Carbon-ceramic brake disc with double friction layers and preparation method of carbon-ceramic brake disc
By adopting a double-layer friction layer structure on the carbon ceramic brake disc, the distribution of silicon carbide and silicon content is optimized, and the problem of poor bonding between the friction layer and the substrate layer is solved, the wear resistance and service life of the brake disc is improved, and the Production process.
Patent Information
- Application Number
- CN202411063771.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The friction layer of the existing carbon ceramic brake disc is not well combined with the substrate layer, which causes the friction layer to peel off easily during use, affecting the wear resistance and service life of the brake disc.
A double-layer friction layer structure is adopted, in which the second friction layer has a high silicon carbide content, a large particle size and a large thermal expansion coefficient. As the outermost layer, the inner layer is the first friction layer and the silicon carbide content is low. By adjusting the friction layer thickness The thickness of the second friction layer is optimized with the relationship between silicon carbide and silicon content, and the bonding force between the friction layer and the substrate layer is improved.
It effectively improves the wear resistance of the brake disc and the bonding strength between the friction layer and the substrate layer, avoids the peeling of the friction layer, extends the service life of the brake disc, simplifies the production process, and reduces the difficulty of detection.
Smart Images

Figure BDA0004978772140000021 
Figure BDA0004978772140000051 
Figure BDA0004978772140000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of brake disc manufacturing, and in particular to a carbon-ceramic brake disc with a double friction layer and a preparation method thereof. Background Art
[0002] Brake discs are mainly used to slow down or stop cars in an emergency. They are particularly important because they are related to human life safety in emergencies. Since braking will produce a short-term large impact friction and generate a lot of heat energy, the material of the brake disc should have properties such as heat resistance, impact resistance, fatigue resistance, and high strength. Cf / SiC composites can be used as brake parts in the aviation and high-end automotive industries due to their high hardness, superior friction performance, and the ability to significantly reduce the mass of friction brake materials. Carbon ceramic brake discs combine the physical properties of carbon fiber and polycrystalline silicon carbide. The elongation at break of C / SiC materials ranges from 0.1% to 0.3%, which is an extremely high value for ceramic materials. At the same time, due to its light weight, good hardness, stability under high pressure and high temperature conditions, thermal shock resistance, and iso-toughness shear fracture characteristics, it not only extends the service life of the brake disc, but also avoids most of the problems caused by load.
[0003] At present, the preparation process of carbon ceramic brake discs is needle puncture-carbonization-high temperature treatment-chemical vapor deposition-high temperature treatment-application of friction layer-processing-siliconization-processing, wherein the application of the friction layer is to improve the wear resistance of the brake disc and stabilize the friction coefficient. The silicon carbide content and fiber content of the friction layer and the brake disc are very different. Due to the high wear resistance requirements of the friction layer, it often does not contain carbon fiber and the silicon carbide content reaches more than 80%, resulting in a large difference in thermal expansion coefficient between it and the matrix. During the cooling process, there is a large residual stress in the friction layer, which makes the friction layer easy to peel off during use. In this regard, a carbon ceramic brake disc with a double friction layer is proposed to improve the bonding problem between the friction layer and the matrix layer. Summary of the invention
[0004] The purpose of the present invention is to provide a carbon-ceramic brake disc with a double friction layer and a preparation method thereof. By setting two friction layers, the thickness of the friction layer is optimized, the bonding force between the friction layer and the substrate is improved, the bonding strength between the friction layer and the substrate layer is effectively improved, and the wear resistance of the brake disc is improved.
[0005] To achieve this object, the present invention provides a carbon-ceramic brake disc with a double friction layer, the carbon-ceramic brake disc comprises a base layer and a friction layer, the friction layer comprises a first friction layer and a second friction layer, the first friction layer is located between the base layer and the second friction layer; the thickness of the first friction layer is t fr1 , silicon carbide content is v SiC1 , silicon content is v Si1; The thickness of the second friction layer is t fr2 , silicon carbide content is v SiC2 , silicon content is v Si2 , then the thickness of the second friction layer t fr2 Satisfies the following formula:
[0006]
[0007] Among them, the coefficient β is 0.9 or 5, ΔT is the difference between the siliconizing temperature and the room temperature, and ΔT is 1600k.
[0008] Preferably, the silicon carbide content in the first friction layer is 50-80%, and the silicon content is 20-50%; the silicon carbide content in the second friction layer is 70-95%, and the silicon content is 5-30%.
