Preparation method of laser cladding and heat treatment reinforced FeCoCrNiMn high-entropy alloy wear-resistant coating

Through laser cladding and heat treatment processes, the problems of low hardness and poor wear resistance of FeCoCrNiMn high-entropy alloys are solved, and the preparation of high-density coatings is realized, which improves wear resistance and economy, and is suitable for applications in the field of tribology.

CN119040878AActive Publication Date: 2024-11-29XIAN UNIV OF TECH

Patent Information

Application Number
CN202411170050.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Due to its low hardness and poor wear resistance, FeCoCrNiMn high-entropy alloys have limited their application in the field of tribology, and traditional metallurgical preparation is difficult to achieve the production and application of large-format coatings.

Method used

The coordinated process of laser cladding and heat treatment is adopted to prepare FeCoCrNiMn high-entropy alloy coating through substrate surface pretreatment and laser cladding, grinding and polishing, and annealing to form a high density wear-resistant coating.

Benefits of technology

It significantly improves the surface hardness and wear resistance of FeCoCrNiMn high-entropy alloy, simplifies the process flow, reduces costs, and realizes the preparation of large-format coatings, with good economics and industrial application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040878A_ABST
    Figure CN119040878A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a FeCoCrNiMn high-entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment. The preparation method comprises the following steps: firstly, pretreating the surface of a matrix; then, a FeCoCrNiMn high-entropy alloy coating is prepared through laser cladding; the FeCoCrNiMn high-entropy alloy coating is ground and polished, and a flat surface is obtained; and finally, annealing treatment is conducted, and the FeCoCrNiMn high-entropy alloy wear-resistant coating is obtained. The high-strength fine-grain FeCoCrNiMn high-entropy alloy prepared through the method solves the technical problems that the FeCoCrNiMn high-entropy alloy is low in relative hardness and poor in abrasion resistance, and particularly solves the technical problem that production and application of a large-area coating are difficult to achieve through a traditional metallurgy preparation technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of FeCoCrNiMn series high entropy alloy wear-resistant coatings, and specifically relates to a method for preparing a FeCoCrNiMn high entropy alloy wear-resistant coating by laser cladding and heat treatment strengthening. Background Art

[0002] The ratio of the main elements of high entropy alloys is close to equimolar. By precisely controlling the composition and content of the elements, it is easy to form a single-phase solid solution phase of face-centered cubic structure (FCC), body-centered cubic structure (BCC) or hexagonal close-packed structure (HCP). It has excellent properties such as high hardness / strength, high fatigue resistance and fracture toughness, high temperature oxidation resistance, and corrosion resistance. In recent years, FeCoCrNiMn alloy has attracted widespread attention due to its stable face-centered cubic (FCC) single-phase structure and excellent machinability. It is considered to be an excellent material that can be used in aerospace and marine equipment manufacturing. However, FeCoCrNiMn alloy has limited its application in the field of tribology due to its low hardness and poor wear resistance. According to the relationship between microstructure and performance, the strengthening and toughening of FeCoCrNiMn can be achieved by changing the internal structure and other processes. For example, by adding a sixth element, it can induce the structure to change from face-centered cubic (FCC) to body-centered cubic (BCC), increase the grain dislocation degree, and improve its surface hardness and wear resistance. However, this technology has a long process flow and the process parameters involved have a great impact on the alloy properties, and the cost is high.

[0003] Laser cladding is a process in which a high-energy-density laser beam is used to melt the substrate and powder simultaneously to form a molten pool under a protective atmosphere, and then rapidly cools the cladding layer to obtain a cladding layer with better plasticity, impact resistance, and corrosion resistance than the substrate. The comprehensive performance of the substrate material can be significantly improved by preparing a high-entropy alloy coating on an alloy substrate through laser cladding. In view of this, the present invention proposes a method for preparing a FeCoCrNiMn high-entropy alloy wear-resistant coating by combining laser cladding with a heat treatment process. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a FeCoCrNiMn high-entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment, and to prepare a fine-grained FeCoCrNiMn high-entropy alloy with high strength to solve its relatively low hardness and poor wear resistance, especially to solve the technical problems that traditional metallurgical preparation technology is difficult to achieve the production and application of large-area coatings.

