High-strength steel surface hydrogen-resistant coating and preparation method thereof
Through the close combination of Al, Cr and Zr amorphous coatings and high-strength steel substrates, magnetron sputtering technology is used to build an efficient hydrogen resistance coating, which solves the problems of hydrogen embrittlement and insufficient coating performance, and achieves high-efficiency hydrogen resistance Improvement of performance and mechanical properties.
Patent Information
- Application Number
- CN202411174319.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
High-strength steel materials are prone to hydrogen embrittlement in hydrogen environment, resulting in a decrease in mechanical strength and elongation, limiting their application in the field of hydrogen energy. The existing hydrogen-resistance coating materials are prone to cracks at high temperatures, the preparation process is complex and costly. High, difficult to meet performance requirements.
Using an amorphous structure coating composed of three elements: Al, Cr and Zr, the chemical composition and microstructure are accurately controlled through magnetron sputtering technology, to build a tortuous hydrogen diffusion path and high hydrogen diffusion barrier, and optimize the coating and high-strength steel matrix. The combination of the application needs is adapted to different application needs.
It effectively prevents hydrogen penetration, improves the mechanical properties and reliability of the material, ensures that the coating is closely integrated with the surface of high-strength steel, greatly broadens the scope of application and processability, and avoids the problems of hydrogen diffusion channels and lattice distortion.
Smart Images

Figure CN119040838A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal material surface modification, and particularly relates to a high-strength steel surface hydrogen barrier coating and a preparation method thereof. Background Art
[0002] With the transformation of the global energy structure and the demand for sustainable development, hydrogen energy, as a clean and efficient energy carrier, is increasingly being used in a variety of fields. In particular, in key facilities such as hydrogen fuel vehicles, hydrogen refueling stations, and future nuclear power plants, high-strength steel materials are widely used as structural materials due to their excellent mechanical properties. However, the application in a hydrogen environment poses severe challenges to high-strength steel materials. Hydrogen atoms, as the smallest atoms in nature, can easily penetrate into the lattice structure of metal materials, and even at extremely low concentrations, they can cause severe hydrogen embrittlement. This hydrogen embrittlement phenomenon can cause a significant decrease in the mechanical strength and elongation of the material, increase the risk of structural failure, and limit the application and development of high-strength steel materials in the field of hydrogen energy.
[0003] Traditional solutions usually focus on the selection and design of materials to improve their inherent resistance to hydrogen embrittlement. However, these methods often fail to meet the growing performance requirements. In order to effectively prevent the penetration and diffusion of hydrogen, researchers have begun to explore methods of applying hydrogen barrier coatings on the surface of high-strength steel. As a surface modification technology, hydrogen barrier coatings aim to reduce hydrogen penetration and improve the safety and reliability of materials by forming a protective layer with low hydrogen permeability on the surface of the material.
[0004] Although a variety of hydrogen barrier coating materials and preparation technologies have been proposed, such as metal and alloy coatings, oxide coatings, aluminide coatings, etc., they still face some challenges in practical applications. For example, some coating materials may not match the thermal expansion coefficient of the substrate material, causing the coating to easily crack and fall off at high temperatures; the preparation process of some coatings is complex and costly, making it difficult to achieve industrial production; and some coatings, although having good hydrogen barrier properties, may sacrifice other properties of the material, such as toughness, corrosion resistance or bending properties. Summary of the invention
[0005] In view of the deficiencies in the above-mentioned prior art, the present invention provides a high-strength steel surface hydrogen barrier coating and a preparation method thereof. The coating utilizes the difference in binding energy between the three elements Al, Cr, and Zr and hydrogen to construct a coating structure with a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier. Through magnetron sputtering technology, the chemical composition and microstructure of the coating can be precisely controlled to achieve close bonding between the coating and the high-strength steel substrate and excellent hydrogen barrier properties. In addition, the present invention also optimizes the preparation process of the coating to adapt to different application requirements and improve the actual application effect of the coating.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] In one aspect, the present invention provides a hydrogen barrier coating on the surface of a high-strength steel, wherein the hardness of the high-strength steel is HV300-HV600, the tensile strength is 900-1200 MPa, and the thermal expansion coefficient can be up to (8-20)×10 -6 / K, and an elastic modulus between 100-200 GPa; the hydrogen barrier coating is composed of three elements, Al, Cr, and Zr, and the molar ratio of each element is not less than 30%; the hydrogen barrier coating is an amorphous structure.
