High-temperature-resistant and high-pressure-resistant concave-convex surface flange and machining process thereof

The flange is solved at high temperature and high pressure by using alloy materials containing chromium, carbon, manganese, silicon, nickel, nitrogen and molybdenum and anticorrosion coatings of modified cerium oxide, polyaniline, aqueous epoxy resin and molybdenum disulfide composites The problems of dimensional changes and performance degradation in the environment achieve higher hardness, strength and corrosion resistance.

CN119040757APending Publication Date: 2024-11-29JIANGYIN RUNFANG MASCH MFG CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411165872.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing flanges are prone to dimensional changes and performance degradation in high temperature and high pressure environments, especially the creep of molybdenum powder and the oxidation of manganese sulfide, which affects its service life and performance.

Method used

Using alloy materials containing chromium, carbon, manganese, silicon, nickel, nitrogen and molybdenum, and using modified cerium oxide, polyaniline, aqueous epoxy resin and molybdenum disulfide composite materials in the surface coating, through smelting and surface molding The treatment process prepares a concave and convex flange that is resistant to high temperature and high pressure.

Benefits of technology

It improves the hardness, strength, toughness and corrosion resistance of the flange, enhances its tolerance to high temperature and high pressure environments, and extends its service life with anti-corrosion coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007859510000141
    Figure BDA0005007859510000141
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant and high-pressure-resistant concave-convex face flange and a machining process thereof, and relates to the technical field of flange machining. The concave-convex surface flange resistant to high temperature and high pressure comprises the following components in percentage by mass: 18.0%-20.0% of chromium, 0.65%-0.75% of carbon, 1.0%-1.50% of manganese, 0.5%-0.75% of silicon, 8.0%-10.5% of nickel, less than or equal to 0.03% of phosphorus, less than or equal to 0.02% of sulfur, 0.10%-0.16% of nitrogen, 2.0%-3.0% of molybdenum and the balance of iron. An anti-corrosion coating is arranged on the surface of the concave-convex surface flange and is prepared by mixing modified cerium oxide, polyaniline, waterborne epoxy resin and a molybdenum disulfide composite material, and the modified cerium oxide is prepared from graphene oxide and cerium oxide, so that the compactness of the coating is enhanced, and a corrosion medium is effectively prevented from permeating the coating; and the manufactured finished product flange has good corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flange processing, and in particular to a high-temperature and high-pressure resistant concave-convex flange and a processing technology thereof. Background Art

[0002] Flange, also known as flange flange or flange, is a part that connects shafts to each other. It can be used for connection between ports or between two devices.

[0003] Chinese patent CN112813358A discloses a material for flange and a preparation method thereof, wherein the raw materials include at least one of iron or copper, carbon, manganese sulfide, and molybdenum powder.

[0004] However, molybdenum powder is a rare metal powder with a high price. It will creep when used at high temperature for a long time, causing the flange size to change and affecting its performance. In addition, manganese sulfide is easily oxidized in humid air, and long-term use in a specific environment may affect the flange performance. Therefore, we propose a high temperature and high pressure resistant concave and convex flange and its processing technology. Summary of the invention

[0005] The object of the present invention is to provide a high temperature and high pressure resistant concave and convex surface flange and a processing technology thereof, so as to solve the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: A high temperature and high pressure resistant concave and convex flange, comprising the following components: in mass percentage, 18.0% to 20.0% chromium, 0.65% to 0.75% carbon, 1.0% to 1.50% manganese, 0.5% to 0.75% silicon, 8.0% to 10.5% nickel, phosphorus: ≤0.03%, sulfur: ≤0.02%, 0.10% to 0.16% nitrogen, 2.0% to 3.0% molybdenum, and the balance is iron.