[0005] The technical solution adopted by the present invention is a method for preparing a FeCoCrNiMn high entropy alloy wear-resistant coating by laser cladding and heat treatment strengthening, which is specifically implemented according to the following steps:

[0006] Step 1: pretreatment of substrate surface;

[0007] Step 2: preparing FeCoCrNiMn high entropy alloy coating by laser cladding;

[0008] Step 3, grinding and polishing the FeCoCrNiMn high entropy alloy coating to obtain a smooth surface;

[0009] Step 4: annealing to obtain a FeCoCrNiMn high entropy alloy wear-resistant coating.

[0010] The present invention is also characterized in that:

[0011] Step 1 is implemented according to the following steps:

[0012] Step 1.1, polish the surface of the sample to remove the oxide layer on the surface;

[0013] Step 1.2, cleaning the substrate obtained in step 1 to remove surface lipids, organic matter and metal residues;

[0014] Step 1.3: Rinse the substrate surface after step 1.2 to remove the residual anhydrous ethanol on the surface, and wait for the surface to dry before use.

[0015] Step 2 is implemented as follows:

[0016] Step 2.1, weighing cladding powders of Fe: 15%-25%, Cr: 15%-20%, Ni: 15%-25%, Mn: 15%-25%, Co: 15%-20%, the sum of the mass percentages of the above powders is 100%, the purity of the powders is greater than 99%, and the particle size range is 100-250μm;

[0017] Step 2.2: Stir for 2 h to 6 h to make the powder diameter range 50-100 μm.

[0018] Step 2.3: Dry the mixed powder after step 2.2, cool it after heat preservation, and take it out after cooling to room temperature.

[0019] Step 2.4, placing the dried FeCoCrNiMn high entropy alloy powder in a powder feeder, and spraying the powder on the surface to be clad by a powder feeding gas, wherein the powder feeding gas is an inert gas such as nitrogen or argon;

[0020] Step 2.5: Use high-speed laser cladding equipment to clad the surface of the substrate to generate a FeCoCrNiMn high-entropy alloy coating. The laser power is 1-2.5 kW, the scanning speed is 2-3 m / min, and the powder feeding rate is 12-13 g / min.

[0021] In step 2.3, the drying temperature is 80°C-150°C, and the insulation time is 4h-14h.

[0022] Step 3 is implemented as follows:

[0023] The surface of the FeCoCrNiMn high entropy alloy coating obtained in step 2 is surface treated using the treatment method of step 1, and finally a flat surface of the FeCoCrNiMn high entropy alloy coating is obtained.

[0024] Step 4 is implemented according to the following steps:

[0025] Step 4.1, preparing the test piece with the FeCoCrNiMn high entropy alloy coating on the surface obtained in step 3 for annealing;

[0026] Step 4.2, set the temperature of the resistance furnace to 500-900°C, start heating, gradually raise the furnace temperature to the set temperature, and use nitrogen as the protective gas in the furnace;

[0027] Step 4.3, annealing at 500-900°C for 2-14 hours;

[0028] Step 4.4, after the insulation is completed, the heating is stopped, and the FeCoCrNiMn high entropy alloy wear-resistant coating is obtained after natural cooling in the furnace.

[0029] The beneficial effect of the present invention is that the method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment has the following advantages: (1) The high entropy alloy coating prepared by the laser cladding method has the advantages of concentrated energy, fast cooling rate, low dilution rate, small heat-affected zone, etc., so as to prepare a large-area coating with high density, while reducing the use of high entropy alloy powder and improving economy. (2) The alloy coating strengthened by annealing treatment has excellent surface hardness, which can effectively improve wear resistance and service life. (3) Since the preparation process is simple and economical and efficient, and does not require other complex equipment, it has great application potential in industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The surface metallographic structures of the embodiments 1, 2 and 3 of the method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment of the present invention;

[0031] Figure 2 The friction coefficient curves of Examples 1, 2 and 3 of the method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment of the present invention;

[0032] Figure 3 is the volume wear rate of Examples 1, 2, and 3 of the method for preparing a FeCoCrNiMn high entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment of the present invention;

[0033] Figure 4 It is the microhardness of Examples 1, 2 and 3 of the method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment of the present invention. DETAILED DESCRIPTION

[0034] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] The method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating by laser cladding and heat treatment strengthening of the present invention is specifically implemented according to the following steps:

[0036] Step 1: pretreatment of substrate surface;

[0037] Step 1 is implemented according to the following steps:

[0038] Step 1.1, use 200#, 600#, and 800# metallographic sandpaper to polish the sample surface to remove the surface oxide layer;

[0039] Step 1.2, cleaning the substrate obtained in step 1 in an ultrasonic cleaning machine using anhydrous ethanol as a solvent for 5-10 minutes to remove surface lipids, organic matter and metal residues;

[0040] Step 1.3: Rinse the substrate surface after step 1.2 with deionized water to remove the residual anhydrous ethanol on the surface, and wait for the surface to dry before use.