[0009] Preferably, the first friction layer comprises coarse silicon carbide with a particle size of 40-80 microns and fine silicon carbide with a particle size of 0.5-30 microns.
[0010] Preferably, the volume ratio of the coarse silicon carbide to the fine silicon carbide is 1:1-10:1.
[0011] Preferably, the second friction layer comprises second coarse silicon carbide with a particle size of 80-150 microns and second fine silicon carbide with a particle size of 0.5-30 microns.
[0012] Preferably, the volume ratio of the second coarse silicon carbide to the second fine silicon carbide is 1:1-10:1.
[0013] The present invention also provides a method for preparing a carbon-ceramic brake disc having a double friction layer, which is used to prepare the carbon-ceramic brake disc having a double friction layer, comprising the following steps:
[0014] S1: Repeatedly overlap the carbon fiber unidirectional cloth and the carbon fiber mesh tire to obtain a carbon fiber preform, and each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh tire are stacked and needle-punched, with a needle-punching density of 50-200 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°;
[0015] S2: impregnating the carbon fiber preform in a 40 wt % phenolic resin alcohol solution, and drying the preform until the alcohol is completely volatilized to obtain an impregnated body;
[0016] S3: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900° C. for 6 hours;
[0017] S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours;
[0018] S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, evenly laying the first friction layer pressed powder on the graphitized green body, and pressing at a temperature of 90° C. for 30 minutes to obtain a first green body with a pressure greater than 10 MPa;
[0019] S6: mixing silicon carbide powder and phenolic powder evenly to obtain second friction layer pressed powder, evenly laying the second friction layer pressed powder on the first green body, pressing at a temperature of 150° C. for 60 minutes to completely solidify it to obtain a second green body, and the pressure is greater than 10 MPa;
[0020] S7: machining the second blank to obtain a brake disc blank;
[0021] S8: Put the brake disc blank into a boron nitride crucible and then into a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and the size is processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible. The siliconizing treatment temperature is 1600-1700°C, the insulation time is 2-4h, and the furnace pressure is less than 1000Pa.
[0022] Preferably, steps S2 and S3 are performed at least once to make the density of the carbonized body reach 1.25-1.45 g / cm 3 .
[0023] Preferably, the silicon carbide particle size in the pressed powder of the first friction layer is 40-80 microns, the silicon carbide powder content is 35-55 vol%, and the phenolic powder content is 45-65 vol%.
[0024] Preferably, the silicon carbide particle size in the pressed powder of the second friction layer is 80-150 microns, the silicon carbide powder content is 45-75 vol%, and the phenolic powder content is 25-55 vol%.
[0025] Beneficial effect: The carbon ceramic brake disc with double friction layers provided by the present invention has two friction layers, the outermost friction layer is the second friction layer, the second friction layer has a high silicon carbide content, a large thermal expansion coefficient, a large particle size, and good wear resistance, and the inner friction layer is the first friction layer, the silicon carbide content of the first friction layer is lower than that of the second friction layer, and has a lower thermal expansion coefficient, which effectively alleviates the problem of stress concentration caused by the connection between the high silicon carbide friction layer and the substrate, thereby avoiding the phenomenon of separation of the friction layer and the substrate layer due to stress concentration in the working state. Further, by establishing a relationship between the silicon carbide, silicon content and thickness between the first friction layer and the second friction layer, the preferred range of the thickness of the second friction layer under different conditions can be obtained, and the bonding strength of the friction layer and the substrate layer can be improved by adjusting the thickness of the friction layer, which not only improves the friction resistance of the brake disc but also prevents the friction layer from detaching, achieving a win-win situation. According to this relationship, during the production process, the theoretical thickness range of the second friction layer can be calculated by testing the silicon carbide content, silicon content, actual thickness value of the first friction layer and the silicon carbide content and silicon content of the second friction layer of the product. By comparing the actual value of the second friction layer with the theoretical value of the friction layer thickness, technical personnel can be assisted in judging the qualification of the brake disc and reducing the difficulty of detection.
