Measurement method of atomic-scale microscopic thermal conductivity
Through the combination of focusing ion beam technology and scanning transmission electron microscopy, the problem that the existing technology cannot measure the microscopic thermal conductivity at the nano and atomic scale is solved, and high-precision microscopic thermal conductivity analysis is achieved, which is suitable for complex material systems.
Patent Information
- Application Number
- CN202410960660.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art cannot measure microscopic thermal conductivity on nano and atomic scales, and it is difficult to analyze complex material systems, mainly due to insufficient spatial resolution and lack of effective micro-nano processing methods.
The micro-nano processing is carried out using focusing ion beam technology to construct thermal conduction path strips, and the local temperature gradient and phonon vibration spectrum of the sample are obtained by in-situ heating and electron energy loss spectrum in scanning transmission electron microscopy, according to Fourier thermal conductivity law Calculate the microscopic thermal conductivity.
Microscopic thermal conductivity measurements at nano and even atomic scales are achieved, with high accuracy and spatial resolution, suitable for samples of complex structures and multiple material systems.
Smart Images

Figure CN119044241A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal conductivity measurement, and in particular to a method for measuring atomic-scale microscopic thermal conductivity. Background Art
[0002] Thermal conductivity is one of the basic properties of materials. It is defined as the heat flux density under unit temperature gradient and describes the ability of materials to conduct heat in a non-equilibrium state. The unit of bulk thermal conductivity is usually Watt per meter per Kelvin (Wm -1 K -1 ), and the interfacial thermal conductivity is watts per meter per Kelvin (Wm -2 K -1 ). The value of thermal conductivity provides important information about the thermal conductivity and heat transfer characteristics of materials, which is of great significance for thermal management, heat dissipation design and thermal conduction applications. With the continuous integration and miniaturization of electronic devices, measuring the microscopic thermal conductivity of materials is of greater significance for thermal management and optimizing the internal heat transport of materials: with the reduction of device size and the increase of internal structural complexity, the thermal resistance at the interface begins to dominate, and measuring the microscopic thermal conductivity at the interface is crucial for designing heat dissipation systems, thermal interface materials and thermal barrier materials; for new temperature-sensitive power electronic devices, optimizing the microscopic thermal conductivity of heat dissipation materials can improve device performance and life, and for new thermoelectric materials, understanding the internal microscopic thermal conductivity is crucial for optimizing thermoelectric performance. Traditional thermal conductivity measurement methods such as heat flow meter method and laser flash method can obtain the macroscopic thermal conductivity of materials, reflecting their average thermal conductivity, but do not have spatial resolution and cannot obtain the microscopic thermal conductivity of specific locations. In recent years, many new measurement methods have been developed based on various microscopes and spectroscopy to obtain microscopic thermal conductivity, but they have certain limitations.
[0003] The photothermal Raman method heats the sample at the light spot by changing the laser power, and measures the temperature value at the light spot by using the frequency shift of the Raman spectrum or the ratio of the Stokes peak to the anti-Stokes peak, thereby inferring the thermal conductivity at the light spot, which can be used to measure the thermal conductivity of single-layer graphene. Its limitations are that due to the diffraction limit of light, it does not have a spatial resolution below 100 nanometers, and it is necessary to know the power of laser absorption at various locations of the material, which makes it difficult to analyze complex systems. Time domain thermoreflectance (TDTR) uses pump laser heating and simultaneously measures the reflectivity of the surface metal. Through the corresponding relationship between reflectivity and temperature, the change of temperature over time is obtained, and the thermal conductivity is calculated, which can be used to measure the interface thermal conductivity of heterojunctions. However, this method requires the sample size to be above micrometers, lacks spatial resolution, and is difficult to analyze the thermal conductivity at various locations for complex material systems. Scanning thermal microscopy (SThM) uses a micro-resistance thermometer and heater at the end of the scanning probe to scan the temperature distribution on the sample surface, and can also directly analyze the micro-area thermal conductivity through the temperature drop of the thermal probe, with a spatial resolution of up to 50nm. Its disadvantage is that only the surface of the material can be analyzed, and the unknown contact thermal resistance between the probe and the surface cannot be ignored.
