Polyetherimide-based dielectric film and preparation method thereof

By covalently connecting the double-ended alkenyl polyphenylene ether cladding in polyetherimide materials, the problem of easy agglomeration of nanoceramic fillers is solved, the dielectric performance and high-temperature energy storage performance are improved, and the breakdown field is enhanced powerful.

CN119039781APending Publication Date: 2024-11-29WUZHEN LABORATORY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411165498.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, when improving the dielectric properties of polyetherimide materials, nanoceramic fillers are prone to agglomeration, making it difficult to achieve better dielectric properties and high-temperature energy storage performance, and a large amount of addition will lead to a decrease in the breakdown field strength.

Method used

By covalently connecting the double-ended alkenyl polyphenylene ether coating on the surface of the hydroxylated dielectric filler, covalent connection is formed using thiol silane coupling agent to improve the dispersion and compatibility of the dielectric filler, reduce interface defects, and enhance Dielectric performance and high-temperature energy storage performance.

Benefits of technology

It has achieved improvements in dielectric performance and improvements in high-temperature energy storage performance, reduced dielectric loss and dielectric constant, and enhanced breakdown field strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007755960000151
    Figure BDA0005007755960000151
Patent Text Reader

Abstract

The invention relates to the technical field of dielectric films, and discloses a polyetherimide-based dielectric film and a preparation method thereof. The dielectric film comprises a polyetherimide matrix and a modified dielectric filler dispersed in the polyetherimide matrix, the modified dielectric filler is composed of a hydroxylated dielectric filler and a double-terminal alkenyl polyphenyl ether coating layer coating the hydroxylated dielectric filler, and the hydroxylated dielectric filler and the double-terminal alkenyl polyphenyl ether coating layer are covalently connected through a sulfydryl silane coupling agent. In the dielectric film disclosed by the invention, the double-terminal alkenyl polyphenyl ether coating layer is covalently connected to the surface of the hydroxylated dielectric filler by utilizing the sulfydryl silane coupling agent, so that the dielectric film can be endowed with better dielectric property and high-temperature energy storage property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dielectric films, and in particular to a polyetherimide-based dielectric film and a preparation method thereof. Background Art

[0002] Film capacitors are an important basic electronic component. Compared with ceramic capacitors, aluminum / tantalum capacitors, film capacitors have high insulation resistance, high withstand voltage, low dielectric loss, excellent frequency characteristics, and self-healing properties. At present, the most commonly used film dielectric in film capacitors is BOPP, which has a temperature resistance of about 105°C and a relative dielectric constant of only 2-3. Therefore, even under high field strength, its energy storage density is less than 2J / cm 3 , which means that a large volume is required to meet certain energy storage requirements.

[0003] Polyetherimide (PEI) is a transparent or translucent polymer with a slightly amber color. It can be used for a long time at 150°C, has good thermal stability, hydrolysis resistance, good dimensional stability, small molding shrinkage, and can maintain excellent mechanical properties even at high temperatures. It also has excellent electrical properties over a wide range of temperature and frequency, and is one of the most promising high-temperature resistant dielectric film polymers.

[0004] However, the relative dielectric constant of pure polyetherimide material is low, and the dielectric constant of the composite material is generally improved by adding nano-ceramic fillers with high dielectric constant to polyetherimide. In the prior art, when nano-ceramic particles are used to composite with a polymer matrix, a large amount of addition is generally required to make the composite material have a higher dielectric constant and better high-temperature energy storage performance. However, a large amount of addition will cause the nanoparticles to agglomerate together due to a strong force, which will not only limit its effect of improving the dielectric constant and reducing dielectric loss, but also significantly reduce the breakdown field strength of the composite material, resulting in poor high-temperature energy storage performance of the film, which is not conducive to its application in film capacitors. Summary of the invention

[0005] In order to solve the above technical problem, that is, when adding nano-ceramic fillers to improve the dielectric properties of PEI materials, nanoparticles are easy to agglomerate, making it difficult to achieve good dielectric properties and high-temperature energy storage performance, the present invention provides a polyetherimide-based dielectric film and a preparation method thereof. In the dielectric film, a bi-terminal vinyl polyphenylene ether coating layer is covalently connected to the surface of the hydroxylated dielectric filler using a mercaptosilane coupling agent, which can give the dielectric film better dielectric properties and high-temperature energy storage performance.

[0006] The specific technical scheme of the present invention is: In the first aspect, the present invention provides a polyetherimide-based dielectric film, comprising a polyetherimide matrix and a modified dielectric filler dispersed in the polyetherimide matrix; the modified dielectric filler is composed of a hydroxylated dielectric filler and a double-terminal vinyl polyphenylene ether coating layer coated on the hydroxylated dielectric filler, and the hydroxylated dielectric filler and the double-terminal vinyl polyphenylene ether coating layer are covalently connected through a mercaptosilane coupling agent.

