Repair method for shaft parts
By combining electrical pulse and ultrasonic rolling technology in the laser cladding repair of wind power spindles, the microstructure structure is regulated, residual stress and overlapping trace problems are solved, and the mechanical performance and service life of the spindle are improved.
Patent Information
- Application Number
- CN202411185726.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
AI Technical Summary
The existing technology has residual tensile stress and overlapping marks in the laser cladding repair of wind power spindles, resulting in reduced service performance and service life of parts. The ultrasonic rolling method is not ideal for high-hardness materials, and it is impossible to deeply improve mechanical properties.
After laser cladding is used to form the cladding layer, electrical pulses are applied and ultrasonic rolling and post-treatment are combined to regulate the microstructure structure through electroplastic effects, skin effects and thermal effects, increase the surface compressive stress, deepen the strengthening layer, and reduce surface roughness. degree and residual stress.
It significantly improves the surface hardness, fatigue resistance, wear resistance and corrosion resistance of the spindle, extends the service life, is simple in process and is suitable for industrial production.
Smart Images

Figure CN119040880A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material surface strengthening processing, in particular to a method for repairing shaft parts. Background Art
[0002] The main material used in wind turbine main shafts is alloy structural steel, which is used to meet the requirements of high-speed rotation and large loads. Alloy structural steel has excellent strength and toughness. More importantly, it has good fatigue resistance in low temperature environments, which can ensure the stability and life of the main shaft during operation. After a period of operation, the damaged parts of the wind turbine main shaft need to be repaired. At present, the damaged main shaft is mainly repaired by surfacing welding. The residual stress of the main shaft after surfacing welding is high, and the surface hardness of the surfacing layer is high. The hardness decreases with the distance from the surface layer. Laser cladding technology is a process method that uses a high-energy density laser beam to melt and solidify the powder and the substrate at the same time and achieve good metallurgical bonding. It has been widely used in the fields of material surface modification, remanufacturing engineering and additive manufacturing. However, due to factors such as uneven laser energy distribution, large differences in the thermophysical properties of powder and substrate, and fast melting and solidification rate of cladding materials, the temperature gradient between the cladding layer and the substrate is large, resulting in uneven solidification structure, inconsistent material shrinkage, and easy formation of residual tensile stress. The existence of residual tensile stress in the cladding layer and the overlap marks left after multiple cladding passes can easily induce cracks, reducing the service performance, service life and reliability of parts.
[0003] In order to obtain an ideal stress distribution state on the surface of the laser cladding layer, one method is to optimize the repair process, such as optimizing the laser cladding process parameters to obtain an ideal microstructure and performance; another method is to perform comprehensive organizational regulation through post-processing. Although residual stress can be released and the surface hardness of the cladding layer can be reduced by heat treatment, the heat treatment process cannot be carried out at the repair site, and the environmental protection investment is large, which is not suitable for on-site operations. Both hammering and shot peening can reduce stress concentration. The hammering method is widely used and more flexible, but the labor intensity is high, the controllability and surface quality are poor, and the effect is unstable. Shot peening can obtain relatively good mechanical properties, good controllability and effect, but the disadvantage is that the equipment is complex and large, the processing cost is high, and the flexibility is poor.
[0004] Ultrasonic rolling surface strengthening technology uses a smooth ball with high hardness to roll the surface of a metal material, and at the same time applies ultrasonic vibration of a certain frequency to the ball along the normal direction of the workpiece surface, combining the ultrasonic impact energy with the rolling action, and producing severe plastic deformation and work hardening on the surface of the metal material, thereby refining the grains on the surface of the material to form a surface strengthening layer, while generating a high surface compressive stress, and greatly reducing the surface roughness of the material, thereby obtaining a metal surface with high hardness, high wear resistance, high fatigue life, high surface finish and stress corrosion resistance. However, the existing ultrasonic rolling strengthening method has certain shortcomings: on the one hand, the hardness of the metal material is limited, and on the other hand, the depth of the introduced residual compressive stress layer is shallow, and there is still a lot of room for improvement in the mechanical properties of the metal material. In addition, for some high-hardness materials, due to their difficulty in plastic deformation, the effect of ultrasonic rolling is not very ideal, and ultrasonic rolling technology alone cannot achieve the expected purpose. Therefore, it is necessary to seek a more complete repair method for shaft parts.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide powder for laser cladding repair, a method for preparing the powder for laser cladding repair, and a method for repairing shaft parts.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides a method for repairing a shaft part, comprising: forming a cladding layer on the shaft part by laser cladding;
[0009] Electric pulses are applied to the shaft parts covered by the cladding layer, and ultrasonic rolling and post-processing are performed on the cladding layer to complete the repair of the shaft parts.
[0010] In an optional embodiment, the laser cladding step satisfies at least one of the following features ae:
[0011] a. The power of laser cladding equipment is 1~6kW;
[0012] b. The laser spot diameter of the laser cladding equipment is 0.5-2mm, the scanning rate is 20-200m / min, and the overlap rate is 45-60%;
[0013] c. The laser cladding step is carried out under a protective gas atmosphere;
[0014] d. The powder feeding gas pressure for laser cladding repair is 0.05~0.9MPa;
[0015] e. The thickness of the cladding layer is 0.5 to 5 mm.
[0016] In an optional embodiment, the pulse waveform of the electric pulse is a sharp wave, the electric pulse frequency is 200-700 Hz, the pulse width is 30-5000 μs, and the average current density is 0.5-30.0 A / mm 2 , Peak current density 5~60A / mm 2 .
[0017] In an optional embodiment, the ultrasonic rolling satisfies at least one of the following characteristics A to C:
[0018] A. Rolling speed is 5-100m / min, feed rate is 0.05-0.8mm / r;
[0019] B. Ultrasonic frequency 10-100kHz, amplitude 3-8μm;
[0020] C. The curvature radius of the rolling head is 5 to 7 mm, the static pressure is 200 to 2500 N, and the processing is 5 to 30 times.
