Water-coal-slurry gasification furnace lining material based on high-chromium castable and preparation method of water-coal-slurry gasification furnace lining material
By using high chromium castable and magnesium-chromium spinel aggregate in the water coal slurry gasifier furnace lining materials, combining hydrated alumina and lightly burned magnesium sand, the existing materials are solved under high temperature, high pressure and chemical erosion environments. The problems of uneven performance and high cost have achieved high pressure resistance, thermal shock resistance and slag resistance.
Patent Information
- Application Number
- CN202411056605.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The existing water-coal slurry gasifier furnace lining materials have problems such as uneven performance, poor thermal shock resistance, and insufficient slag corrosion resistance in high temperature, high pressure and chemical erosion environments, and the production cost is relatively high.
Using materials based on high chromium castables, chemical components include electromelted chromium oxide particles, magnesium chromium spinel particles, chromium oxide fine powder, α-alumina fine powder, lightly burned magnesium sand fine powder and hydrated alumina fine powder , combined with polycarboxylate as water reducer, molding through casting process, avoiding expensive molding equipment and nano-aluminum sol costs, and hydrated alumina and lightly burned magnesium sand to form magnesium-aluminum hydrotalcite phase to improve sintering density and compressive resistance. .
It has achieved a significant improvement in the material's high pressure resistance, low porosity, good chemical stability, excellent thermal shock resistance, slag corrosion resistance and slag permeability, while reducing production costs.
Smart Images

Figure CN119059828A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water-coal slurry gasification furnace lining materials, and in particular relates to a water-coal slurry gasification furnace lining material based on high-chromium castable and a preparation method thereof. Background Art
[0002] my country is a country with abundant coal resources. In terms of resource distribution, it presents a situation of "more coal and less gas". However, directly burning coal resources for power generation will generate a lot of pollution. Gasification technology is a process of producing synthesis gas and chemical raw materials from carbon-containing raw materials (mainly coal and petroleum coke). It is an important way to convert coal cleanly and efficiently. The water-coal slurry gasifier is a container where carbon-containing raw materials, water and oxygen react under a high temperature and strong reducing atmosphere. The operating environment inside the water-coal slurry gasifier is complex, with high temperature, high pressure and a strong reducing atmosphere dominated by H2 and CO. In addition, the furnace wall of the water-coal slurry gasifier must also withstand temperature fluctuations caused by the circulation of high-temperature gas, as well as the scouring and chemical erosion of slag. In order to meet the use requirements of the water-coal slurry gasifier, the stability and longevity of its lining material is an important prerequisite for the efficient operation of the water-coal slurry gasifier.
[0003] Chromium-containing refractories are widely used in water-coal slurry gasifiers because Cr2O3 has good physical and chemical stability, ultra-low solubility in corrosive media, and ultra-high thermochemical stability. At present, the lining material of water-coal slurry gasifiers is mainly phosphate-bonded Cr2O3-Al2O3-ZrO2 bricks. However, phosphates as binders will migrate from the hot surface to the cold surface during service. Aluminum phosphate will be affected by reducing gases on the hot surface, decompose to produce oxygen and phosphorus pentoxide, increase the porosity of the material close to the hot surface, aggravate the penetration of slag, and reduce the service life of the material. In addition, the high-chromium bricks obtained by machine pressing will produce uneven performance due to uneven force on the periphery and center of the bricks, resulting in lower performance on the outside of the bricks than on the inside, making the outer part of the bricks more easily damaged, thereby reducing the service life of the material. Therefore, the development of high-chromium refractories for water-coal slurry gasifiers with excellent performance has attracted the attention of technicians in this field.
[0004] The patented technology of "Chrome-zirconium bricks for water-coal slurry gasification furnace and preparation method thereof (CN101591189A)" uses 85-90wt% Cr2O3, 3-8wt% ZrO2, 3-6wt% Al2O3, 0.1-1wt% Y2O3 and 2-3wt% binder as raw materials. The high-chrome bricks made in an inert atmosphere have little pollution to the environment and a long service life. However, the slag of the water-coal slurry gasification furnace contains a large amount of SiO2, which reacts with ZrO2 to generate zircon and dissolves in the slag, which reduces the thermal shock resistance of the bricks. At the same time, its binder is phenolic resin, which will react with water vapor to produce pores during service, exacerbating the penetration of slag liquid.
[0005] The patented technology of "A 95 chromium aluminum zirconium brick for a water-coal slurry pressurized gasification furnace and its production method (CN101913886A)" uses fused chromium oxide, chromium oxide green, zirconium oxide powder, α-Al2O3, powder and binder as raw materials to produce chromium aluminum zirconium bricks with a chromium oxide mass fraction of 95wt%. Compared with 90 chromium aluminum zirconium bricks, it has better room temperature compressive strength, corrosion resistance and scouring performance. However, the chromium oxide content of the product is high. A high content of chromium oxide will lead to an increase in production costs, and there are still problems such as the decomposition of the binder used (aluminum dihydrogen phosphate or dextrin) to produce pores and uneven brick performance caused by the machine pressing method.