[0004] In summary, existing technologies cannot obtain microscopic thermal conductivity at the nano and atomic scales, and it is difficult to analyze multi-material systems. This is mainly due to the insufficient spatial resolution of the characterization methods and the lack of an effective method for micro-nano processing of samples. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for measuring atomic-scale micro-thermal conductivity, which is used to measure temperature distribution at the nano and atomic scales, analyze micro-heat transport, and obtain micro-region thermal conductivity and interface thermal conductivity.
[0006] The principle of the present invention is to obtain the temperature gradient at each location by measuring the local temperature distribution at the nanometer and atomic scales for a sample with a stable temperature gradient, and then obtain the local microscopic thermal conductivity according to Fourier's law of thermal conductivity.
[0007] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0008] A method for measuring atomic-scale microscopic thermal conductivity comprises the following steps:
[0009] S1. Pre-treating the sample to be characterized for microscopic thermal conductivity to obtain a pre-treated sample, and obtaining the macroscopic average thermal conductivity of a component of the pre-treated sample;
[0010] S2. Use focused ion beam technology to perform micro-nano processing on the pretreated sample described in S1 to construct a thermal conductive path strip of the microstructure or interface to be characterized, deposit a circuit at one end of the path strip and connect it to the electrode heating area to form a hot end, and connect the other end to the substrate for heat dissipation to form a cold end, so as to make a transmission electron microscope sample with local heating to generate a temperature gradient;
[0011] S3. Characterize the transmission electron microscope sample described in S2 in the transmission electron microscope using an in-situ heating system, apply a set current to the sample, heat the hot end of the path strip, and dissipate the heat at the cold end, so as to establish a stable temperature gradient on the path strip of the transmission electron microscope sample to be measured for microscopic thermal conductivity;
[0012] S4. using a scanning transmission electron microscope to collect the electron energy loss spectrum at each location of the path strip of the transmission electron microscope sample that generates the temperature gradient described in S3, and obtain the phonon vibration spectrum at different locations of the sample path strip; using the obtained phonon vibration spectrum to calculate the temperature and temperature gradient at each location of the sample path strip that generates the temperature gradient according to the phonon peak intensity of the Bose distribution;
[0013] S5. According to the inverse relationship between thermal conductivity and temperature gradient in the one-dimensional thermal conductivity model, the relative value of the microscopic thermal conductivity of the sample path strip is obtained.
[0014] Preferably,
[0015] The S4 is specifically:
[0016] The sample path strip is continuously scanned point by point in space from the cold end to the hot end to collect the electron energy loss spectrum. The background signal is removed from the electron energy loss part on the right side of the zero loss peak and the electron energy gain part on the left side of the zero loss peak to obtain the loss spectrum Loss(ω) and gain spectrum Gain(ω);
[0017] The gain spectrum comes from the inelastic scattered electrons that gain energy when the transmitted electrons interact with the phonons of the sample material, corresponding to the annihilation process of phonons, which is equal to the phonon state density D(ω) multiplied by the number of excited state phonons <n>The loss spectrum comes from the inelastic scattered electrons that lose energy when the transmitted electrons interact with the phonons of the sample material. It corresponds to the phonon generation process and is the sum of the phonon state density D(ω) multiplied by the number of phonons in the excited state and the ground state. <n>+1; among them <n>is the statistical average number of excited state phonons, which increases with increasing temperature. Phonons obey the Bose distribution. <n>It can be expressed as
[0018]
[0019] in, is the energy of the phonon, equivalent to the energy lost or gained by the electron in the electron energy loss spectrum, k B is the Boltzmann constant, T is the temperature;
[0020] For the phonon spectrum collected at any position, there is a proportional relationship between its loss spectrum Loss(ω) and gain spectrum Gain(ω), and the proportional function It is related to the temperature T at that point, that is
[0021]
[0022] Temperature-dependent residual spectrum Theoretically, it should be zero, and the temperature value corresponding to this point is obtained by least square fitting;
[0023] The temperature is calculated by collecting the phonon spectrum of each point in the spatial range, and the temperature distribution T(x,y) within a certain spatial range is obtained, and then the temperature gradient can be calculated.
[0024] Preferably,
[0025] The S5 is specifically:
[0026] The sample path strip is treated as a one-dimensional heat conduction model, which is applicable to the one-dimensional Fourier heat transfer law.