[0007] The mercaptosilane coupling agent can form a covalent connection between the hydroxylated dielectric filler and the double-terminal alkenyl polyphenylene ether coating layer in the following manner: the silane alkoxy group (i.e., the alkoxy group connected to the silicon atom) in the mercaptosilane coupling agent can undergo a hydrolysis condensation reaction with the hydroxyl group on the surface of the hydroxylated dielectric filler to form a covalent connection, and the mercapto group in the mercaptosilane coupling agent can undergo a click reaction with the terminal alkenyl group in the double-terminal alkenyl polyphenylene ether to form a covalent connection. Through the above-mentioned method, the polyphenylene ether can form a relatively stable coating layer outside the dielectric filler. After being added to the PEI matrix, the dispersibility and compatibility of the dielectric filler in the PEI matrix can be effectively improved, and the interface defects can be reduced. At the same time, the agglomeration of the dielectric filler can be reduced, and its effect can be improved, thereby improving the dielectric properties of the dielectric film (achieving lower dielectric loss and higher dielectric constant) and high-temperature energy storage performance.

[0008] In addition, polyphenylene ether has the characteristics of low dielectric loss, high heat resistance and low water absorption (only about 0.06%, much lower than PEI). Therefore, after polyphenylene ether is introduced into the PEI-based dielectric film, polyphenylene ether itself will not cause too much adverse effect on the dielectric properties and heat resistance of the film. At the same time, it can also prevent the surface of the dielectric filler from absorbing water, thereby reducing the dielectric loss of the film and increasing the breakdown field strength, thereby improving the high-temperature energy storage performance.

[0009] Preferably, the hydroxylated dielectric filler is formed by hydroxylating BaTiO3 and BN nanosheets in a mass ratio of 1:0.05 to 0.19.

[0010] Barium titanate (BaTiO3) has the characteristics of high dielectric constant and high energy density. It can effectively improve the dielectric constant of PEI-based dielectric film when added to it. However, when the amount added is large, it will cause a significant decrease in the breakdown field strength of the film at high temperature, thereby affecting its high-temperature energy storage performance. Boron nitride (BN) nanosheets have a wide band gap and high dielectric strength, and have good mechanical strength and thermal conductivity. When they are directly added to PEI-based dielectric film, they cannot effectively improve the dielectric properties and high-temperature energy storage performance of the film. However, when polyphenylene ether is wrapped around it in the manner of the present invention, it can better capture the fluid in the film, suppress leakage current, thereby reducing the dielectric loss of the film and improving its high-temperature energy storage performance.

[0011] The present invention adopts a specific mass ratio (1:0.05-0.19) of BaTiO3 and BN nanosheets to give the PEI-based dielectric film better dielectric properties and high-temperature energy storage performance. Among these two dielectric fillers, when the proportion of BaTiO3 is too large, the dielectric loss of the dielectric film will be large and the high-temperature energy storage performance will be poor; and when the proportion of BN nanosheets is too large, it will have an adverse effect on the dielectric constant of the dielectric film.

[0012] Preferably, the number average molecular weight of the diolefinic polyphenylene ether is 1000 to 5000 Da.

[0013] The present invention uses a biolefinic polyphenylene ether to coat a dielectric filler to improve the dielectric properties and high-temperature energy storage performance of a PEI-based dielectric film. By using a biolefinic polyphenylene ether with a number average molecular weight of 1000 to 5000 Da, the dielectric properties and high-temperature energy storage performance of the dielectric film can be further improved. When the molecular chain of the biolefinic polyphenylene ether is too short (the number average molecular weight is too small), the coating effect on the dielectric filler is poor, which will cause the coating layer to have a relatively poor effect on improving the dielectric properties and high-temperature energy storage performance of the film; when the molecular chain of the biolefinic polyphenylene ether is too long (the number average molecular weight is too large), the reaction activity is low, which will also have an adverse effect on its coating effect, thereby affecting the improvement of the dielectric properties and high-temperature energy storage performance of the film.

[0014] Preferably, the particle size of the BaTiO3 is 30 to 500 nm.

[0015] Preferably, the mass ratio of the polyetherimide matrix to the modified dielectric filler is 100:5-55.

[0016] In a second aspect, the present invention provides a method for preparing the polyetherimide-based dielectric film, comprising the following steps: (1) performing surface hydroxylation modification on the dielectric filler to obtain a hydroxylated dielectric filler; (2) using a hydroxylated dielectric filler and a mercaptosilane coupling agent as raw materials, performing a hydrolysis condensation reaction between hydroxyl groups and silaneoxy groups to obtain a mercapto-containing dielectric filler; (3) using the thiolated dielectric filler and the double-terminal olefinic polyphenylene ether as raw materials, performing a click reaction between the thiol group and the olefinic group, forming a double-terminal olefinic polyphenylene ether coating layer outside the thiolated dielectric filler, and obtaining a modified dielectric filler; (4) The modified dielectric filler and the polyetherimide resin are mixed and prepared into a film.

[0017] In the above preparation process: in step (1), hydroxyl groups can be introduced on the surface of the dielectric filler by surface hydroxylation modification; in step (2), the mercaptosilane coupling agent can be covalently grafted onto the dielectric filler by the reaction of silanol groups with silanoxy groups, thereby introducing mercapto groups on the surface of the dielectric filler; in step (3), the terminal alkenyl polyphenylene ether can be covalently linked to the surface of the dielectric filler by the reaction of mercapto groups with alkenyl groups. In the above manner, the stable coating of polyphenylene ether on the surface of the dielectric filler can be achieved.

[0018] Preferably, in step (2), the mass ratio of the hydroxylated dielectric filler to the mercaptosilane coupling agent is 1:0.5-0.7; in step (3), the mass ratio of the mercapto dielectric filler to the double-terminal alkenyl polyphenylene ether is 1:0.5-1.

