Green multi-slow-release biological dispersion glue, preparation method and application

By developing green multiple sustained release biodispersible glue, using polymer functional polymers and natural polymers and other components, the existing polymer frozen glue has solved the problems of high toxicity and environmental hazards in oil fields, and achieved high efficiency Blocking and deep migration meet the development needs of medium and high permeability conglomerate reservoirs.

CN119039727AActive Publication Date: 2024-11-29PETROCHINA CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202310616668.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

During the application process, the existing polymer frozen glue has defects such as high toxicity, high environmental hazards, easy volatility and inconvenient transportation. It cannot effectively seal the flow channel, and the glue formation time is short and the long-term stability is poor, which cannot meet the needs of the medium and low oil fields. Requirements for the development of seepage layers.

Method used

Develop a green multiple sustained release biodispersant glue, which adopts polymer functional polymers, natural polymers, biocrosslinking agents and other components, and forms multiple crosslinking delays and green environmental protection through preferred ratio and polymerization reaction. The colloid has good properties and viscoelasticity, and the glue formation time is adjustable and is used for sealing different reservoirs.

Benefits of technology

It has achieved efficient sealing rate (sealing rate above 99%), strong deep migration capacity, no harm to different reservoirs, meets the needs of medium and high permeability sand and conglomerate reservoirs, and has controllable glue formation time and high viscosity, which improves Recovery and well stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004254068230000101
    Figure BDA0004254068230000101
  • Figure BDA0004254068230000111
    Figure BDA0004254068230000111
Patent Text Reader

Abstract

The invention belongs to the technical field of oilfield chemistry, and particularly relates to green multiple slow-release biological dispersion glue, a preparation method and application. The composition comprises the following components in percentage by mass: 0.2%-1% of a high-molecular functional polymer; 0.3%-1% of a natural high-molecular polymer; 0.5%-5% of polyethyleneimine; 0.1%-1% of a biological cross-linking agent; 0.1%-0.5% of an inorganic cross-linking agent; 0.02%-0.2% of a selective retardant; 0.02 to 0.6 percent of a biological solid enhancer; 0.03%-0.12% of a heat stabilizer; 0.05-0.5% of an antioxidant bacteriostatic agent and the balance of water. All the components are mixed to obtain the green multiple slow-release biological dispersion adhesive which is temperature-resistant, salt-resistant, formaldehyde-free, chromium-free, low in toxicity and environment-friendly. The green multiple slow-release biological dispersion glue has no damage to matrixes of different reservoirs, and can meet the plugging requirements of different channels such as fracture channels, dominant channels and secondary channels of medium-high permeability glutenite reservoirs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oilfield chemistry, and in particular relates to a green multiple sustained-release biodispersible gel, a preparation method and an application thereof. Background Art

[0002] At present, due to the strong heterogeneity of the oil reservoir, long-term water drive development, strong injection and strong production and other reasons, the injected water forms multi-directional crossflow at different levels in the formation, and the low permeability reservoir cannot be effectively utilized, resulting in a significant decrease in the actual single well oil production. Therefore, how to develop and manufacture green and environmentally friendly gel plugging agents to plug different types of crossflow channels and improve the sweep efficiency of low permeability layers has become one of the key research directions for significantly improving the recovery rate.

[0003] Water plugging and profile control technology is an important means to improve the effect of water injection and tertiary oil recovery, and to achieve water control, oil stabilization and increased recovery. Water plugging and profile control technology mainly includes mechanical water plugging and chemical water plugging. Among them, chemical water plugging has become the main stable production measure for water plugging and profile control in oil fields at home and abroad. Polymer gel is composed of high molecular polymers, cross-linking agents and additives. It is the most widely used and economically effective method in chemical water plugging. As far as the cross-linking system of existing polymer gel is concerned, it is mainly divided into inorganic metal cross-linking agents and organic cross-linking agents. Among them, inorganic metal cross-linking agents are mainly high-valent metal ions (Cr 6+ 、Zr 4 + ) is the most widely used, but has defects such as short gelation time, poor temperature resistance, serious environmental pollution and high toxicity; organic crosslinking agents are mainly liquid formaldehyde, phenolic resin prepolymers and other liquid aldehyde derivatives. Due to the high volatility, irritation, toxicity and environmental pollution of liquid phenols and aldehydes, large-scale water plugging applications are greatly restricted. Therefore, the selection of low-toxic, aldehyde-free and chromium-free environmentally friendly green crosslinking agents has become the core goal of oil and water well water plugging in the future.

[0004] Chinese invention patent application CN111892918A discloses a gel-type water plugging and profile control agent and its preparation method, wherein the profile control agent is composed of agent A and agent B; agent A includes the following components in mass percentage: trivalent chromium salt 16%-23%, complexing agent 10%-15%, antioxidant 1%-4%, emulsifier 1%-4%, pH adjuster 4%-8%, retarder 0.5%-1.5%, and the balance is water; agent B includes the following components in mass percentage: polyacrylamide 0.3%-0.5%, and the balance is water. There is trivalent chromium salt in it, which is highly toxic and environmentally harmful.