[0006] The patented technology of "a chromium-aluminum-magnesium-zirconium refractory brick and its preparation method (CN116332631A)" introduces zirconium-magnesium-chromium spinel and chromium oxide composite frit during the preparation of the chromium oxide brick matrix. Compared with the traditional chromium oxide brick, the high-chrome brick produced has excellent thermal shock resistance by utilizing the difference in thermal expansion coefficient between the magnesia-chromium spinel and the chromium oxide particles of solid-dissolved alumina, while the slag erosion resistance is not reduced. However, the zirconium-magnesium-chromium spinel used in this technology has high preparation cost, which increases production cost.
[0007] The patented technology of "a vacuum cast high chrome brick and its preparation process (CN114230351A)" uses plate-shaped corundum, fused chrome corundum sand, fused chrome sand, chrome green powder, zirconium oxide powder, spherical corundum powder, nano-alumina sol, saponin powder and polycarboxylic acid as raw materials, and forms them by vacuum casting process after mixing them in proportion. After demolding and drying, they are kept at 1550-1590℃ for 8-12 hours and fired. The obtained high chrome brick has good integrity, low apparent porosity and excellent slag erosion resistance, and the number of water quenching cycles is more than 15 times. Although the high chrome bricks prepared by vibration molding are better than the high chrome bricks formed by machine pressing in terms of performance uniformity, on the one hand, the vacuum casting technology and the use of nano-alumina sol increase the production cost of high chrome bricks; on the other hand, the corundum and chrome corundum raw materials used in this technology are not as good as fused chromium oxide in slag erosion resistance, and no data on the slag erosion resistance and slag penetration resistance of high chrome bricks are shown. Summary of the invention
[0008] The present invention aims to overcome the defects of the prior art and aims to provide a method for preparing a water-coal slurry gasifier lining material based on a high-chromium castable with a simple process and low production cost. The water-coal slurry gasifier lining material based on a high-chromium castable prepared by the method has high compressive strength, low apparent porosity, good chemical stability, excellent thermal shock resistance, excellent slag erosion resistance and excellent slag penetration resistance.
[0009] To achieve the above object, the technical solution adopted by the present invention is:
[0010] The chemical composition of the water-coal slurry gasifier lining material based on high-chromium castable is: 57-64wt% of fused chromium oxide particles and 5-10wt% of fused magnesia-chromium spinel particles are used as aggregates, 14-21wt% of fused chromium oxide fine powder, 3-6wt% of chromium oxide green fine powder, 2-4wt% of α-alumina fine powder, 1-3wt% of light-burned magnesia sand fine powder and 3-4wt% of hydrated alumina fine powder are used as a matrix; and 0.15-0.2wt% of polycarboxylates as a water reducer are added, which is the sum of the aggregates and the matrix.
[0011] The preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable is as follows: the aggregate, the matrix and the water reducer are mixed, and then 3.5-5wt% of water of the sum of the aggregate and the matrix is added, stirred evenly, vibrated to form, cured for 1-3 days under the conditions of temperature of 40-80°C and humidity of 70-80%, demolded, baked, and kept warm for 3-8h under the conditions of 1400-1700°C, so as to obtain the water-coal slurry gasification furnace lining material based on high-chromium castable.
[0012] The particle gradation of the fused chromium oxide particles is as follows: the fused chromium oxide particles with a particle size greater than or equal to 3 mm and less than 5 mm account for 35-45wt%, the fused chromium oxide particles with a particle size greater than or equal to 1 mm and less than 3 mm account for 25-40wt%, and the fused chromium oxide particles with a particle size greater than or equal to 0.1 mm and less than 1 mm are the remainder; the Cr2O3 content of the fused chromium oxide particles is ≥99wt%.
[0013] The particle size of the fused magnesia-chromium spinel particles is greater than or equal to 3 mm and less than 5 mm; the Cr2O3 content of the fused magnesia-chromium spinel particles is greater than or equal to 72wt%.
[0014] The particle size of the fused chromium oxide fine powder is ≤0.074 mm; the Cr2O3 content of the fused chromium oxide fine powder is ≥99wt%.
[0015] The particle size of the chromium oxide green fine powder is ≤1 um; the Cr2O3 content of the chromium oxide green fine powder is ≥99wt%.
[0016] The particle size of the α-alumina fine powder is ≤5um; the Al2O3 content of the α-alumina fine powder is ≥99wt%.
[0017] The particle size of the light-burned magnesia fine powder is ≤7um; and the MgO content of the light-burned magnesia fine powder is ≥97wt%.
[0018] The particle size of the hydrated alumina fine powder is ≤8um; the Al2O3 content of the hydrated alumina fine powder is ≥97wt%.
[0019] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:
[0020] 1. The present invention adopts a pouring construction method, which is not only simple in process, but also avoids the expensive molding equipment required for the finalized product and reduces the uneven performance of the brick. The binder used in the present invention is hydrated alumina, which avoids the generation of a large amount of hexavalent chromium in the product and the increase in the cost of nano-alumina sol due to the use of calcium aluminate cement. In addition, under the curing temperature condition of 40-80°C, hydrated alumina reacts with water to generate nano-hydrated phases of bayerite and boehmite, which decompose into nano-alumina at 500-600°C, promote the formation of chromium-aluminum solid solution and the sintering of the product, increase the internal density, and thus improve the mechanical properties and physical properties of the product.