[0007] In the above technical solution, chromium can form chromium compounds in steel. These compounds can improve the hardness and strength of steel, reduce the oxidation rate of steel, and make the performance of steel less susceptible to high-temperature oxidation. Chromium can also improve the grain size and grain boundary clarity of steel, making the structure of steel more uniform, thereby improving its mechanical properties. Carbon can form a solid solution structure to improve the strength of steel, and at the same time form a carbide structure to improve the hardness and wear resistance of steel. High-carbon steel has a high carbon content and has high hardness and strength. Manganese can form hard interstitial compounds to improve the strength and hardness of steel, while improving the toughness of steel, improving cold work hardening performance, effectively inhibiting the carbonization tendency of steel, and improving the heat treatment performance of steel. While improving the strength, hardness and toughness of steel, silicon can also reduce the cold brittleness tendency of steel, improve the thermal rigidity and heat resistance of steel. The appropriate silicon content can effectively reduce the oxidation rate of steel and improve the high-temperature stability of the material. Nickel can significantly improve the yield strength and tensile strength of steel, and can also improve the plasticity of steel. In addition, nickel has a low chemical affinity with iron, which can reduce the potential of steel and enhance the corrosion resistance of steel. An appropriate amount of phosphorus can improve the hardness and strength of steel, but excessive phosphorus will reduce the plasticity and toughness of steel. An appropriate amount of sulfur can improve the machinability and processing performance of steel, but excessive sulfur will reduce the toughness and plasticity of steel, making it more susceptible to thermal cracking. Nitrogen can make the grain boundaries in steel thinner and form nitride phases, thereby effectively improving the hardness and toughness of steel. Nitrides have high thermal stability and can maintain a certain strength and hardness in high temperature environments. Molybdenum can improve the strength, rigidity, heat resistance and corrosion resistance of carbon steel, and can also effectively prevent intergranular corrosion and deformation of steel. Iron combines with carbon elements to form various carbides, thereby improving the hardness, strength and wear resistance of steel. The combination of carbon content and alloy elements improves the hardness and strength of the steel, making the steel's performance less susceptible to high-temperature oxidation. It can also increase the steel's yield strength and tensile strength, making the flange material have high strength, plasticity and thermomechanical properties, and the flange has good resistance to high temperature and high pressure.

[0008] Furthermore, the surface of the concave and convex flange is provided with an anti-corrosion coating.

[0009] A processing technology for high temperature and high pressure resistant concave and convex flanges comprises the following steps:

[0010] The steel is melted and formed to obtain a flange rough product, an anti-corrosion coating is applied to the surface-treated flange rough product, and after drying and curing, a high-temperature and high-pressure resistant concave and convex surface flange is obtained.

[0011] Further, the drying temperature is 70-80°C and the time is 15-20 minutes;

[0012] The curing temperature is 115-125°C and the curing time is 3.5-5 minutes.

[0013] Further, the smelting and forming process is as follows:

[0014] The steel is smelted, poured into a concave and convex flange casting mold after melting, kept warm for 40 to 50 minutes, demolded and slowly cooled in a pit, and taken out of the furnace after 45 to 50 hours to obtain a rough flange product.

[0015] Further, the melting temperature is 1490-1540°C;

[0016] The flange casting mold is preheated to 290-310°C and the pouring temperature is 1490-1510°C.

[0017] Furthermore, the process conditions for slow cooling in the pit are as follows:

[0018] The slow cooling time is 36 to 48 hours, and the exit temperature is 150 to 200°C.

[0019] Further, the specific process of surface treatment is as follows:

[0020] Soak the rough flange product in the rust remover for 1 to 2 hours, wash the rust-removed flange with clean water, then perform ultrasonic washing, and then dry to obtain the surface-treated flange.

[0021] Furthermore, the ultrasonic washing frequency is 20 to 30 Hz, and the time is 0.5 to 1 h.

[0022] Furthermore, the rust remover model: XS-533, comes from Shanghai Xinsheng Chemical New Materials Co., Ltd.

[0023] Furthermore, the anti-corrosion coating is made by mixing modified cerium oxide, polyaniline, water-based epoxy resin, and molybdenum disulfide composite material, and the specific process is as follows:

[0024] The modified cerium oxide, polyaniline, waterborne epoxy resin and molybdenum disulfide composite material are mixed and deionized water is added. After stirring for 0.8 to 1.2 hours, a curing agent is added, stirring is continued for 20 to 30 minutes, and the mixture is allowed to stand until there are no bubbles to obtain an anti-corrosion coating.

[0025] Furthermore, the mass ratio of modified cerium oxide, polyaniline, water-based epoxy resin, molybdenum disulfide composite material, curing agent, and deionized water is (0.1-0.5):2:2:(1-3):1:(0.6-1).

[0026] Further, polyaniline CAS number: 5612-44-2, from Hubei Longxin Chemical Industry Co., Ltd.;

[0027] Waterborne epoxy resin CAS number: 38891-59-7, viscosity: 500-3000mpa·s, from Guangzhou Tanhua Materials Co., Ltd.;

[0028] The curing agent is 2,4,6-tris(dimethylaminomethyl)phenol, CAS number: 90-72-2, amine value: 600-630 mgkOH / g, derived from Xindian Chemistry.

