Medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristic as well as preparation method and application of medium-carbon low-alloy semi-hard magnetic steel

Through medium-carbon low alloying design and specific heat treatment technology, the medium-carbon low alloy semi-hard magnetic steel produced has excellent mechanical and magnetic properties at room temperature, which solves the difficulty of existing semi-hard magnetic alloys to have both coercivity. , the problems of high residual magnetic induction strength and high mechanical properties have achieved higher residual magnetic properties and impact mechanical properties.

CN119040768APending Publication Date: 2024-11-29ADVANCED TECHNOLOGY & MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411061714.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing semi-hard magnetic alloys are difficult to have both suitable coercive forces, high residual magnetic induction strength and high mechanical properties, and cannot meet actual needs.

Method used

Adopt medium-carbon low alloying design, including chemical components Mn: 0.3% to 1.5%, Cr: 0.5% to 1.0%, Mo: 0.1% to 0.3%, Ni: 0.5% to 2.0%, C: 0.25% to 0.60% , Si: 0.20%~0.50%, P: < 0.010%, S: < 0.010%, O: < 0.0015%, the balance is Fe and inevitable impurities, and smelting through converter, electric furnace or vacuum induction furnace, and refining outside the furnace , forging, air-cooling treatment and specific heat treatment processes to produce medium-carbon low-alloy semi-hard magnetic steel with high residual magnetic characteristics.

Benefits of technology

At room temperature, medium-carbon low-alloy semi-hard magnets have excellent mechanical properties and magnetic properties, with yield strength Rp0.2 greater than 800MPa, tensile strength Rm greater than 900MPa, magnetic induction strength B8000 greater than 1.70T, and residual magnetic induction strength Br8000 greater than 1.40T The coercive force Hc8000 is 1100~1400A/m, filling the gap in performance of existing semi-hard magnetic alloys in China.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040768A_ABST
    Figure CN119040768A_ABST
Patent Text Reader

Abstract

The invention discloses medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristic and a preparation method and application thereof, and belongs to the technical field of semi-hard magnetic alloys, and the medium-carbon low-alloy semi-hard magnetic steel comprises the following chemical components in percentage by mass: 0.3%-1.5% of Mn, 0.5%-1.0% of Cr, 0.1%-0.3% of Mo, 0.5%-2.0% of Ni, 0.25%-0.60% of C, 0.20%-0.50% of Si, less than 0.010% of P, less than 0.010% of S, less than 0.0015% of O, less than 0.008% of N and the balance of Fe and inevitable impurities. Meanwhile, in the preparation process of the semi-hard magnetic steel, after heat treatment of quenching and tempering, a tempered totsonite structure can be obtained, so that the prepared medium-carbon low-alloy semi-hard magnetic steel has proper coercive force and excellent mechanical property on the basis of achieving high residual magnetic induction intensity, and is suitable for being used as a material for manufacturing an iron core of a magnetic control mechanism.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of semi-hard magnetic alloys, and in particular relates to a medium-carbon low-alloy semi-hard magnetic steel with high remanence properties and a preparation method and application thereof. Background Art

[0002] The electromagnetic conversion linear motion vacuum circuit breaker control mechanism has the advantages of few parts, simple and reliable structure, small size and controllable motion process. It is widely used in synchronous drive devices of vacuum circuit breaker electrical equipment and other automatic systems for power transmission. Semi-hard magnetic alloy is often used in the production of iron core of bistable vacuum circuit breaker control mechanism. Its characteristics are that the iron core is driven to attract by low-power excitation pulse current to complete the closing action. After excitation, the high remanence characteristics of the semi-hard magnetic alloy keep the closing state. After the reverse low-power current is passed, the iron core is demagnetized, and the opening process is completed under the action of the built-in spring elastic force.