[0005] Chinese invention patent application CN101531890A discloses a method for preparing a profile control agent using phenolic resin, organic chromium, glacial acetic acid, resorcinol and polyacrylamide as raw materials. By adding different crosslinking agents, the gelling time of the profile control agent can be controlled during use, and the gelling time is 8-48 hours; the gelling strength is high, it is not easy to break the gel, and the effective period is 1-2 years. However, due to the Cr in the organic chromium crosslinking agent, 3+ ,Cr 6+ They transform into each other during the gelation process and are identified as heavy metal pollutants in the new environmental protection law. They seriously pollute groundwater and deep soil and are greatly affected by environmental restrictions.

[0006] Chinese invention patent application CN114517082A discloses a heat-resistant and salt-resistant black liquor phenolic gel profile control agent and a preparation method thereof, which relates to the technical field of oil and gas field profile control agents. The gel profile control agent comprises: alkaline cotton pulp black liquor, phenol, formaldehyde and polyacrylamide, wherein the mass ratio of alkaline cotton pulp black liquor to phenol is 2:1-1:1; the molar ratio of phenol to formaldehyde is 3.5-4:1; the mass ratio of alkaline cotton pulp black liquor to polyacrylamide is 10-15:1; during preparation, alkaline cotton pulp black liquor and formaldehyde are alternately added to molten phenol in sequence to obtain resin, which is then reacted with polyacrylamide solution to form gel. Since the phenol and formaldehyde used are highly irritating and toxic, and the liquid is volatile, transportation is difficult.

[0007] Due to the various types of inorganic crosslinking agents (Cr 3+ The crosslinking agents mainly (organic chromium, phenolic aldehyde, formaldehyde) and organic crosslinking agents (organic chromium, phenolic aldehyde, formaldehyde) have defects such as high toxicity, high environmental hazards, easy volatility and inconvenient transportation during application. The polymer gel crosslinked with the polymer has a short gelling time, poor long-term stability, serious reservoir pollution and weak colloidal strength, and cannot achieve the purpose of blocking the cross-flow channel. Therefore, it is urgent to develop a biodispersible gel that is formaldehyde-free and chromium-free, has good multiple delayed crosslinking effects, is stable in nature, non-toxic and environmentally friendly. Summary of the invention

[0008] In order to solve the above-mentioned technical problems, the present invention provides a green multiple slow-release biodispersible gel and a preparation method thereof. The green multiple slow-release biodispersible gel has the advantages of good multiple cross-linking delay, good green environmental protection, good viscoelasticity (>150Pa), good biodegradability, strong deep migration and plugging ability (plugging rate of more than 99%) and adjustable gelling time (2h-8h). It has no damage to the matrix of different reservoirs and can meet the plugging needs of different channels such as fracture channels, dominant channels and secondary channels in medium and high permeability conglomerate oil reservoirs.

[0009] In order to achieve the above-mentioned purpose of the present invention, the specific technical solution adopted by the present invention is:

[0010] The present invention provides a green multiple sustained-release biodispersible gel, which comprises the following components by mass percentage:

[0011] High molecular functional polymer, 0.2%-1%; natural high molecular polymer, 0.3%-1%; polyethyleneimine, 0.5%-5%; biological cross-linking agent, 0.1%-1%; inorganic cross-linking agent, 0.1%-0.5%; selective retarder, 0.02%-0.2%; biological stiffener, 0.02-0.6%; thermal stabilizer, 0.03%-0.12%; antioxidant and antibacterial agent, 0.05-0.5%; water, the balance.

[0012] Preferably, the high molecular weight functional polymer comprises 30%-50% sodium caseinate, 10%-20% hydrophobic associating polymer and 30%-60% sodium polyacrylate, by mass percentage.

[0013] Further preferably, the viscosity-average molecular weights of the sodium caseinate, the hydrophobically associating polymer and the sodium polyacrylate are 80,000-350,000, 15,000-30,000,000 and 5,000-15,000,000 respectively.

[0014] Further preferably, the monomers in the hydrophobically associating polymer are selected from one or more of N-dodecyl acrylamide, N-hexadecyl acrylamide, N-phenylethyl acrylamide, and behenyl allyl dibromide tetramethylethylenediamine.

[0015] Preferably, the raw materials of the natural high molecular polymer include 30%-40% carboxymethyl xylan, 20%-30% konjac glucomannan and 30%-50% carboxymethyl fennel gum in terms of mass percentage.

[0016] Further preferably, the viscosity-average molecular weights of the carboxymethyl xylan, konjac glucomannan and carboxymethyl fennel gum are 15-20 million, 10-30 million and 15-20 million respectively.

[0017] Preferably, the viscosity average molecular weight of the polyethyleneimine is 3-5 million.

[0018] Preferably, the biocrosslinking agent comprises 20%-30% potassium humate, 30%-40% sodium hyaluronate and 30%-50% sodium alginate by mass percentage.

[0019] More preferably, the number average molecular weights of the sodium hyaluronate and sodium alginate are 500,000-700,000 Daltons and 32,000-250,000 Daltons, respectively.

[0020] Preferably, the inorganic cross-linking agent comprises, by mass percentage, 30%-50% sodium alginate, 10%-20% potassium pentaborate and 30%-60% disodium edetate.

[0021] More preferably, the viscosity average molecular weight of the sodium alginate is 50,000-70,000.