[0041] Step 2: preparing FeCoCrNiMn high entropy alloy coating by laser cladding;

[0042] Step 2 is implemented as follows:

[0043] Step 2.1, weighing cladding powders of Fe: 15%-25%, Cr: 15%-20%, Ni: 15%-25%, Mn: 15%-25%, Co: 15%-20%, the sum of the mass percentages of the above powders is 100%, the purity of the powders is greater than 99%, and the particle size range is 100-250μm;

[0044] Step 2.2: In order to make the powder have good fluidity, the mixed powder is placed in a ball mill, and then stirred in a planetary vertical ball mill at a speed of 50-500 r / min for 2h-6h to make the powder diameter range 50-100 μm.

[0045] Step 2.3, drying the mixed powder after step 2.2 in a drying oven protected by nitrogen or argon, with a drying temperature of 80°C-150°C and a holding time of 4h-14h to remove moisture and volatile substances in the powder. After the holding is completed, nitrogen or argon is continuously introduced into the drying oven for cooling, and the powder is taken out after cooling to room temperature.

[0046] Step 2.4, placing the dried FeCoCrNiMn high entropy alloy powder in a powder feeder, and spraying the powder on the surface to be clad by a powder feeding gas, wherein the powder feeding gas is an inert gas such as nitrogen or argon;

[0047] Step 2.5: Use high-speed laser cladding equipment to clad the surface of the substrate to generate a FeCoCrNiMn high-entropy alloy coating. The laser power is 1-2.5 kW, the scanning speed is 2-3 m / min, and the powder feeding rate is 12-13 g / min.

[0048] Step 3, grinding and polishing the FeCoCrNiMn high entropy alloy coating to obtain a smooth surface;

[0049] Step 3 is implemented as follows:

[0050] The surface of the FeCoCrNiMn high entropy alloy coating obtained in step 2 is surface treated by the treatment method of step 1, see step 1 for details; finally, a flat surface of the FeCoCrNiMn high entropy alloy coating is obtained.

[0051] Step 4: annealing to obtain a FeCoCrNiMn high entropy alloy wear-resistant coating;

[0052] Step 4 is implemented according to the following steps:

[0053] Step 4.1, placing the test piece with the FeCoCrNiMn high entropy alloy coating on the surface obtained in step 3 into a box-type resistance furnace for annealing treatment;

[0054] Step 4.2, set the temperature of the resistance furnace to 500-900°C, start heating, gradually raise the furnace temperature to the set temperature, and use nitrogen as the protective gas in the furnace;

[0055] Step 4.3, annealing at 500-900°C for 2-14 hours;

[0056] Step 4.4, after the insulation is completed, the heating is stopped, and the FeCoCrNiMn high entropy alloy wear-resistant coating is obtained after natural cooling in the furnace.

[0057] In order to study the influence of annealing process parameters on the performance of FeCoCrNiMn high entropy alloy wear-resistant coating, the surface hardness was tested by microhardness tester, the load of hardness test was 50g and loaded for 15s, and the wear resistance of FeCoCrNiMn high entropy alloy wear-resistant coating was characterized by dry friction experiment. The load was set to 5N, the sliding speed was 0.04m / s, the reciprocating distance was 5mm, and the experimental time was 30min. In order to ensure the accuracy of the experiment, the steel ball and disc samples were ultrasonically cleaned with anhydrous ethanol before and after the experiment, and the impurities such as oil stains on the surface of the sample were dried to remove them. After the experiment, the wear scar profile was measured using a laser confocal microscope, and the volume wear rate was calculated. Through the above test, the high entropy alloy wear-resistant coating of the present invention has excellent wear resistance.

[0058] Example 1

[0059] The specimen selected for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating is 45 steel with a thickness of 10 mm, and a 45 steel sample of 20×20×5 (mm) is selected. The following is a specific example of preparing the FeCoCrNiMn high entropy alloy wear-resistant coating.