[0008] Furthermore, the thickness of the hydrogen barrier coating is 100-200 μm.
[0009] On the other hand, the present invention provides a method for preparing the above-mentioned hydrogen barrier coating, comprising: selecting high-strength steel and a target material, and pretreating the surface of the high-strength steel to be coated; and coating the surface to be coated by magnetron sputtering.
[0010] Furthermore, the target material includes an AlCr target and a Zr target.
[0011] Furthermore, the pretreatment includes: using 400# to 5000# SiC sandpaper to polish the surface of the high-strength steel to be coated step by step until there are no voids and large scratches on the surface, and then mirror polishing with diamond polishing paste. The surface roughness of the prepared product is less than 0.16μm. Finally, the sample is soaked and cleaned with deionized water, anhydrous ethanol and acetone in an ultrasonic cleaner for 10-30 minutes and then dried.
[0012] Furthermore, the magnetron sputtering process includes vacuuming, bias cleaning and coating; the vacuum degree after vacuuming is not greater than 2.0×10 -3 Pa.
[0013] Furthermore, the bias cleaning process is as follows: the substrate is heated at a preparation temperature of 180-220°C, and the vacuum degree in the chamber is not greater than 1.8×10 -3 When 0.04 Pa, the stop valve was opened, the limiting valve parameter was set to 100°, the argon flow rate was set to 30 sccm, and the voltage was set to -900 V to keep the pressure in the chamber above 1.0 Pa for bias cleaning.
[0014] Furthermore, the coating process includes primary deposition and secondary deposition; the primary deposition is: the argon flow rate is set to 30sccm, the AlCr target power is 140-160W, the Zr target power is 90-110W, the chamber working pressure is 0.4-0.6Pa, the substrate rotation speed is 9-11r / min, the deposition temperature is 180-220°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100V, and the deposition is performed for 10-15min; the secondary deposition is: the Zr target power is adjusted to 140-160W, the chamber working pressure is 0.9-1.1Pa, and then the deposition is performed for 10-20min.
[0015] Furthermore, in the first deposition, the power ratio of the AlCr target to the Zr target is 3:2; in the second deposition, the power ratio of the AlCr target to the Zr target is 1:1.
[0016] Compared with the prior art, the technical solution provided by the present invention brings the following beneficial effects:
[0017] (1) The three elements Al, Cr and Zr used in the present invention have significant differences in their binding energies with hydrogen. This difference is the basis for constructing a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier, which is crucial for slowing down the diffusion rate of hydrogen in the material. The AlCrZr coating with an amorphous structure lacks grain boundaries, thereby reducing the rapid diffusion channel of hydrogen and further improving the hydrogen barrier efficiency of the coating. Compared with a single metal coating, the AlCrZr coating not only improves the density and cohesion of the coating through the synergistic effect of multiple elements, but also enhances the coating's ability to adsorb and capture hydrogen, thereby performing better in inhibiting hydrogen penetration. The high entropy alloy coating in the prior art has problems such as complex interactions between elements, difficult-to-control lattice distortion and the unpredictable hydrogen diffusion behavior caused by its multi-element composition. The AlCrZr medium entropy alloy coating optimizes the interactions between elements and reduces adverse lattice distortion through a carefully designed element composition, thereby providing a more stable hydrogen diffusion path.
[0018] (2) With respect to the high-strength steel of the prior art, the high-strength steel has the following physical properties: hardness of HV300-HV600, tensile strength of 900-1200 MPa, and thermal expansion coefficient of up to (8-20)×10 -6 / K, due to the high mechanical performance indicators, it is difficult to directly plate the coating through the technical solutions disclosed in the prior art, and in order to meet the subsequent processing requirements, a certain degree of processing is required after the coating is plated. The hydrogen barrier coating prepared by the technical solution of the present application can meet the requirement that when the thickness of the high-strength steel is within 5mm, the minimum bending radius is 2cm, and no cracks will be generated between the coating and the surface of the high-strength steel, which greatly broadens the scope of application and machinability of subsequent products. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 This is a SEM image of the surface morphology of the hydrogen barrier coating provided in Example 1 of the present invention, where a is the coating surface and b is the cross section;
[0021] Figure 2 XRD diagram of the hydrogen barrier coating provided in the embodiment of the present invention;
[0022] Figure 3 This is a hydrogen permeation curve of the hydrogen barrier coating provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. The specific implementation of the present invention is not limited to the specific embodiments given here, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the disclosed specific embodiments.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and do not limit the present invention.