[0019] Preferably, step (1) specifically comprises: dispersing the dielectric filler into a H2O2 solution, reacting at 95-105°C for 2-4 hours, separating the product, and obtaining a hydroxylated dielectric filler.

[0020] Preferably, step (2) specifically comprises: dispersing the thiolated dielectric filler into a reaction solvent I, adding a mercaptosilane coupling agent, reacting at 20 to 80° C. for 8 to 24 hours, separating the product, and obtaining the thiolated dielectric filler.

[0021] Preferably, step (3) specifically comprises: dissolving the double-terminal olefinic polyphenylene ether and the click reaction catalyst into the reaction solvent II, adding the thiol-modified dielectric filler, and after uniform dispersion, reacting under ultraviolet light for 30 to 60 minutes, separating the product, and obtaining the modified dielectric filler.

[0022] Preferably, step (4) specifically comprises: (4.1) dissolving a polyetherimide resin in an organic solvent to obtain a polyetherimide solution; (4.2) dispersing the modified dielectric filler into the polyetherimide solution to obtain a composite solution; (4.3) The composite solution is scraped onto the substrate to form a thin film, which is then dried and peeled off from the substrate.

[0023] Preferably, in step (4.1), the mass concentration of the polyetherimide solution is 10 to 50%.

[0024] Preferably, step (4.2) specifically comprises: adding the modified dielectric filler into the polyetherimide solution, stirring, and then ultrasonically dispersing at 1500-2200W for 10-40min to obtain a composite solution.

[0025] Preferably, in step (4.3), the composite solution is coated on the substrate to a thickness of 30 to 80 μm.

[0026] Compared with the prior art, the present invention has the following advantages: (1) In the present invention, a diolefinic polyphenylene ether coating layer is covalently linked to the surface of the hydroxylated dielectric filler by using a mercaptosilane coupling agent, which can improve the dispersibility and compatibility of the dielectric filler in the PEI matrix. The polyphenylene ether itself will not cause excessive adverse effects on the dielectric properties of the PEI-based dielectric film, and can also prevent the surface of the dielectric filler from absorbing water. Therefore, the dielectric properties and high-temperature energy storage performance of the PEI-based dielectric film can be improved to a large extent.

[0027] (2) In the present invention, BaTiO3 and BN nanosheets are compounded in a certain ratio as dielectric fillers, which can give the PEI-based dielectric film better dielectric properties and high-temperature energy storage performance. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with the embodiments.

[0029] Overall embodiment A polyetherimide-based dielectric film comprises a polyetherimide matrix and a modified dielectric filler dispersed in the polyetherimide matrix; the modified dielectric filler is composed of a hydroxylated dielectric filler and a biolefinic polyphenylene ether coating layer coated on the hydroxylated dielectric filler, and the hydroxylated dielectric filler and the biolefinic polyphenylene ether coating layer are covalently connected via a mercaptosilane coupling agent.

[0030] As a specific implementation, the hydroxylated dielectric filler is formed by hydroxylating BaTiO3 and BN nanosheets in a mass ratio of 1:0.05-0.19; the particle size of the BaTiO3 is 30-500 nm.

[0031] As a specific implementation, the number average molecular weight of the double-terminal olefinic polyphenylene ether is 1000 to 5000 Da.

[0032] As a specific implementation manner, the mass ratio of the polyetherimide matrix to the modified dielectric filler is 100:5-55.

[0033] A method for preparing the polyetherimide-based dielectric film comprises the following steps: (1) performing surface hydroxylation modification on the dielectric filler to obtain a hydroxylated dielectric filler; (2) using a hydroxylated dielectric filler and a mercaptosilane coupling agent as raw materials, performing a hydrolysis condensation reaction between hydroxyl groups and silaneoxy groups to obtain a mercapto-containing dielectric filler; (3) using the thiolated dielectric filler and the double-terminal olefinic polyphenylene ether as raw materials, performing a click reaction between the thiol group and the olefinic group, forming a double-terminal olefinic polyphenylene ether coating layer outside the thiolated dielectric filler, and obtaining a modified dielectric filler; (4) The modified dielectric filler and the polyetherimide resin are mixed and prepared into a film.

[0034] As a specific implementation, step (1) specifically includes: dispersing the dielectric filler into a H2O2 solution, reacting at 95-105°C for 2-4 hours, separating the product, and obtaining a hydroxylated dielectric filler.

[0035] As a specific implementation, step (2) specifically includes: dispersing the thiolated dielectric filler into the reaction solvent I, then adding a mercaptosilane coupling agent, reacting at 20 to 80° C. for 8 to 24 hours, separating the product, and obtaining the thiolated dielectric filler; the mass ratio of the hydroxylated dielectric filler to the mercaptosilane coupling agent is 1:0.5 to 0.7.

[0036] As a specific implementation method, step (3) specifically includes: dissolving the double-terminal olefinic polyphenylene ether and the click reaction catalyst into the reaction solvent II, then adding the thiolated dielectric filler, and after uniform dispersion, reacting under ultraviolet light for 30 to 60 minutes, separating the product, and obtaining the modified dielectric filler; the mass ratio of the thiolated dielectric filler to the double-terminal olefinic polyphenylene ether is 1:0.5 to 1.