[0021] 2. The light-burned magnesia introduced in the present invention can react with hydrated alumina during the hydration process to form a layered magnesium-aluminum hydrotalcite phase [Mg x Al y (OH) 2×+2y ](CO3) y / 2 ·nH2O], this in-situ generated magnesium aluminum hydrotalcite phase can give the product higher early strength and promote the microporous internal structure. In addition, magnesium aluminum hydrotalcite dehydrates at high temperature to form magnesium aluminum spinel, which can react with chromium oxide to form magnesium aluminum chromium spinel solid solution, promote the sintering of the product, improve the compressive strength and reduce the apparent porosity of the product.
[0022] 3. The magnesium-chromium spinel aggregate introduced in the present invention can, on the one hand, react with Fe2O3, FeO, MgO and Al2O3 in the slag to form a spinel solid solution, thereby preventing it from reacting with the chromium-aluminum solid solution in the matrix to form spinel, causing expansion, destroying the internal structure of the material, and further causing spalling, thereby improving the product's resistance to slag erosion; on the other hand, by reducing the content of Fe2O3, FeO, MgO and Al2O3 in the slag, the viscosity of the slag liquid is increased, the penetration of the slag liquid is slowed down, and the product's resistance to slag penetration is improved. In addition, the thermal expansion coefficients between magnesium-chromium spinel and chromium oxide do not match, so that microcracks are generated between the magnesium-chromium spinel aggregate and the chromium oxide matrix, thereby improving the thermal shock resistance of the product. Moreover, the price of magnesium-chromium spinel is lower than that of chromium oxide, and the use of magnesium-chromium spinel aggregate to replace part of the chromium oxide aggregate can reduce the production cost of the product.
[0023] 4. The water-coal slurry gasifier lining material based on high-chromium castable prepared by the present invention has been tested: the room-temperature flexural strength after baking is 10.82-14.97MPa; the room-temperature compressive strength after baking is 60.8-79.3MPa; the apparent porosity after baking is 5.09-7.43%; the room-temperature flexural strength after high-temperature heat treatment is 15.44-17.23MPa; the room-temperature compressive strength after high-temperature heat treatment is 135.3-149.2MPa; the apparent porosity after high-temperature heat treatment is 14.5-16.7%; the number of thermal shock water cooling is 8-11 times; after a static crucible test at 1600°C×3h, the erosion index of the crucible sample is 1.08-1.22%, and the permeability index is 5.16-7.35%, which are lower than the erosion index (1.61%) and permeability index (7.84%) of phosphate-bonded high-chromium bricks under the same conditions.
[0024] Therefore, the process of the present invention is simple and the cost is low. The prepared water-coal slurry gasification furnace lining material based on high-chromium castable has the characteristics of high compressive strength, low apparent porosity, good chemical stability, excellent thermal shock resistance, excellent slag erosion resistance and excellent slag penetration resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is an XRD diagram of a hydration product of a water-coal slurry gasifier lining material based on a high-chromium castable prepared by the present invention;
[0026] Figure 2 yes Figure 1 The microstructure of the hydration product of hydrated alumina (ρ-Al2O3) of the water-coal slurry gasifier lining material based on high chromium castable is shown;
[0027] Figure 3 yes Figure 1 The microstructure of the hydration product of hydrated alumina (ρ-Al2O3) mixed with light-burned magnesia (MgO) in the water-coal slurry gasifier lining material based on high chromium castable. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the accompanying drawings and today's implementation methods, but is not intended to limit the scope of protection thereof.
[0029] A water-coal slurry gasifier lining material based on high-chromium castable and a preparation method thereof. The preparation method described in this specific embodiment is:
[0030] The chemical composition of the water-coal slurry gasifier lining material based on high-chromium castable is: 57-64wt% of fused chromium oxide particles and 5-10wt% of fused magnesia-chromium spinel particles are used as aggregates, 14-21wt% of fused chromium oxide fine powder, 3-6wt% of chromium oxide green fine powder, 2-4wt% of α-alumina fine powder, 1-3wt% of light-burned magnesia sand fine powder and 3-4wt% of hydrated alumina fine powder are used as a matrix; and 0.15-0.2wt% of polycarboxylates as a water reducer are added, which is the sum of the aggregates and the matrix.
[0031] The preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable is as follows: the aggregate, the matrix and the water reducer are mixed, and then 3.5-5wt% of water of the sum of the aggregate and the matrix is added, stirred evenly, vibrated to form, cured for 1-3 days under the conditions of temperature of 40-80°C and humidity of 70-80%, demolded, baked, and kept warm for 3-8h under the conditions of 1400-1700°C, so as to obtain the water-coal slurry gasification furnace lining material based on high-chromium castable.