[0027]
[0028] Where j is the heat flux density, which is the heat flow per unit cross-sectional area; k is the thermal conductivity, is the temperature gradient in the direction of the heat transfer path; ignoring the heat dissipation on the heat transfer path, the total heat flow is considered constant, the width of the strip path is constant, and the thickness is considered uniform. The heat flux density is approximately the same everywhere, so the microscopic thermal conductivity at each position is inversely proportional to the temperature gradient at that location.
[0029]
[0030] Where K is the interfacial thermal conductivity, ΔT 界面 is the temperature difference across the interface;
[0031] Calculate the temperature gradient at any point based on the phonon vibration spectrum The microscopic thermal conductivity at these points is inversely proportional to the temperature gradient, and the relative value of the microscopic thermal conductivity at each location is obtained.
[0032] Preferably,
[0033] The S2 is specifically:
[0034] S2.1 Select a sampling area on the pretreated sample described in S1, and use ion beam to etch pits with a depth of more than 15 μm above and below the sampling area, respectively. The upper and lower widths of the two etching areas are between 10 μm and 20 μm, and the left and right widths exceed the width of the sampling area; use ion beam to etch the upper and lower sides of the sampling area close to the sampling area to make the upper and lower sides of the sampling area flat;
[0035] S2.2 Insert the probe, the probe tip contacts the upper side of the sampling area, and carbon is deposited at the tip of the probe to weld the probe to the sampling area, so that the sampling area is completely separated from the sample;
[0036] S2.3 Etch a groove slightly larger than the size of the sampling area at the electrode position of the four-electrode substrate, and its depth is slightly smaller than the thickness of the sampling area, embed the sampling area into the groove, deposit carbon at the four corners of the sample in the sampling area so that they are connected to the four electrodes respectively, weld the sample in the sampling area into the groove of the substrate, etch away the carbon deposited on the probe needle tip, separate the needle tip from the sample in the sampling area, and thin out the excess carbon on the upper surface to make the upper surface of the sample flat;
[0037] S2.4 Select a set area and thin it up and down to make the thickness of the thin area less than 50nm, etch a path strip parallel to the heat transfer direction on the thin area, deposit a large amount of carbon at one end of the thin area to connect with the substrate base to build a heat dissipation channel, deposit thinner carbon at the other end of the thin area as a heating resistor, and additionally deposit a large amount of carbon at the electrode to concentrate the resistance in the heating circuit below the thin area.
[0038] Preferably,
[0039] According to the relative value of the microscopic thermal conductivity obtained by S5, the proportional relationship of the microscopic thermal conductivity at different positions of the sample path strip is obtained; by querying or measuring the absolute value of the macroscopic thermal conductivity of any component of the sample, the absolute value of the microscopic thermal conductivity at that location is calibrated as a standard value, thereby obtaining the absolute values of the microscopic thermal conductivity at all other locations.
[0040] Preferably,
[0041] Combined with the absolute value of the macroscopic thermal conductivity, the absolute values of the microscopic thermal conductivity and interface thermal conductivity at each location of the sample are calculated; the absolute value of the interface thermal conductivity is expressed as
[0042]
[0043] Where k1 is the bulk thermal conductivity of sample material one.
[0044] Preferably,
[0045] In view of the uneven thickness of the sample path strip, the electron energy loss spectrum is used to calculate the thickness of the sample path strip at each location, and the microscopic thermal conductivity is corrected. The corresponding formula becomes
[0046]
[0047] Here, t is the thickness at different locations, which is calculated by collecting the plasmon spectrum of the sample area in the electron microscope.
[0048] Preferably,
[0049] The sample pretreatment in S1 includes cutting the sample into small pieces that can be placed in a scanning electron microscope, wherein each size of the small pieces is less than 1 cm, grinding and polishing, and spraying carbon or gold on the surface to make it conductive.
[0050] Preferably,
[0051] The transmission electron microscope in the S4 is equipped with a spherical aberration corrector and a monochromator, with a spatial resolution of more than 60 pm and an energy resolution of less than 7 meV.