[0037] As a specific implementation, step (4) specifically includes: (4.1) dissolving a polyetherimide resin in an organic solvent to obtain a polyetherimide solution having a mass concentration of 10 to 50%; (4.2) adding a modified dielectric filler to the polyetherimide solution, stirring, and then ultrasonically dispersing at 1500 to 2200 W for 10 to 40 minutes to obtain a composite solution; (4.3) The composite solution is scraped onto the substrate to form a thin film with a thickness of 30 to 80 μm, which is then dried and peeled off from the substrate. Specific embodiments The present invention is described below by specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Without departing from the spirit and scope of the inventive concept, changes and advantages that can be thought of by those skilled in the art are included in the present invention, and the attached claims and any equivalents thereof are the protection scope of the present invention.

[0039] Unless otherwise defined, all technical terms and scientific terms used in the present invention have the same meanings as those commonly understood by ordinary technicians in the field to which the present disclosure belongs. Unless otherwise specified, the raw materials and equipment used in the present invention are conventional raw materials and equipment in the field and can be obtained from conventional commercial channels; unless otherwise specified, the methods used in the present invention are conventional methods in the field.

[0040] Example 1 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0041] (2) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.1 to a hydrogen peroxide solution with a concentration of 30 wt %, and the ratio of the total mass of the nano-barium titanate and the boron nitride nanosheets to the volume of the hydrogen peroxide solution is 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 100° C. for 3 h. The product is separated, washed, and dried to obtain a hydroxylated dielectric filler.

[0042] (3) Ultrasonic dispersion of the hydroxylated dielectric filler in a mixed solvent of water and ethanol in a volume ratio of 1:9, and then adding 3-mercaptopropyltrimethoxysilane. The mass volume ratio of the hydroxylated dielectric filler, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.4 g:10 mL. The reaction is stirred at 60° C. for 12 h. The product is separated, washed and dried to obtain the thiolated dielectric filler.

[0043] (4) A biolefinic polyphenylene ether with a number average molecular weight of 1000Da was dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then a thiolated dielectric filler was added, the mass volume ratio of the thiolated dielectric filler, the biolefinic polyphenylene ether and the mixed solvent was 1g:1g:20mL, stirred and ultrasonically dispersed for 20min, and then a catalyst benzoin dimethyl ether was added, the mass ratio of benzoin dimethyl ether to the thiolated dielectric filler was 0.01:1, stirred evenly, and reacted under ultraviolet light for 40min, and the product was separated, washed and dried to obtain a modified dielectric filler.

[0044] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0045] (6) The modified dielectric filler was added to the PEI solution, with the mass ratio of the modified dielectric filler to the PEI resin being 10:100, and the mixture was stirred for 30 min, and then ultrasonicated at a power of 1800 W for 20 min to obtain a uniform composite solution.

[0046] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0047] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0048] Example 2 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0049] (2) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.05 to a hydrogen peroxide solution with a concentration of 30 wt %. The ratio of the total mass of the nano-barium titanate and the boron nitride nanosheets to the volume of the hydrogen peroxide solution is 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 95° C. for 4 h. The product is separated, washed and dried to obtain a hydroxylated dielectric filler.

[0050] (3) Ultrasonic dispersion of the hydroxylated dielectric filler in a mixed solvent of water and ethanol in a volume ratio of 2:8, and then adding 3-mercaptopropyltrimethoxysilane. The mass volume ratio of the hydroxylated dielectric filler, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.3 g:10 mL. The reaction is stirred at 25° C. for 24 h. The product is separated, washed and dried to obtain the thiolated dielectric filler.

[0051] (4) A double-terminal olefinic polyphenylene ether with a number average molecular weight of 2500Da is dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then a thiolated dielectric filler is added, the mass volume ratio of the thiolated dielectric filler, the double-terminal olefinic polyphenylene ether and the mixed solvent is 1g:0.5g:20mL, stirred and ultrasonically dispersed for 20min, and then a catalyst benzoin dimethyl ether is added, the mass ratio of benzoin dimethyl ether to the thiolated dielectric filler is 0.01:1, stirred evenly, reacted under ultraviolet light for 40min, and the product was separated, washed and dried to obtain a modified dielectric filler.

[0052] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0053] (6) The modified dielectric filler was added to the PEI solution, with the mass ratio of the modified dielectric filler to the PEI resin being 20:100, and the mixture was stirred for 30 min, and then ultrasonicated at a power of 1800 W for 20 min to obtain a uniform composite solution.

[0054] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0055] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0056] Example 3 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0057] (2) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.19 to a hydrogen peroxide solution with a concentration of 30 wt %. The ratio of the total mass of the nano-barium titanate and the boron nitride nanosheets to the volume of the hydrogen peroxide solution is 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 105° C. for 2 h. The product is separated, washed and dried to obtain a hydroxylated dielectric filler.

[0058] (3) Ultrasonic dispersion of the hydroxylated dielectric filler in a mixed solvent of water and ethanol in a volume ratio of 3:7, and then adding 3-mercaptopropyltrimethoxysilane. The mass volume ratio of the hydroxylated dielectric filler, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.5 g:10 mL. The reaction is stirred at 80° C. for 8 h. The product is separated, washed and dried to obtain the thiolated dielectric filler.