[0032] The particle gradation of the fused chromium oxide particles is as follows: the fused chromium oxide particles with a particle size greater than or equal to 3 mm and less than 5 mm account for 35-45wt%, the fused chromium oxide particles with a particle size greater than or equal to 1 mm and less than 3 mm account for 25-40wt%, and the fused chromium oxide particles with a particle size greater than or equal to 0.1 mm and less than 1 mm are the remainder; the Cr2O3 content of the fused chromium oxide particles is ≥99wt%.
[0033] The Cr2O3 content of the fused magnesia-chromium spinel particles is ≥72wt%.
[0034] The Cr2O3 content of the fused chromium oxide fine powder is ≥99wt%.
[0035] The Cr2O3 content of the chromium oxide green fine powder is ≥99wt%.
[0036] The Al2O3 content of the α-alumina fine powder is ≥99wt%.
[0037] The MgO content of the light-burned magnesia fine powder is ≥97wt%.
[0038] The Al2O3 content of the hydrated alumina fine powder is ≥97wt%.
[0039] In this specific implementation mode:
[0040] The particle size of the fused magnesia-chromium spinel particles is greater than or equal to 3 mm and less than 5 mm;
[0041] The particle size of the fused chromium oxide fine powder is ≤0.074 mm;
[0042] The particle size of the chromium oxide green fine powder is ≤1um;
[0043] The particle size of the α-alumina fine powder is ≤5um;
[0044] The particle size of the light-burned magnesia fine powder is ≤7um;
[0045] The particle size of the hydrated alumina fine powder is ≤8um.
[0046] This will not be described in detail in the embodiments.
[0047] Example 1
[0048] A water-coal slurry gasifier lining material based on high-chromium castable and a preparation method thereof. The preparation method described in this embodiment is:
[0049] The chemical composition of the water-coal slurry gasifier lining material based on high-chromium castable is: 64wt% of fused chromium oxide particles and 8wt% of fused magnesia-chromium spinel particles as aggregates, 14wt% of fused chromium oxide fine powder, 6wt% of chromium oxide green fine powder, 2wt% of α-alumina fine powder, 3wt% of light-burned magnesia sand fine powder and 3wt% of hydrated alumina fine powder as a matrix; and 0.15wt% of polycarboxylates as a water reducer, the sum of the aggregates and the matrix.
[0050] The preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable is as follows: the aggregate, the matrix and the water reducer are mixed, and then 4.5wt% of water of the sum of the aggregate and the matrix is added, stirred evenly, vibrated to form, cured for 2 days at a temperature of 40°C and a humidity of 75%, demolded, baked, and kept warm at 1700°C for 5h to obtain the water-coal slurry gasification furnace lining material based on high-chromium castable.
[0051] The particle gradation of the fused chromium oxide particles is as follows: the fused chromium oxide particles with a particle size greater than or equal to 3 mm and less than 5 mm account for 45wt%, the fused chromium oxide particles with a particle size greater than or equal to 1 mm and less than 3 mm account for 40wt%, and the fused chromium oxide particles with a particle size greater than or equal to 0.1 mm and less than 1 mm are the remainder; the Cr2O3 content of the fused chromium oxide particles is 99.1wt%.
[0052] The fused magnesia-chromium spinel particles have a Cr2O3 content of 72.0 wt%.
[0053] The Cr2O3 content of the fused chromium oxide fine powder is 99.0wt%.
[0054] The Cr2O3 content of the chromium oxide green fine powder is 99.5wt%.
[0055] The Al2O3 content of the α-alumina fine powder is 99.3 wt%.
[0056] The MgO content of the light-burned magnesia fine powder is 97.0 wt %.
[0057] The Al2O3 content of the hydrated alumina fine powder is 97.8 wt%.
[0058] The water-coal slurry gasification furnace lining material based on high chromium castable prepared in this embodiment has been tested: the room temperature flexural strength after baking is 10.82MPa; the room temperature compressive strength after baking is 60.8MPa; the apparent porosity after baking is 7.43%; the room temperature flexural strength after high temperature heat treatment is 15.44MPa; the room temperature compressive strength after high temperature heat treatment is 135.3MPa; the apparent porosity after high temperature heat treatment is 16.7%; the number of thermal shock water cooling is 8 times; after a static crucible test at 1600℃×3h, the erosion index of the crucible sample is 1.22%, and the permeability index is 7.35%, which are lower than the erosion index (1.61%) and permeability index (7.84%) of phosphate-bonded high chromium bricks under the same conditions.
[0059] Example 2
[0060] A water-coal slurry gasifier lining material based on high-chromium castable and a preparation method thereof. The preparation method described in this embodiment is:
[0061] The chemical composition of the water-coal slurry gasification furnace lining material based on high-chromium castable is: 57wt% of fused chromium oxide particles and 10wt% of fused magnesia-chromium spinel particles as aggregates, 17wt% of fused chromium oxide fine powder, 6wt% of chromium oxide green fine powder, 4wt% of α-alumina fine powder, 3wt% of light-burned magnesia sand fine powder and 3wt% of hydrated alumina fine powder as a matrix; and 0.2wt% of polycarboxylates as a water reducer, the sum of the aggregates and the matrix.