[0060] The FeCoCrNiMn high entropy alloy wear-resistant coating preparation method of the present invention can be achieved by the following technical scheme:

[0061] Step 1: pretreatment of substrate surface;

[0062] Step 1 is as follows:

[0063] Step 1.1, use 200#, 600#, and 800# metallographic sandpaper to polish the sample surface to remove the surface oxide layer;

[0064] Step 1.2, cleaning the substrate obtained in step 1 in an ultrasonic cleaning machine using anhydrous ethanol as a solvent for 5-10 minutes to remove surface lipids, organic matter and metal residues;

[0065] Step 1.3: Rinse the substrate surface after step 1.2 with deionized water to remove the residual anhydrous ethanol on the surface, and wait for the surface to dry before use.

[0066] Step 2: Prepare FeCoCrNiMn high entropy alloy by cladding on the surface of the substrate.

[0067] Step 2 is as follows:

[0068] Step 2.1, the chemical composition of FeCoCrNiMn high entropy alloy powder is Fe: 15%-25%, Cr: 15%-20%, Ni: 15%-25%, Mn: 15%-25%, Co: 15%-20%. The purity of the powder is greater than 99%, and the particle size range is 100-250μm.

[0069] Step 2.2: In order to make the powder have good fluidity, the mixed powder is placed in a ball mill, and then stirred in a planetary vertical ball mill at a speed of 50-500 r / min for 2h-6h to make the powder diameter range 50-100 μm.

[0070] Step 2.3, the FeCoCrNiMn high entropy alloy powder is dried in a drying oven protected by nitrogen or argon. The drying temperature is 80℃-150℃, and the insulation time is 4h-14h to remove moisture and volatile substances in the powder. After the insulation is completed, nitrogen or argon is continuously introduced into the drying oven for cooling, and the powder is taken out after cooling to room temperature.

[0071] Step 2.4, placing the dried FeCoCrNiMn high entropy alloy powder in a powder feeder, and spraying the powder on the surface to be clad by a powder feeding gas, wherein the powder feeding gas is an inert gas such as nitrogen or argon;

[0072] Step 2.5: Use high-speed laser cladding equipment to prepare FeCoCrNiMn high-entropy alloy coating, laser power: 1-82.33 kW, scanning speed: 2.90 m / min, powder feeding rate: 12.46 g / min.

[0073] Step 3: grinding and polishing the surface of the sample after laser cladding;

[0074] Step 3 is as follows:

[0075] Step 3.1, the surface of the cladding layer obtained in step 2 is treated by the treatment method of step 1, see step 2 for details;

[0076] Step 4: annealing to obtain a FeCoCrNiMn high entropy alloy wear-resistant coating;

[0077] Step 4 is as follows:

[0078] Step 4.1, placing the high entropy alloy specimen obtained in step 3 into a box-type resistance furnace;

[0079] Step 4.2: Set the temperature of the resistance furnace to 700°C, start the heating system, gradually raise the furnace temperature to the set temperature, and use nitrogen as the protective gas in the furnace.

[0080] Step 4.3, annealing at 700°C for 2h;

[0081] Step 4.4: After the insulation is completed, turn off the resistance furnace heating system and let the furnace cool naturally;

[0082] Then the FeCoCrNiMn high entropy alloy wear-resistant coating is obtained. Figure 1, wherein (a) is the surface structure morphology of Example 1, (b) is the surface structure morphology of Example 2, (c) is the surface structure morphology of Example 3, (d) is the grain size frequency distribution diagram of Example 1, (e) is the grain size frequency distribution diagram of Example 2, and (f) is the grain size frequency distribution diagram of Example 3. Figure 1 It can be seen that after annealing at 700℃ for 2h, about 76% of the grains on the surface of the sample have a size less than 150μm, and all grains are less than 250μm. Figure 2 It can be seen that the friction coefficient curve of Example 1 fluctuates violently, with a fluctuation range of about 0.15, and its average friction coefficient is 0.706. Figure 3 and Figure 4 It can be seen that the volume wear rate of the coating after the 5N-4Hz friction test is about 1.35×10 -4 , the surface microhardness is about 240.5HV. In summary, the high entropy alloy wear-resistant coating preparation technology of the present invention can refine the FeCoCrNiMn coating grains and improve the wear resistance.