[0021] Every time a cladding layer is formed on a shaft part by laser cladding, ultrasonic rolling is performed on the cladding layer.
[0022] In an optional embodiment, the alloy powder used in the laser cladding step includes 80-90 wt.% of high entropy alloy powder and 10-20 wt.% of titanium carbide reinforcement particles;
[0023] The chemical composition of the high entropy alloy powder includes, by mass percentage, Ti: 28-34wt.%, Zr: 26-29wt.%, Hf: 26-29.5wt.%, Nb: 4-6wt.%, Ta: 4-6wt.% and V: 2-4wt.%.
[0024] In an optional embodiment, the particle size of the high entropy alloy powder is 16 to 50 μm, the sphericity is ≥ 90%, and the oxygen content is ≤ 150 ppm;
[0025] And / or, the particle size of the titanium carbide reinforcement particles is 5 to 20 μm.
[0026] In an optional embodiment, the method for preparing the alloy powder comprises: ball milling and sieving a mixture of a high entropy alloy powder raw material and a titanium carbide reinforced particle raw material to obtain the powder for laser cladding repair.
[0027] Preferably, the ball milling speed is 10 to 400 r / min, the ball milling time is 2 to 16 h, and the ball milling atmosphere is an inert gas atmosphere;
[0028] Preferably, the particle size of the high entropy alloy powder raw material is 20 to 35 μm, and the particle size of the titanium carbide reinforced particle raw material is 8 to 12 μm.
[0029] In an optional embodiment, the shaft part to be repaired is subjected to a preheating treatment before forming the cladding layer; the preheating treatment satisfies at least one of the following characteristics ① to ③:
[0030] ① Preheating the surface temperature of the shaft parts to be repaired to 200-300°C;
[0031] ② The preheating treatment adopts a laser fast scanning preheating method, wherein the laser power is 4 to 6 kW;
[0032] ③ Before the preheating treatment, the shaft parts to be repaired are also cleaned and inspected to remove rust stains, failure sites, and fatigue layers on the surface, and then subjected to flaw detection and turning until there is no wear or crack layer on the surface.
[0033] In an optional embodiment, the post-processing step includes: sequentially performing laser cleaning, annealing correction, machining and strengthening on the shaft parts to be repaired after the cladding layer preparation and ultrasonic rolling; the post-processing satisfies at least one of the following characteristics ④ to ⑥:
[0034] ④ The laser cleaning power is 1-2kW, and the cleaning speed is 0.5-5m / min;
[0035] ⑤ In the annealing correction step, the surface temperature of the shaft parts to be repaired is 900-1000°C, and then air cooling is performed;
[0036] ⑥ The strengthening step adopts the electric pulse coupled ultrasonic rolling method.
[0037] The present invention has the following beneficial effects:
[0038] The repaired spindle surface of the present invention has high surface hardness, fatigue resistance, wear resistance and corrosion resistance, etc., which can effectively increase the service life of the spindle and achieve the purpose of repair. The process has high efficiency, simple operation, wide application range, and is convenient for industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0040] Figure 1 It is a schematic diagram of the electric pulse ultrasonic rolling laser cladding surface repair process of the present invention.
[0041] Figure 2 Microstructure of laser cladding surface strengthened and repaired by electric pulse assisted ultrasonic rolling.
[0042] Figure 3 Microstructure of the laser cladding surface repaired by traditional methods.
[0043] In the figure: 1-spindle to be repaired; 2-ultrasonic system; 3-manipulator; 4-conductive brush; 5-pulse power supply; 6-laser light source. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0045] An embodiment of the present invention provides a method for repairing a shaft part, comprising:
[0046] The cladding layer formed on shaft parts by laser cladding;
[0047] Electric pulses are applied to the shaft parts covered by the cladding layer, and ultrasonic rolling and post-processing are performed on the cladding layer to complete the repair of the shaft parts.
[0048] The embodiment of the present invention applies pulse current to the processing area of shaft parts, and uses the electroplastic effect, skin effect and thermal effect of the pulse current to sharply reduce the plastic deformation resistance of the surface layer of the processing area, and further regulate and optimize the microstructure of the material. Compared with the simple ultrasonic rolling processing technology, the surface of the cladding layer is strengthened by electric pulse-assisted ultrasonic rolling, which can obtain higher surface compressive stress, increase the depth of the strengthening layer, inhibit the initiation of surface microcracks during ultrasonic rolling, and obtain a higher quality surface, thereby greatly improving the material's fatigue resistance, friction and wear resistance, and corrosion resistance, and obtaining a higher damage tolerance.
[0049] The electroplastic effect, skin effect and thermal effect of pulse current can significantly reduce the resistance to plastic deformation of the surface layer of metal workpieces, reduce the degree of work hardening of the surface layer of workpieces, make the deformation layer undergo dynamic recovery or dynamic recrystallization, and further refine the surface grains of the workpiece, thereby further improving the surface hardness of the workpiece. At the same time, due to the reduction in the degree of work hardening of the surface layer, the plastic deformation capacity of the sub-surface layer of the workpiece is enhanced, and the grain refinement layer extends deeper into the surface layer under the action of ultrasonic rolling, further deepening the thickness of the strengthening layer. By applying ultrasonic rolling technology on the coating surface, the residual stress distribution state in the coating is changed, the coating microstructure is refined and homogenized, the surface roughness of the coating is significantly reduced, the overlap marks of multiple laser cladding are eliminated, the subsequent processing steps and costs are reduced, and the wear resistance, corrosion resistance and fatigue resistance of the coating are further improved.