[0052] The beneficial effects of the present invention are:
[0053] The method provided by the present invention can measure local temperature information at the nanometer or even atomic scale, thereby quantitatively analyzing the microscopic thermal conductivity of each structure at different positions inside the sample. It has the advantages of accurate measurement, high spatial resolution, and the ability to study nanoscale heat transport and micro-area thermal conductivity. It is suitable for samples with complex structures and various material systems. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0055] Figure 1 It is a schematic diagram of a method for realizing local heating of a sample in a scanning transmission electron microscope; Figure 1 a is an in-situ heated sample rod, which is used to carry the sample and introduce current into the sample through internal wires and probe electrodes; Figure 1 b is a four-electrode substrate with four independent electrodes and a groove for carrying micro-samples. The inset shows the distance between the electrodes. Figure 1 c is a schematic diagram of local heating of the sample, where the sample is welded and fixed to the groove in the middle of the four-electrode substrate and connected to the electrodes, and local heating of one end is achieved by applying current to two of the electrodes; Figure 1 d is a schematic diagram of the sample structure that can achieve local heating to build a stable temperature gradient.
[0056] Figure 2 Scanning electron beam (and ion beam) image of the localized heating sample preparation process based on focused ion beam technology; operations include moving and tilting the sample stage, deposition (white dashed box), etching and thinning (black cross box), and moving the manipulation probe.
[0057] Figure 3 It is a schematic diagram of the principle of measuring temperature and interface thermal conductivity based on scanning and collecting electron energy loss spectrum; Figure 3 a is a scanning transmission electron micrograph of a strip-shaped thin region containing an interface in a heterojunction sample. The black text identifies the interface position and the positions of the two different materials, as well as the heating at the right end and the heat dissipation at the left end; Figure 3 b is a series of electron energy loss spectra collected in the white dashed box area in 3a. The spectrum lines from bottom to top correspond to the white arrows in 3a from left to right. The dashed line is the zero loss peak, representing the background signal of the transmitted electrons. The signal on the left is the electron energy gain spectrum, and the signal on the right is the electron energy loss spectrum. Figure 3 c is a schematic diagram of a one-dimensional strip heat transfer model, and the heat conduction on the sample structure can be simplified to this model; Figure 3 d is the spatial distribution of temperature in the heat transfer direction under the ideal state corresponding to the one-dimensional strip model.
[0058] Figure 4 This is an experimental data diagram of measuring the interface thermal conductivity of the aluminum nitride / silicon carbide heterojunction interface at different temperatures in the example; Figure 4 a and Figure 4 b is the temperature distribution diagram of the interface area, where the horizontal and vertical axes represent the position and the color represents the temperature; Figure 4 c is a graph of temperature varying with space.
[0059] Figure 5 The method flow chart of the present invention is DETAILED DESCRIPTION
[0060] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the following embodiments are provided only for the purpose of illustration and are not intended to limit the scope of the present invention. Those skilled in the art may make various modifications and substitutions to the present invention without departing from the purpose and spirit of the present invention.
[0061] The present invention provides a method for measuring atomic-scale micro-thermal conductivity, which locally heats a sample in a scanning transmission electron microscope to generate a temperature gradient, thereby measuring micro-thermal conductivity at the atomic scale. The method is mainly based on a focused ion beam sample preparation method and an electron energy loss spectrum based on a scanning transmission electron microscope.
[0062] Specifically, the sample is micro-nano processed to construct a long strip of heat conduction path, on which there is a microstructure or interface to be studied. A circuit is deposited at one end of the path and connected to an electrode for heating, while the other end dissipates heat to build a stable temperature gradient on the path. The electron energy loss spectrum of a scanning transmission electron microscope is used to obtain the phonon vibration spectrum at different positions of the sample, and then the temperature at each position is calculated based on the Bose distribution of the phonons, and then the local temperature gradient is obtained, with a spatial resolution of sub-nanometers. Since the sample is in a high vacuum, it can be approximated as an adiabatic boundary condition, and the heat flow on the heat conduction path is consistent everywhere. According to Fourier's law of heat conduction, the local thermal conductivity is inversely proportional to the temperature gradient at that location, so the relative values of thermal conductivity at different locations can be obtained. Combined with the thermal conductivity of a component of a known heat conduction path or the overall average thermal conductivity as a reference, the absolute value of the microscopic thermal conductivity can be derived. Since the spatial distribution diagram of temperature provides all the information except the heat flow value under steady-state heat transport, the method provided by the present invention can measure the local temperature information at the nanometer or even atomic scale, thereby quantitatively analyzing the microscopic thermal conductivity of each structure at different positions inside the sample.