[0029] Furthermore, the modified cerium oxide is prepared from graphene oxide and cerium oxide, and the specific process is as follows:

[0030] Graphene oxide, cerium oxide and citric acid are mixed, placed on a magnetic stirrer for heating and stirring to obtain a mixture, the mixture is placed in a drying oven for drying, and then calcined in a muffle furnace to obtain modified cerium oxide.

[0031] Furthermore, the mass ratio of graphene oxide, cerium oxide and citric acid is (1-5):(1-4):20.

[0032] Furthermore, citric acid is added in the form of an aqueous solution with a solution concentration of 0.6 mol / L; CAS number of citric acid: 77-92-9, sourced from Suzhou Renpin Chemical Technology Co., Ltd.

[0033] Furthermore, graphene oxide has a thickness of 0.55 to 1.2 nm, a diameter of 0.5 to 3 μm, item number: 102740, and is sourced from Beijing Dekedaojin Technology Co., Ltd.;

[0034] The particle size of cerium oxide is 15 μm, which comes from Zibo Rongruida Powder Material Factory.

[0035] Furthermore, the stirring temperature is 160-200°C and the stirring time is 80-100 min;

[0036] The drying oven temperature is 90-100°C and the drying time is 20-24 hours;

[0037] The calcination temperature is 480-500°C and the time is 0.8-1h.

[0038] In the above technical solution, cerium oxide has a corrosion inhibition effect on metals, but it is easy to agglomerate and has low density. Adding graphene oxide can improve the dispersion stability and compatibility of cerium oxide particles while further enhancing the density of the coating and preventing the penetration of corrosive media into the coating. Polyaniline has a passivating effect on metals and can delay corrosion. Polyaniline forms a stronger chemical interface with water-based epoxy resin, which improves the barrier performance of the coating.

[0039] Furthermore, the molybdenum disulfide composite material is composed of molybdenum disulfide and graphene, and the specific process is as follows:

[0040] The graphene was mixed with deionized water, and ultrasonically treated for 1.5 to 2 hours. Ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide were then added to obtain a mixed solution, and ultrasonically treated for 0.5 to 1 hour. The mixed solution was stirred during the ultrasonic process, and the pH value was adjusted to 0.5 to 1 with concentrated hydrochloric acid. The mixed solution was transferred to a reactor and heated in an oven. The solution after the reaction was centrifuged and then washed with deionized water for 3 times to obtain a precursor solution. The precursor solution was placed in a low-temperature refrigerator for pre-freezing treatment. After completion, it was placed in a vacuum freeze dryer for treatment to obtain a molybdenum disulfide composite material.

[0041] Furthermore, the mass ratio of graphene, deionized water, ammonium molybdate tetrahydrate, thiourea, and hexadecyltrimethylammonium bromide is (0.03-0.05):(10-16):(0.5-1):(1-3):(0.02-0.05).

[0042] Further, the oven temperature is 200-240°C, and the heating time is 20-24h;

[0043] The temperature of the low-temperature refrigerator is -10 to -20°C, and the pre-freezing time is 10 to 15 hours;

[0044] The temperature of the vacuum freeze dryer is -50 to -60°C and the time is 8 to 12 hours.

[0045] Further, graphene CAS number: 7440-44-0, thickness 1-6 nm, sourced from Jiangsu Xianfeng Nanomaterials Co., Ltd.;

[0046] Ammonium molybdate tetrahydrate CAS number: 12054-85-2, from Guangdong Wengjiang Chemical Reagent Co., Ltd.;

[0047] Thiourea CAS number: 62-56-6, from Qingzhou Jinhui Chemical Plant;

[0048] Hexadecyltrimethylammonium bromide CAS number: 57-09-0, from Hubei Yamade Biopharmaceutical Co., Ltd.

[0049] Concentrated hydrochloric acid CAS number: 7647-01-0, from Merck reagent.

[0050] In the above technical scheme, molybdenum disulfide is prone to agglomeration, and the dispersion stability in the coating is reduced. In addition, the large number of dangling bonds on the surface of molybdenum disulfide makes it easy to oxidize during friction and high-temperature environment. Graphene is loaded on molybdenum disulfide by freeze-drying, which improves the dispersion stability of molybdenum disulfide and helps prevent molybdenum disulfide from oxidizing during friction, so that the prepared composite material has better wear reduction and anti-wear properties.