[0083] Example 2

[0084] The specimen selected for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating is 45 steel with a thickness of 10 mm, and a 45 steel sample of 20×20×5 (mm) is selected. The following is a specific example of preparing the FeCoCrNiMn high entropy alloy wear-resistant coating.

[0085] The FeCoCrNiMn high entropy alloy wear-resistant coating preparation method of the present invention can be achieved by the following technical scheme:

[0086] Step 1: pretreatment of substrate surface;

[0087] Step 1 is as follows:

[0088] Step 1.1, use 200#, 600#, and 800# metallographic sandpaper to polish the surface of the sample to remove the oxide layer on the surface;

[0089] Step 1.2, cleaning the substrate obtained in step 1 in an ultrasonic cleaning machine using anhydrous ethanol as a solvent for 5-10 minutes to remove surface lipids, organic matter and metal residues;

[0090] Step 1.3: Rinse the substrate surface after step 1.2 with deionized water to remove the residual anhydrous ethanol on the surface, and wait for the surface to dry before use.

[0091] Step 2: Prepare FeCoCrNiMn high entropy alloy by cladding on the surface of the substrate.

[0092] Step 2 is as follows:

[0093] Step 2.1, the chemical composition of FeCoCrNiMn high entropy alloy powder is Fe: 15%-25%, Cr: 15%-20%, Ni: 15%-25%, Mn: 15%-25%, Co: 15%-20%. The purity of the powder is greater than 99%, and the particle size range is 100-250μm.

[0094] Step 2.2: In order to make the powder have good fluidity, the mixed powder is placed in a ball mill, and then stirred in a planetary vertical ball mill at a speed of 50-500 r / min for 2h-6h to make the powder diameter range 50-100 μm.

[0095] Step 2.3, the FeCoCrNiMn high entropy alloy powder is dried in a drying oven protected by nitrogen or argon. The drying temperature is 80℃-150℃, and the insulation time is 4h-14h to remove moisture and volatile substances in the powder. After the insulation is completed, nitrogen or argon is continuously introduced into the drying oven for cooling, and the powder is taken out after cooling to room temperature.

[0096] Step 2.4, placing the dried FeCoCrNiMn high entropy alloy powder in a powder feeder, and spraying the powder on the surface to be clad by a powder feeding gas, wherein the powder feeding gas is an inert gas such as nitrogen or argon;

[0097] Step 2.5: Use high-speed laser cladding equipment to prepare FeCoCrNiMn high-entropy alloy coating, laser power: 1-82.33 kW, scanning speed: 2.90 m / min, powder feeding rate: 12.46 g / min.

[0098] Step 3: grinding and polishing the surface of the sample after laser cladding;

[0099] Step 3 is as follows:

[0100] Step 3.1, the surface of the cladding layer obtained in step 2 is treated by the treatment method of step 1, see step 2 for details;

[0101] Step 4: annealing to obtain a FeCoCrNiMn high entropy alloy wear-resistant coating;

[0102] Step 4 is as follows:

[0103] Step 4.1, placing the high entropy alloy specimen obtained in step 3 into a box-type resistance furnace;

[0104] Step 4.2: Set the temperature of the resistance furnace to 700°C, start the heating system, gradually raise the furnace temperature to the set temperature, and use nitrogen as the protective gas in the furnace.

[0105] Step 4.3, annealing at 700°C for 8h;

[0106] Step 4.4: After the insulation is completed, turn off the resistance furnace heating system and let the furnace cool naturally;

[0107] Then the FeCoCrNiMn high entropy alloy wear-resistant coating is obtained. Figure 1 It can be seen that about 79.6% of the grain sizes on the coating surface are below 150μm, and the proportion below 250μm is 96%. Figure 2 It can be seen that the friction coefficient of the sample annealed at 700℃ for 8h increased rapidly to 0.65 at the beginning of the experiment, dropped to 0.55 after a short running-in period, and then began to increase, with an average friction coefficient of 0.635. Figure 3 and Figure 4 It can be seen that the volume wear rate of the coating is about 8.14×10-5 mm3 / N·m, and the microhardness is about 250.8 HV. In summary, the hardness and wear resistance of the FeCoCrNiMn coating can be improved by the high entropy alloy wear-resistant coating preparation technology of the present invention.

[0108] Example 3

[0109] The specimen selected for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating is 45 steel with a thickness of 10 mm, and a 45 steel sample of 20×20×5 (mm) is selected. The following is a specific example of preparing the FeCoCrNiMn high entropy alloy wear-resistant coating.