[0063] The present invention has the advantages of accurate measurement, high spatial resolution, and the ability to study nanoscale heat transport and micro-area thermal conductivity, and is suitable for samples of complex structures and various material systems.
[0064] Example 1 Measurement of the interface thermal conductivity of silicon carbide / aluminum nitride heterojunction
[0065] The method of the present invention comprises the steps of:
[0066] A. Pre-process the sample, including cutting into small pieces, grinding and polishing, and sticking it on the sample stage with conductive glue.
[0067] For different research and measurement purposes, the processing details of the sample will also be somewhat different. The sample in this case is aluminum nitride grown directly on a silicon carbide substrate, where silicon carbide is a single crystal 4H phase, and the thermal conductivity of the bulk is known (obtained from the literature). Only a small piece needs to be prepared for the subsequent micro-nano processing using a focused ion beam. For other samples with unknown thermal conductivity, it is also necessary to measure their macroscopic average thermal conductivity.
[0068] B. Use focused ion beam (FIB) technology to produce samples that can be locally heated to produce temperature gradients and are suitable for scanning transmission electron microscopy.
[0069] This step is carried out in the Helios G4 instrument, which integrates an ion beam and a scanning electron microscope. The instrument can realize operations such as moving and tilting the sample stage, depositing carbon and metal, inserting and moving the probe, and rotating the probe. The specific implementation method is as follows:
[0070] B1. Select an area of about 25μm×5μm (hereinafter referred to as the sampling area) at an appropriate position of the bulk sample, and deposit about 2μm of amorphous carbon on the surface of the area, such as Figure 2 a is shown in the white dotted box; and ion beams are used to etch pits with a depth of more than 15 μm above and below the sampling area. The upper and lower widths of the two etching areas are between 10 μm and 20 μm, and the left and right widths need to exceed the width of the sampling area by 25 μm; and ion beams are continued to etch just above and below the sampling area to make the upper and lower sides of the sampling area flat. Figure 2 The black box in a is shown;
[0071] B2. Cut the sampling area with an ion beam from the upper side, along Figure 2 At the black frame position of b, cut through the edge of the sample to separate the left, right and bottom of the sampling area from the block sample, but leave a small section on the right side without cutting off;
[0072] B3. Insert the probe and move it until the tip contacts the upper side of the sampling area. Figure 2 As shown in c. Figure 2 As shown in d, carbon is deposited at the needle tip to weld the needle to the sampling area firmly, and a small section on the right side of the sampling area is cut off to completely separate it from the bulk sample. Finally, the probe is manipulated to take out the small sample from the sampling area.
[0073] B4. Figure 2 As shown in Fig. e, a groove slightly larger than the size of the small sample (25 μm × 15 μm) is etched at the electrode position of the four-electrode substrate, and its depth is slightly smaller than the thickness of the small sample. Figure 2 As shown in f, the probe is manipulated to embed a small piece of sample into the groove. Figure 2 As shown in Figure g, carbon is deposited on the four corners of the sample to connect them to the four electrodes respectively, and the sample is firmly welded in the groove of the substrate. Then the carbon deposited on the needle tip in the previous step is etched away to separate the needle tip from the sample. Figure 2 The engraving shown in h thins out the excess carbon on the upper surface to make the upper surface of the sample flat;
[0074] B5. Figure 2 As shown in Fig. i, a region with a width of about 6 μm is selected and thinned up and down to make the thickness of the thin region less than 50 nm to be suitable for SEM observation, and a gap parallel to the heat transfer direction is etched on the thin region to make it present a stripe structure, as shown in Fig. Figure 2 j. At the same time, at one end of the thin area ( Figure 2 A large amount of carbon is deposited on the top of the thin area to connect with the substrate to construct a heat dissipation channel, and a thinner carbon is deposited on the other end of the thin area as a heating resistor. At the same time, a large amount of carbon is additionally deposited at the electrode to concentrate the resistance in the heating circuit below the thin area.