[0051] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0052] 1. Cerium oxide itself has a corrosion inhibition effect on metals, but it is easy to agglomerate, has low density, and has poor dispersibility and compatibility in epoxy resin. Adding graphene oxide can improve the dispersion stability and compatibility of cerium oxide particles, enhance the density of the coating, and prevent the penetration of corrosive media into the coating. Polyaniline itself has a passivating effect on metals and can delay corrosion. The addition of water-based epoxy resin forms a stronger chemical interface and improves the barrier performance of the coating.

[0053] 2. Loading graphene on molybdenum disulfide by freeze-drying can improve the dispersion stability of molybdenum disulfide, improve the disadvantage of easy agglomeration of molybdenum disulfide, and prevent molybdenum disulfide from oxidizing in high temperature environment and friction process, so that the prepared composite material has better wear reduction and anti-wear properties, and further improves its lubrication performance. DETAILED DESCRIPTION

[0054] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0055] In the following specific implementations,

[0056] Rust remover model: XS-533, from Shanghai Xinsheng Chemical New Materials Co., Ltd.;

[0057] Polyaniline CAS number: 5612-44-2, from Hubei Longxin Chemical Industry Co., Ltd.;

[0058] Waterborne epoxy resin CAS number: 38891-59-7, viscosity: 500-3000mpa·s, from Guangzhou Tanhua Materials Co., Ltd.;

[0059] The curing agent is 2,4,6-tris(dimethylaminomethyl)phenol, CAS number: 90-72-2, amine value: 600-630mgkOH / g, from Xindian Chemical;

[0060] Graphene oxide thickness 0.55 ~ 1.2nm, diameter 0.5 ~ 3μm, item number: 102740, from Beijing Dekedaojin Technology Co., Ltd.;

[0061] The particle size of cerium oxide is 15 μm, which comes from Zibo Rongruida Powder Material Factory;

[0062] Graphene CAS number: 7440-44-0, thickness 1-6nm, from Jiangsu Xianfeng Nanomaterials Co., Ltd.;

[0063] Ammonium molybdate tetrahydrate CAS number: 12054-85-2, from Guangdong Wengjiang Chemical Reagent Co., Ltd.;

[0064] Thiourea CAS number: 62-56-6, from Qingzhou Jinhui Chemical Plant;

[0065] Hexadecyltrimethylammonium bromide CAS number: 57-09-0, from Hubei Yamade Biopharmaceutical Co., Ltd.

[0066] Concentrated hydrochloric acid CAS number: 7647-01-0, from Merck reagent;

[0067] Embodiment 1: A high temperature and high pressure resistant concave and convex flange and a processing technology thereof, comprising the following processes:

[0068] Step (1) Preparation of flange crude product:

[0069] The steel is melted at a melting temperature of 1490°C, and after melting, it is poured into a concave and convex flange mold preheated to 290°C, and the pouring temperature is 1490°C. After keeping warm for 40 minutes, the steel is demolded and slowly cooled in a pit, and then taken out of the furnace after 45 hours to obtain a rough flange product; the slow cooling time is 36 to 48 hours, and the temperature out of the pit is 150 to 200°C; the rough flange product includes the following components: in terms of mass percentage, 18.0% chromium, 0.65% carbon, 1.0% manganese, 0.5% silicon, 8.0% nickel, 0.01% phosphorus, 0.01% sulfur, 0.10% nitrogen, 2.0% molybdenum, and the balance is iron.

[0070] Step (2) Preparation of anti-corrosion coating:

[0071] Graphene oxide, cerium oxide and citric acid were mixed, placed on a magnetic stirrer, heated to 160° C. and stirred for 80 min to obtain a mixture, the mixture was placed in a drying oven at 90° C. for 20 h, and calcined in a muffle furnace at 480° C. for 0.8 h to obtain modified cerium oxide;

[0072] The graphene was mixed with deionized water, and ultrasonically treated for 1.5 hours. Then, ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide were added to obtain a mixed solution, and ultrasonically treated for 0.5 hours. The mixed solution was stirred during the ultrasonic process, and the pH was adjusted to 0.5 with concentrated hydrochloric acid. The mixed solution was transferred to a reactor and heated in an oven at 200°C for 20 hours. The solution after the reaction was centrifuged and then washed with deionized water for 3 times to obtain a precursor solution. The precursor solution was placed in a low-temperature refrigerator at -10°C for pre-freezing treatment for 10 hours. After completion, it was placed in a -50°C vacuum freeze dryer for treatment for 8 hours to obtain a molybdenum disulfide composite material. The mass ratio of graphene, deionized water, ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide was 0.03:10:0.5:1:0.02.