[0003] The iron core made of semi-hard magnetic alloy is used repeatedly during service, so it must have excellent mechanical properties to resist repeated attraction and collision, high remanence characteristics to maintain the stability of the attraction state, and appropriate coercivity to resist the interference of external magnetic fields in the service environment. However, excessive coercivity will also put forward higher requirements for driving electrical equipment. Common semi-hard magnetic alloys in China mainly include Fe-Co-Ni-V series, Fe-Co-V series, Fe-Co-Mo series, and Fe-Mn-Ni-Mo series semi-hard magnetic alloys specified in "GB / T 14988-2008 Hysteresis Alloys". The coercivity is much greater than 1000A / m and the residual magnetic induction intensity is required to be less than 1.40T, which is difficult to meet actual needs.

[0004] Therefore, in order to solve the above problems, it is necessary for the present invention to provide a medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics and a preparation method thereof. The present invention reduces the manufacturing cost and improves the mechanical properties of the semi-hard magnetic steel through low alloying design, and combines a specific heat treatment method to obtain the semi-hard magnetic steel. The semi-hard magnetic steel obtained by the present invention has excellent mechanical properties. At room temperature, its yield strength Rp 0.2 Greater than 800MPa, tensile strength R m Greater than 900MPa, elongation A>10%, while taking into account excellent magnetic properties, among which the magnetic induction intensity B 8000 Greater than 1.70T, residual magnetic induction intensity Br 8000 Greater than 1.40T, and appropriate coercivity Hc 8000 It is 1100~1400A / m, filling the performance gap of existing semi-hard magnetic alloys in China. Summary of the invention

[0005] The main purpose of the present invention is to provide a medium-carbon low-alloy semi-hard magnetic steel with high remanent magnetic properties and its preparation method and application, so as to solve the problem that existing semi-hard magnetic alloys are difficult to simultaneously have suitable coercive force, high residual magnetic induction intensity and high mechanical properties.

[0006] In order to achieve the above-mentioned purpose, the present invention provides a medium-carbon low-alloy semi-hard magnetic steel with high remanence properties, which includes the following chemical components in percentage by mass: Mn: 0.3%~1.5%, Cr: 0.5%~1.0%, Mo: 0.1%~0.3%, Ni: 0.5%~2.0%, C: 0.25%~0.60%, Si: 0.20%~0.50%, P: <0.010%, S: <0.010%, O: <0.0015%, N: <0.008%, and the balance is Fe and unavoidable impurities.

[0007] Furthermore, the medium carbon low alloy semi-hard magnetic steel has the following combination of magnetic properties and mechanical properties at room temperature: 8000 Greater than 1.7T, Br 8000 Greater than 1.4T, remanence ratio greater than 0.8, coercivity Hc 8000 1100~1400A / m, yield strength Rp 0.2 Greater than 800MPa, tensile strength R m Greater than 900MPa, elongation A>10%.

[0008] Another aspect of the present invention provides a method for preparing medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics, comprising the following steps:

[0009] The semi-hard magnetic steel raw materials of the formula amount are smelted in a converter, an electric furnace or a vacuum induction furnace;

[0010] The smelted material is refined outside the furnace, and after refining, continuous casting or mold casting is performed to obtain a casting billet;

[0011] The ingot is forged after being opened, and then air-cooled;

[0012] The air-cooled forging material is heat-treated to obtain the medium-carbon low-alloy semi-hard magnetic steel with high remanence properties.

[0013] Furthermore, the heat treatment includes: first quenching the forging material in a quenching medium to obtain a martensitic structure, and then performing a tempering treatment to obtain the medium-carbon low-alloy semi-hard magnetic steel with high remanence properties and a tempered troostite structure.

[0014] Furthermore, the quenching temperature is 750-900° C., and the heating and insulation time is 30-300 min.

[0015] Furthermore, the temperature of the tempering treatment is 300-600° C., and the heating and heat preservation time is 30-300 min.

[0016] Furthermore, the quenching medium is one or more of water, water mist or oil; and the tempering treatment is air-cooled after tempering.

[0017] Another aspect of the present invention provides an application of the above-mentioned medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics in the material for the core of a magnetron mechanism.