[0059] (4) A double-terminal olefinic polyphenylene ether with a number average molecular weight of 5000Da is dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then a thiolated dielectric filler is added, the mass volume ratio of the thiolated dielectric filler, the double-terminal olefinic polyphenylene ether and the mixed solvent is 1g:1g:20mL, stirred and ultrasonically dispersed for 20min, and then a catalyst benzoin dimethyl ether is added, the mass ratio of benzoin dimethyl ether to the thiolated dielectric filler is 0.01:1, stirred evenly, reacted under ultraviolet light for 40min, and the product was separated, washed and dried to obtain a modified dielectric filler.

[0060] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0061] (6) The modified dielectric filler was added to the PEI solution, with the mass ratio of the modified dielectric filler to the PEI resin being 30:100, and the mixture was stirred for 30 min, and then ultrasonicated at a power of 1800 W for 20 min to obtain a uniform composite solution.

[0062] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0063] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0064] Example 4 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0065] (2) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.1 to a hydrogen peroxide solution with a concentration of 30 wt %, and the ratio of the total mass of the nano-barium titanate and the boron nitride nanosheets to the volume of the hydrogen peroxide solution is 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 100° C. for 3 h. The product is separated, washed, and dried to obtain a hydroxylated dielectric filler.

[0066] (3) Ultrasonic dispersion of the hydroxylated dielectric filler in a mixed solvent of water and ethanol in a volume ratio of 1:9, and then adding 3-mercaptopropyltrimethoxysilane. The mass volume ratio of the hydroxylated dielectric filler, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.4 g:10 mL. The reaction is stirred at 60° C. for 12 h. The product is separated, washed and dried to obtain the thiolated dielectric filler.

[0067] (4) A double-terminal olefinic polyphenylene ether with a number average molecular weight of 1000Da is dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then a thiolated dielectric filler is added, the mass volume ratio of the thiolated dielectric filler, the double-terminal olefinic polyphenylene ether and the mixed solvent is 1g:1g:20mL, stirred and ultrasonically dispersed for 20min, and then a catalyst benzoin dimethyl ether is added, the mass ratio of benzoin dimethyl ether to the thiolated dielectric filler is 0.01:1, stirred evenly, reacted under ultraviolet light for 40min, and the product was separated, washed and dried to obtain a modified dielectric filler.

[0068] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0069] (6) The modified dielectric filler was added to the PEI solution, with the mass ratio of the modified dielectric filler to the PEI resin being 40:100, and the mixture was stirred for 30 minutes, and then ultrasonicated at a power of 1800 W for 20 minutes to obtain a uniform composite solution.

[0070] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0071] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0072] Example 5 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0073] (2) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.1 to a hydrogen peroxide solution with a concentration of 30 wt %, and the ratio of the total mass of the nano-barium titanate and the boron nitride nanosheets to the volume of the hydrogen peroxide solution is 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 100° C. for 3 h. The product is separated, washed, and dried to obtain a hydroxylated dielectric filler.

[0074] (3) Ultrasonic dispersion of the hydroxylated dielectric filler in a mixed solvent of water and ethanol in a volume ratio of 1:9, and then adding 3-mercaptopropyltrimethoxysilane. The mass volume ratio of the hydroxylated dielectric filler, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.4 g:10 mL. The reaction is stirred at 60° C. for 12 h. The product is separated, washed and dried to obtain the thiolated dielectric filler.

[0075] (4) A double-terminal olefinic polyphenylene ether with a number average molecular weight of 1000Da is dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then a thiolated dielectric filler is added, the mass volume ratio of the thiolated dielectric filler, the double-terminal olefinic polyphenylene ether and the mixed solvent is 1g:1g:20mL, stirred and ultrasonically dispersed for 20min, and then a catalyst benzoin dimethyl ether is added, the mass ratio of benzoin dimethyl ether to the thiolated dielectric filler is 0.01:1, stirred evenly, reacted under ultraviolet light for 40min, and the product was separated, washed and dried to obtain a modified dielectric filler.

[0076] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0077] (6) The modified dielectric filler was added to the PEI solution, with the mass ratio of the modified dielectric filler to the PEI resin being 50:100, and the mixture was stirred for 30 min, and then ultrasonicated at a power of 1800 W for 20 min to obtain a uniform composite solution.

[0078] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0079] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0080] Comparative Example 1 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) PEI resin was added to N-methylpyrrolidone, heated to 60° C. and stirred until completely dissolved, to obtain a PEI solution with a mass concentration of 20%.

[0081] (2) The PEI solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The PEI film was obtained by scraping. The glass substrate with the PEI film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven for drying at 220°C for 4 h.

[0082] (3) The glass substrate with the PEI film was taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the PEI film was peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0083] Comparative Example 2 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0084] (2) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0085] (3) Add nano-barium titanate (purchased from McLean Company, particle size 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.1 to the PEI solution, and the total mass ratio of nano-barium titanate and boron nitride nanosheets to the mass ratio of PEI is 10:100. Stir for 30 minutes, and then ultrasonicate at a power of 1800 W for 20 minutes to obtain a uniform composite solution.

[0086] (4) The composite solution is evenly dropped onto the glass substrate using a dropper, and the scraper height is adjusted to 50 μm. The composite film is scraped to obtain a uniform composite film. The glass substrate with the composite film is first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0087] (5) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0088] Comparative Example 3 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) to a 30 wt% hydrogen peroxide solution, with the mass volume ratio of nano-barium titanate to hydrogen peroxide solution being 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 100° C. for 3 h. The product is separated, washed, and dried to obtain hydroxylated nano-barium titanate.