[0073] The modified cerium oxide, polyaniline, water-based epoxy resin, and molybdenum disulfide composite material were mixed and deionized water was added, and after stirring for 0.8 hours, a curing agent was added, and the mixture was stirred for 20 minutes and allowed to stand until there were no bubbles, thereby obtaining an anti-corrosion coating; the mass ratio of the modified cerium oxide, polyaniline, water-based epoxy resin, molybdenum disulfide composite material, curing agent, and deionized water was 0.1:2:2:1:1:0.6;

[0074] Step (3) Preparation of finished flange:

[0075] The rough flange product is placed in the rust remover and soaked for 1 hour. The rust-removed flange is cleaned with clean water, then ultrasonically washed, and then dried to obtain the surface-treated flange; the ultrasonic washing frequency is 20 Hz and the time is 0.5 h;

[0076] The anti-corrosion coating is applied to the surface treated flange, and the finished flange is obtained after drying and curing; the drying temperature is 70°C and the time is 15 minutes; the curing temperature is 115°C and the time is 3.5 minutes.

[0077] Embodiment 2: A high temperature and high pressure resistant concave and convex flange and a processing technology thereof, comprising the following processes:

[0078] Step (1) Preparation of flange crude product:

[0079] The steel is melted at a melting temperature of 1520°C, and after melting, it is poured into a concave and convex flange mold preheated to 300°C, with a pouring temperature of 1500°C. After keeping warm for 45 minutes, it is demolded and put into a pit for slow cooling, and taken out of the furnace after 48 hours to obtain a flange rough product; the slow cooling time is 36 to 48 hours, and the pit exit temperature is 150 to 200°C; the flange rough product includes the following components: by mass percentage, 19.0% chromium, 0.70% carbon, 1.3% manganese, 0.6% silicon, 9.0% nickel, 0.02% phosphorus, 0.02% sulfur, 0.13% nitrogen, 2.5% molybdenum, and the balance is iron.

[0080] Step (2) Preparation of anti-corrosion coating:

[0081] Graphene oxide, cerium oxide and citric acid were mixed, placed on a magnetic stirrer, heated to 180°C and stirred for 90 minutes to obtain a mixture, the mixture was placed in a drying oven at 95°C for 22 hours, and calcined in a muffle furnace at 490°C for 0.9 hours to obtain modified cerium oxide;

[0082] The graphene was mixed with deionized water, and ultrasonically treated for 1.8 hours. Then, ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide were added to obtain a mixed solution, and ultrasonically treated for 0.8 hours. The mixed solution was stirred during the ultrasonic process, and the pH was adjusted to 0.7 with concentrated hydrochloric acid. The mixed solution was transferred to a reactor and heated in an oven at 220°C for 22 hours. The solution after the reaction was centrifuged and then washed with deionized water for 3 times to obtain a precursor solution. The precursor solution was placed in a low-temperature refrigerator at -15°C for pre-freezing treatment for 13 hours. After completion, it was placed in a -55°C vacuum freeze dryer for treatment for 10 hours to obtain a molybdenum disulfide composite material; the mass ratio of graphene, deionized water, ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide was 0.04:13:0.8:2:0.04;

[0083] The modified cerium oxide, polyaniline, water-based epoxy resin, and molybdenum disulfide composite material were mixed and deionized water was added, and after stirring for 1 hour, a curing agent was added, and the stirring was continued for 25 minutes, and the mixture was allowed to stand until there were no bubbles, thereby obtaining an anti-corrosion coating; the mass ratio of the modified cerium oxide, polyaniline, water-based epoxy resin, molybdenum disulfide composite material, curing agent, and deionized water was 0.3:2:2:2:1:0.8;

[0084] Step (3) Preparation of finished flange:

[0085] The rough flange product is placed in the rust remover and soaked for 1.5 hours. The rust-removed flange is cleaned with clean water, then ultrasonically washed, and then dried to obtain the surface-treated flange; the ultrasonic washing frequency is 25 Hz, and the time is 0.8 hours;

[0086] The anti-corrosion coating is applied to the surface treated flange, and the finished flange is obtained after drying and curing; the drying temperature is 75°C and the time is 17 minutes; the curing temperature is 120°C and the time is 4 minutes.