[0018] The functions and proportions of the elements of the present invention are as follows:

[0019] Carbon: One of the most important strengthening elements. Too high a carbon content will significantly reduce the plasticity and toughness of semi-hard magnetic steel. The high carbon embrittlement effect is not conducive to the impact resistance of semi-hard magnetic steel during repeated absorption and collision. Too low a carbon content will lack the solid solution strengthening and precipitation strengthening effects brought by carbon atoms. The decrease in hardness and rigidity will cause the material to deform easily during the absorption and collision process, resulting in material failure. Therefore, the present invention controls the C content to 0.25-0.60%.

[0020] Chromium: Adding appropriate Cr to the steel of the present invention can not only significantly improve the hardenability of the steel, but also improve the uniformity of the structure, improve the oxidation resistance and corrosion resistance of the steel, and the carbide of chromium will increase the coercive force of the steel. However, excessive Cr is easy to form carbides such as Cr7C3, which reduces the plasticity and toughness of the steel. Therefore, the Cr content of the present invention is controlled to be 0.5% to 1.0%.

[0021] Manganese: It is one of the main deoxidizing elements in steel. It improves the strength of steel through solid solution strengthening, significantly improves the hardenability of steel, and reduces quenching cracking and deformation of semi-hard magnetic steel. Too high Mn is not conducive to the magnetic properties of semi-hard magnetic steel. Therefore, the present invention controls the Mn content to 0.3% to 1.5%.

[0022] Molybdenum: improves the tempering stability of steel. When Mo, Cr and Mn coexist, it inhibits the temper brittleness caused by Cr and Mn. Therefore, the Mo content in the present invention is controlled to be Mo: 0.1% to 0.3%.

[0023] Nickel: Improves the hardening performance of steel, reduces the diffusion rate of various elements in steel, improves hardenability, and is the most effective alloy element for improving the toughness of steel. It combines the alloy cost and its synergy with other alloy elements in terms of toughness and hardenability. At the same time, Ni can optimize the stability of magnetic properties. Therefore, the content of Ni in the present invention is controlled to be: Ni: 0.5% to 2.0%.

[0024] Silicon: has a significant solid solution strengthening effect, but at the same time it will damage toughness, play a deoxidation role, reduce magnetic resistance and crystal anisotropy. Therefore, the content of Si in the present invention is controlled to be: Si: 0.20% to 0.50%.

[0025] Nitrogen: It often forms second phase particles with microalloying elements such as Nb, V, and Ti to strengthen the matrix. This article does not involve the addition of microalloying elements. Therefore, the control range of N element is N: <0.008%.

[0026] Phosphorus: In the steel of the present invention, P is controlled as an impurity element, and the content thereof is P<0.010%.

[0027] Sulfur: In the steel of the present invention, S is controlled as an impurity element, and the content of S is S<0.010%.

[0028] Oxygen: has formed inclusions. The present invention controls O as an impurity element with a content of O<0.015%.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The invention provides a medium carbon low alloy semi-hard magnetic steel with high remanence characteristics and a preparation method thereof. In terms of chemical composition, a low alloying design with medium carbon and total alloy element content less than 5% by mass is adopted, and the price is low.

[0031] The medium-carbon low-alloy semi-hard magnetic steel of the present invention can obtain a tempered troostite structure after appropriate heat treatment, and has excellent mechanical properties and residual magnetic properties required for the service state of the iron core of the magnetron mechanism. Compared with the common Fe-Co-Ni-V series, Fe-Co-V series, Fe-Co-Mo series, and Fe-Mn-Ni-Mo series semi-hard magnetic alloys, it has better impact resistance mechanical properties and higher residual magnetic properties. The residual magnetic induction intensity Br of the steel of the present invention is 8000 >1.40T.