[0026] The present invention also proposes a method for preparing a carbon ceramic brake disc with a double friction layer, which is pressed twice after carbonization treatment, and each pressing adopts a pressing powder mixed with different contents of silicon carbide powder and phenolic powder, thereby realizing the manufacture of two friction layers. The pressing temperature of the outer friction layer is higher and the pressing time is longer. The two-step pressing is beneficial to improve the connection strength between the two friction layers and the substrate, and reduce the probability of separation between the friction layer and the substrate layer. The entire preparation process is simple, does not require chemical vapor deposition treatment, adopts low-temperature graphite conversion, has a simple process, is relatively low in process difficulty, and is easy to mass produce. DETAILED DESCRIPTION
[0027] The embodiments described below are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] This embodiment provides a carbon-ceramic brake disc with a double friction layer, the carbon-ceramic brake disc includes a base layer and a friction layer, the friction layer includes a first friction layer and a second friction layer, the first friction layer is located between the base layer and the second friction layer; the thickness of the first friction layer is t fr1 , silicon carbide content is v SiC1 , silicon content is v Si1 ; The thickness of the second friction layer is t fr2 , silicon carbide content is v SiC2 , silicon content is vSi2 , then the thickness of the second friction layer t fr2 Satisfies the following formula:
[0029]
[0030] Among them, the coefficient β is 0.9 or 5, ΔT is the difference between the siliconizing temperature and the room temperature, and ΔT is 1600k.
[0031] The silicon carbide content in the first friction layer is 50-80%, and the silicon content is 20-50%; the silicon carbide content in the second friction layer is 70-95%, and the silicon content is 5-30%.
[0032] The first friction layer includes coarse silicon carbide with a particle size of 40-80 microns and fine silicon carbide with a particle size of 0.5-30 microns.
[0033] The volume ratio of the coarse silicon carbide to the fine silicon carbide is 1:1-10:1. The volume ratio of the coarse silicon carbide to the fine silicon carbide includes but is not limited to 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1. Further preferably, the volume ratio of the coarse silicon carbide to the fine silicon carbide is selected to be 2:1 or 3:1 or 4:1 or 5:1 or 6:1, because within this ratio range, the coarse / fine silicon carbide mixture has a higher packing density (the fine powder exists between the gaps of the coarse powder, and the packing density is high).
[0034] The second friction layer includes second coarse silicon carbide with a particle size of 80-150 microns and second fine silicon carbide with a particle size of 0.5-30 microns.
[0035] The volume ratio of the second coarse silicon carbide to the second fine silicon carbide is 1:1-10:1. The volume ratio of the second coarse silicon carbide to the second fine silicon carbide includes but is not limited to 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1. Further preferably, the volume ratio of coarse silicon carbide to fine silicon carbide is 2:1 or 3:1 or 4:1 or 5:1 or 6:1.
[0036] The present invention also provides a method for preparing a carbon-ceramic brake disc having a double friction layer, which is used to prepare the carbon-ceramic brake disc having a double friction layer, comprising the following steps:
[0037] S1: Repeatedly overlap the carbon fiber unidirectional cloth and the carbon fiber mesh tire to obtain a carbon fiber preform, and each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh tire are stacked and needle-punched, with a needle-punching density of 50-200 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°;
[0038] S2: impregnating the carbon fiber preform in a 40wt% phenolic resin alcohol solution, and drying the impregnated body after impregnation until the alcohol is completely volatilized, wherein the impregnation time is generally 2-5h, preferably 3-4h, and the impregnation time is selected based on the standard of soaking the carbon fiber preform;
[0039] S3: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900° C. for 6 hours;
[0040] S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours;
[0041] S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, evenly laying the first friction layer pressed powder on the graphitized green body, and pressing at a temperature of 90° C. for 30 minutes to obtain a first green body with a pressure greater than 10 MPa;
[0042] S6: mixing silicon carbide powder and phenolic powder evenly to obtain second friction layer pressed powder, evenly laying the second friction layer pressed powder on the first green body, pressing at a temperature of 150° C. for 60 minutes to completely solidify it to obtain a second green body, and the pressure is greater than 10 MPa;
[0043] S7: machining the second blank to obtain a brake disc blank;
[0044] S8: Put the brake disc blank into a boron nitride crucible and then into a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and the size is processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible. The siliconizing treatment temperature is 1600-1700°C, the insulation time is 2-4h, and the furnace pressure is less than 1000Pa.
[0045] Steps S2 and S3 are performed at least once, so that the density of the carbonized body reaches 1.25-1.45 g / cm 3 .
[0046] The silicon carbide particle size in the pressed powder of the first friction layer is 40-80 microns, the silicon carbide powder content is 35-55 vol%, and the phenolic powder content is 45-65 vol%.