[0050] The present invention performs laser cladding repair on the main shaft parts that have failed due to fatigue damage, and then regulates the repaired microstructure through electric-thermal-mechanical coupling ultrasonic rolling to greatly improve the anti-fatigue and friction and wear performance of the main shaft. The production process is simple and has good prospects for industrial production.
[0051] In an optional embodiment, the laser cladding step satisfies at least one of the following features ae:
[0052] a. The power of laser cladding equipment is 1-6kW; appropriate laser power helps to control the shape and size of the molten pool and improve the bonding strength of the cladding layer.
[0053] b. The laser spot diameter of the laser cladding equipment is 0.5-2mm, the scanning rate is 20-200m / min, and the overlap rate is 45-60%; the size of the spot diameter will affect the size and shape of the molten pool. A smaller spot diameter can produce a more concentrated heat source, which helps to form a finer cladding layer structure. The scanning speed affects the cooling rate of the molten pool and the thickness of the cladding layer.
[0054] c. The laser cladding step is carried out under a protective gas atmosphere;
[0055] d. The powder feeding gas pressure for laser cladding repair is 0.05~0.9MPa. The gas feeding pressure will affect the powder feeding rate and thus affect the thickness of the cladding layer.
[0056] e. The thickness of the cladding layer is 0.5 to 5 mm.
[0057] In an optional embodiment, the pulse waveform of the electric pulse is a sharp wave, the electric pulse frequency is 200-700 Hz, the pulse width is 30-5000 μs, and the average current density is 0.5-30.0 A / mm 2 , Peak current density 5~60A / mm 2 .
[0058] When the frequency, pulse width, average current density and peak current density of the electric pulse meet the above requirements, it is beneficial to control the electroplastic effect, skin effect and thermal effect of the pulse current within a reasonable range, thereby facilitating the acquisition of a metal surface with high hardness, high wear resistance, high fatigue life and high surface finish. In addition, the pulse waveform of the electric pulse is a sharp wave, which is beneficial to reduce the thermal effect to a certain extent, better control the change of current density, maintain a good electroplastic effect and reduce the skin effect.
[0059] In an optional embodiment, the ultrasonic rolling satisfies at least one of the following characteristics A to C:
[0060] A. The rolling speed is 5-100m / min, and the feed rate is 0.05-0.8mm / r; slower rolling speed and smaller feed rate help improve surface quality, but will reduce production efficiency; faster rolling speed and larger feed rate will reduce the impact of ultrasonic vibration on the surface.
[0061] B. Ultrasonic frequency 10-100kHz, amplitude 3-8μm;
[0062] C. The curvature radius of the rolling head is 5 to 7 mm, the static pressure is 200 to 2500 N, and the processing is 5 to 30 times. If the pressure applied during rolling is too small, the depth and hardness of the cladding layer surface will be reduced, and if it is too large, the surface of the workpiece will be damaged or deformed.
[0063] Each time a cladding layer is formed on a shaft part by laser cladding, the cladding layer is subjected to ultrasonic rolling. After laser cladding a layer, electric pulse ultrasonic rolling is performed alternately to ensure that each cladding layer is fully acted upon by electricity, heat, force and ultrasound.
[0064] In an optional embodiment, the alloy powder used in the laser cladding step includes 80-90 wt.% of high entropy alloy powder and 10-20 wt.% of titanium carbide reinforcement particles;
[0065] The chemical composition of the high entropy alloy powder includes, by mass percentage, Ti: 28-34wt.%, Zr: 26-29wt.%, Hf: 26-29.5wt.%, Nb: 4-6wt.%, Ta: 4-6wt.% and V: 2-4wt.%.
[0066] During the laser cladding process, high entropy alloy elements can quickly dissolve into the matrix material to form a supersaturated solid solution. This solid solution structure can effectively improve the hardness and strength of the repair layer. In particular, the addition of interstitial atoms can significantly increase the electron density between adjacent atoms and the elastic modulus of the multi-principal solid solution, thereby achieving a good solid solution strengthening effect. In addition to introducing alloying elements and interstitial elements to strengthen the matrix, titanium carbide reinforcement particles are added as new nucleation cores inside the grains, which can effectively inhibit the growth of grains and improve the performance of the cladding layer. The TaNbHfZrVTi cladding layer has a simple body-centered cubic supersaturated solid solution structure, and the hardness decreases less under high-temperature service conditions, showing good thermal stability. The precipitated phases formed in the high entropy alloy can hinder the movement of dislocations, especially the inhomogeneous precipitated phases, which can provide additional heterogeneous deformation-induced toughening effects during deformation, thereby improving the toughness of the coating.
[0067] High entropy alloy powder and ceramic reinforcement particles are used to repair and strengthen the damaged position of the damaged spindle surface by laser cladding, which can achieve continuous multi-layer repair, breaking through the limitation of the number of repair layers of conventional powder and process, and the dimensional accuracy of the repaired parts is high. The laser cladding layer can significantly improve the toughness of the repair layer by introducing high entropy alloy, which is mainly due to the combined effect of the solid solution strengthening, fine grain strengthening, grain boundary strengthening and precipitation phase strengthening mechanisms of high entropy alloy. The repaired structure is dense, without cracks and unmelted powder, etc., there is no obvious height difference between the welds and the bonding is good. The repaired spindle surface has high surface hardness, fatigue resistance, wear resistance and corrosion resistance, etc., which can effectively improve the service life of the spindle and achieve the purpose of repair. The process is highly efficient, simple to operate, has a wide range of applications, and is convenient for industrial production and application.
[0068] In an optional embodiment, the particle size of the high entropy alloy powder is 16 to 50 μm, the sphericity is ≥ 90%, and the oxygen content is ≤ 150 ppm;
[0069] And / or, the particle size of the titanium carbide reinforcement particles is 5 to 20 μm.