[0062] The preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable is as follows: the aggregate, the matrix and the water reducer are mixed, and then 5wt% of water of the sum of the aggregate and the matrix is added, stirred evenly, vibrated to form, cured for 3 days at a temperature of 40°C and a humidity of 70%, demolded, baked, and kept warm at 1400°C for 8h to obtain the water-coal slurry gasification furnace lining material based on high-chromium castable.
[0063] The particle gradation of the fused chromium oxide particles is as follows: the fused chromium oxide particles with a particle size greater than or equal to 3 mm and less than 5 mm account for 43wt%, the fused chromium oxide particles with a particle size greater than or equal to 1 mm and less than 3 mm account for 38wt%, and the fused chromium oxide particles with a particle size greater than or equal to 0.1 mm and less than 1 mm are the remainder; the Cr2O3 content of the fused chromium oxide particles is 99.3wt%.
[0064] The fused magnesia-chromium spinel particles have a Cr2O3 content of 73.2 wt%.
[0065] The Cr2O3 content of the fused chromium oxide fine powder is 99.1wt%.
[0066] The Cr2O3 content of the chromium oxide green fine powder is 99.2wt%.
[0067] The Al2O3 content of the α-alumina fine powder is 99.5 wt%.
[0068] The MgO content of the light-burned magnesia fine powder is 97.5 wt %.
[0069] The Al2O3 content of the hydrated alumina fine powder is 97.1 wt%.
[0070] The water-coal slurry gasification furnace lining material based on high chromium castable prepared in this embodiment has been tested: the room temperature flexural strength after baking is 12.89MPa; the room temperature compressive strength after baking is 65.4MPa; the apparent porosity after baking is 6.84%; the room temperature flexural strength after high temperature heat treatment is 16.32MPa; the room temperature compressive strength after high temperature heat treatment is 137.2MPa; the apparent porosity after high temperature heat treatment is 15.7%; the number of thermal shock water cooling is 11 times; after the static crucible test at 1600℃×3h, the erosion index of the crucible sample is 1.19%, and the permeability index is 6.48%, which are lower than the erosion index (1.61%) and permeability index (7.84%) of phosphate-bonded high chromium bricks under the same conditions.
[0071] Example 3
[0072] A water-coal slurry gasifier lining material based on high-chromium castable and a preparation method thereof. The preparation method described in this embodiment is:
[0073] The chemical composition of the water-coal slurry gasification furnace lining material based on high-chromium castable is: 62wt% of fused chromium oxide particles and 10wt% of fused magnesia-chromium spinel particles as aggregates, 16wt% of fused chromium oxide fine powder, 3wt% of chromium oxide green fine powder, 3wt% of α-alumina fine powder, 2wt% of light-burned magnesia sand fine powder and 4wt% of hydrated alumina fine powder as a matrix; and 0.2wt% of polycarboxylates as a water reducer, the sum of the aggregates and the matrix.
[0074] The preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable is as follows: the aggregate, the matrix and the water reducer are mixed, and then 4wt% of water of the sum of the aggregate and the matrix is added, stirred evenly, vibrated to form, cured for 2 days at a temperature of 80°C and a humidity of 80%, demolded, baked, and kept warm at 1600°C for 5h to obtain the water-coal slurry gasification furnace lining material based on high-chromium castable.
[0075] The particle gradation of the fused chromium oxide particles is as follows: the fused chromium oxide particles with a particle size greater than or equal to 3 mm and less than 5 mm account for 40wt%, the fused chromium oxide particles with a particle size greater than or equal to 1 mm and less than 3 mm account for 25wt%, and the fused chromium oxide particles with a particle size greater than or equal to 0.1 mm and less than 1 mm are the remainder; the Cr2O3 content of the fused chromium oxide particles is 99.2wt%.
[0076] The Cr2O3 content of the fused magnesia-chromium spinel particles is 75.0wt%.
[0077] The Cr2O3 content of the fused chromium oxide fine powder is 993wt%.
[0078] The Cr2O3 content of the chromium oxide green fine powder is 99.3wt%.
[0079] The Al2O3 content of the α-alumina fine powder is 99.2 wt%.
[0080] The MgO content of the light-burned magnesia fine powder is 97.4 wt %.
[0081] The Al2O3 content of the hydrated alumina fine powder is 97.6 wt%.
[0082] The water-coal slurry gasifier lining material based on high-chromium castable prepared in this embodiment has been tested: the room-temperature flexural strength after baking is 13.31MPa; the room-temperature compressive strength after baking is 70.1MPa; the apparent porosity after baking is 6.26%; the room-temperature flexural strength after high-temperature heat treatment is 16.84MPa; the room-temperature compressive strength after high-temperature heat treatment is 142.8MPa; the apparent porosity after high-temperature heat treatment is 15.2%; the number of thermal shock water cooling is 10 times; after a static crucible test at 1600℃×3h, the erosion index of the crucible sample is 1.14%, and the permeability index is 6.25%, which are lower than the erosion index (1.61%) and permeability index (7.84%) of phosphate-bonded high-chromium bricks under the same conditions.