[0089] (2) Ultrasonic dispersion of hydroxylated nano-barium titanate in a mixed solvent of water and ethanol in a volume ratio of 1:9, and then adding 3-mercaptopropyltrimethoxysilane, the mass volume ratio of hydroxylated nano-barium titanate, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.4 g:10 mL, stirring the reaction at 60° C. for 12 h, separating, washing and drying the product to obtain thiolated nano-barium titanate.

[0090] (3) A double-terminal olefinic polyphenylene ether with a number average molecular weight of 1000Da was dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then thiolated nano-barium titanate was added, the mass volume ratio of thiolated nano-barium titanate, double-terminal olefinic polyphenylene ether and mixed solvent was 1g:1g:20mL, stirred and ultrasonically dispersed for 20min, and then catalyst benzoin dimethyl ether was added, the mass ratio of benzoin dimethyl ether to thiolated nano-barium titanate was 0.01:1, stirred evenly, reacted under ultraviolet light for 40min, and the product was separated, washed and dried to obtain modified nano-barium titanate.

[0091] (4) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0092] (5) Add the modified nano-barium titanate to the PEI solution, with the mass ratio of the modified nano-barium titanate to the PEI resin being 10:100, stir for 30 minutes, and then ultrasonicate for 20 minutes at a power of 1800 W to obtain a uniform composite solution.

[0093] (6) The composite solution is evenly dropped onto the glass substrate using a dropper, and the scraper height is adjusted to 50 μm. The composite film is scraped to obtain a uniform composite film. The glass substrate with the composite film is first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0094] (7) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0095] Comparative Example 4 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0096] (1) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) to a 30 wt% hydrogen peroxide solution, with the mass volume ratio of nano-barium titanate to hydrogen peroxide solution being 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 100° C. for 3 h. The product is separated, washed, and dried to obtain hydroxylated nano-barium titanate.

[0097] (2) Ultrasonic dispersion of hydroxylated nano-barium titanate in a mixed solvent of water and ethanol in a volume ratio of 1:9, and then adding 3-mercaptopropyltrimethoxysilane, the mass volume ratio of hydroxylated nano-barium titanate, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.4 g:10 mL, stirring the reaction at 60° C. for 12 h, separating, washing and drying the product to obtain thiolated nano-barium titanate.

[0098] (3) A double-terminal olefinic polyphenylene ether with a number average molecular weight of 1000Da was dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then thiolated nano-barium titanate was added, the mass volume ratio of thiolated nano-barium titanate, double-terminal olefinic polyphenylene ether and mixed solvent was 1g:1g:20mL, stirred and ultrasonically dispersed for 20min, and then catalyst benzoin dimethyl ether was added, the mass ratio of benzoin dimethyl ether to thiolated nano-barium titanate was 0.01:1, stirred evenly, reacted under ultraviolet light for 40min, and the product was separated, washed and dried to obtain modified nano-barium titanate.

[0099] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0100] (6) Adding the modified nano-barium titanate and boron nitride nanosheets into the PEI solution, the mass ratio of nano-barium titanate to boron nitride nanosheets is 1:0.1, and the mass ratio of modified nano-barium titanate to PEI resin is 10:100, stirring for 30 minutes, and then ultrasonicating at a power of 1800 W for 20 minutes to obtain a uniform composite solution.

[0101] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0102] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0103] Comparative Example 5 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0104] (2) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.33 to a hydrogen peroxide solution with a concentration of 30 wt %, and the ratio of the total mass of the nano-barium titanate and the boron nitride nanosheets to the volume of the hydrogen peroxide solution is 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 100° C. for 3 h. The product is separated, washed, and dried to obtain a hydroxylated dielectric filler.

[0105] (3) Ultrasonic dispersion of the hydroxylated dielectric filler in a mixed solvent of water and ethanol in a volume ratio of 1:9, and then adding 3-mercaptopropyltrimethoxysilane. The mass volume ratio of the hydroxylated dielectric filler, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.4 g:10 mL. The reaction is stirred at 60° C. for 12 h. The product is separated, washed and dried to obtain the thiolated dielectric filler.

[0106] (4) A biolefinic polyphenylene ether with a number average molecular weight of 1000Da was dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then a thiolated dielectric filler was added, the mass volume ratio of the thiolated dielectric filler, the biolefinic polyphenylene ether and the mixed solvent was 1g:1g:20mL, stirred and ultrasonically dispersed for 20min, and then a catalyst benzoin dimethyl ether was added, the mass ratio of benzoin dimethyl ether to the thiolated dielectric filler was 0.01:1, stirred evenly, and reacted under ultraviolet light for 40min, and the product was separated, washed and dried to obtain a modified dielectric filler.

[0107] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0108] (6) The modified dielectric filler was added to the PEI solution, with the mass ratio of the modified dielectric filler to the PEI resin being 10:100, and the mixture was stirred for 30 min, and then ultrasonicated at a power of 1800 W for 20 min to obtain a uniform composite solution.

[0109] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0110] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0111] Comparative Example 6 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0112] (2) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.1 to a hydrogen peroxide solution with a concentration of 30 wt %, and the ratio of the total mass of the nano-barium titanate and the boron nitride nanosheets to the volume of the hydrogen peroxide solution is 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 100° C. for 3 h. The product is separated, washed, and dried to obtain a hydroxylated dielectric filler.