[0075] C. Using an in-situ heating system and electron energy loss spectroscopy of a scanning transmission electron microscope, a temperature gradient is constructed and detected on the strip sample to obtain the interface temperature difference and calculate the interface thermal conductivity.
[0076] The in-situ heating system consists of an in-situ heating rod, connecting wires, a control power supply and supporting control software. It can add different currents to the sample in the electron microscope and monitor the changes in voltage resistance. Using a scanning transmission electron microscope (Nion U-HERMES200) with a spherical aberration corrector and a monochromator, the spatial resolution can reach 60pm, achieving atomic resolution; the energy resolution can reach below 7meV, which is used to obtain the lattice vibration spectrum of the sample, that is, the phonon spectrum. Since phonons obey the Bose distribution, the temperature of the point can be calculated based on the intensity of the phonon peak. The specific implementation method is:
[0077] C1. Place the sample in the in-situ heating rod and place it in the scanning transmission electron microscope for characterization. Use a software-controlled power supply meter to add an appropriate current to the sample and wait for the sample to reach a steady state in the electron microscope where it no longer drifts. At this time, the temperature of each part no longer changes with time. Since one end of the strip-shaped thin area on the sample is connected to the heating area and the other end is connected to the substrate for heat dissipation, a stable temperature gradient has been generated in the spatial range containing the thermal conductivity of the interface to be measured;
[0078] C2. Figure 3 As shown in a, the electron energy loss spectrum is collected by scanning point by point within a certain spatial range including the interface. Figure 3 b shows a series of electron energy loss spectra collected in continuous space from the cold end to the hot end. The background signal is removed from the electron energy loss part on the right side of the zero loss peak and the electron energy gain part on the left side of the zero loss peak to obtain the loss spectrum Loss(ω) and the gain spectrum Gain(ω). The gain spectrum comes from the inelastic scattered electrons that gain energy when the transmitted electrons interact with the material phonons, corresponding to the annihilation process of phonons, which is equal to the phonon state density D(ω) multiplied by the number of excited state phonons <n>, while the loss spectrum comes from the inelastic scattered electrons that lose energy when the transmitted electrons interact with the material phonons. It corresponds to the phonon generation process and is the phonon state density D(ω) multiplied by the sum of the number of phonons in the excited state and the ground state. <n>+1. <n>is the statistical average of the number of excited state phonons, which increases with increasing temperature. Since phonons obey the Bose distribution, <n>It can be expressed as
[0079]
[0080] in, is the energy of the phonon (equivalent to the energy lost or gained by the electron in the electron energy loss spectrum), k B is the Boltzmann constant, and T is the temperature. For the phonon spectrum collected at any position, there is a proportional relationship between its loss spectrum Loss(ω) and gain spectrum Gain(ω), and the proportional function It is related to the temperature T at that point, that is
[0081]
[0082] Temperature-dependent residual spectrum Theoretically, it should be zero. Therefore, the temperature value corresponding to the point is obtained by least square fitting. The phonon spectrum of each point in the spatial range is collected to calculate the temperature, and the temperature change graph within a certain spatial range is obtained. Ideally, it should be similar to Figure 3 As shown in d;
[0083] C3. Figure 3 c shows that the sample in the experiment can be treated according to the one-dimensional heat conduction model, which is applicable to the one-dimensional Fourier heat transfer law.
[0084]
[0085] Where j is the heat flux density, which is the heat flow per unit cross-sectional area; k is the thermal conductivity, is the temperature gradient in the direction of the heat transfer path. Ignoring the heat dissipation on the heat transfer path, the total heat flow can be considered constant. Since the width of the strip-shaped path is constant and the thickness is considered uniform, the heat flux density can be approximately considered to be consistent everywhere. Therefore, the thermal conductivity at each position is inversely proportional to the temperature gradient at that location.
[0086]
[0087] Where K is the interfacial thermal conductivity, ΔT 界面 is the temperature difference on both sides of the interface. Based on the temperature distribution obtained in the previous step, the temperature gradient at any point can be calculated The microscopic thermal conductivity at these points is inversely proportional to the temperature gradient, and the relative size of the microscopic thermal conductivity at each location can be obtained. Combined with the bulk thermal conductivity obtained in step A, the absolute values of the microscopic thermal conductivity and interface thermal conductivity at each location can be calculated. Figure 3 d, the absolute value of the interface thermal conductivity can be expressed as
[0088]
[0089] Where k1 is the bulk thermal conductivity of material 1.