[0047] The silicon carbide particle size in the pressed powder of the second friction layer is 80-150 microns, the silicon carbide powder content is 45-75 vol%, and the phenolic powder content is 25-55 vol%.
[0048] The stress formula between the first friction layer and the second friction layer is as follows:
[0049]
[0050] E is Young's modulus, P is Poisson's coefficient;
[0051] For the interface between the first friction layer and the second friction layer, the residual stress generated by the mismatch of thermal expansion coefficients is:
[0052]
[0053] Where E fr1 is the Young's modulus of the first friction layer, P fr1 is the Poisson coefficient of the first friction layer, t fr1 is the thickness of the first friction layer;
[0054] E fr2 is the Young's modulus of the second friction layer, P fr2 is the Poisson coefficient of the second friction layer, t fr2 is the thickness of the second friction layer.
[0055] E fr2 =v SiC2 E SiC2 +v Si2 E Si2 =440v SiC2 +190v Si2
[0056] P fr2 =v SiC2 P SiC2 +v Si2 P Si2 =0.22v SiC2 +0.28v Si2
[0057] α fr2 =v SiC2 α SiC +v Si2 α Si =4×10 -6 v SiC2 +2.4×10 -6 v Si2
[0058] E fr1 =v SiC1 E SiC1 +v Si1 E Si1 =440v SiC1 +190v Si1
[0059] P fr1 =v SiC1 P SiC1 +vSi1 P Si1 =0.22v SiC1 +0.28v Si1
[0060] α fr1 =v SiC1 α SiC +v Si1 α Si =4×10 -6 v SiC1 +2.4×10 -6 v Si1
[0061] Bring in:
[0062]
[0063] We can get:
[0064]
[0065] Among them, ΔT is 1600k, σ c It should be between 20-60MPa. If the second friction layer is too thin, large residual stress is likely to occur, causing the friction layer to peel off. Experimental measurements show that residual stress of the friction layer between 20-60MPa will cause cracking of the friction layer. To avoid cracking, we use the minimum residual stress value for calculation:
[0066]
[0067] Multiply the above formula by the coefficient β. The thickness calculated without adding the empirical coefficient 0.9-5 is the thickness of the friction layer when the residual stress is within a limited range (i.e., no cracks appear). During preparation, microscopic defects may cause local gravity concentration and lead to cracking, which is difficult to avoid. Therefore, we increase the coefficient β, that is, the thickness of the second friction layer calculated within the maximum and minimum range of β, which can better ensure the strength of the friction layer and is not easy to cause cracking of the friction layer even in the presence of cracks.
[0068] If the thickness of the second friction layer is too thick, it will not only increase the weight of the brake disc, but also easily cause the friction layer to peel off under the shear force of friction. Therefore, the maximum value of the second friction layer shall not exceed 10mm.
[0069] Example 1
[0070] This embodiment provides a carbon-ceramic brake disc with a double friction layer. The steps of preparing the carbon-ceramic brake disc with a double friction layer are as follows:
[0071] S1: The carbon fiber unidirectional cloth and the carbon fiber mesh are repeatedly overlapped to obtain a carbon fiber preform. Each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh are overlapped and then needle-punched. The needle-punching density is 150 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°;
[0072] S2: impregnating the carbon fiber preform in a 40 wt % phenolic resin alcohol solution, and drying the preform until the alcohol is completely volatilized to obtain an impregnated body;
[0073] S3: The impregnated body is carbonized to obtain a carbonized body at a carbonization temperature of 900°C for 6 hours. Steps S2 and S3 are repeated until the density of the carbonized body reaches 1.4 g / cm 3 ;
[0074] S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours;
[0075] S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, wherein the silicon carbide particle size of the first friction layer pressed powder is 50 μm, the silicon carbide content is 45 vol%, and the phenolic powder is 55 vol%, and the first friction layer pressed powder is evenly laid on the graphitized blank, and pressed at a temperature of 90° C. for 30 min to obtain a first blank, the pressure is 12 MPa, and the thickness after pressing is 0.22 mm;
[0076] S6: mixing silicon carbide powder and phenolic powder evenly to obtain a second friction layer pressed powder, wherein the silicon carbide particle size of the second friction layer pressed powder is 100 μm, the silicon carbide content is 60 vol%, and the phenolic powder is 40 vol%. The second friction layer pressed powder is evenly laid on the first blank, and pressed at a temperature of 150° C. for 60 min to completely solidify it to obtain a second blank, and the pressure is 14 MPa, and the thickness after pressing is 0.8 mm;
[0077] S7: Mechanically processing the second blank to obtain a brake disc blank, and preparing features such as ventilation channels of the product;
[0078] S8: The brake disc blank is placed in a boron nitride crucible and then in a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and dimensionally processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the insulation time is 3h, and the furnace pressure is less than 1000Pa.