[0025] The embodiment of the present invention provides a hydrogen barrier coating on the surface of a high-strength steel, wherein the hardness of the high-strength steel is HV300-HV600, the tensile strength is 900-1200 MPa, and the thermal expansion coefficient can be up to (8-20)×10 -6 / K, and an elastic modulus between 100-200 GPa; the hydrogen barrier coating is composed of three elements, Al, Cr, and Zr, and the molar ratio of each element is not less than 30%; the hydrogen barrier coating is an amorphous structure.
[0026] First, the three elements Al, Cr and Zr used in the present invention have significant differences in their binding energies with hydrogen. This difference is the basis for constructing a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier, which is crucial for slowing down the diffusion rate of hydrogen in the material. The AlCrZr coating with an amorphous structure lacks grain boundaries, thereby reducing the rapid diffusion channel of hydrogen and further improving the hydrogen barrier efficiency of the coating. Compared with a single metal coating, the AlCrZr coating not only improves the density and cohesion of the coating through the synergistic effect of multiple elements, but also enhances the coating's ability to adsorb and capture hydrogen, thereby performing better in inhibiting hydrogen penetration. The high entropy alloy coating in the prior art has complex interactions between elements, difficult-to-control lattice distortion, and unpredictable hydrogen diffusion behavior due to its multi-element composition, while the AlCrZr medium entropy alloy coating optimizes the interactions between elements and reduces adverse lattice distortion through a carefully designed element composition, thereby providing a more stable hydrogen diffusion path. Secondly, for the high-strength steel in the prior art, the high-strength steel has the following physical properties: hardness of HV300-HV600, tensile strength of 900-1200 MPa, and thermal expansion coefficient of up to (8-20)×10 -6 / K, due to the high mechanical performance indicators, it is difficult to directly plate the coating through the technical solutions disclosed in the prior art, and in order to meet the subsequent processing requirements, a certain degree of processing is required after the coating is plated. The hydrogen barrier coating prepared by the technical solution of the present application can meet the requirement that when the thickness of the high-strength steel is within 5mm, the minimum bending radius is 2cm, and no cracks will be generated between the coating and the surface of the high-strength steel, which greatly broadens the scope of application and machinability of subsequent products.
[0027] It should be noted that the high-strength steel in the present invention is 12Cr2Mo1R steel or 17-4PH.
[0028] Specifically, the thickness of the hydrogen barrier coating is 100-200 μm. The hydrogen barrier coating should not be too thin. Although it increases the manufacturing efficiency, the hydrogen barrier performance is weakened. It should be pointed out that there is no element transition distance between the hydrogen barrier coating and the high-strength steel substrate, which is easy to cause cracks between the coating and the high-strength steel substrate during the subsequent bending process. However, the hydrogen barrier coating should not be too thick. Too thick increases the preparation time and increases the probability of cracks on the outer surface of the coating.
[0029] The present invention also provides a method for preparing the above-mentioned hydrogen barrier coating, comprising:
[0030] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.
[0031] Specifically, for illustration, in the present invention, the high-strength steel is selected from 12Cr2Mo1R and 17-4PH, and the components of the 12Cr2Mo1R steel and their mass percentages are as follows: C: 0.14%, Si: 0.12%, Mn: 0.57%, P: 0.01%, Cr: 2.64%, Ni: 0.02%, Co: 3.67%, Nb: 0.01%, Al: 0.07%.
[0032] The components of the 17-4PH and their mass percentages are as follows: C: 0.03%, Si: 0.56%, Mn: 0.51%, P: 0.02%, Cr: 16.75%, Ni: 3.99%, Cu: 3.67%, Nb: 0.28%.
[0033] The target material is a 99.99% pure metal AlCr composite target (φ76.2×5mm 3 ) and a Zr target with a purity of 99.99% (φ76.2×5mm 3 ).
[0034] The pretreatment includes: using 400# to 5000# SiC sandpaper to grind the surface of the 12Cr2Mo1R steel to be coated step by step until there are no cavities and large scratches on the surface, and then using diamond polishing paste to perform mirror polishing. The surface roughness of the prepared product is less than 0.16μm. Finally, using an ultrasonic cleaner to soak and clean the sample with deionized water, anhydrous ethanol and acetone in turn for 10-30 minutes and then drying.