[0110] The FeCoCrNiMn high entropy alloy wear-resistant coating preparation method of the present invention can be achieved by the following technical scheme:

[0111] Step 1: pretreatment of substrate surface;

[0112] Step 1 is as follows:

[0113] Step 1.1, use 200#, 600#, and 800# metallographic sandpaper to polish the surface of the sample to remove the oxide layer on the surface;

[0114] Step 1.2, cleaning the substrate obtained in step 1 in an ultrasonic cleaning machine using anhydrous ethanol as a solvent for 5-10 minutes to remove surface lipids, organic matter and metal residues;

[0115] Step 1.3: Rinse the substrate surface after step 1.2 with deionized water to remove the residual anhydrous ethanol on the surface, and wait for the surface to dry before use.

[0116] Step 2: Prepare FeCoCrNiMn high entropy alloy by cladding on the surface of the substrate.

[0117] Step 2 is as follows:

[0118] Step 2.1, the chemical composition of FeCoCrNiMn high entropy alloy powder is Fe: 15%-25%, Cr: 15%-20%, Ni: 15%-25%, Mn: 15%-25%, Co: 15%-20%. The purity of the powder is greater than 99%, and the particle size range is 100-250μm.

[0119] Step 2.2: In order to make the powder have good fluidity, the mixed powder is placed in a ball mill, and then stirred in a planetary vertical ball mill at a speed of 50-500 r / min for 2h-6h to make the powder diameter range 50-100 μm.

[0120] Step 2.3, the FeCoCrNiMn high entropy alloy powder is dried in a drying oven protected by nitrogen or argon. The drying temperature is 80℃-150℃, and the insulation time is 4h-14h to remove moisture and volatile substances in the powder. After the insulation is completed, nitrogen or argon is continuously introduced into the drying oven for cooling, and the powder is taken out after cooling to room temperature.

[0121] Step 2.4, placing the dried FeCoCrNiMn high entropy alloy powder in a powder feeder, and spraying the powder on the surface to be clad by a powder feeding gas, wherein the powder feeding gas is an inert gas such as nitrogen or argon;

[0122] Step 2.5: Use high-speed laser cladding equipment to prepare FeCoCrNiMn high-entropy alloy coating, laser power: 1-82.33 kW, scanning speed: 2.90 m / min, powder feeding rate: 12.46 g / min.

[0123] Step 3: grinding and polishing the surface of the sample after laser cladding;

[0124] Step 3 is as follows:

[0125] Step 3.1, the surface of the cladding layer obtained in step 2 is treated by the treatment method of step 1, see step 2 for details;

[0126] Step 4: annealing to obtain a FeCoCrNiMn high entropy alloy wear-resistant coating;

[0127] Step 4 is as follows:

[0128] Step 4.1, placing the high entropy alloy specimen obtained in step 3 into a box-type resistance furnace;

[0129] Step 4.2: Set the temperature of the resistance furnace to 700°C, start the heating system, gradually raise the furnace temperature to the set temperature, and use nitrogen as the protective gas in the furnace.

[0130] Step 4.3, annealing at 700°C for 14 hours;

[0131] Step 4.4: After the insulation is completed, turn off the resistance furnace heating system and let the furnace cool naturally;

[0132] It can be seen from the attached drawings that Figure 1 (a) is the surface structure morphology of Example 1, (b) is the surface structure morphology of Example 2, (c) is the surface structure morphology of Example 3, (d) is the grain size frequency distribution diagram of Example 1, (e) is the grain size frequency distribution diagram of Example 2, and (f) is the grain size frequency distribution diagram of Example 3; Figure 2 The friction coefficient curves of Examples 1, 2 and 3 of the method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment of the present invention; Figure 3 is the volume wear rate of Examples 1, 2, and 3 of the method for preparing a FeCoCrNiMn high entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment of the present invention; Figure 4 The microhardness of the FeCoCrNiMn high entropy alloy wear-resistant coating preparation method of the present invention is shown in Examples 1, 2, and 3. As can be seen from the above figures, about 69.4% of the grain size on the coating surface is below 150μm, and the proportion below 250μm is 93%. The friction coefficient curve of the coating that has been annealed at 700℃-14h is more stable during the entire experiment, with an average friction coefficient of 0.670 and a volume wear rate of about 2.76×10-4mm 3 / N·m microhardness is about 185.4HV. It can be seen that the tribological properties of FeCoCrNiMn can be improved by the high entropy alloy wear-resistant coating preparation technology of the present invention.