[0083] Example 4
[0084] A water-coal slurry gasifier lining material based on high-chromium castable and a preparation method thereof. The preparation method described in this embodiment is:
[0085] The chemical composition of the water-coal slurry gasification furnace lining material based on high-chromium castable is: 62wt% of fused chromium oxide particles and 5wt% of fused magnesia-chromium spinel particles as aggregates, 20wt% of fused chromium oxide fine powder, 6wt% of chromium oxide green fine powder, 2wt% of α-alumina fine powder, 1wt% of light-burned magnesia sand fine powder and 4wt% of hydrated alumina fine powder as a matrix; and 0.15wt% of polycarboxylates as a water reducer, the sum of the aggregates and the matrix.
[0086] The preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable is as follows: the aggregate, the matrix and the water reducer are mixed, and then 4.2wt% of water of the sum of the aggregate and the matrix is added, stirred evenly, vibrated to form, cured for 1 day at a temperature of 60°C and a humidity of 75%, demolded, baked, and kept warm at 1650°C for 3h to obtain the water-coal slurry gasification furnace lining material based on high-chromium castable.
[0087] The particle gradation of the fused chromium oxide particles is as follows: the fused chromium oxide particles with a particle size greater than or equal to 3 mm and less than 5 mm account for 38wt%, the fused chromium oxide particles with a particle size greater than or equal to 1 mm and less than 3 mm account for 30wt%, and the fused chromium oxide particles with a particle size greater than or equal to 0.1 mm and less than 1 mm are the remainder; the Cr2O3 content of the fused chromium oxide particles is 99.0wt%.
[0088] The Cr2O3 content of the fused magnesia-chromium spinel particles is 73.9wt%.
[0089] The Cr2O3 content of the fused chromium oxide fine powder is 99.2wt%.
[0090] The Cr2O3 content of the chromium oxide green fine powder is 99.0wt%.
[0091] The Al2O3 content of the α-alumina fine powder is 99.1 wt%.
[0092] The MgO content of the light-burned magnesia fine powder is 97.2 wt %.
[0093] The Al2O3 content of the hydrated alumina fine powder is 97.3 wt%.
[0094] The water-coal slurry gasification furnace lining material based on high chromium castable prepared in this embodiment has been tested: the room temperature flexural strength after baking is 14.97MPa; the room temperature compressive strength after baking is 79.3MPa; the apparent porosity after baking is 5.09%; the room temperature flexural strength after high temperature heat treatment is 17.23MPa; the room temperature compressive strength after high temperature heat treatment is 149.2MPa; the apparent porosity after high temperature heat treatment is 14.5%; the number of thermal shock water cooling is 10 times; after a static crucible test at 1600℃×3h, the erosion index of the crucible sample is 1.08%, and the permeability index is 5.16%, which are lower than the erosion index (1.61%) and permeability index (7.84%) of phosphate-bonded high chromium bricks under the same conditions.
[0095] Example 5
[0096] A water-coal slurry gasifier lining material based on high-chromium castable and a preparation method thereof. The preparation method described in this embodiment is:
[0097] The chemical composition of the water-coal slurry gasifier lining material based on high-chromium castable is: 62wt% of fused chromium oxide particles and 5wt% of fused magnesia-chromium spinel particles as aggregates, 21wt% of fused chromium oxide fine powder, 5wt% of chromium oxide green fine powder, 2wt% of α-alumina fine powder, 1wt% of light-burned magnesia sand fine powder and 4wt% of hydrated alumina fine powder as a matrix; and 0.15wt% of polycarboxylates as a water reducer, the sum of the aggregates and the matrix.
[0098] The preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable is as follows: the aggregate, the matrix and the water reducer are mixed, and then 4wt% of water of the sum of the aggregate and the matrix is added, stirred evenly, vibrated to form, cured for 1 day at a temperature of 60°C and a humidity of 75%, demolded, baked, and kept warm at 1500°C for 3h to obtain the water-coal slurry gasification furnace lining material based on high-chromium castable.
[0099] The particle gradation of the fused chromium oxide particles is as follows: the fused chromium oxide particles with a particle size greater than or equal to 3 mm and less than 5 mm account for 35wt%, the fused chromium oxide particles with a particle size greater than or equal to 1 mm and less than 3 mm account for 35wt%, and the fused chromium oxide particles with a particle size greater than or equal to 0.1 mm and less than 1 mm are the remainder; the Cr2O3 content of the fused chromium oxide particles is 99.5wt%.
[0100] The fused magnesia-chromium spinel particles have a Cr2O3 content of 76.0 wt%.
[0101] The Cr2O3 content of the fused chromium oxide fine powder is 99.5wt%.
[0102] The Cr2O3 content of the chromium oxide green fine powder is 99.1wt%.
[0103] The Al2O3 content of the α-alumina fine powder is 99.0 wt%.
[0104] The MgO content of the light-burned magnesia fine powder is 97.9 wt %.