[0035] S2 uses magnetron sputtering to coat the surface to be coated.
[0036] The magnetron sputtering process includes vacuuming, bias cleaning and coating; the vacuum degree after vacuuming is not greater than 2.0×10 -3 Pa.
[0037] The bias cleaning process is as follows: setting the preparation temperature to 180-220°C to heat the substrate, and when the vacuum degree in the chamber is not greater than 1.8×10 -3 When the pressure is 0.04 Pa, open the stop valve, set the flow limit valve parameter to 100°, set the argon flow rate to 30 sccm, set the voltage to -900 V, keep the pressure in the chamber above 1.0 Pa for bias cleaning, and the cleaning time is not less than 10 minutes. Ensure that the contaminants on the substrate surface can be removed, the substrate surface can be activated, and the adhesion of the coating can be guaranteed.
[0038] The coating process includes primary deposition and secondary deposition;
[0039] The primary deposition is as follows: the argon flow rate is set to 30sccm, the AlCr target power is 140-160W, the Zr target power is 90-110W, the chamber working pressure is 0.4-0.6Pa, the substrate rotation speed is 9-11r / min, the deposition temperature is 180-220°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100V, and the deposition is 10-15min. A uniform and relatively dense coating base layer is formed, low gas pressure helps to reduce gas impurities in the coating, and moderate bias helps to improve the adhesion between the coating and the substrate, and enhances the bonding strength between the coating and the high-strength steel substrate.
[0040] The secondary deposition is as follows: adjust the Zr target power to 140-160W, make the chamber working pressure 0.9-1.1Pa, and then deposit for 10-20min. Increase the thickness of the coating to 100-200μm to achieve the required hydrogen barrier performance. Increasing the Zr target power and chamber pressure will increase the deposition rate of the Zr element in the coating. At the same time, the increased pressure helps the continuity of the coating growth and forms a thicker coating. The above process parameters ensure that the molar ratio of each element is not less than 30%.
[0041] Preferably, in the first deposition, the power ratio of the AlCr target to the Zr target is 3:2; in the second deposition, the power ratio of the AlCr target to the Zr target is 1:1.
[0042] In the embodiment of the present invention, the performance of the prepared hydrogen barrier coating is tested, including:
[0043] Penetration current density: Tested in accordance with the national standard “Determination of hydrogen permeability of metallic materials Part 1: Steady-state current method” (GB / T 35439.1-2017).
[0044] In order to further illustrate the present invention, a wide temperature range multiphase low expansion lightweight aluminum-based composite material provided by the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0045] Example 1
[0046] The embodiment of the present invention prepares a high-strength steel surface hydrogen barrier coating, and the preparation method thereof includes:
[0047] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.
[0048] 12Cr2Mo1R steel and target material are used to polish and clean the surface of the 12Cr2Mo1R steel to be coated.
[0049] S2 uses magnetron sputtering to coat the surface to be coated.
[0050] Turn on the magnetron sputtering equipment, place the substrate material on the sample stage of the substrate stage, close the chamber door and evacuate the chamber to a vacuum degree of 2.0×10 -3 Below Pa.
[0051] The bias cleaning process is as follows: 12Cr2Mo1R steel is heated and bias cleaned. The preparation temperature is set to 200°C and the 12Cr2Mo1R steel is heated. When the predetermined temperature is reached and the vacuum degree in the chamber is 1.8×10 -3 When 0.04°C / 6.08°C is reached, the stop valve is opened, the flow limiting valve parameter is set to 100° (the adjustment range is 0-1000°), the argon flow rate is set to 30 sccm, and the voltage is set to -900 V to keep the pressure in the chamber above 1.0 Pa for bias cleaning. The surface of 12Cr2Mo1R steel is first bombarded with Ar+ particles for 10 minutes to ensure that the contaminants on the surface of 12Cr2Mo1R steel can be removed, the surface of 12Cr2Mo1R steel can be activated, and the adhesion of the coating can be guaranteed.