Claims

1. A method for preparing a FeCoCrNiMn high entropy alloy wear-resistant coating strengthened by laser cladding and heat treatment, characterized in that: Follow the steps below to implement it: Step 1: pretreatment of substrate surface; Step 2: preparing FeCoCrNiMn high entropy alloy coating by laser cladding; Step 3, grinding and polishing the FeCoCrNiMn high entropy alloy coating to obtain a smooth surface; Step 4: annealing to obtain a FeCoCrNiMn high entropy alloy wear-resistant coating.

2. The method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating by laser cladding and heat treatment strengthening according to claim 1, characterized in that: The step 1 is specifically implemented according to the following steps: Step 1.1, polish the surface of the sample to remove the oxide layer on the surface; Step 1.2, cleaning the substrate obtained in step 1 to remove surface lipids, organic matter and metal residues; Step 1.3: Rinse the substrate surface after step 1.2 to remove the residual anhydrous ethanol on the surface, and wait for the surface to dry before use.

3. The method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating by laser cladding and heat treatment strengthening according to claim 2, characterized in that: The step 2 is specifically implemented according to the following steps: Step 2.1, weighing cladding powders of Fe: 15%-25%, Cr: 15%-20%, Ni: 15%-25%, Mn: 15%-25%, Co: 15%-20%, the sum of the mass percentages of the above powders is 100%, the purity of the powders is greater than 99%, and the particle size range is 100-250μm; Step 2.2, stirring for 2h-6h, so that the powder diameter ranges from 50 to 100μm; Step 2.3, drying the mixed powder after step 2.2, cooling it after the heat preservation is completed, and taking it out after cooling it to room temperature; Step 2.4, placing the dried FeCoCrNiMn high entropy alloy powder in a powder feeder, and spraying the powder on the surface to be clad by a powder feeding gas, wherein the powder feeding gas is an inert gas such as nitrogen or argon; Step 2.5: Use high-speed laser cladding equipment to clad the surface of the substrate to generate a FeCoCrNiMn high-entropy alloy coating. The laser power is 1-2.5 kW, the scanning speed is 2-3 m / min, and the powder feeding rate is 12-13 g / min.

4. The method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating by laser cladding and heat treatment strengthening according to claim 2, characterized in that: In the step 2.3, the drying temperature is 80° C.-150° C., and the insulation time is 4 h-14 h.

5. The method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating by laser cladding and heat treatment strengthening according to claim 3, characterized in that: The step 3 is specifically implemented according to the following steps: The surface of the FeCoCrNiMn high entropy alloy coating obtained in step 2 is surface treated using the treatment method of step 1, and finally a flat surface of the FeCoCrNiMn high entropy alloy coating is obtained.

6. The method for preparing the FeCoCrNiMn high entropy alloy wear-resistant coating by laser cladding and heat treatment strengthening according to claim 4, characterized in that: The step 4 is specifically implemented according to the following steps: Step 4.1, preparing the test piece with the FeCoCrNiMn high entropy alloy coating on the surface obtained in step 3 for annealing; Step 4.2, set the temperature of the resistance furnace to 500-900°C, start heating, gradually raise the furnace temperature to the set temperature, and use nitrogen as the protective gas in the furnace; Step 4.3, annealing at 500-900°C for 2-14 hours; Step 4.4, after the insulation is completed, the heating is stopped, and the FeCoCrNiMn high entropy alloy wear-resistant coating is obtained after natural cooling in the furnace.

Citation Information

Patent Citations

  • High entropy alloy coating as well as preparation method and application thereof

    CN107299342A

  • High-entropy alloy coating and preparation method thereof

    CN111850544A

  • Preparation method of FCC-BCC double-phase high-entropy alloy gradient material

    CN112323058A

  • Heat treatment method of laser cladding coating material

    CN112410782A

  • Method for strengthening high-entropy alloy cladding layer through ceramic particles and application

    CN113493913A

Cited By

  • Method for preparing high-entropy alloy composite coating based on nitrogen / MnN double-source synergy and high-entropy alloy composite coating

    CN120249970A

  • High-temperature wear-resistant high-entropy alloy-based composite coating and preparation method thereof

    CN120796813A