[0087] Embodiment 3: A high temperature and high pressure resistant concave and convex flange and a processing technology thereof, comprising the following processes:

[0088] Step (1) Preparation of flange crude product:

[0089] The steel is melted at a melting temperature of 1540°C, and after melting, it is poured into a concave and convex flange casting mold preheated to 310°C, with a pouring temperature of 1510°C. After keeping warm for 50 minutes, it is demolded and slowly cooled in a pit, and then taken out of the furnace after 50 hours to obtain a rough flange product; the slow cooling time is 36 to 48 hours, and the pit exit temperature is 150 to 200°C; the rough flange product includes the following components: in terms of mass percentage, 20.0% chromium, 0.75% carbon, 1.50% manganese, 0.75% silicon, 10.5% nickel, 0.03% phosphorus, 0.02% sulfur, 0.16% nitrogen, 3.0% molybdenum, and the balance is iron.

[0090] Step (2) Preparation of anti-corrosion coating:

[0091] Graphene oxide, cerium oxide and citric acid were mixed, placed on a magnetic stirrer, heated to 200°C and stirred for 100 minutes to obtain a mixture, the mixture was placed in a drying oven at 100°C for 24 hours, and calcined in a muffle furnace at 500°C for 1 hour to obtain modified cerium oxide;

[0092] The graphene was mixed with deionized water, and ultrasonically treated for 2 hours. Then, ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide were added to obtain a mixed solution, and ultrasonically treated for 1 hour. The mixed solution was stirred during the ultrasonic process, and the pH was adjusted to 1 with concentrated hydrochloric acid. The mixed solution was transferred to a reactor and heated in an oven at 240°C for 24 hours. The solution after the reaction was centrifuged and then washed with deionized water for 3 times to obtain a precursor solution. The precursor solution was placed in a low-temperature refrigerator at -20°C for pre-freezing treatment for 15 hours. After completion, it was placed in a -60°C vacuum freeze dryer for treatment for 12 hours to obtain a molybdenum disulfide composite material. The mass ratio of graphene, deionized water, ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide was 0.05:16:1:3:0.05.

[0093] The modified cerium oxide, polyaniline, water-based epoxy resin, and molybdenum disulfide composite material were mixed and deionized water was added, and after stirring for 1.2 hours, a curing agent was added, and the stirring was continued for 30 minutes, and the mixture was allowed to stand until there were no bubbles, thereby obtaining an anti-corrosion coating; the mass ratio of the modified cerium oxide, polyaniline, water-based epoxy resin, molybdenum disulfide composite material, curing agent, and deionized water was 0.5:2:2:3:1:1;

[0094] Step (3) Preparation of finished flange:

[0095] The rough flange product is placed in the rust remover and soaked for 2 hours. The rust-removed flange is cleaned with clean water, then ultrasonically washed, and then dried to obtain the surface-treated flange; the ultrasonic washing frequency is 30 Hz and the time is 1 hour;

[0096] The anti-corrosion coating is applied to the surface treated flange, and after drying and curing, a finished flange is obtained; the drying temperature is 80°C and the time is 20 minutes; the curing temperature is 125°C and the time is 5 minutes.

[0097] Comparative Example 1: Taking Example 1 as a control, the molybdenum disulfide composite material is replaced with ordinary molybdenum powder, a high temperature and high pressure resistant concave and convex flange and a processing technology thereof, including the following processes:

[0098] Step (1) Preparation of flange crude product: the same as in Example 1;

[0099] Step (2) Preparation of anti-corrosion coating:

[0100] Graphene oxide, cerium oxide and citric acid were mixed, placed on a magnetic stirrer, heated to 160° C. and stirred for 80 min to obtain a mixture, the mixture was placed in a drying oven at 90° C. for 20 h, and calcined in a muffle furnace at 480° C. for 0.8 h to obtain modified cerium oxide;

[0101] The modified cerium oxide, polyaniline, water-based epoxy resin and molybdenum powder were mixed and deionized water was added, and after stirring for 0.8 hours, a curing agent was added, and the mixture was stirred for 20 minutes and allowed to stand until there were no bubbles to obtain an anti-corrosion coating; the mass ratio of the modified cerium oxide, polyaniline, water-based epoxy resin, molybdenum powder, curing agent and deionized water was 0.1:2:2:1:1:0.6;

[0102] Step (3) Preparation of finished flange: Same as in Example 1.