[0052] The coating process is as follows: set the argon flow rate to 30sccm, the AlCr target power to 150W, the Zr target power to 100W, the chamber working pressure to 0.5Pa, the substrate speed to 10r / min, the deposition temperature to 200℃, adjust the bias voltage of the magnetron sputtering equipment to -100V, and deposit for 10min; then adjust the Zr target power to 150W, make the chamber working pressure 1.0Pa, and deposit for another 10min. The morphology of the prepared hydrogen barrier coating is shown in the figure below: Figure 1 As shown in a and 1b, the thickness of the prepared hydrogen barrier coating is 141 μm.
[0053] like Figure 2 , “-100V”, “-150V” and “-50V” represent the bias voltage of the magnetron sputtering equipment. It can be seen that the prepared coating is an amorphous structure; Figure 3 As shown in Figure 2, the permeation current density was measured to be 0.68 μA·cm -2 ; Through testing, when the thickness of high-strength steel is 5mm, the minimum bending radius is 2cm, and there is no crack at the interface between the hydrogen barrier coating and the 12Cr2Mo1R steel substrate.
[0054] Example 2
[0055] The embodiment of the present invention prepares a high-strength steel surface hydrogen barrier coating, and the preparation method thereof includes:
[0056] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.
[0057] 12Cr2Mo1R steel and target material are used to polish and clean the surface of the 12Cr2Mo1R steel to be coated.
[0058] S2 uses magnetron sputtering to coat the surface to be coated.
[0059] Turn on the magnetron sputtering equipment, place the substrate material on the sample stage of the substrate stage, close the chamber door and evacuate the chamber to a vacuum degree of 2.0×10 -3 Below Pa.
[0060] The bias cleaning process is as follows: 12Cr2Mo1R steel is heated and bias cleaned. The preparation temperature is set to 180°C and the 12Cr2Mo1R steel is heated. When the predetermined temperature is reached and the vacuum degree in the chamber is 1.8×10 -3 When 0.04°C / 6.08°C is reached, the stop valve is opened, the flow limiting valve parameter is set to 100° (the adjustment range is 0-1000°), the argon flow rate is set to 30 sccm, and the voltage is set to -900 V to keep the pressure in the chamber above 1.0 Pa for bias cleaning. The surface of 12Cr2Mo1R steel is first bombarded with Ar+ particles for 10 minutes to ensure that the contaminants on the surface of 12Cr2Mo1R steel can be removed, the surface of 12Cr2Mo1R steel can be activated, and the adhesion of the coating can be guaranteed.
[0061] The coating process is as follows: set the argon flow rate to 30sccm, the AlCr target power to 140W, the Zr target power to 90W, the chamber working pressure to 0.4Pa, the substrate rotation speed to 9r / min, the deposition temperature to 180°C, adjust the bias voltage of the magnetron sputtering equipment to -100V, and deposit for 10 minutes; then adjust the Zr target power to 140W, make the chamber working pressure 1.0Pa, and deposit for another 10 minutes. The thickness of the prepared hydrogen barrier coating is 101μm.
[0062] The prepared coating has an amorphous structure. The permeation current density is measured to be 0.74 μA·cm -2 ; Through mechanical property testing, when the thickness of high-strength steel is 5mm, the minimum bending radius is 2cm, and there is no crack at the interface between the hydrogen barrier coating and the 12Cr2Mo1R steel substrate.
[0063] Example 3
[0064] The embodiment of the present invention prepares a high-strength steel surface hydrogen barrier coating, and the preparation method thereof includes:
[0065] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.
[0066] 12Cr2Mo1R steel and target material are used to polish and clean the surface of the 12Cr2Mo1R steel to be coated.
[0067] S2 uses magnetron sputtering to coat the surface to be coated.
[0068] Turn on the magnetron sputtering equipment, place the substrate material on the sample stage of the substrate stage, close the chamber door and evacuate the chamber to a vacuum degree of 2.0×10 -3 Below Pa.
[0069] The bias cleaning process is as follows: 12Cr2Mo1R steel is heated and bias cleaned. The preparation temperature is set to 200°C and the 12Cr2Mo1R steel is heated. When the predetermined temperature is reached and the vacuum degree in the chamber is 1.8×10 -3 When 0.04°C / 6.08°C is reached, the stop valve is opened, the flow limiting valve parameter is set to 100° (the adjustment range is 0-1000°), the argon flow rate is set to 30 sccm, and the voltage is set to -900 V to keep the pressure in the chamber above 1.0 Pa for bias cleaning. The surface of 12Cr2Mo1R steel is first bombarded with Ar+ particles for 10 minutes to ensure that the contaminants on the surface of 12Cr2Mo1R steel can be removed, the surface of 12Cr2Mo1R steel can be activated, and the adhesion of the coating can be guaranteed.