[0022] Preferably, the selective retarder comprises 20%-40% sodium carbamate, 10%-30% potassium sorbate and 30%-70% sodium glycinate by mass percentage.

[0023] Preferably, the bio-stiffener comprises, by mass percentage, 10%-30% of elm bark powder, 30%-50% of sesbania powder and 20%-60% of bay leaf powder.

[0024] Preferably, the heat stabilizer comprises, by mass percentage, 30%-50% of 2-methylimidazolyl-1-ethyl urea, 20%-30% of sodium starch octenylsuccinate, and 20%-50% of potassium metaborate.

[0025] Preferably, the antioxidant and antibacterial agent comprises, by mass percentage, 20%-40% sodium dichloroisocyanurate, 20%-30% sodium perborate and 30%-60% potassium ferrate.

[0026] The present invention also relates to a method for preparing the green multiple sustained-release biodispersible gel, comprising the following steps:

[0027] (1) mixing high molecular weight functional polymer powder and natural high molecular weight polymer powder and dissolving them in water to obtain a polymer base liquid;

[0028] (2) adding polyethyleneimine, a biocrosslinking agent, and an inorganic crosslinking agent to a polymer base liquid respectively, and stirring to obtain a polymer crosslinking solution;

[0029] (3) dissolving the selective retarder, the heat stabilizer, and the antioxidant and antibacterial agent in water to obtain a uniform and stable dispersion;

[0030] (4) The polymerization cross-linking solution and the dispersion are mixed, and a bio-strengthening agent is added to obtain a green multiple sustained-release bio-dispersible gel after a polymerization reaction.

[0031] Preferably, the stirring speed in step (4) is 700-900 r / min, the stirring time is 20-30 min, and the reaction temperature is 30-120°C.

[0032] The present invention also relates to the application of the green multiple slow-release biological dispersible gel or the dispersible gel prepared by the preparation method of the dispersible gel in the technical field of oil field profile control and water plugging.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The present invention obtains a green multiple sustained-release biodispersible glue that is temperature-resistant and salt-resistant, formaldehyde-free and chromium-free, low-toxic and environmentally friendly by selecting multiple low-toxic functional components and optimizing the ratio;

[0035] (2) The high molecular weight functional polymer and the natural high molecular weight polymer in the present invention are used together to produce a synergistic effect, which can effectively improve the plugging rate; the use of the bio-crosslinking agent significantly increases the viscosity of the dispersed gel;

[0036] (3) The green multiple slow-release biodispersible gel has the advantages of good multiple cross-linking delay, good green environmental protection, good viscoelasticity (>150Pa), good biodegradability, strong deep migration and plugging ability (plugging rate of more than 99%), and adjustable gelling time (2h-8h). It has no damage to the matrix of different reservoirs and can meet the plugging needs of different channels such as fracture channels, dominant channels and secondary channels in medium and high permeability conglomerate reservoirs. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are further clearly described. The described embodiments are only a part of the present invention and are used to explain the present invention but not to limit the present invention. Therefore, other embodiments obtained by other technicians in the field without creative work all belong to the protection scope of the present invention.

[0038] Sodium caseinate, hydrophobically associating polymer, and sodium polyacrylate were purchased from Aisen (Rudong) Chemical Co., Ltd.;

[0039] Polyethyleneimine was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0040] Carboxymethyl xylan, konjac glucomannan, and carboxymethyl fennel gum were purchased from Beijing Hengju Chemical Group Co., Ltd.;

[0041] Sodium hyaluronate, sodium alginate, and sodium alginate were purchased from Sichuan Weiqi Biotechnology Co., Ltd.;

[0042] Elm bark powder (FDBL) and geranium leaf powder (FDFG) were purchased from Xi'an Feida Biotechnology Co., Ltd.;

[0043] Sesbania sesbania powder was purchased from Nanjing Ximenuo Biotechnology Co., Ltd.

[0044] The reagents not particularly described in the following examples are all conventional reagents in the art and are commercially available.

[0045] Example 1

[0046] A green multiple sustained-release biodispersible gel, the components of which are, by mass percentage, 1% high molecular weight functional polymer; 1% natural high molecular weight polymer; 2% polyethyleneimine; 1% biological cross-linking agent; 0.5% inorganic cross-linking agent; 0.2% selective retarder; 0.6% biological stiffener; 0.12% thermal stabilizer; 0.5% antioxidant and antibacterial agent; and 93.08% water.

[0047] The high molecular weight functional polymer is a mixture of 30% sodium caseinate (viscosity average molecular weight is 350,000), 10% hydrophobic associating polymer (viscosity average molecular weight is 30 million, the monomer is N-hexadecyl acrylamide) and 60% sodium polyacrylate (viscosity average molecular weight is 15 million) by mass percentage;

[0048] The natural high molecular polymer is a mixture of 30% carboxymethyl xylan (viscosity average molecular weight is 20 million), 20% konjac glucomannan (viscosity average molecular weight is 30 million) and 50% carboxymethyl fennel gum (viscosity average molecular weight is 20 million);

[0049] Polyethyleneimine, viscosity average molecular weight is 5 million;

[0050] The biocrosslinking agent is a mixture of 20% potassium humate, 30% sodium hyaluronate (number average molecular weight of 700,000 Daltons) and 50% sodium alginate (number average molecular weight of 250,000 Daltons);