[0113] (3) Ultrasonic dispersion of the hydroxylated dielectric filler in a mixed solvent of water and ethanol in a volume ratio of 1:9, and then adding 3-mercaptopropyltrimethoxysilane. The mass volume ratio of the hydroxylated dielectric filler, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.4 g:10 mL. The reaction is stirred at 60° C. for 12 h. The product is separated, washed and dried to obtain the thiolated dielectric filler.

[0114] (4) A double-terminal olefinic polyphenylene ether with a number average molecular weight of 500 Da was dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then a thiolated dielectric filler was added, the mass volume ratio of the thiolated dielectric filler, the double-terminal olefinic polyphenylene ether and the mixed solvent was 1g:1g:20mL, stirred and ultrasonically dispersed for 20 minutes, and then a catalyst benzoin dimethyl ether was added, the mass ratio of benzoin dimethyl ether to the thiolated dielectric filler was 0.01:1, stirred evenly, and reacted under ultraviolet light for 40 minutes. The product was separated, washed and dried to obtain a modified dielectric filler.

[0115] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0116] (6) The modified dielectric filler was added to the PEI solution, with the mass ratio of the modified dielectric filler to the PEI resin being 10:100, and the mixture was stirred for 30 min, and then ultrasonicated at a power of 1800 W for 20 min to obtain a uniform composite solution.

[0117] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0118] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0119] Comparative Example 7 A method for preparing a polyetherimide-based dielectric film comprises the following steps: (1) Hexagonal boron nitride (h-BN) is added to a mixed solvent of deionized water and ethanol in a volume ratio of 1:1, stirred at high speed for 30 minutes, and then passed into a micron channel of a high-pressure homogenizer for circulation 50 times. After standing, the upper clear layer is separated, filtered, and dried to obtain boron nitride nanosheets with a thickness of 5 to 20 nm and a width of 100 to 400 nm.

[0120] (2) Add nano-barium titanate (purchased from McLean Company, with a particle size of 30-500 nm) and boron nitride nanosheets in a mass ratio of 1:0.1 to a hydrogen peroxide solution with a concentration of 30 wt %, and the ratio of the total mass of the nano-barium titanate and the boron nitride nanosheets to the volume of the hydrogen peroxide solution is 1 g:50 mL. After ultrasonic dispersion, the mixture is refluxed at 100° C. for 3 h. The product is separated, washed, and dried to obtain a hydroxylated dielectric filler.

[0121] (3) Ultrasonic dispersion of the hydroxylated dielectric filler in a mixed solvent of water and ethanol in a volume ratio of 1:9, and then adding 3-mercaptopropyltrimethoxysilane. The mass volume ratio of the hydroxylated dielectric filler, 3-mercaptopropyltrimethoxysilane and the mixed solvent is 1 g:0.4 g:10 mL. The reaction is stirred at 60° C. for 12 h. The product is separated, washed and dried to obtain the thiolated dielectric filler.

[0122] (4) A double-terminal olefinic polyphenylene ether with a number average molecular weight of 8000Da was dissolved in a mixed solvent of toluene and butanone in a volume ratio of 1:1, and then a thiolated dielectric filler was added, the mass volume ratio of the thiolated dielectric filler, the double-terminal olefinic polyphenylene ether and the mixed solvent was 1g:1g:20mL, stirred and ultrasonically dispersed for 20min, and then a catalyst benzoin dimethyl ether was added, the mass ratio of benzoin dimethyl ether to the thiolated dielectric filler was 0.01:1, stirred evenly, and reacted under ultraviolet light for 40min. The product was separated, washed and dried to obtain a modified dielectric filler.

[0123] (5) Add PEI resin to N-methylpyrrolidone, heat to 60° C. and stir until completely dissolved to obtain a PEI solution with a mass concentration of 20%.

[0124] (6) The modified dielectric filler was added to the PEI solution, with the mass ratio of the modified dielectric filler to the PEI resin being 10:100, and the mixture was stirred for 30 min, and then ultrasonicated at a power of 1800 W for 20 min to obtain a uniform composite solution.

[0125] (7) The composite solution was evenly dropped onto the glass substrate using a dropper, and the scraper height was adjusted to 50 μm. The composite film was obtained by scraping. The glass substrate with the composite film was first placed in a 50°C vacuum oven for vacuum drying for 2 h, then heated to 80°C for vacuum drying for 2 h, and then transferred to a high-temperature forced air oven at 220°C for drying for 4 h.

[0126] (8) The glass substrate with the composite film is taken out from the high-temperature forced air oven and placed in deionized water. After 10 minutes, the composite film is peeled off from the glass substrate and placed in a vacuum oven and dried under vacuum at 60° C. for 2 hours to obtain a polyetherimide-based dielectric film.

[0127] Test Case The dielectric constant and dielectric loss of the dielectric films prepared in the embodiments and comparative examples were tested, and the energy storage density was tested at a frequency of 10 KHz. The results are shown in Table 1.

[0128] Table 1 Performance test results of dielectric films From Table 1 we can see that: (1) The dielectric constant and energy storage density of the dielectric films obtained by using the method of the present invention in Examples 1 to 5 are significantly improved compared with the pure polyetherimide film in Comparative Example 1, and have lower dielectric loss.