[0079] Example 2
[0080] This embodiment provides a carbon-ceramic brake disc with a double friction layer. The steps of preparing the carbon-ceramic brake disc with a double friction layer are as follows:
[0081] S1: The carbon fiber unidirectional cloth and the carbon fiber mesh are repeatedly overlapped to obtain a carbon fiber preform. Each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh are overlapped and then needle-punched. The needle-punching density is 150 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°;
[0082] S2: impregnating the carbon fiber preform in a 40 wt % phenolic resin alcohol solution, and drying the preform until the alcohol is completely volatilized to obtain an impregnated body;
[0083] S3: The impregnated body is carbonized to obtain a carbonized body at a carbonization temperature of 900°C for 6 hours. Steps S2 and S3 are repeated until the density of the carbonized body reaches 1.4 g / cm 3 ;
[0084] S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours;
[0085] S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, wherein the silicon carbide particle size in the first friction layer pressed powder is 50 μm, the silicon carbide content is 45 vol%, and the phenolic powder is 55 vol%, and the first friction layer pressed powder is evenly laid on the graphitized blank, and pressed at a temperature of 90° C. for 30 min to obtain a first blank, the pressure is 12 MPa, and the thickness after pressing is 0.33 mm;
[0086] S6: mixing silicon carbide powder and phenolic powder evenly to obtain a second friction layer pressed powder, wherein the silicon carbide particle size of the second friction layer pressed powder is 100 μm, the silicon carbide content is 60 vol%, and the phenolic powder is 40 vol%. The second friction layer pressed powder is evenly laid on the first blank, and pressed at a temperature of 150° C. for 60 min to completely solidify it to obtain a second blank, and the pressure is 14 MPa, and the thickness after pressing is 1.0 mm;
[0087] S7: Mechanically processing the second blank to obtain a brake disc blank, and preparing features such as ventilation channels of the product;
[0088] S8: The brake disc blank is placed in a boron nitride crucible and then in a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and dimensionally processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the insulation time is 3h, and the furnace pressure is less than 1000Pa.
[0089] Example 3
[0090] This embodiment provides a carbon-ceramic brake disc with a double friction layer. The steps of preparing the carbon-ceramic brake disc with a double friction layer are as follows:
[0091] S1: The carbon fiber unidirectional cloth and the carbon fiber mesh are repeatedly overlapped to obtain a carbon fiber preform. Each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh are overlapped and then needle-punched. The needle-punching density is 150 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°;
[0092] S2: impregnating the carbon fiber preform in a 40 wt % phenolic resin alcohol solution, and drying the preform until the alcohol is completely volatilized to obtain an impregnated body;
[0093] S3: The impregnated body is carbonized to obtain a carbonized body at a carbonization temperature of 900°C for 6 hours. Steps S2 and S3 are repeated until the density of the carbonized body reaches 1.4 g / cm 3 ;
[0094] S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours;
[0095] S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, wherein the silicon carbide particle size of the first friction layer pressed powder is 50 μm, the silicon carbide content is 45 vol%, and the phenolic powder is 55 vol%, and the first friction layer pressed powder is evenly laid on the graphitized blank, and pressed at a temperature of 90° C. for 30 min to obtain a first blank, the pressure is 12 MPa, and the thickness after pressing is 0.12 mm;
[0096] S6: mixing silicon carbide powder and phenolic powder evenly to obtain a second friction layer pressed powder, wherein the silicon carbide particle size of the second friction layer pressed powder is 100 μm, the silicon carbide content is 60 vol%, and the phenolic powder is 40 vol%. The second friction layer pressed powder is evenly laid on the first blank, and pressed at a temperature of 150° C. for 60 min to completely solidify it to obtain a second blank. The pressure is 14 MPa and the thickness after pressing is 0.5 mm;
[0097] S7: Mechanically processing the second blank to obtain a brake disc blank, and preparing features such as ventilation channels of the product;
[0098] S8: The brake disc blank is placed in a boron nitride crucible and then in a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and dimensionally processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the insulation time is 3h, and the furnace pressure is less than 1000Pa.