[0051] The inorganic cross-linking agent is a mixture of 30% sodium alginate (viscosity average molecular weight is 70,000), 10% potassium pentaborate and 60% disodium edetate;

[0052] The selective retarder is a mixture of 20% sodium carbamate, 10% potassium sorbate and 70% sodium glycinate;

[0053] The bioreinforcement agent is a mixture of 10% elm bark powder, 30% sesbania powder and 60% bay leaf powder;

[0054] The heat stabilizer is a mixture of 30% 2-methylimidazolyl-1-ethylurea, 20% sodium starch octenylsuccinate and 50% potassium metaborate;

[0055] The antioxidant and antibacterial agent is a mixture of 20% sodium dichloroisocyanurate, 20% sodium perborate and 60% potassium ferrate.

[0056] The preparation method of the green multiple sustained-release biodispersible gel is as follows:

[0057] (1) mixing high molecular weight functional polymer powder and natural high molecular weight polymer powder and dissolving them in water to obtain a polymer base liquid;

[0058] (2) adding polyethyleneimine, a biocrosslinking agent, and an inorganic crosslinking agent to the above solution respectively, and stirring evenly to obtain a polymerized crosslinking solution;

[0059] (3) dissolving the selective retarder, the heat stabilizer, and the antioxidant and antibacterial agent in water to obtain a uniform and stable dispersion;

[0060] (4) The polymerization cross-linking solution and the dispersion were mixed at 80° C., the bio-strengthening agent was added, and the polymerization reaction was carried out by stirring at 800 r / min. After 30 minutes, a green multiple sustained-release bio-dispersible gel was obtained.

[0061] Example 2

[0062] A green multiple sustained-release biodispersible gel, the components of which are, by mass percentage, 1% high molecular weight functional polymer; 0.8% natural high molecular weight polymer; 1% polyethyleneimine; 0.8% biological cross-linking agent; 0.4% inorganic cross-linking agent; 0.15% selective retarder; 0.4% biological reinforcing agent; 0.08% thermal stabilizer; 0.3% antioxidant and antibacterial agent; and 95.07% water.

[0063] The high molecular weight functional polymer is a mixture of 40% sodium caseinate (viscosity average molecular weight is 250,000), 15% hydrophobic associating polymer (viscosity average molecular weight is 20 million, the monomer is N-phenylethyl acrylamide) and 45% sodium polyacrylate (viscosity average molecular weight is 10 million) by mass percentage;

[0064] The natural high molecular polymer is a mixture of 35% carboxymethyl xylan (viscosity average molecular weight is 18 million), 25% konjac glucomannan (viscosity average molecular weight is 15 million) and 40% carboxymethyl fennel gum (viscosity average molecular weight is 18 million);

[0065] Polyethyleneimine, viscosity average molecular weight is 4 million;

[0066] The biocrosslinking agent is a mixture of 25% potassium humate, 35% sodium hyaluronate (number average molecular weight of 600,000 Daltons) and 40% sodium alginate (number average molecular weight of 200,000 Daltons);

[0067] The inorganic cross-linking agent is a mixture of 40% sodium alginate (viscosity average molecular weight is 60,000), 15% potassium pentaborate and 45% disodium edetate;

[0068] The selective retarder is a mixture of 30% sodium carbamate, 20% potassium sorbate and 50% sodium glycinate;

[0069] The bioreinforcement agent is a mixture of 20% elm bark powder, 40% sesbania powder and 40% bay leaf powder;

[0070] The heat stabilizer is a mixture of 40% 2-methylimidazolyl-1-ethylurea, 25% sodium starch octenylsuccinate and 35% potassium metaborate;

[0071] The antioxidant and antibacterial agent is a mixture of 30% sodium dichloroisocyanurate, 35% sodium perborate and 45% potassium ferrate.

[0072] The reaction conditions in step (4) of this embodiment are: stirring speed of 900 r / min, stirring time of 20 min, reaction temperature of 120° C., and other preparation steps are the same as those in Example 1.

[0073] Example 3

[0074] A green multiple sustained-release biodispersible gel, the components of which are, by mass percentage, 0.5% of high molecular weight functional polymer, 0.5% of natural high molecular weight polymer, 1% of polyethyleneimine, 0.4% of biological cross-linking agent, 0.3% of inorganic cross-linking agent, 0.08% of selective retarder, 0.2% of biological reinforcing agent, 0.04% of thermal stabilizer, 0.1% of antioxidant and antibacterial agent, and 96.88% of water.