[0070] The coating process is as follows: set the argon flow rate to 30sccm, the AlCr target power to 160W, the Zr target power to 110W, the chamber working pressure to 0.6Pa, the substrate rotation speed to 11r / min, the deposition temperature to 220°C, adjust the bias voltage of the magnetron sputtering equipment to -100V, and deposit for 15min; then adjust the Zr target power to 160W, make the chamber working pressure to 1.1Pa, and deposit for another 20min. The thickness of the prepared hydrogen barrier coating is 198μm.
[0071] The prepared coating has an amorphous structure. The permeation current density is measured to be 0.87 μA·cm -2 ; Through testing, when the thickness of high-strength steel is 5mm, the minimum bending radius is 2cm, and there is no crack at the interface between the hydrogen barrier coating and the 12Cr2Mo1R steel substrate.
[0072] Example 4
[0073] The embodiment of the present invention prepares a high-strength steel surface hydrogen barrier coating, and the preparation method thereof includes:
[0074] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.
[0075] Using 17-4PH steel and target material, the surface of 17-4PH steel to be coated is polished and cleaned.
[0076] S2 uses magnetron sputtering to coat the surface to be coated.
[0077] Turn on the magnetron sputtering equipment, place the substrate material on the sample stage of the substrate stage, close the chamber door and evacuate the chamber to a vacuum degree of 2.0×10 -3 Below Pa.
[0078] The bias cleaning process is as follows: 17-4PH steel is heated and bias cleaned. The preparation temperature is set to 200°C and the 17-4PH steel is heated. When the predetermined temperature is reached and the vacuum degree in the chamber is 1.8×10 -3 When 0.04 Pa, open the stop valve, set the flow limiting valve parameter to 100° (adjustment range is 0-1000°), set the argon flow rate to 30 sccm, set the voltage to -900 V, and keep the pressure in the chamber above 1.0 Pa for bias cleaning. First, bombard the surface of 17-4PH steel with Ar+ particles for 10 minutes to ensure that the contaminants on the surface of 17-4PH steel can be removed, the surface of 17-4PH steel can be activated, and the adhesion of the coating can be guaranteed.
[0079] The coating process is as follows: set the argon flow rate to 30sccm, the AlCr target power to 150W, the Zr target power to 100W, the chamber working pressure to 0.5Pa, the substrate rotation speed to 10r / min, the deposition temperature to 200°C, adjust the bias voltage of the magnetron sputtering equipment to -100V, and deposit for 10 minutes; then adjust the Zr target power to 150W, make the chamber working pressure 1.0Pa, and deposit for another 10 minutes. The thickness of the prepared hydrogen barrier coating is 143μm.
[0080] The prepared coating has an amorphous structure. The permeation current density is measured to be 0.64 μA·cm -2 ; Through testing, when the thickness of high-strength steel is 5mm, the minimum bending radius is 2cm, and there is no crack at the interface between the hydrogen barrier coating and the 12Cr2Mo1R steel substrate.
[0081] Comparative Example 1
[0082] Different from Example 1, in step S2 of this comparative example, the AlCr target power is 150 W, the Zr target power is 100 W, and the co-deposition time is 20 min.
[0083] The prepared coating has an amorphous structure; through testing, it was found that when the thickness of the high-strength steel was 5 mm and the bending radius was 10 cm, cracks existed at the interface between the hydrogen barrier coating and the 12Cr2Mo1R steel substrate.
[0084] Comparative Example 2
[0085] Different from Example 1, in step S2 of this comparative example, the AlCr target power is 150 W, the Zr target power is 150 W, and the co-deposition is carried out for 20 min.
[0086] The prepared coating has an amorphous structure; through testing, it was found that when the thickness of the high-strength steel was 5 mm and the bending radius was 15 cm, cracks existed at the interface between the hydrogen barrier coating and the 12Cr2Mo1R steel substrate.
[0087] Comparative Example 3
[0088] Different from Example 1, in step S2 of this comparative example, the time for the first deposition is 8 minutes, and the time for the second deposition is 12 minutes.
[0089] The prepared coating has an amorphous structure; through testing, it was found that when the thickness of the high-strength steel was 5 mm and the bending radius was 20 cm, cracks existed on the outer surface of the hydrogen barrier coating.