[0070] In an optional embodiment, the method for preparing the alloy powder comprises: ball milling and sieving a mixture of a high entropy alloy powder raw material and a titanium carbide reinforced particle raw material to obtain the powder for laser cladding repair.
[0071] Preferably, the ball milling speed is 10 to 400 r / min, the ball milling time is 2 to 16 h, and the ball milling atmosphere is an inert gas atmosphere;
[0072] Preferably, the particle size of the high entropy alloy powder raw material is 20 to 35 μm, and the particle size of the titanium carbide reinforced particle raw material is 8 to 12 μm.
[0073] In an optional embodiment, the shaft part to be repaired is subjected to a preheating treatment before forming the cladding layer; the preheating treatment satisfies at least one of the following characteristics ① to ③:
[0074] ① Preheating to a surface temperature of 200-300°C of the shaft parts to be repaired; preheating can reduce thermal stress and prevent the generation of cracks.
[0075] ② The preheating treatment adopts a laser fast scanning preheating method, wherein the laser power is 4 to 6 kW;
[0076] ③ Before the preheating treatment, the shaft parts to be repaired are also cleaned and inspected to remove rust stains, failure sites, and fatigue layers on the surface, and then subjected to flaw detection and turning until there is no wear or crack layer on the surface.
[0077] In an optional embodiment, the post-processing step includes: sequentially performing laser cleaning, annealing correction, machining and strengthening on the shaft parts to be repaired after the cladding layer preparation and ultrasonic rolling; the post-processing satisfies at least one of the following characteristics ④ to ⑥:
[0078] ④ The laser cleaning power is 1-2kW, and the cleaning speed is 0.5-5m / min;
[0079] ⑤ In the annealing correction step, the surface temperature of the shaft parts to be repaired is 900-1000℃, and then air-cooled; annealing correction is beneficial to eliminate stress, refine grains, improve organizational structure, and thus help improve the hardness, wear resistance, and bonding strength between shaft parts and the cladding layer.
[0080] ⑥ The strengthening step adopts the electric pulse coupled ultrasonic rolling method.
[0081] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0082] Example 1
[0083] The present invention provides a method for strengthening and repairing shaft parts by ultra-high-speed laser cladding, the method comprising the following steps:
[0084] S1. Inspection and preprocessing
[0085] The surface of the wind turbine main shaft is sandblasted to remove the oil and rust attached to the surface, and then the remaining rust is cleaned with sandpaper; the wear and failure parts and fatigue layer on the main shaft surface are then removed by turning, and a flaw detection inspection is performed every 0.5mm of turning until there is no wear or cracks on the surface; then the overall circular runout, ovality, wear degree and hardness test of the main shaft are checked; before laser cladding repair, the main shaft is laser preheated with a laser preheating power of 4kW and a scanning time of 10min.
[0086] S2, laser cladding and electric pulse ultrasonic rolling (schematic diagram as shown Figure 1 (shown)
[0087] Argon with a purity greater than 99.99% is used as the protective gas, the powder feeding pressure is 0.3MPa, and the powder feeding amount is 20g / min; the repair powder is baked and dried at a temperature of 160°C for 2 hours; the repair powder and ultra-high-speed laser cladding equipment are used for surface repair, and the laser power emitted by the laser light source 6 is 2kW; the thickness of the cladding layer is 2mm. The path trajectory of the laser cladding adopts a spiral trajectory (positive and negative) motion mode, and the laser cladding and electric pulse ultrasonic rolling are carried out alternately. The manipulator 3 is used to fix the main shaft 1 to be repaired, and the conductive brush 4 is respectively placed at both ends of the main shaft 1 to be repaired and connected to the positive and negative electrodes of the pulse power supply 5. Among them, the laser spot diameter is 1mm, the scanning rate is 20m / min, and the overlap rate is 50%. The ultrasonic system 2 emits an ultrasonic frequency of 30kHz and an amplitude of 8μm; the rolling speed is 15m / min, the feed amount is 0.3mm / r, and the preload force is 200N. The electric pulse waveform is a sharp wave, the electric pulse frequency is 300Hz, the pulse width is 50μs, and the average current density is 25A / mm 2 , Peak current density 50A / mm 2 . The preparation of the laser cladding repair powder used includes: weighing 80% of high entropy alloy powder (Ti: 29wt.%, Zr: 28wt.%, Hf: 29wt.%, Nb: 5wt.%, Ta: 5wt.%, V: 4wt.%) and 20% of titanium carbide reinforcement particles in proportion and mixing them evenly. A planetary ball mill is used with a speed of 200r / min and a ball milling time of 12h. Argon is introduced during the ball milling process for protection. After the ball milling is completed, the repair powder with a particle size of 15 to 50μm is obtained by sieving and grading through a 400-mesh sieve.
[0088] S3. Correction and post-processing
[0089] The spindle straightness and roundness after laser cladding repair are laser cleaned and corrected. The spindle laser cleaning power is 1.5kW, the cleaning speed is 1m / min, the spindle surface temperature is 950℃ for annealing correction, and then air cooling is performed; the turning thickness is 0.1mm, and then grinding is performed. The surface roughness of the spindle after grinding is Ra≤0.3, followed by electric pulse ultrasonic rolling. The appearance, dimensional accuracy and performance of the spindle are tested, and there should be no cracks, pores and bumps on the appearance surface. The dimensional accuracy must meet the upper deviation of 0 and the lower deviation of -0.03mm; the surface hardness is HRC 62.
[0090] The laser cladding repair strengthening layer prepared in this embodiment has a dense structure without cracks, and the bonding strength between the repair layer and the substrate is 525 MPa. Its average surface hardness is HRC 67, the surface roughness is Ra 0.18, and the residual internal stress is -221 MPa.