[0075] The high molecular weight functional polymer is a mixture of 50% sodium caseinate (viscosity average molecular weight of 80,000), 20% hydrophobic associating polymer (viscosity average molecular weight of 15 million, monomer is N-dodecyl acrylamide) and 30% sodium polyacrylate (viscosity average molecular weight of 5 million) by mass percentage;

[0076] The natural high molecular polymer is a mixture of 40% carboxymethyl xylan (viscosity average molecular weight is 15 million), 30% konjac glucomannan (viscosity average molecular weight is 10 million) and 30% carboxymethyl guar gum (viscosity average molecular weight is 15 million);

[0077] Polyethyleneimine, viscosity average molecular weight is 3 million;

[0078] The biocrosslinking agent is a mixture of 30% potassium humate, 40% sodium hyaluronate (number average molecular weight of 500,000 Daltons) and 30% sodium alginate (number average molecular weight of 150,000 Daltons);

[0079] The inorganic cross-linking agent is a mixture of 50% sodium alginate (viscosity average molecular weight is 50,000), 20% potassium pentaborate and 30% disodium edetate;

[0080] The selective retarder is a mixture of 40% sodium carbamate, 30% potassium sorbate and 30% sodium glycinate;

[0081] The bioreinforcement agent is a mixture of 30% elm bark powder, 50% sesbania powder and 20% bay leaf powder;

[0082] The heat stabilizer is a mixture of 50% 2-methylimidazolyl-1-ethylurea, 30% sodium starch octenylsuccinate and 20% potassium metaborate;

[0083] The antioxidant and antibacterial agent is a mixture of 40% sodium dichloroisocyanurate, 30% sodium perborate and 30% potassium ferrate.

[0084] The reaction conditions in step (4) of this embodiment are: stirring speed of 700 r / min, stirring time of 30 min, reaction temperature of 60° C., and other preparation steps are the same as those in Example 1.

[0085] Example 4

[0086] A green multiple sustained-release biodispersible gel, the components of which are, by mass percentage, 0.6% of high molecular weight functional polymer, 0.5% of natural high molecular weight polymer, 2.5% of polyethyleneimine, 0.5% of biological cross-linking agent, 0.25% of inorganic cross-linking agent, 0.12% of selective retarder, 0.3% of biological reinforcing agent, 0.07% of thermal stabilizer, 0.3% of antioxidant and antibacterial agent, and 94.86% of water.

[0087] The high molecular weight functional polymer is a mixture of 30% sodium caseinate (viscosity average molecular weight is 80,000), 10% hydrophobic associating polymer (viscosity average molecular weight is 15 million, the monomer is dicosyl allyl dibromide tetramethylethylenediamine) and 60% sodium polyacrylate (viscosity average molecular weight is 5 million) by mass percentage;

[0088] The natural high molecular polymer is a mixture of 30% carboxymethyl xylan (viscosity average molecular weight is 15 million), 20% konjac glucomannan (viscosity average molecular weight is 10 million) and 50% carboxymethyl guar gum (viscosity average molecular weight is 15 million);

[0089] Polyethyleneimine, viscosity average molecular weight is 4 million;

[0090] The biocrosslinking agent is a mixture of 20% potassium humate, 30% sodium hyaluronate (number average molecular weight of 500,000 Daltons) and 50% sodium alginate (number average molecular weight of 100,000 Daltons);

[0091] The inorganic cross-linking agent is a mixture of 30% sodium alginate (viscosity average molecular weight is 50,000), 10% potassium pentaborate and 60% disodium edetate;

[0092] The selective retarder is a mixture of 20% sodium carbamate, 10% potassium sorbate and 70% sodium glycinate;

[0093] The bioreinforcement agent is a mixture of 10% elm bark powder, 30% sesbania powder and 60% bay leaf powder;

[0094] The heat stabilizer is a mixture of 30% 2-methylimidazolyl-1-ethylurea, 20% sodium starch octenylsuccinate and 50% potassium metaborate;

[0095] The antioxidant and antibacterial agent is a mixture of 20% sodium dichloroisocyanurate, 20% sodium perborate and 60% potassium ferrate.

[0096] The reaction conditions in step (4) of this embodiment are: stirring speed of 900 r / min, stirring time of 30 min, reaction temperature of 30° C., and other preparation steps are the same as those in Example 1.

[0097] Example 5

[0098] A green multiple sustained-release biodispersible gel, the components of which are, by mass percentage, 0.5% of high molecular weight functional polymer, 0.5% of natural high molecular weight polymer, 1% of polyethyleneimine, 0.4% of biological cross-linking agent, 0.3% of inorganic cross-linking agent, 0.08% of selective retarder, 0.2% of biological reinforcing agent, 0.04% of thermal stabilizer, 0.1% of antioxidant and antibacterial agent, and 96.88% of water.

[0099] The high molecular weight functional polymer is a mixture of 40% sodium caseinate (viscosity average molecular weight is 300,000), 15% hydrophobic associating polymer (viscosity average molecular weight is 15 million, the monomer is N-phenylethyl acrylamide) and 45% sodium polyacrylate (viscosity average molecular weight is 5 million) by mass percentage;

[0100] The natural high molecular polymer is a mixture of 35% carboxymethyl xylan (viscosity average molecular weight is 15 million), 25% konjac glucomannan (viscosity average molecular weight is 10 million) and 40% carboxymethyl guar gum (viscosity average molecular weight is 15 million);

[0101] Polyethyleneimine, viscosity average molecular weight is 3.5 million;

[0102] The biocrosslinking agent is a mixture of 25% potassium humate, 35% sodium hyaluronate (number average molecular weight of 600,000 Daltons) and 40% sodium alginate (number average molecular weight of 32,000 Daltons);

[0103] The inorganic cross-linking agent is a mixture of 40% sodium alginate (viscosity average molecular weight is 50,000), 15% potassium pentaborate and 45% disodium edetate;

[0104] The selective retarder is a mixture of 30% sodium carbamate, 20% potassium sorbate and 50% sodium glycinate;

[0105] The bioreinforcement agent is a mixture of 20% elm bark powder, 40% sesbania powder and 40% bay leaf powder;

[0106] The heat stabilizer is a mixture of 40% 2-methylimidazolyl-1-ethylurea, 25% sodium starch octenylsuccinate and 35% potassium metaborate;

[0107] The preparation process of the green multiple sustained-release biodispersible gel in this example is the same as that in Example 1.