[0129] (2) In Comparative Example 2, barium titanate and boron nitride nanosheets are directly compounded with PEI resin, and the dielectric constant of the dielectric film is reduced compared with that of Example 1, and the dielectric loss is significantly higher than that of Example 1, and the energy storage density is significantly lower than that of Example 1. This is because: coating the barium titanate and boron nitride nanosheets with polyphenylene ether can improve the dispersibility and compatibility of the barium titanate and boron nitride nanosheets in the PEI matrix, reduce interface defects and leakage current, and increase the breakdown field strength of the film at high temperature, thereby improving the dielectric properties and high-temperature energy storage performance of the film.

[0130] (3) No boron nitride nanosheets were added in Comparative Example 3, and the boron nitride nanosheets in Comparative Example 4 were directly composited with PEI resin without modification. Compared with Comparative Example 3, the dielectric properties and high-temperature energy storage performance of Comparative Example 4 were not significantly improved, while the dielectric loss of Example 1 was reduced and the energy storage density was increased. This is because: after the boron nitride nanosheets were coated with polyphenylene ether by the method of the present invention, they could effectively capture carriers in the film and suppress leakage current, thereby improving the dielectric loss and high-temperature energy storage performance of the PEI-based dielectric film.

[0131] (4) The dielectric constant of the dielectric film of Comparative Example 5 is smaller than that of Example 1. This indicates that when the proportion of boron nitride nanosheets in barium titanate and boron nitride nanosheets is too large, the dielectric constant of the PEI-based dielectric film will decrease.

[0132] (5) The dielectric properties and high-temperature energy storage properties of Comparative Examples 6 and 7 are higher than those of Comparative Example 2, but lower than those of Example 1. This indicates that when the molecular weight of the bi-terminal olefinic polyphenylene ether is too large or too small, it will have an adverse effect on the effect of the coating layer on improving the dielectric properties and high-temperature energy storage properties of the film. This is because: when its molecular weight is too small, the coating effect on the dielectric filler is poor; when its molecular weight is too large, the reaction activity is low, which will also have an adverse effect on the coating effect.

[0133] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A polyetherimide-based dielectric film, characterized in that: The invention comprises a polyetherimide matrix and a modified dielectric filler dispersed in the polyetherimide matrix; the modified dielectric filler is composed of a hydroxylated dielectric filler and a double-terminal vinyl polyphenylene ether coating layer coated on the hydroxylated dielectric filler; the hydroxylated dielectric filler and the double-terminal vinyl polyphenylene ether coating layer are covalently connected via a mercaptosilane coupling agent.

2. The polyetherimide-based dielectric film according to claim 1, characterized in that: The hydroxylated dielectric filler is formed by hydroxylating BaTiO3 and BN nanosheets in a mass ratio of 1:0.05-0.

19.

3. The polyetherimide-based dielectric film according to claim 1, characterized in that: The number average molecular weight of the double-terminal olefinic polyphenylene ether is 1000-5000 Da.

4. The polyetherimide-based dielectric film according to claim 2, characterized in that: The particle size of the BaTiO3 is 30-500nm.

5. The polyetherimide-based dielectric film according to claim 1, characterized in that: The mass ratio of the polyetherimide matrix to the modified dielectric filler is 100:5-55.

6. A method for preparing a polyetherimide-based dielectric film according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Surface hydroxylation modification of dielectric fillers to obtain hydroxylated dielectric fillers; (2) using a hydroxylated dielectric filler and a mercaptosilane coupling agent as raw materials, carrying out a hydrolysis condensation reaction between hydroxyl groups and silaneoxy groups to obtain a mercapto-containing dielectric filler; (3) using the thiolated dielectric filler and the double-terminal olefinic polyphenylene ether as raw materials, performing a click reaction between the thiol group and the olefinic group to form a double-terminal olefinic polyphenylene ether coating layer outside the thiolated dielectric filler, thereby obtaining a modified dielectric filler; (4) The modified dielectric filler and the polyetherimide resin are mixed and prepared into a film.

7. The preparation method according to claim 6, characterized in that: In step (2), the mass ratio of the hydroxylated dielectric filler to the mercaptosilane coupling agent is 1:0.5-0.7; in step (3), the mass ratio of the mercapto dielectric filler to the double-terminal olefinic polyphenylene ether is 1:0.5-1.

8. The preparation method according to claim 6, characterized in that: Step (1) specifically comprises: dispersing the dielectric filler into a H2O2 solution, reacting at 95-105°C for 2-4 hours, separating the product, and obtaining a hydroxylated dielectric filler.

9. The preparation method according to claim 6 or 7, characterized in that: Step (3) specifically comprises: dissolving the double-terminal olefinic polyphenylene ether and the click reaction catalyst into the reaction solvent II, then adding the thiol-modified dielectric filler, dispersing them uniformly, reacting them under ultraviolet light for 30 to 60 minutes, separating the product, and obtaining the modified dielectric filler.

10. The preparation method according to claim 6, characterized in that: Step (4) specifically includes: (4.1) dissolving a polyetherimide resin in an organic solvent to obtain a polyetherimide solution; (4.2) dispersing the modified dielectric filler into the polyetherimide solution to obtain a composite solution; (4.3) The composite solution is scraped onto the substrate to form a thin film, which is then dried and peeled off from the substrate.

Citation Information

Cited By

  • Modified polytetrafluoroethylene resin composition as well as preparation method and application thereof

    CN119529452A