[0091] Example 2
[0092] The present invention provides a method for strengthening and repairing shaft parts by ultra-high-speed laser cladding, the method comprising the following steps:
[0093] S1. Inspection and preprocessing
[0094] The spindle surface is sandblasted to remove oil and rust attached to the surface, and then the remaining rust is cleaned with sandpaper; the wear and failure parts and fatigue layer on the spindle surface are removed by turning, and a flaw detection inspection is performed every 0.5mm of turning until there is no wear or cracks on the surface; then the overall circular runout, ovality, wear degree and hardness test of the spindle are checked; before laser cladding repair, the spindle is laser preheated with a laser preheating power of 4kW and a scanning time of 10min.
[0095] S2, Laser Cladding and Electric Pulse Ultrasonic Rolling
[0096] Argon with a purity greater than 99.99% is used as the protective gas, the powder feeding pressure is 0.3MPa, and the powder feeding amount is 20g / min; the repair powder is baked and dried at a temperature of 160°C for 2 hours; the repair powder and ultra-high-speed laser cladding equipment are used for surface repair, the laser power is 2kW; the thickness of the cladding layer is 3mm. The path trajectory of the laser cladding adopts a spiral trajectory (forward and reverse) motion mode, and the laser cladding and electric pulse ultrasonic rolling are carried out alternately. The brushes are placed at both ends of the shaft and connected to the positive and negative poles of the pulse power supply 5. The laser spot diameter is 1mm, the scanning rate is 30m / min, and the overlap rate is 50%. The ultrasonic system 2 emits an ultrasonic frequency of 30kHz and an amplitude of 8μm. The rolling speed is 15m / min, the feed rate is 0.3mm / r, and the preload force is 200N. The electric pulse waveform is a sharp wave, the electric pulse frequency is 300Hz, the pulse width is 50μs, and the average current density is 25A / mm 2 , Peak current density 50A / mm 2 The preparation method of the powder for laser cladding repair includes weighing 85% of high entropy alloy powder (Ti: 29wt.%, Zr: 28wt.%, Hf: 29wt.%, Nb: 5wt.%, Ta: 4wt.%, V: 5wt.%) and 15% of titanium carbide reinforcement particles in proportion and mixing them uniformly. The powder is milled in a planetary ball mill at a speed of 200r / min for 12h, and argon gas is introduced during the milling process for protection. After the milling is completed, the powder is sieved and graded through a 400-mesh sieve to obtain a repair powder with a particle size of 15 to 50μm.
[0097] S3. Correction and post-processing
[0098] The spindle straightness and roundness after laser cladding repair are laser cleaned and corrected. The spindle laser cleaning power is 1.5kW, the cleaning speed is 1m / min, the spindle surface temperature is 950℃ for annealing correction, and then air cooling is performed; the turning thickness is 0.1mm, and then grinding is performed. The surface roughness of the spindle after grinding is Ra≤0.3, followed by electric pulse ultrasonic rolling. The appearance, dimensional accuracy and performance of the spindle are tested, and there should be no cracks, pores and bumps on the appearance surface. The dimensional accuracy must meet the upper deviation of 0 and the lower deviation of -0.03mm; the surface hardness is HRC 62.
[0099] The laser cladding repair strengthening layer prepared in this embodiment has a dense structure without cracks, and the bonding strength between the repair layer and the substrate is 547 MPa. Its average surface hardness is HRC 65, the surface roughness is Ra 0.15, and the residual internal stress is -194 MPa.
[0100] Example 3
[0101] The present invention provides a method for strengthening and repairing shaft parts by ultra-high-speed laser cladding, the method comprising the following steps:
[0102] S1. Inspection and preprocessing
[0103] The spindle surface is sandblasted to remove oil and rust attached to the surface, and then the remaining rust is cleaned with sandpaper; the wear and failure parts and fatigue layer on the spindle surface are removed by turning, and a flaw detection inspection is performed every 0.5mm of turning until there is no wear or cracks on the surface; then the overall circular runout, ovality, wear degree and hardness test of the spindle are checked; before laser cladding repair, the spindle is laser preheated with a laser preheating power of 4kW and a scanning time of 10min.
[0104] S2, Laser Cladding and Electric Pulse Ultrasonic Rolling
[0105] Argon with a purity greater than 99.99% is used as the protective gas, the powder feeding pressure is 0.3MPa, and the powder feeding amount is 20g / min; the repair powder is baked and dried at a temperature of 160°C for 2 hours; the repair powder and ultra-high-speed laser cladding equipment are used for surface repair, the laser power is 2kW; the thickness of the cladding layer is 4mm. The path trajectory of the laser cladding adopts a spiral trajectory (positive and negative) motion mode, and the laser cladding and electric pulse ultrasonic rolling are carried out alternately. The brushes are placed at both ends of the shaft and connected to the positive and negative poles of the pulse power supply 5. The laser spot diameter is 1mm, the scanning rate is 40m / min, and the overlap rate is 50%. The ultrasonic system 2 emits an ultrasonic frequency of 30kHz and an amplitude of 8μm. The rolling speed is 15m / min, the feed rate is 0.3mm / r, and the preload force is 200N. The electric pulse waveform is a sharp wave, the electric pulse frequency is 300Hz, the pulse width is 50μs, and the average current density is 25A / mm 2 , Peak current density 50A / mm 2 The preparation method of the powder for laser cladding repair includes weighing 90% of high entropy alloy powder (Ti: 32wt.%, Zr: 27wt.%, Hf: 28wt.%, Nb: 4wt.%, Ta: 4wt.%, V: 5wt.%) and 10% of titanium carbide reinforcement particles in proportion and mixing them uniformly. The powder is milled in a planetary ball mill at a speed of 200r / min for 12h, and argon gas is introduced for protection during the milling process. After the milling is completed, the powder is sieved and graded through a 400-mesh sieve to obtain a repair powder with a particle size of 15 to 50μm.