[0103] Comparative Example 2: Taking Example 1 as a control, no modified cerium oxide is added to the anti-corrosion coating, a high temperature and high pressure resistant concave and convex flange and a processing technology thereof, including the following processes:

[0104] Step (1) Preparation of flange crude product: the same as in Example 1;

[0105] Step (2) Preparation of anti-corrosion coating:

[0106] The graphene was mixed with deionized water, and ultrasonically treated for 1.5 hours. Then, ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide were added to obtain a mixed solution, and ultrasonically treated for 0.5 hours. The mixed solution was stirred during the ultrasonic process, and the pH was adjusted to 0.5 with concentrated hydrochloric acid. The mixed solution was transferred to a reactor and heated in an oven at 200°C for 20 hours. The solution after the reaction was centrifuged and then washed with deionized water for 3 times to obtain a precursor solution. The precursor solution was placed in a low-temperature refrigerator at -10°C for pre-freezing treatment for 10 hours. After completion, it was placed in a -50°C vacuum freeze dryer for treatment for 8 hours to obtain a molybdenum disulfide composite material. The mass ratio of graphene, deionized water, ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide was 0.03:10:0.5:1:0.02.

[0107] The polyaniline, waterborne epoxy resin and molybdenum disulfide composite material were mixed and deionized water was added, and after stirring for 0.8 hours, a curing agent was added, and the stirring was continued for 20 minutes, and the mixture was allowed to stand until there were no bubbles, thereby obtaining an anti-corrosion coating; the mass ratio of polyaniline, waterborne epoxy resin, molybdenum disulfide composite material, curing agent and deionized water was 2:2:1:1:0.6;

[0108] Step (3) Preparation of finished flange: Same as in Example 1.

[0109] Comparative Example 3: Using Example 1 as a control, without using an anti-corrosion coating, a high-temperature and high-pressure resistant concave-convex flange and a processing technology thereof include the following processes:

[0110] Step (1) Preparation of flange crude product: the same as in Example 1;

[0111] Step (2) Preparation of finished flange:

[0112] The rough flange product is soaked in the rust remover for 1 hour, the rust-removed flange is cleaned with clean water, then ultrasonically washed, and then dried to obtain the finished flange; the ultrasonic washing frequency is 20 Hz and the time is 0.5 h.

[0113] experiment:

[0114] The flanges obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were taken to prepare samples, and their performances were tested and the test results were recorded:

[0115] Tensile strength test: using the tensile test bar method, tensile test bars were pressed with the corresponding formulations in the embodiments and comparative examples, and the mechanical properties were tested;

[0116] Hardness test at high temperature: The steel materials in the above embodiments and comparative examples were selected to make specimens with a thickness of 4 mm and a size of 200 mm×200 mm, and the specimens were placed in a high temperature hardness tester at 600°C for hardness test;

[0117] High-pressure fracture toughness test: The fracture toughness test was carried out in a high-pressure hydrogen atmosphere at a pressure of 115 MPa and a constant displacement speed of 2.5 μm / min.

[0118] Corrosion resistance test: The corrosion resistance of the sample was detected by polarization test sample method. The neutral corrosion environment was 3.5% NaCl solution. The reference electrode was saturated calomel electrode, the auxiliary electrode was platinum electrode, the potential scanning rate was 1mV / s, and the self-corrosion potential was selected to characterize the corrosion resistance of the sample.

[0119]

[0120] According to the data in the above table, we can clearly draw the following conclusions:

[0121] The flanges obtained in Examples 1-3 are compared with the flanges obtained in Comparative Examples 1-3. The test results show that:

[0122] Compared with Comparative Example 1, the flanges obtained in Examples 1 to 3 have better tensile strength, stronger high temperature resistant hardness, better toughness and stronger corrosion resistance, which fully demonstrates that in the present invention, the selected steel and the anti-corrosion coating set can improve the tensile strength, high temperature and high pressure resistance, and corrosion resistance of the manufactured flanges.