[0108] Comparative Example 1

[0109] A green multiple sustained-release biodispersible gel, the components of which are, by mass percentage, 2% natural high molecular polymer; 2% polyethyleneimine; 1% biocrosslinking agent; 0.5% inorganic crosslinking agent; 0.2% selective retarder; 0.6% bioreinforcement agent; 0.12% thermal stabilizer; 0.5% antioxidant and antibacterial agent; and 93.08% water.

[0110] The natural high molecular polymer is a mixture of 30% carboxymethyl xylan (viscosity average molecular weight is 20 million), 20% konjac glucomannan (viscosity average molecular weight is 30 million) and 50% carboxymethyl fennel gum (viscosity average molecular weight is 20 million) by mass percentage;

[0111] Polyethyleneimine, viscosity average molecular weight is 5 million;

[0112] The biocrosslinking agent is a mixture of 20% potassium humate, 30% sodium hyaluronate (number average molecular weight of 700,000 Daltons) and 50% sodium alginate (number average molecular weight of 250,000 Daltons);

[0113] The inorganic cross-linking agent is a mixture of 30% sodium alginate (viscosity average molecular weight is 70,000), 10% potassium pentaborate and 60% disodium edetate;

[0114] The selective retarder is a mixture of 20% sodium carbamate, 10% potassium sorbate and 70% sodium glycinate;

[0115] The bioreinforcement agent is a mixture of 10% elm bark powder, 30% sesbania powder and 60% bay leaf powder;

[0116] The heat stabilizer is a mixture of 30% 2-methylimidazolyl-1-ethylurea, 20% sodium starch octenylsuccinate and 50% potassium metaborate;

[0117] The antioxidant and antibacterial agent is a mixture of 20% sodium dichloroisocyanurate, 20% sodium perborate and 60% potassium ferrate.

[0118] The preparation method of the green multiple sustained-release biodispersible gel is as follows:

[0119] (1) dissolving natural high molecular polymer powder in water, then adding polyethyleneimine, a biocrosslinking agent, and an inorganic crosslinking agent, and stirring evenly to obtain a polymer crosslinking solution;

[0120] (2) dissolving the selective retarder, the heat stabilizer, and the antioxidant and antibacterial agent in water to obtain a uniform and stable dispersion;

[0121] (3) The polymerization cross-linking solution and the dispersion were mixed at 80° C., the bio-strengthening agent was added, and the polymerization reaction was carried out by stirring at 800 r / min. After 30 minutes, a green multiple sustained-release bio-dispersible gel was obtained.

[0122] Comparative Example 2

[0123] A green multiple sustained-release biodispersible gel, the components of which are, by mass percentage, 2% high molecular functional polymer; 2% polyethyleneimine; 1% biological cross-linking agent; 0.5% inorganic cross-linking agent; 0.2% selective retarder; 0.6% biological reinforcing agent; 0.12% thermal stabilizer; 0.5% antioxidant and antibacterial agent; and 93.08% water.

[0124] The high molecular weight functional polymer is a mixture of 30% sodium caseinate (viscosity average molecular weight is 350,000), 10% hydrophobic associating polymer (viscosity average molecular weight is 30 million, the monomer is N-hexadecyl acrylamide) and 60% sodium polyacrylate (viscosity average molecular weight is 15 million) by mass percentage;

[0125] Polyethyleneimine, viscosity average molecular weight is 5 million;

[0126] The biocrosslinking agent is a mixture of 20% potassium humate, 30% sodium hyaluronate (number average molecular weight of 700,000 Daltons) and 50% sodium alginate (number average molecular weight of 250,000 Daltons);

[0127] The inorganic cross-linking agent is a mixture of 30% sodium alginate (viscosity average molecular weight is 70,000), 10% potassium pentaborate and 60% disodium edetate;

[0128] The selective retarder is a mixture of 20% sodium carbamate, 10% potassium sorbate and 70% sodium glycinate;

[0129] The bioreinforcement agent is a mixture of 10% elm bark powder, 30% sesbania powder and 60% bay leaf powder;

[0130] The heat stabilizer is a mixture of 30% 2-methylimidazolyl-1-ethylurea, 20% sodium starch octenylsuccinate and 50% potassium metaborate;

[0131] The antioxidant and antibacterial agent is a mixture of 20% sodium dichloroisocyanurate, 20% sodium perborate and 60% potassium ferrate.