[0106] S3. Correction and post-processing
[0107] The spindle straightness and roundness after laser cladding repair are laser cleaned and corrected. The spindle laser cleaning power is 1.5kW, the cleaning speed is 1m / min, the spindle surface temperature is 950℃ for annealing correction, and then air cooling is performed; the turning thickness is 0.1mm, and then grinding is performed. The surface roughness of the spindle after grinding is Ra≤0.3, followed by electric pulse ultrasonic rolling. The appearance, dimensional accuracy and performance of the spindle are tested, and there should be no cracks, pores and bumps on the appearance surface. The dimensional accuracy must meet the upper deviation of 0 and the lower deviation of -0.03mm; the surface hardness is HRC 62.
[0108] The laser cladding repair strengthening layer prepared in this embodiment has a dense structure without cracks, and the bonding strength between the repair layer and the substrate is 563 MPa. Its average surface hardness is HRC 64, the surface roughness is Ra 0.14, and the residual internal stress is -208 MPa.
[0109] Example 4
[0110] The difference between this embodiment and embodiment 1 is mainly that the electric pulse parameters are different, and the following steps are included:
[0111] S1. Inspection and preprocessing
[0112] The surface of the wind turbine main shaft is sandblasted to remove the oil and rust attached to the surface, and then the remaining rust is cleaned with sandpaper; the wear and failure parts and fatigue layer on the main shaft surface are then removed by turning, and a flaw detection inspection is performed every 0.5mm of turning until there is no wear or cracks on the surface; then the overall circular runout, ovality, wear degree and hardness test of the main shaft are checked; before laser cladding repair, the main shaft is laser preheated with a laser preheating power of 4kW and a scanning time of 10min.
[0113] S2, Laser Cladding and Electric Pulse Ultrasonic Rolling
[0114] Argon with a purity greater than 99.99% is used as the protective gas, the powder feeding pressure is 0.3MPa, and the powder feeding amount is 20g / min; the repair powder is baked and dried at a temperature of 160°C for 2 hours; the repair powder and ultra-high-speed laser cladding equipment are used for surface repair, and the laser power emitted by the laser light source 6 is 2kW; the thickness of the cladding layer is 2mm. The path trajectory of the laser cladding adopts a spiral trajectory (positive and negative) motion mode, and the laser cladding and electric pulse ultrasonic rolling are carried out alternately. The manipulator 3 is used to fix the main shaft 1 to be repaired, and the conductive brush 4 is respectively placed at both ends of the main shaft 1 to be repaired and connected to the positive and negative electrodes of the pulse power supply 5. Among them, the laser spot diameter is 1mm, the scanning rate is 20m / min, and the overlap rate is 50%. The ultrasonic system 2 emits an ultrasonic frequency of 30kHz and an amplitude of 8μm; the rolling speed is 15m / min, the feed amount is 0.3mm / r, and the preload force is 200N. The electric pulse waveform is a sharp wave, the electric pulse frequency is 500Hz, the pulse width is 50μs, and the average current density is 20A / mm 2 , Peak current density 50A / mm 2 . The preparation of the laser cladding repair powder used includes: weighing 80% of high entropy alloy powder (Ti: 29wt.%, Zr: 28wt.%, Hf: 29wt.%, Nb: 5wt.%, Ta: 5wt.%, V: 4wt.%) and 20% of titanium carbide reinforcement particles in proportion and mixing them evenly. A planetary ball mill is used with a speed of 200r / min and a ball milling time of 12h. Argon is introduced during the ball milling process for protection. After the ball milling is completed, the repair powder with a particle size of 15 to 50μm is obtained by sieving and grading through a 400-mesh sieve.
[0115] S3. Correction and post-processing
[0116] The spindle straightness and roundness after laser cladding repair are laser cleaned and corrected. The spindle laser cleaning power is 1.5kW, the cleaning speed is 1m / min, the spindle surface temperature is 950℃ for annealing correction, and then air cooling is performed; the turning thickness is 0.1mm, and then grinding is performed. The surface roughness of the spindle after grinding is Ra≤0.3, followed by electric pulse ultrasonic rolling. The appearance, dimensional accuracy and performance of the spindle are tested, and there should be no cracks, pores and bumps on the appearance surface. The dimensional accuracy must meet the upper deviation of 0 and the lower deviation of -0.03mm; the surface hardness is HRC 62.
[0117] The laser cladding repair strengthening layer prepared in this embodiment has a dense structure without cracks, and the bonding strength between the repair layer and the substrate is 554 MPa. Its average surface hardness is HRC 62, the surface roughness is Ra 0.21, and the residual internal stress is -196 MPa.
[0118] Comparative Example 1
[0119] The main difference between this comparative example and Example 1 is that no electric pulse and ultrasonic rolling treatment are applied to the spindle, and the following steps are included:
[0120] A laser cladding repair powder is prepared by weighing 80% of high entropy alloy powder (Ti: 29wt.%, Zr: 28wt.%, Hf: 29wt.%, Nb: 5wt.%, Ta: 5wt.%, V: 4wt.%) and 20% of titanium carbide reinforcement particles in proportion and uniformly mixing them. A planetary ball mill is used with a rotation speed of 200r / min and a ball milling time of 12h. Argon is introduced during the ball milling process for protection. After the ball milling is completed, the repair powder is sieved and classified through a 400-mesh screen to obtain a particle size of 15 to 50μm.
[0121] The present invention provides a method for strengthening and repairing shaft parts by ultra-high-speed laser cladding, the method comprising the following steps:
[0122] S1. Inspection and preprocessing
[0123] The spindle surface is sandblasted to remove oil and rust attached to the surface, and then the remaining rust is cleaned with sandpaper; the wear and failure parts and fatigue layer on the spindle surface are removed by turning, and a flaw detection inspection is performed every 0.5mm of turning until there is no wear or cracks on the surface; then the overall circular runout, ovality, wear degree and hardness test of the spindle are checked; before laser cladding repair, the spindle is laser preheated with a laser preheating power of 4kW and a scanning time of 10min.