[0099] Example 4
[0100] This embodiment provides a carbon-ceramic brake disc with a double friction layer. The steps of preparing the carbon-ceramic brake disc with a double friction layer are as follows:
[0101] S1: The carbon fiber unidirectional cloth and the carbon fiber mesh are repeatedly overlapped to obtain a carbon fiber preform. Each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh are overlapped and then needle-punched. The needle-punching density is 150 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°;
[0102] S2: impregnating the carbon fiber preform in a 40 wt % phenolic resin alcohol solution, and drying the preform until the alcohol is completely volatilized to obtain an impregnated body;
[0103] S3: The impregnated body is carbonized to obtain a carbonized body at a carbonization temperature of 900°C for 6 hours. Steps S2 and S3 are repeated until the density of the carbonized body reaches 1.4 g / cm 3 ;
[0104] S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours;
[0105] S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, wherein the silicon carbide particle size of the first friction layer pressed powder is 50 μm, the silicon carbide content is 45 vol%, and the phenolic powder is 55 vol%, and the first friction layer pressed powder is evenly laid on the graphitized blank, and pressed at a temperature of 90° C. for 30 min to obtain a first blank, the pressure is 12 MPa, and the thickness after pressing is 0.22 mm;
[0106] S6: mixing silicon carbide powder and phenolic powder evenly to obtain a second friction layer pressed powder, wherein the silicon carbide particle size of the second friction layer pressed powder is 100 μm, the silicon carbide content is 65 vol%, and the phenolic powder is 35 vol%. The second friction layer pressed powder is evenly laid on the first blank, and pressed at a temperature of 150° C. for 60 min to completely solidify it to obtain a second blank. The pressure is 14 MPa and the thickness after pressing is 0.8 mm;
[0107] S7: Mechanically processing the second blank to obtain a brake disc blank, and preparing features such as ventilation channels of the product;
[0108] S8: The brake disc blank is placed in a boron nitride crucible and then in a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and dimensionally processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the insulation time is 3h, and the furnace pressure is less than 1000Pa.
[0109] Comparative Example 1
[0110] This embodiment provides a carbon-ceramic brake disc with a double friction layer. The steps of preparing the carbon-ceramic brake disc with a double friction layer are as follows:
[0111] S1: The carbon fiber unidirectional cloth and the carbon fiber mesh are repeatedly overlapped to obtain a carbon fiber preform. Each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh are overlapped and then needle-punched. The needle-punching density is 150 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°;
[0112] S2: impregnating the carbon fiber preform in a 40 wt % phenolic resin alcohol solution, and drying the preform until the alcohol is completely volatilized to obtain an impregnated body;
[0113] S3: The impregnated body is carbonized to obtain a carbonized body at a carbonization temperature of 900°C for 6 hours. Steps S2 and S3 are repeated until the density of the carbonized body reaches 1.4 g / cm 3 ;
[0114] S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours;
[0115] S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, wherein the silicon carbide particle size of the first friction layer pressed powder is 50 μm, the silicon carbide content is 45 vol%, and the phenolic powder is 55 vol%, and the first friction layer pressed powder is evenly laid on the graphitized blank, and pressed at a temperature of 90° C. for 30 min to obtain a first blank, the pressure is 12 MPa, and the thickness after pressing is 0.22 mm;
[0116] S6: mixing silicon carbide powder and phenolic powder evenly to obtain a second friction layer pressed powder, wherein the silicon carbide particle size of the second friction layer pressed powder is 100 μm, the silicon carbide content is 60 vol%, and the phenolic powder is 40 vol%. The second friction layer pressed powder is evenly laid on the first blank, and pressed at a temperature of 150° C. for 60 min to completely solidify it to obtain a second blank. The pressure is 14 MPa and the thickness after pressing is 0.44 mm;
[0117] S7: Mechanically processing the second blank to obtain a brake disc blank, and preparing features such as ventilation channels of the product;
[0118] S8: The brake disc blank is placed in a boron nitride crucible and then in a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and dimensionally processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the insulation time is 3h, and the furnace pressure is less than 1000Pa.