[0032] The steel coercivity of the carbon low alloy semi-hard magnetic steel of the present invention is lower than that of the common semi-hard magnetic alloy. 8000 The current is 1100-1400A / m, and the saturation magnetization process and demagnetization process can be completed under low-power pulse current excitation, with fast response speed. It is more friendly to the control of electrical equipment and has promotion potential in other fields of automatic control systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is an optical microstructure photograph of the medium-carbon low-alloy semi-hard magnetic steel after quenching heat treatment during the preparation process of Example 2 of the present invention;

[0034] Figure 2 This is an optical microstructure photograph of the medium-carbon low-alloy semi-hard magnetic steel after tempering heat treatment during the preparation process of Example 2 of the present invention. DETAILED DESCRIPTION

[0035] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0036] An embodiment of the present invention provides a medium-carbon low-alloy semi-hard magnetic steel with high remanence properties, which includes the following chemical components in percentage by mass: Mn: 0.3% to 1.5%, Cr: 0.5% to 1.0%, Mo: 0.1% to 0.3%, Ni: 0.5% to 2.0%, C: 0.25% to 0.60%, Si: 0.20% to 0.50%, P: <0.010%, S: <0.010%, O: <0.0015%, N: <0.008%, and the remainder is Fe and unavoidable impurities.

[0037] The chemical composition of the high remanence medium-carbon low-alloy semi-hard magnetic steel involved in the present invention comprises Mn, Cr, Mo, Ni, C, Si, P, S, O and N, and the remainder is Fe and inevitable impurities.

[0038] The role of alloying elements and the basis for alloy design are as follows:

[0039] C: Taking into account the mechanical properties and magnetic properties of the material, the steel of the present invention adopts a medium carbon design, and the C content of the steel of the present invention is controlled in the range of 0.25-0.60%.

[0040] Cr: It improves the hardenability of steel and improves the uniformity of the structure. However, excessive Cr will form chromium carbides, which is not conducive to the plasticity and toughness of the steel. At the same time, excessive Cr will affect the magnetic properties of the material. The Cr content of the steel of the present invention is controlled in the range of 0.5-1.0%.

[0041] Mn: plays a deoxidizing role and significantly improves the hardenability of steel. Like Cr, excessive Mn will affect the magnetic properties of the material. The Mn content of the steel of the present invention is controlled within the range of 0.3-1.5%.

[0042] Mo: Mo can improve the tempering stability of steel. When Mo coexists with Cr and Mn elements, it can inhibit the tempering brittleness caused by Cr and Mn. The Mo content of the steel of the present invention is controlled within the range of 0.1% to 0.3%.

[0043] Ni: Considering the alloy cost and its synergy with other elements in terms of strength, toughness and hardenability, the Ni content of the steel of the present invention is controlled in the range of 0.5-2.0%.

[0044] N: <0.008%, N often forms a second phase particle-reinforced matrix with microalloying elements such as Nb, V, and Ti. This article does not involve the addition of microalloying elements.

[0045] Preferably, P, S and O are used as impurity elements, and the impurity element contents in the steel of the present invention are controlled to be P < 0.010%, S < 0.010%, and O < 0.0015%.

[0046] The present invention specially designs the alloy element ratio, and the total alloy element content is less than 5%. Based on the synergistic effect between the alloy elements of Mn, Cr, Mo, Ni and the elements of C and Si, the medium-carbon low-alloy semi-hard magnetic steel of the present invention has excellent magnetic properties, mechanical properties and suitable coercive force. The medium-carbon low-alloy semi-hard magnetic steel of the present invention has the following magnetic properties and mechanical properties at room temperature: Room temperature B 8000 Greater than 1.7T, Br 8000 Greater than 1.4T, remanence ratio greater than 0.8, coercivity Hc 8000 1100~1400A / m, yield strength Rp 0.2 Greater than 800MPa, tensile strength R m Greater than 900MPa, elongation A>10%.

[0047] The embodiment of the present invention further provides a method for preparing the aforementioned medium carbon low alloy semi-hard magnetic steel with high remanence properties, comprising the following steps:

[0048] The semi-hard magnetic steel raw materials of the formula amount are smelted in a converter, an electric furnace or a vacuum induction furnace;

[0049] The smelted material is refined outside the furnace, and after refining, continuous casting or mold casting is performed to obtain a casting billet;

[0050] The ingot is forged after being opened, and then air-cooled;

[0051] The air-cooled forging material is heat-treated to obtain the medium-carbon low-alloy semi-hard magnetic steel with high remanence properties.