[0132] The preparation method of the green multiple sustained-release biodispersible gel is as follows:

[0133] (1) dissolving a high molecular weight functional polymer powder in water, then adding polyethyleneimine, a biocrosslinking agent, and an inorganic crosslinking agent, and stirring evenly to obtain a polymer crosslinking solution;

[0134] (2) dissolving the selective retarder, the heat stabilizer, and the antioxidant and antibacterial agent in water to obtain a uniform and stable dispersion;

[0135] (3) The polymerization cross-linking solution and the dispersion were mixed at 80° C., the bio-strengthening agent was added, and the polymerization reaction was carried out by stirring at 800 r / min. After 30 minutes, a green multiple sustained-release bio-dispersible gel was obtained.

[0136] Comparative Example 3

[0137] A green multiple sustained-release biodispersible gel, the components of which are, by mass percentage, 1% high molecular weight functional polymer; 1% natural high molecular weight polymer; 2% polyethyleneimine; 1.5% inorganic crosslinking agent; 0.2% selective retarder; 0.6% bioreinforcement agent; 0.12% thermal stabilizer; 0.5% antioxidant and antibacterial agent; and 93.08% water.

[0138] The high molecular weight functional polymer is a mixture of 30% sodium caseinate (viscosity average molecular weight is 350,000), 10% hydrophobic associating polymer (viscosity average molecular weight is 30 million, the monomer is N-hexadecyl acrylamide) and 60% sodium polyacrylate (viscosity average molecular weight is 15 million) by mass percentage;

[0139] The natural high molecular polymer is a mixture of 30% carboxymethyl xylan (viscosity average molecular weight is 20 million), 20% konjac glucomannan (viscosity average molecular weight is 30 million) and 50% carboxymethyl fennel gum (viscosity average molecular weight is 20 million);

[0140] Polyethyleneimine, viscosity average molecular weight is 5 million;

[0141] The inorganic cross-linking agent is a mixture of 30% sodium alginate (viscosity average molecular weight is 70,000), 10% potassium pentaborate and 60% disodium edetate;

[0142] The selective retarder is a mixture of 20% sodium carbamate, 10% potassium sorbate and 70% sodium glycinate;

[0143] The bioreinforcement agent is a mixture of 10% elm bark powder, 30% sesbania powder and 60% bay leaf powder;

[0144] The heat stabilizer is a mixture of 30% 2-methylimidazolyl-1-ethylurea, 20% sodium starch octenylsuccinate and 50% potassium metaborate;

[0145] The antioxidant and antibacterial agent is a mixture of 20% sodium dichloroisocyanurate, 20% sodium perborate and 60% potassium ferrate.

[0146] The preparation method of the green multiple sustained-release biodispersible gel is as follows:

[0147] (1) mixing high molecular weight functional polymer powder and natural high molecular weight polymer powder and dissolving them in water to obtain a polymer base liquid;

[0148] (2) adding polyethyleneimine and an inorganic crosslinking agent to the above solution respectively, stirring evenly to obtain a polymerized crosslinking solution;

[0149] (3) dissolving the selective retarder, the heat stabilizer, and the antioxidant and antibacterial agent in water to obtain a uniform and stable dispersion;

[0150] (4) The polymerization cross-linking solution and the dispersion were mixed at 80° C., the bio-strengthening agent was added, and the polymerization reaction was carried out by stirring at 800 r / min. After 30 minutes, a green multiple sustained-release bio-dispersible gel was obtained.

[0151] Effect evaluation

[0152] The dispersions prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention were tested.

[0153] The parameters such as gelling time and viscosity were measured according to the standard "SY / T 5590-2004 Performance Evaluation Method of Profile Control Agents"; the viscoelasticity of the dispersed gel was measured according to the standard "SY / T 6296-1997 Determination of the strength of polymer gel for oil production. Rheological parameter method", and the plugging rate was calculated by core displacement experiment. The test results are shown in Table 1.

[0154] Table 1 Test results of green multiple sustained-release biodispersible gel properties of examples and comparative examples

[0155]

[0156]

[0157] It can be seen from the data in Table 1 that the green multiple sustained-release biodispersible gel of the embodiment of the present invention has the advantages of good multiple cross-linking delay, good green environmental protection, good viscoelasticity (>150Pa), good biodegradability, strong deep migration plugging (plugging rate of more than 99%), adjustable gelling time (2h-8h), etc., has no damage to the matrix of different reservoirs, and can meet the plugging needs of different channels such as fracture channels, dominant channels and secondary channels in medium and high permeability conglomerate reservoirs.

[0158] A green multiple sustained-release biodispersible gel developed by the present invention is mainly composed of high molecular polymers. By adding a preferred cross-linking agent, a high-viscosity dispersible gel system is formed. The viscosity is increased by 10 times compared with the conventional sludge suspension system, and the core plugging rate is increased by 30%. It can effectively carry sludge into the deep formation to form plugging for medium and high permeability channels. At present, the profile adjustment system has been applied in the Che 510 well area of ​​the first oil production plant. From October to December 2022, a total of 4 wells have been implemented. So far, the effect of increasing oil and reducing water content has begun to show, and the absolute increase in oil production has been verified to be 270 tons, and the maximum water content has been reduced by 7 percentage points.

[0159] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.