[0119] Comparative Example 2
[0120] This embodiment provides a carbon-ceramic brake disc with a double friction layer. The steps of preparing the carbon-ceramic brake disc with a double friction layer are as follows:
[0121] S1: The carbon fiber unidirectional cloth and the carbon fiber mesh are repeatedly overlapped to obtain a carbon fiber preform. Each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh are overlapped and then needle-punched. The needle-punching density is 150 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°;
[0122] S2: impregnating the carbon fiber preform in a 40 wt % phenolic resin alcohol solution, and drying the preform until the alcohol is completely volatilized to obtain an impregnated body;
[0123] S3: The impregnated body is carbonized to obtain a carbonized body at a carbonization temperature of 900°C for 6 hours. Steps S2 and S3 are repeated until the density of the carbonized body reaches 1.4 g / cm 3 ;
[0124] S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours;
[0125] S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, wherein the silicon carbide particle size of the first friction layer pressed powder is 50 μm, the silicon carbide content is 45 vol%, and the phenolic powder is 55 vol%, and the first friction layer pressed powder is evenly laid on the graphitized blank, and pressed at a temperature of 90° C. for 30 min to obtain a first blank, the pressure is 12 MPa, and the thickness after pressing is 0.22 mm;
[0126] S6: mixing silicon carbide powder and phenolic powder evenly to obtain a second friction layer pressed powder, wherein the silicon carbide particle size of the second friction layer pressed powder is 100 μm, the silicon carbide content is 60 vol%, and the phenolic powder is 40 vol%, and the second friction layer pressed powder is evenly laid on the first blank, and pressed at a temperature of 150° C. for 60 min to completely solidify it to obtain a second blank, the pressure is 14 MPa, and the thickness after pressing is 5 mm;
[0127] S7: Mechanically processing the second blank to obtain a brake disc blank, and preparing features such as ventilation channels of the product;
[0128] S8: The brake disc blank is placed in a boron nitride crucible and then in a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and dimensionally processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the insulation time is 3h, and the furnace pressure is less than 1000Pa.
[0129] The carbon ceramic brake discs with double friction layers prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-2 were tested. The dynamic friction coefficient and wear rate of the carbon ceramic brake disc samples were tested using an MM-1000 friction tester. The effective friction surface of the test ring had an outer diameter of D75 mm / inner diameter of D55 mm×10 mm, and a specific pressure of 98 N / cm 2 , inertia is 3kgf·cm·s 2 , linear speed is 25m / s.
[0130] The test data is shown in Table 1.
[0131] Table 1 Test data of carbon ceramic brake discs with double friction layers prepared in Examples 1-4 and Comparative Examples 1-2
[0132]
[0133] It can be seen from the above embodiments and comparative data that the second friction layer is located at the outermost layer of the brake disc, and increasing the silicon carbide content in the second friction layer can reduce the amount of wear, indicating that increasing the silicon carbide content in the friction layer is beneficial to improving the wear resistance of the friction layer. It can be seen from comparative example 1 and embodiment 1 that when the thickness of the second friction layer is less than the minimum value of the theoretical friction layer thickness, the performance of the friction layer is greatly reduced, and the friction layer peels off. It can be seen from comparative example 2 and embodiment 1 that when the thickness of the second friction layer is greater than the theoretical value, it will also cause the friction layer to peel off. It means that when the actual thickness of the second friction layer is between the minimum theoretical value of the friction layer and the maximum theoretical value of the friction layer, the friction layer has better performance and is more stable. The thickness of the second friction layer is closely related to the thickness of the first friction layer and the silicon carbide content and silicon content of the two friction layers. Flexible setting of the thickness of the second friction layer is more conducive to improving the comprehensive performance of the brake disc.
[0134] The above disclosures are only several preferred embodiments of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention are still within the scope covered by the present invention.
Claims
1. A carbon ceramic brake disc with a double friction layer, characterized in that: The carbon ceramic brake disc comprises a base layer and a friction layer, wherein the friction layer comprises a first friction layer and a second friction layer, wherein the first friction layer is located between the base layer and the second friction layer; and the thickness of the first friction layer is t fr1 , silicon carbide content is v SiC1 , silicon content is v Si1 ; The thickness of the second friction layer is t fr2 , silicon carbide content is v SiC2 , silicon content is v Si2 , then the thickness of the second friction layer t fr2 Satisfies the following formula: Among them, the coefficient β is the thickness coefficient, the value range is 0.9 or 5, ΔT is the difference between the siliconizing temperature and the room temperature, and ΔT is 1600k.
2. The carbon-ceramic brake disc with a double friction layer as claimed in claim 1, characterized in that: The silicon carbide content in the first friction layer is 50-80%, and the silicon content is 20-50%; the silicon carbide content in the second friction layer is 70-95%, and the silicon content is 5-30%.