[0052] In order to further improve the magnetic properties and mechanical properties of the steel of the present invention, in a preferred embodiment of the present invention, the heat treatment includes: first quenching the forging material in a quenching medium to obtain a martensitic structure, and then tempering it to obtain a medium-carbon low-alloy semi-hard magnetic steel with high remanence properties of a tempered troostite structure.

[0053] The present invention obtains medium-carbon low-alloy semi-hard magnetic steel with tempered troostite structure through the above-mentioned heat treatment process. The tempered troostite structure is a characteristic structure corresponding to the high remanence property of semi-hard magnetic steel. Only this structure can have high remanence, high remanence ratio and excellent mechanical properties. Changes in the structure type under other heat treatment processes will deteriorate its magnetic properties.

[0054] In a preferred embodiment of the present invention, the quenching temperature is 750-900°C, and the heating and heat preservation time is 30-300min. The quenching temperature can be, for example, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C. The heating and heat preservation time can be, for example, 30min, 40min, 50min, 60min, 80min, 100min, 120min, 140min, 150min, 160min, 180min, 200min, 210min, 220min, 240min, 250min, 260min, 280min, 300min.

[0055] The present invention selects a quenching temperature of 750-900°C for austenitization, the purpose of which is to eliminate the uneven structure in the forging process, while dissolving the second phase particles in the semi-hard magnetic steel and homogenizing the alloy elements. The quenching medium can be used for rapid cooling, and the martensitic structure can be obtained through the above treatment.

[0056] In a preferred embodiment of the present invention, the temperature of the tempering treatment is 300-600°C, and the heating and heat preservation time is 30-300min. The tempering temperature can be, for example, 300°C, 320°C, 340°C, 350°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C, 600°C. The heating and heat preservation time can be, for example, 30min, 40min, 50min, 60min, 80min, 100min, 120min, 140min, 150min, 160min, 180min, 200min, 210min, 220min, 240min, 250min, 260min, 280min, 300min.

[0057] The present invention controls the tempering temperature within the above range, so that the high remanent magnetic properties of the medium-carbon low-alloy semi-hard magnetic steel can be converted into a tempered troostite structure. If the tempering temperature is lower than 300°C, the martensite cannot be converted into tempered troostite. If it is higher than 600°C, the carbides in the tempered troostite coarsen to form granular pearlite. Only by tempering within the above temperature range can the semi-hard magnetic steel with the highest remanent magnetic properties and remanent magnetic ratio be obtained.

[0058] In a preferred embodiment of the present invention, the quenching medium is one or more of water, water mist or oil; and in the tempering treatment, air cooling is performed after tempering.

[0059] An embodiment of the present invention also provides an application of the aforementioned medium-carbon low-alloy semi-hard magnetic steel with high remanence properties in the material for the core of a magnetron mechanism.

[0060] The medium-carbon low-alloy semi-hard magnetic steel of the present invention is particularly suitable as a material for the iron core of a magnetron mechanism. The medium-carbon low-alloy semi-hard magnetic steel of the present invention has excellent mechanical properties, can resist repeated attraction and collision of the magnetron mechanism, has high residual magnetic properties, can maintain the stability of the attraction state of the magnetron mechanism, has suitable coercive force, can resist the interference of the external magnetic field in the service environment, and has a fast response speed to complete the saturation magnetization process and the demagnetization process, and is more friendly to the requirements for controlling electrical equipment.

[0061] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0062] Three specific embodiments are given below, and the chemical compositions are shown in Table 1.

[0063] Table 1 Chemical composition of carbon low alloy semi-hard magnetic steel (mass percentage %)

[0064]

[0065]

[0066] The processing techniques used for the chemical composition raw materials in the above embodiments are all the same: they are all prepared by the steps of smelting in a vacuum induction furnace → refining outside the furnace followed by continuous casting or die casting → blanking and forging → heat treatment.