[0124] S2. Laser cladding
[0125] Argon with a purity greater than 99.99% is used as the protective gas, the powder feeding pressure is 0.3MPa, and the powder feeding amount is 20g / min; the repair powder is baked and dried at a temperature of 160°C for 2 hours; the repair powder and ultra-high-speed laser cladding equipment are used for surface repair, the laser power is 2kW; the cladding layer thickness is 2mm. The laser spot diameter is 1mm, the scanning rate is 20m / min, and the overlap rate is 50%.
[0126] S3. Correction and post-processing
[0127] The spindle straightness and roundness after laser cladding repair are laser cleaned and corrected. The spindle laser cleaning power is 1.5kW, the cleaning speed is 1m / min, the spindle surface temperature is 950℃ for annealing correction, and then air cooling is performed; the turning thickness is 0.1mm, and then grinding is performed. The surface roughness of the spindle after grinding is Ra≤0.3. The appearance, dimensional accuracy and performance of the spindle are tested, and there should be no cracks, pores and bumps on the appearance surface. The dimensional accuracy must meet the upper deviation of 0 and the lower deviation of -0.03mm; the surface hardness is HRC 62.
[0128] The laser cladding repair layer prepared in this comparative example has a dense structure with microcracks, a bonding strength of 529 MPa between the repair layer and the substrate, an average surface hardness of HRC 62, a surface roughness of Ra 0.44, and a residual internal stress of 239 MPa.
[0129] Comparative Example 2
[0130] The main difference between this comparative example and Example 1 is that no electric pulse is applied to the spindle during the ultrasonic rolling process, and specifically includes the following steps:
[0131] S1. Inspection and preprocessing
[0132] The surface of the wind turbine main shaft is sandblasted to remove the oil and rust attached to the surface, and then the remaining rust is cleaned with sandpaper; the wear and failure parts and fatigue layer on the main shaft surface are then removed by turning, and a flaw detection inspection is performed every 0.5mm of turning until there is no wear or cracks on the surface; then the overall circular runout, ovality, wear degree and hardness test of the main shaft are checked; before laser cladding repair, the main shaft is laser preheated with a laser preheating power of 4kW and a scanning time of 10min.
[0133] S2, Laser Cladding and Ultrasonic Rolling
[0134] Argon with a purity greater than 99.99% is used as the protective gas, the powder feeding pressure is 0.3MPa, and the powder feeding amount is 20g / min; the repair powder is baked and dried at a temperature of 160°C for 2 hours; the repair powder and ultra-high-speed laser cladding equipment are used for surface repair, and the laser power emitted by the laser light source 6 is 2kW; the thickness of the cladding layer is 2mm. The path trajectory of the laser cladding adopts a spiral trajectory (positive and negative) motion mode, and the laser cladding and ultrasonic rolling are carried out alternately. The manipulator 3 is used to fix the main shaft 1 to be repaired. Among them, the laser spot diameter is 1mm, the scanning rate is 20m / min, and the overlap rate is 50%. The ultrasonic system 2 emits an ultrasonic frequency of 30kHz and an amplitude of 8μm; the rolling speed is 15m / min, the feed rate is 0.3mm / r, and the preload force is 200N. The preparation of the laser cladding repair powder used includes: weighing 80% of high entropy alloy powder (Ti: 29wt.%, Zr: 28wt.%, Hf: 29wt.%, Nb: 5wt.%, Ta: 5wt.%, V: 4wt.%) and 20% of titanium carbide reinforcement particles in proportion and mixing them uniformly. A planetary ball mill is used at a speed of 200r / min and a ball milling time of 12h. Argon is introduced during the ball milling process for protection. After the ball milling is completed, the repair powder with a particle size of 15 to 50μm is obtained by sieving and grading through a 400-mesh screen.
[0135] S3. Correction and post-processing
[0136] The spindle straightness and roundness after laser cladding repair are laser cleaned and corrected. The spindle laser cleaning power is 1.5kW, the cleaning speed is 1m / min, the spindle surface temperature is 950℃ for annealing correction, and then air cooling is performed; the turning thickness is 0.1mm, and then grinding is performed. The surface roughness of the spindle after grinding is Ra≤0.3, followed by electric pulse ultrasonic rolling. The appearance, dimensional accuracy and performance of the spindle are tested, and there should be no cracks, pores and bumps on the appearance surface. The dimensional accuracy must meet the upper deviation of 0 and the lower deviation of -0.03mm; the surface hardness is HRC 62.
[0137] The laser cladding repair layer prepared in this comparative example has a dense structure with microcracks, a bonding strength of 531 MPa between the repair layer and the substrate, an average surface hardness of HRC 63, a surface roughness of Ra 0.47, and a residual internal stress of 254 MPa.
[0138] Some properties of the repaired spindles in the above embodiments and comparative examples are shown in Table 1.