[0123] Compared with Example 1, in Comparative Example 1, the molybdenum disulfide composite material is replaced by ordinary molybdenum powder, which is easy to agglomerate and affect the product quality; in Comparative Example 2, cerium oxide is not added to the anti-corrosion coating, which reduces the protective effect of the anti-corrosion coating on the metal, reduces the density of the coating, and makes it easier for the corrosive medium to penetrate the coating; in Comparative Example 3, no anti-corrosion coating is used, and without coating protection, the tensile strength of the flange decreases, the wear volume increases, and the self-corrosion potential decreases; it can be seen that the setting of the process and the materials used in this application can promote the improvement of the tensile strength, high temperature and high pressure resistance and corrosion resistance of the manufactured flange.

[0124] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A high temperature and high pressure resistant concave and convex flange, characterized in that: The invention comprises the following mass components: by mass percentage, 18.0% to 20.0% chromium, 0.65% to 0.75% carbon, 1.0% to 1.50% manganese, 0.5% to 0.75% silicon, 8.0% to 10.5% nickel, phosphorus: ≤0.03%, sulfur: ≤0.02%, 0.10% to 0.16% nitrogen, 2.0% to 3.0% molybdenum, and the balance is iron; The surface of the concave-convex flange is provided with an anti-corrosion coating.

2. A high temperature and high pressure resistant concave and convex flange according to claim 1, characterized in that: The anti-corrosion coating is prepared by mixing modified cerium oxide, polyaniline, waterborne epoxy resin and molybdenum disulfide composite material.

3. The high temperature and high pressure resistant concave and convex flange according to claim 2, characterized in that: The modified cerium oxide is prepared from graphene oxide and cerium oxide.

4. The high temperature and high pressure resistant concave and convex flange according to claim 2, characterized in that: The molybdenum disulfide composite material consists of molybdenum disulfide and graphene.

5. A processing technology for high temperature and high pressure resistant concave and convex flanges, characterized in that: Including the following processes: The steel is melted and formed to obtain a flange rough product, an anti-corrosion coating is applied to the surface-treated flange rough product, and after drying and curing, a high-temperature and high-pressure resistant concave and convex flange is obtained.

6. The processing technology of the high temperature and high pressure resistant concave and convex flange according to claim 5 is characterized in that: The anti-corrosion coating is prepared by the following process: The modified cerium oxide, polyaniline, waterborne epoxy resin and molybdenum disulfide composite material are mixed and deionized water is added. After stirring for 0.8 to 1.2 hours, a curing agent is added, stirring is continued for 20 to 30 minutes, and the mixture is allowed to stand until there are no bubbles to obtain an anti-corrosion coating.

7. The processing technology of the high temperature and high pressure resistant concave and convex flange according to claim 6 is characterized in that: The modified cerium oxide is prepared by the following process: Graphene oxide, cerium oxide and citric acid are mixed, placed on a magnetic stirrer for heating and stirring to obtain a mixture, the mixture is placed in a drying oven for drying, and then calcined in a muffle furnace to obtain modified cerium oxide.

8. The processing technology of the high temperature and high pressure resistant concave and convex flange according to claim 6 is characterized in that: The molybdenum disulfide composite material is prepared by the following process: The graphene was mixed with deionized water, and ultrasonically treated for 1.5 to 2 hours. Ammonium molybdate tetrahydrate, thiourea and hexadecyltrimethylammonium bromide were then added to obtain a mixed solution, and ultrasonically treated for 0.5 to 1 hour. The mixed solution was stirred during the ultrasonic process, and the pH value was adjusted to 0.5 to 1 with concentrated hydrochloric acid. The mixed solution was transferred to a reactor and heated in an oven. The solution after the reaction was centrifuged and then washed with deionized water for 3 times to obtain a precursor solution. The precursor solution was placed in a low-temperature refrigerator for pre-freezing treatment. After completion, it was placed in a vacuum freeze dryer for treatment to obtain a molybdenum disulfide composite material.

9. The processing technology of the high temperature and high pressure resistant concave and convex flange according to claim 5, characterized in that: The process of melting and forming is as follows: The steel is smelted, poured into a concave and convex flange casting mold after melting, kept warm for 40 to 50 minutes, demolded and slowly cooled in a pit, and taken out of the furnace after 45 to 50 hours to obtain a rough flange product.

10. The processing technology of the high temperature and high pressure resistant concave and convex flange according to claim 5, characterized in that: The drying temperature is 70-80°C and the time is 15-20 minutes; the curing temperature is 115-125°C and the time is 3.5-5 minutes.

Citation Information

Cited By

  • High-strength alloy steel plate and processing technology thereof

    CN120210647A

  • High-strength alloy steel plate material and processing technology thereof

    CN120210647B