3. The carbon-ceramic brake disc with a double friction layer as claimed in claim 1, characterized in that: The first friction layer includes coarse silicon carbide with a particle size of 40-80 microns and fine silicon carbide with a particle size of 0.5-30 microns.
4. The carbon-ceramic brake disc with a double friction layer as claimed in claim 3, characterized in that: The volume ratio of the coarse silicon carbide to the fine silicon carbide is 1:1-10:
1.
5. The carbon-ceramic brake disc with a double friction layer as claimed in claim 1, characterized in that: The second friction layer includes second coarse silicon carbide with a particle size of 80-150 microns and second fine silicon carbide with a particle size of 0.5-30 microns.
6. The carbon-ceramic brake disc with a double friction layer as claimed in claim 5, characterized in that: The volume ratio of the second coarse silicon carbide to the second fine silicon carbide is 1:1-10:
1.
7. A method for preparing a carbon-ceramic brake disc with a double friction layer, for preparing a carbon-ceramic brake disc with a double friction layer as claimed in any one of claims 1 to 6, characterized in that: The steps include: S1: Repeatedly overlap the carbon fiber unidirectional cloth and the carbon fiber mesh tire to obtain a carbon fiber preform, and each layer of the carbon fiber unidirectional cloth and each layer of the carbon fiber mesh tire are stacked and needle-punched, with a needle-punching density of 50-200 needles / cm 2 , the carbon fiber directions between the two adjacent carbon fiber unidirectional fabrics above and below each carbon fiber mesh tire form an angle of 90°; S2: impregnating the carbon fiber preform in a 40 wt % phenolic resin alcohol solution, and drying the preform until the alcohol is completely volatilized to obtain an impregnated body; S3: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900° C. for 6 hours; S4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen to obtain a graphitized body, the treatment temperature is 1700° C., and the temperature is kept for 2 hours; S5: mixing silicon carbide powder and phenolic powder evenly to obtain a first friction layer pressed powder, evenly laying the first friction layer pressed powder on the graphitized green body, and pressing at a temperature of 90° C. for 30 minutes to obtain a first green body with a pressure greater than 10 MPa; S6: mixing silicon carbide powder and phenolic powder evenly to obtain second friction layer pressed powder, evenly laying the second friction layer pressed powder on the first green body, pressing at a temperature of 150° C. for 60 minutes to completely solidify it to obtain a second green body, and the pressure is greater than 10 MPa; S7: machining the second blank to obtain a brake disc blank; S8: Put the brake disc blank into a boron nitride crucible and then into a high-temperature vacuum furnace for siliconizing treatment. After the siliconizing treatment, the surface is polished and the size is processed to obtain the carbon-ceramic brake disc with a double friction layer. 1.1 times the mass of the blank is pre-placed in the boron nitride crucible. The siliconizing treatment temperature is 1600-1700°C, the insulation time is 2-4h, and the furnace pressure is less than 1000Pa.
8. The method for preparing a carbon ceramic brake disc with a double friction layer as claimed in claim 7, characterized in that: Steps S2 and S3 are performed at least once, so that the density of the carbonized body reaches 1.25-1.45 g / cm 3 .
9. The method for preparing a carbon-ceramic brake disc with a double friction layer as claimed in claim 5, characterized in that: The silicon carbide particle size in the pressed powder of the first friction layer is 40-80 microns, the silicon carbide powder content is 35-55 vol%, and the phenolic powder content is 45-65 vol%.
10. The method for preparing a carbon ceramic brake disc with a double friction layer as claimed in claim 5, characterized in that: The silicon carbide particle size in the pressed powder of the second friction layer is 80-150 microns, the silicon carbide powder content is 45-75 vol%, and the phenolic powder content is 25-55 vol%.
Citation Information
Patent Citations
C / SiC composite material, preparation method of composite material and friction plate
CN102617178A
Preparation technology of C / C-SiC ventilation brake disc with silicon carbide friction functional layer
CN108299002A
Preparation method of high-bonding-strength coating carbon / ceramic brake disc
CN113816756A
Brake disc, preparation method thereof and traffic equipment
CN114233779A
Silicon carbide porous ceramic corrugated plate as well as preparation method and application thereof
CN118239794A
Cited By
Preparation method of carbon-ceramic brake disc with composite friction layer and carbon-ceramic brake disc
CN119638469A
Preparation method of carbon ceramic brake disc with composite friction layer and carbon ceramic brake disc