[0067] During the heat treatment process, quenching heat treatment is first performed, the quenching medium is selected as water mist, the quenching temperature is selected as 850±10℃ for austenitization, the temperature is kept for 1 to 5 hours, and the martensite structure is obtained by rapid cooling. The structure photo of Example 2 after quenching is shown in Figure 1 As shown. Then, the tempering heat treatment is carried out, the tempering temperature is 500±10℃, and the temperature is kept for 1 to 2 hours. After tempering, it is air-cooled to room temperature. The high remanence structure finally obtained is the tempered troostite structure. The structure photo after tempering in Example 2 is shown as follows Figure 2 shown.

[0068] The present invention can directly process the forging material into a finished iron core device blank for heat treatment, directly process the test sample into a test product, and the device blank after heat treatment can be assembled and used after grinding, surface treatment and other processes.

[0069] The magnetic properties and mechanical properties of the medium carbon low alloy semi-hard magnetic steel prepared by the above process are shown in Table 2. The room temperature magnetic induction intensity B 8000 Greater than 1.70T, residual magnetic induction intensity Br 8000 Greater than 1.40T, coercivity Hc8000 The maximum value is 1100-1400A / m, the yield strength is greater than 800MPa, the yield strength is greater than 900MPa, and the elongation is greater than 10%.

[0070] Table 2 Magnetic properties and mechanical properties of medium carbon low alloy semi-hard magnetic steel The above-described embodiments only represent the embodiments of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. The present invention can also be implemented in other specific ways or other specific forms without departing from the gist or essential features of the present invention. Therefore, the described embodiments should be regarded as illustrative rather than restrictive in any respect. The scope of the present invention should be described by the attached claims, and any changes equivalent to the intention and scope of the claims should also be included in the scope of the present invention.

Claims

1. A medium carbon low alloy semi-hard magnetic steel with high remanence characteristics, It is characterized in that Calculated by mass percentage, it includes the following chemical components: Mn: 0.3%-1.5%, Cr: 0.5%-1.0%, Mo: 0.1%-0.3%, Ni: 0.5%-2.0%, C: 0.25%-0.60%, Si: 0.20%-0.50%, P: <0.010%, S: <0.010%, O: <0.0015%, N: <0.008%, and the balance is Fe and unavoidable impurities.

2. The medium carbon low alloy semi-hard magnetic steel with high remanence characteristics according to claim 1, It is characterized in that The medium carbon low alloy semi-hard magnetic steel has the following combination of magnetic properties and mechanical properties at room temperature: 8000 Greater than 1.7T, Br 8000 Greater than 1.4T, remanence ratio greater than 0.8, coercivity Hc 8000 1100~1400A / m, yield strength Rp 0.2 Greater than 800MPa, tensile strength R m Greater than 900MPa, elongation A>10%.

3. A method for preparing a medium-carbon low-alloy semi-hard magnetic steel with high remanence properties as described in any one of claims 1 to 2, It is characterized in that The steps include: The semi-hard magnetic steel raw materials of the formula amount are smelted in a converter, an electric furnace or a vacuum induction furnace; The smelted material is refined outside the furnace, and after refining, continuous casting or mold casting is performed to obtain a casting billet; The ingot is forged after being opened, and then air-cooled; The air-cooled forging material is heat-treated to obtain the medium-carbon low-alloy semi-hard magnetic steel with high remanence properties.

4. The method for preparing the medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics according to claim 3, It is characterized in that The heat treatment comprises: first quenching the forging material in a quenching medium to obtain a martensitic structure, and then performing a tempering treatment to obtain the medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics and a tempered troostite structure.

5. The method for preparing the medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics according to claim 4, It is characterized in that The quenching temperature is 750-900° C., and the heating and heat preservation time is 30-300 minutes.

6. The method for preparing the medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics according to claim 4, It is characterized in that The temperature of the tempering treatment is 300-600° C., and the heating and heat preservation time is 30-300 minutes.

7. The method for preparing the medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics according to claim 4, It is characterized in that The quenching medium is one or more of water, water mist or oil; in the tempering treatment, air cooling is performed after tempering.

8. Use of the medium-carbon low-alloy semi-hard magnetic steel with high remanence characteristics as claimed in any one of claims 1 to 2 in the material for the core of a magnetron mechanism.