[0090] Comparative Example 4
[0091] Different from Example 1, in step S2 of this comparative example, the time for the first deposition is 12 minutes, and the time for the second deposition is 8 minutes.
[0092] The prepared coating has an amorphous structure. The permeation current density is measured to be 2.47 μA·cm -2 .
[0093] Comparative Example 3
[0094] Different from Example 1, in S2 of this comparative example, the bias voltage of the magnetron sputtering device is -50V. Figure 3 As shown, the measured penetration current density is: 3.40μA·cm -2 .
[0095] Comparative Example 4
[0096] Different from Example 1, in S2 of this comparative example, the bias voltage of the magnetron sputtering device is -150V. Figure 3 As shown, the penetration current density is measured to be: 1.20μA·cm -2 .
[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A hydrogen barrier coating on the surface of high-strength steel, It is characterized in that The hardness of the high-strength steel is HV300-HV600, the tensile strength is 900-1200MPa, and the thermal expansion coefficient can be up to (8-20)×10 -6 / K, elastic modulus between 100-200GPa; The hydrogen barrier coating is composed of three elements: Al, Cr and Zr, and the molar ratio of each element is not less than 30%; The hydrogen barrier coating has an amorphous structure.
2. The hydrogen barrier coating according to claim 1, It is characterized in that The thickness of the hydrogen barrier coating is 100-200 μm.
3. A method for preparing the hydrogen barrier coating according to claim 1 or 2, It is characterized in that include: Selecting high-strength steel and a target material, and pretreating the surface of the high-strength steel to be coated; The surface to be coated is coated by magnetron sputtering.
4. The preparation method according to claim 3, It is characterized in that The target materials include AlCr target and Zr target.
5. The preparation method according to claim 3, It is characterized in that The pretreatment includes: using 400# to 5000# SiC sandpaper to grind the surface of the high-strength steel to be coated step by step until there are no cavities and large scratches on the surface, and then using diamond polishing paste to perform mirror polishing. The surface roughness of the prepared product is less than 0.16μm. Finally, using an ultrasonic cleaner to soak and clean the sample with deionized water, anhydrous ethanol and acetone in turn for 10-30 minutes and then drying.
6. The preparation method according to claim 3, It is characterized in that The magnetron sputtering process includes vacuuming, bias cleaning and coating; The vacuum degree after vacuuming is not greater than 2.0×10 -3 Pa.
7. The preparation method according to claim 6, It is characterized in that The bias cleaning process is as follows: setting the preparation temperature to 180-220°C to heat the substrate, and when the vacuum degree in the chamber is not greater than 1.8×10 -3 When 0.040 ℃, the stop valve was opened, the limiting valve parameter was set to 100°, the argon flow rate was set to 30 sccm, and the voltage was set to -900 V to keep the pressure in the chamber above 1.0 Pa for bias cleaning.
8. The preparation method according to claim 6, It is characterized in that The coating process includes primary deposition and secondary deposition; The primary deposition is as follows: the argon flow rate is set to 30 sccm, the AlCr target power is 140-160 W, the Zr target power is 90-110 W, the chamber working pressure is 0.4-0.6 Pa, the substrate rotation speed is 9-11 r / min, the deposition temperature is 180-220° C., the bias voltage of the magnetron sputtering device is adjusted to -100 V, and the deposition is performed for 10-15 min; The secondary deposition is as follows: the Zr target power is adjusted to 140-160W, the chamber working pressure is set to 0.9-1.1 Pa, and the deposition is continued for 10-20 minutes.
9. The preparation method according to claim 8, It is characterized in that In one deposition, the power ratio of AlCr target to Zr target is 3:2; For secondary deposition, the power ratio of AlCr target to Zr target was 1:1.
Citation Information
Patent Citations
M / MOx composite hydrogen resistance coating and preparation method thereof
CN105729934A
Aluminum-oxide hydrogen-permeation inhibition anti-corrosive insulating layer with high bonding strength as well as preparation method and application thereof
CN108914111A
Compound hydrogen-resistant coating and production method thereof
CN113122842A
Anti-corrosion and anti-hydrogen permeation coating and preparation method thereof
CN114686810A
Ternary composite novel hydrogen / deuterium / tritium permeation resistant coating and preparation method thereof
CN115110067A
Cited By