[0139] Table 1
[0140]
[0141] The microstructures of the laser cladding samples obtained in Example 1 and Comparative Example 1 are compared. Figure 2 and Figure 3 As shown, the sample in Example 1 that uses electric pulse ultrasonic rolling to regulate the repair layer organization is denser and has no microcracks than the sample in Comparative Example 1. This is because the electroplastic effect, skin effect and thermal effect of the pulse current can significantly reduce the plastic deformation resistance of the surface layer of the metal workpiece, reduce the degree of work hardening of the surface layer of the workpiece, and make the machined deformation layer undergo dynamic recovery or dynamic recrystallization, which promotes further refinement of the surface grains of the workpiece, thereby further improving the surface hardness of the workpiece. When the pulse current passes through the metal material, a large number of directional drifting free electrons (electron wind) will be generated. These drifting electron groups frequently and directionally collide with dislocations in the material, generating an electron wind force similar to an applied stress on the dislocations, and promoting the movement of the dislocations on their slip planes. At the same time, the random thermal motion of atoms obtains enough kinetic energy to leave the equilibrium position under the instantaneous impact force of the pulse current, the diffusion capacity of atoms is enhanced, and dislocations are more likely to slip and climb, thereby improving the plasticity of the metal. At the same time, due to the reduction of the degree of surface hardening, the plastic deformation ability of the sub-surface layer of the workpiece is enhanced, and the grain refinement layer expands deeper into the surface under the action of ultrasonic rolling, further deepening the thickness of the strengthening layer. By applying the ultrasonic rolling process on the surface of the repair layer, the residual stress distribution state in the repair layer is changed, the microstructure of the repair layer is refined and homogenized, the surface roughness of the repair layer is significantly reduced, and the overlap marks of multiple laser cladding are eliminated.
[0142] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for repairing shaft parts, characterized in that: Including a cladding layer formed on a shaft part by laser cladding; Electric pulses are applied to the shaft parts covered by the cladding layer, and ultrasonic rolling and post-processing are performed on the cladding layer to complete the repair of the shaft parts.
2. The method for repairing shaft parts according to claim 1, characterized in that: The laser cladding step satisfies at least one of the following features: a. The power of laser cladding equipment is 1~6kW; b. The laser spot diameter of the laser cladding equipment is 0.5-2mm, the scanning rate is 20-200m / min, and the overlap rate is 45-60%; c. Laser cladding is carried out under a protective gas atmosphere; d. The powder feeding gas pressure for laser cladding repair is 0.05~0.9MPa; e. The thickness of the cladding layer is 0.5 to 5 mm.
3. The method for repairing shaft parts according to claim 1, characterized in that: The electric pulse has a sharp waveform, an electric pulse frequency of 200-700 Hz, a pulse width of 30-5000 μs, and an average current density of 0.5-30.0 A / mm 2 , Peak current density 5~60A / mm 2 .
4. The method for repairing shaft parts according to claim 1, characterized in that: The ultrasonic rolling meets at least one of the following characteristics A to C: A. Rolling speed is 5-100m / min, feed rate is 0.05-0.8mm / r; B. Ultrasonic frequency 10-100kHz, amplitude 3-8μm; C. The curvature radius of the rolling head is 5 to 7 mm, the static pressure is 200 to 2500 N, and the processing is 5 to 30 times.
5. The method for repairing shaft parts according to claim 1, characterized in that: Every time a cladding layer is formed on a shaft part by laser cladding, ultrasonic rolling is performed on the cladding layer.
6. The method for repairing shaft parts according to claim 1, characterized in that: The alloy powder used in the laser cladding comprises 80-90wt.% of high entropy alloy powder and 10-20wt.% of titanium carbide reinforcement particles; The chemical composition of the high entropy alloy powder includes, by mass percentage, Ti: 28-34wt.%, Zr: 26-29wt.%, Hf: 26-29.5wt.%, Nb: 4-6wt.%, Ta: 4-6wt.% and V: 2-4wt.%.
7. The method for repairing shaft parts according to claim 6, characterized in that: The high entropy alloy powder has a particle size of 16 to 50 μm, a sphericity of ≥ 90%, and an oxygen content of ≤ 150 ppm; And / or, the particle size of the titanium carbide reinforcement particles is 5 to 20 μm.
8. The method for repairing shaft parts according to claim 6, characterized in that: The preparation method of the alloy powder comprises: ball milling and sieving a mixture of a high entropy alloy powder raw material and a titanium carbide reinforced particle raw material to obtain the powder for laser cladding repair; Preferably, the ball milling speed is 10 to 400 r / min, the ball milling time is 2 to 16 h, and the ball milling atmosphere is an inert gas atmosphere; Preferably, the particle size of the high entropy alloy powder raw material is 20 to 35 μm, and the particle size of the titanium carbide reinforced particle raw material is 8 to 12 μm.
9. The method for repairing shaft parts according to claim 1, characterized in that: The shaft parts to be repaired are preheated before forming the cladding layer; the preheating treatment satisfies at least one of the following characteristics ① to ③: ① Preheating the surface temperature of the shaft parts to be repaired to 200-300°C; ② The preheating treatment adopts a laser fast scanning preheating method, wherein the laser power is 4 to 6 kW; ③ Before the preheating treatment, the shaft parts to be repaired are also cleaned and inspected to remove rust stains, failure sites, and fatigue layers on the surface, and then subjected to flaw detection and turning until there is no wear or crack layer on the surface.
10. The method for repairing shaft parts according to claim 1, characterized in that: The post-processing step includes: sequentially performing laser cleaning, annealing correction, machining and strengthening on the shaft parts to be repaired after the cladding layer preparation and ultrasonic rolling; the post-processing satisfies at least one of the following characteristics ④ to ⑥: ④ The laser cleaning power is 1-2kW, and the cleaning speed is 0.5-5m / min; ⑤ In the annealing correction step, the surface temperature of the shaft parts to be repaired is 900-1000°C, and then air cooling is performed; ⑥ The strengthening step adopts the electric pulse coupled ultrasonic rolling method.
Citation Information
Cited By
Electric arc additive remanufacturing repairing method for sliding bearing of LNG low-temperature immersed pump
CN119820246A
Welding machine for repairing abrasion of main shaft of large equipment and machining method of welding machine
CN120663068A
Large equipment main shaft wear repair welding machine and processing method thereof
CN120663068B
Repair method for shaft parts
CN121131786A