[0105] The Al2O3 content of the hydrated alumina fine powder is 97.0 wt%.
[0106] The water-coal slurry gasifier lining material based on high-chromium castable prepared in this embodiment is tested: the room-temperature flexural strength after baking is 14.02MPa; the room-temperature compressive strength after baking is 74.5MPa; the apparent porosity after baking is 5.56%; the room-temperature flexural strength after high-temperature heat treatment is 17.01MPa; the room-temperature compressive strength after high-temperature heat treatment is 147.6MPa; the apparent porosity after high-temperature heat treatment is 14.9%; the number of thermal shock water cooling is 9 times; after a static crucible test at 1600℃×3h, the erosion index of the crucible sample is 1.12%, and the permeability index is 5.84%, which are lower than the erosion index (1.61%) and permeability index (7.84%) of phosphate-bonded high-chromium bricks under the same conditions.
[0107] Compared with the prior art, this specific implementation has the following positive effects:
[0108] 1. The present invention adopts a pouring construction method, which is not only simple in process, but also avoids the expensive molding equipment required for the finalized product and reduces the uneven performance of the brick. The binder used in the present invention is hydrated alumina, which avoids the generation of a large amount of hexavalent chromium in the product and the increase in the cost of nano-alumina sol due to the use of calcium aluminate cement. In addition, under the curing temperature condition of 40-80°C, hydrated alumina reacts with water to generate nano-hydrated phases of bayerite and boehmite, which decompose into nano-alumina at 500-600°C, promote the formation of chromium-aluminum solid solution and the sintering of the product, increase the internal density, and thus improve the mechanical properties and physical properties of the product.
[0109] 2. The water-coal slurry gasifier lining material based on high chromium castable prepared by the present invention is shown in the attached figure. Figure 1 is the XRD diagram of the hydration product of the water-coal slurry gasifier lining material based on the high chromium castable prepared in Example 4; Figure 2 yes Figure 1 The microstructure of the hydration product of hydrated alumina (ρ-Al2O3) of the water-coal slurry gasifier lining material based on high chromium castable is shown; Figure 3 yes Figure 1 The microstructure of the hydration product of hydrated alumina (ρ-Al2O3) and light-burned magnesia (MgO) mixed in the water-coal slurry gasifier lining material based on high chromium castable. Figure 1 It can be seen that the added light-burned magnesia fine powder and hydrated alumina fine powder react during the hydration process to form a magnesium-aluminum hydrotalcite phase [Mg x Al y (OH) 2×+2y ](CO3) y / 2 ·nH2O], the magnesium-aluminum hydrotalcite phase decomposes to form magnesium-aluminum spinel during the sintering process, and the magnesium-aluminum spinel can react with chromium oxide fine powder to produce spinel solid solution, which promotes the sintering of the product, thereby promoting the improvement of the compressive strength of the product and the reduction of the apparent porosity; Figure 2 and Figure 3 It can be seen that the size of the generated magnesium-aluminum hydrotalcite is between nanometer size and micrometer size, and the shape is layered. These layered magnesium-aluminum hydrotalcites are stacked on each other and fill the pores in the product, which can improve the early strength of the product and reduce its early apparent porosity, thereby promoting the improvement of the compressive strength of the product and the reduction of the apparent porosity.
[0110] Therefore, the magnesium-aluminum hydrotalcite in this specific embodiment will form magnesium-aluminum spinel when dehydrated at high temperature, which can react with chromium oxide to form a magnesium-aluminum-chromium spinel solid solution, promote the sintering of the product, improve the compressive strength and reduce the apparent porosity of the product.
[0111] 3. On the one hand, the magnesium-chromium spinel aggregate introduced in the present invention can react with Fe2O3, FeO, MgO and Al2O3 in the slag to form a spinel solid solution, thereby preventing it from reacting with the chromium-aluminum solid solution in the matrix to form spinel, causing expansion, destroying the internal structure of the material, and then causing spalling, thereby improving the slag erosion resistance of the castable; on the other hand, by reducing the content of Fe2O3, FeO, MgO and Al2O3 in the slag, the viscosity of the slag liquid is increased, the penetration of the slag liquid is slowed down, and the slag penetration resistance of the castable is improved. In addition, the thermal expansion coefficients between magnesium-chromium spinel and chromium oxide do not match, so that microcracks are generated between the magnesium-chromium spinel aggregate and the chromium oxide matrix, thereby improving the thermal shock resistance of the castable. Moreover, the price of magnesium-chromium spinel is lower than that of chromium oxide, and the use of magnesium-chromium spinel aggregate to replace part of the chromium oxide aggregate can reduce the production cost of the castable.