Claims

1. A green multiple sustained-release biodispersible gel, characterized in that: In terms of mass percentage, the components of the green multiple sustained-release dispersible gel include: high molecular functional polymer, 0.2%-1%; Natural polymers, 0.3%-1%; Polyethyleneimine, 0.5%-5%; Biocrosslinker, 0.1%-1%; Inorganic crosslinking agent, 0.1%-0.5%; Selective retarder, 0.02%-0.2%; Bio-strengthening agent, 0.02-0.6%; Heat stabilizer, 0.03%-0.12%; Antioxidant and antibacterial agent, 0.05-0.5%; Water, balance.

2. The dispersion according to claim 1, characterized in that: Calculated by mass percentage, the raw materials of the high molecular functional polymer include 30%-50% sodium caseinate, 10%-20% hydrophobic associating polymer and 30%-60% sodium polyacrylate.

3. The dispersion according to claim 2, characterized in that: The viscosity average molecular weights of the sodium caseinate, the hydrophobic associating polymer and the sodium polyacrylate are 80,000-350,000, 15,000-30,000,000 and 5,000-15,000,000 respectively.

4. The dispersion according to claim 2, characterized in that: The monomers in the hydrophobically associating polymer are selected from one or more of N-dodecyl acrylamide, N-hexadecyl acrylamide, N-phenylethyl acrylamide, and behenyl allyl dibromide tetramethylethylenediamine.

5. The dispersion according to claim 1, characterized in that: Calculated by mass percentage, the raw materials of the natural high molecular polymer include 30%-40% of carboxymethyl xylan, 20%-30% of konjac glucomannan and 30%-50% of carboxymethyl fennel gum.

6. The dispersion according to claim 5, characterized in that: The viscosity average molecular weights of the carboxymethyl xylan, konjac glucomannan and carboxymethyl fennel gum are 15-20 million, 10-30 million and 15-20 million respectively.

7. The dispersion according to claim 1, characterized in that: The viscosity average molecular weight of the polyethyleneimine is 3-5 million.

8. The dispersion according to claim 1, characterized in that: Calculated by mass percentage, the raw materials of the biological cross-linking agent include 20%-30% potassium humate, 30%-40% sodium hyaluronate and 30%-50% sodium alginate.

9. The dispersion according to claim 8, characterized in that: The number average molecular weights of the sodium hyaluronate and sodium alginate are 500,000-700,000 Daltons and 32,000-250,000 Daltons respectively.

10. The dispersion according to claim 1, characterized in that: Calculated by mass percentage, the raw materials of the inorganic cross-linking agent include 30%-50% sodium alginate, 10%-20% potassium pentaborate and 30%-60% disodium edetate.

11. The dispersion according to claim 10, characterized in that: The viscosity average molecular weight of the sodium alginate is 50,000-70,000.

12. The dispersible rubber according to any one of claims 1 to 11, characterized in that: Calculated by mass percentage, the raw materials of the selective retarder include 20%-40% sodium carbamate, 10%-30% potassium sorbate and 30%-70% sodium glycinate.

13. The dispersion according to claim 1, characterized in that: Calculated by mass percentage, the raw materials of the biological reinforcing agent include 10%-30% of elm bark powder, 30%-50% of sesbania powder and 20%-60% of bay leaf powder.

14. The dispersion according to claim 1, characterized in that: Calculated by mass percentage, the raw materials of the heat stabilizer include 30%-50% of 2-methylimidazolyl-1-ethylurea, 20%-30% of sodium octenyl succinate starch and 20%-50% of potassium metaborate.

15. The dispersion according to claim 1, characterized in that: Calculated by mass percentage, the raw materials of the antioxidant and antibacterial agent include 20%-40% of sodium dichloroisocyanurate, 20%-30% of sodium perborate and 30%-60% of potassium ferrate.

16. A method for preparing the green multiple sustained-release biodispersible gel according to any one of claims 1 to 15, characterized in that: The following steps are involved: (1) mixing high molecular weight functional polymer powder and natural high molecular weight polymer powder and dissolving them in water to obtain a polymer base liquid; (2) adding polyethyleneimine, a biocrosslinking agent, and an inorganic crosslinking agent to a polymer base liquid respectively, and stirring to obtain a polymer crosslinking solution; (3) dissolving the selective retarder, the heat stabilizer, and the antioxidant and antibacterial agent in water to obtain a uniform and stable dispersion; (4) The polymerization cross-linking solution and the dispersion are mixed, a bio-strengthening agent is added, and the mixture is stirred to obtain a green multiple sustained-release bio-dispersible gel after a polymerization reaction occurs.

17. The preparation method according to claim 16, characterized in that: The stirring speed in step (4) is 700-900 r / min, the stirring time is 20-30 min, and the reaction temperature is 30-120°C.

18. Use of the dispersoid according to any one of claims 1 to 15 or the dispersoid prepared by the preparation method of the dispersoid according to any one of claims 16 to 17 in the field of oilfield profile control and water plugging technology.

Citation Information

Patent Citations

  • Konjac glucomannan water-base fracturing fluid as well as preparation method and gel breaking method thereof

    CN101735791A

  • Composite dirt blocking remover for oil-water well

    CN101921582A

  • Environment-friendly composite blocking remover composition for oil fields

    CN102399546A

  • Acrylamide graft copolymer oil-displacing agent and preparation method thereof

    CN102876312A

  • Environment-friendly crosslinking and gelling retarding profile control agent and preparation method thereof

    CN102965088A