[0112] 4. The water-coal slurry gasifier lining material based on high-chromium castable prepared by the present invention has been tested: the room-temperature flexural strength after baking is 10.82-14.97MPa; the room-temperature compressive strength after baking is 60.8-79.3MPa; the apparent porosity after baking is 5.09-7.43%; the room-temperature flexural strength after high-temperature heat treatment is 15.44-17.23MPa; the room-temperature compressive strength after high-temperature heat treatment is 135.3-149.2MPa; the apparent porosity after high-temperature heat treatment is 14.5-16.7%; the number of thermal shock water cooling is 8-11 times; after a static crucible test at 1600°C×3h, the erosion index of the crucible sample is 1.08-1.22%, and the permeability index is 5.16-7.35%, which are lower than the erosion index (1.61%) and permeability index (7.84%) of phosphate-bonded high-chromium bricks under the same conditions.
[0113] Therefore, the process of the present invention is simple and the cost is low. The prepared water-coal slurry gasification furnace lining material based on high-chromium castable has the characteristics of high compressive strength, low apparent porosity, good chemical stability, excellent thermal shock resistance, excellent slag erosion resistance and excellent slag penetration resistance.
Claims
1. A method for preparing a water-coal slurry gasifier lining material based on a high-chromium castable, characterized in that: The chemical composition of the water-coal slurry gasifier lining material based on high-chromium castable is: 57-64wt% of fused chromium oxide particles and 5-10wt% of fused magnesia-chromium spinel particles as aggregates, 14-21wt% of fused chromium oxide fine powder, 3-6wt% of chromium oxide green fine powder, 2-4wt% of α-alumina fine powder, 1-3wt% of light-burned magnesia fine powder and 3-4wt% of hydrated alumina fine powder as a matrix; 0.15-0.2wt% of the total of the aggregate and the matrix is added as a polycarboxylate as a water reducer; The preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable is as follows: the aggregate, the matrix and the water reducer are mixed, and then 3.5-5wt% of water of the sum of the aggregate and the matrix is added, stirred evenly, vibrated to form, cured for 1-3 days under the conditions of temperature of 40-80°C and humidity of 70-80%, demolded, baked, and kept warm for 3-8h under the conditions of 1400-1700°C, so as to obtain the water-coal slurry gasification furnace lining material based on high-chromium castable.
2. The method for preparing a water-coal slurry gasifier lining material based on a high chromium castable according to claim 1, characterized in that: The particle gradation of the fused chromium oxide particles is as follows: the fused chromium oxide particles with a particle size greater than or equal to 3 mm and less than 5 mm account for 35-45wt%, the fused chromium oxide particles with a particle size greater than or equal to 1 mm and less than 3 mm account for 25-40wt%, and the fused chromium oxide particles with a particle size greater than or equal to 0.1 mm and less than 1 mm are the remainder; the Cr2O3 content of the fused chromium oxide particles is ≥99wt%.
3. The method for preparing a water-coal slurry gasifier lining material based on a high chromium castable according to claim 1, characterized in that: The particle size of the fused magnesia-chromium spinel particles is greater than or equal to 3 mm and less than 5 mm; the Cr2O3 content of the fused magnesia-chromium spinel particles is greater than or equal to 72wt%.
4. The method for preparing a water-coal slurry gasifier lining material based on a high chromium castable according to claim 1, characterized in that: The particle size of the fused chromium oxide fine powder is ≤0.074 mm; the Cr2O3 content of the fused chromium oxide fine powder is ≥99wt%.
5. The method for preparing a water-coal slurry gasifier lining material based on a high chromium castable according to claim 1, characterized in that: The particle size of the chromium oxide green fine powder is ≤1 um; the Cr2O3 content of the chromium oxide green fine powder is ≥99wt%.
6. The method for preparing a water-coal slurry gasifier lining material based on a high chromium castable according to claim 1, characterized in that: The particle size of the α-alumina fine powder is ≤5um; the Al2O3 content of the α-alumina fine powder is ≥99wt%.
7. The method for preparing a water-coal slurry gasifier lining material based on a high chromium castable according to claim 1, characterized in that: The particle size of the light-burned magnesia fine powder is ≤7um; and the MgO content of the light-burned magnesia fine powder is ≥97wt%.
8. The method for preparing a water-coal slurry gasifier lining material based on a high chromium castable according to claim 1, characterized in that: The particle size of the hydrated alumina fine powder is ≤8um; the Al2O3 content of the hydrated alumina fine powder is ≥97wt%.
9. A water-coal slurry gasifier lining material based on high chromium castable, characterized in that The water-coal slurry gasification furnace lining material based on high-chromium castable is a water-coal slurry gasification furnace lining material based on high-chromium castable prepared by the preparation method of the water-coal slurry gasification furnace lining material based on high-chromium castable according to any one of claims 1 to 8.
Citation Information
Patent Citations
Cr-Zr brick for coal slurry gasifier and method for preparing same
CN101591189A
95 chromium-aluminum-zirconium brick for coal water slurry pressurized gasifier and preparation method thereof
CN101913886A
Vacuum casting high-chromium brick and preparation process thereof
CN114230351A
Plugging brick for top opening of water-coal slurry gasification furnace and preparation process thereof
CN104478442A
Chromium oxide composite spinel brick and preparation method of same
CN108516845A
Cited By
Anti-corrosion composite furnace lining material for fluidizing chlorination of zircon sand and preparation method of anti-corrosion composite furnace lining material