[0090] As a preferred solution, in step C3, the thickness information of the sample at different positions can be used to correct the heat flux density, which is suitable for the case where the sample thickness is uneven. The corresponding formula becomes
[0091]
[0092] Among them, t is the thickness at different positions, which can be directly calculated by collecting the plasmon spectrum of the sample area in the electron microscope.
[0093] The method of the present invention is used to measure the interfacial thermal conductivity of the aluminum nitride / silicon carbide (AlN / SiC) heterojunction interface at different temperatures, wherein the sample preparation is consistent with the description of step A and step B, and the experimental operation is consistent with the description of step C1. By applying different currents to the heating end, steady-state heat transfer at different temperatures and temperature gradients can be obtained. The temperature distribution is detected by scanning the electron energy loss spectrum in the 400nm area near the interface, and the method is consistent with the description of step C2. For the currents of 5mA and 8mA, the results are as follows: Figure 4 a and 4b, the temperature variation curve along the heat transfer path is as follows Figure 4 c. Figure 4 a corresponds Figure 4 c The temperature at the interface is about 460K, and the temperature difference on both sides of the interface is 478K-448K=30K. The temperature gradient of silicon carbide on the left is (442K-425K) / 140nm=1.06E8 K / m. According to the literature (J.Appl.Phys.113,053503(2013)), the bulk thermal conductivity of silicon carbide along the heat flow direction at this temperature is about 110W / (mK). According to the calculation formula in step C3, the interface thermal conductivity at this temperature is 390MW / (m 2 K). Figure 4 b corresponds Figure 4 c The temperature at the interface is about 540K, and the temperature difference on both sides of the interface is 559K-534K=25K. The temperature gradient of silicon carbide on the left is (534K-509K) / 160nm=1.56E8K / m. The bulk thermal conductivity of silicon carbide along the heat flow direction at this temperature is about 80W / (mK). According to the calculation formula in step C3, the interface thermal conductivity at this temperature is 500MW / (m 2 K). The results are consistent with the general rule that the thermal conductivity of the interface increases with increasing temperature.
[0094] The present invention realizes local heating in the micrometer-scale region of the sample, constructs a stable temperature field with a huge temperature gradient (hundreds of Kelvin per micrometer) by locally heating the sample in a scanning transmission electron microscope to generate a temperature gradient, and measures the temperature by electron energy loss spectrum in the electron microscope. It can also realize atomic-resolved phonon spectrum detection and temperature measurement in space, and finds that the temperature mutation at the heterojunction interface actually occurs on a scale within 2nm. This method is sufficient to measure the relative value of microscopic thermal conductivity at the atomic scale, and obtain the absolute value of microscopic thermal conductivity in combination with the macroscopic measurement results of bulk thermal conductivity (reference can be made to the literature).
[0095] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0096] Finally, it should be noted that the above description is only a preferred example of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.< / n> < / n> < / n> < / n> < / n> < / n> < / n> < / n>
Claims
1. A method for measuring atomic-scale microscopic thermal conductivity, characterized in that: The steps are as follows: S1. Pretreat the sample to be characterized for micro-thermal conductivity to obtain a pretreated sample, and obtain the macroscopic average thermal conductivity of a certain component of the pretreated sample; S2. Use the focused ion beam technology to perform micro-nano processing on the pretreated sample in S1, construct a heat conduction path strip for the microstructure or interface to be characterized, deposit a circuit at one end of the path strip and connect it to the electrode heating area to form a hot end, and connect the other end to the substrate for heat dissipation to form a cold end, and fabricate a transmission electron microscope sample with a local heating to generate a temperature gradient; S3. Use an in-situ heating system to characterize the transmission electron microscope sample in S2 in the transmission electron microscope, apply a set current to the sample, heat the hot end of the path strip, and dissipate heat at the cold end to construct a stable temperature gradient on the path strip of the transmission electron microscope sample with the micro-thermal conductivity to be measured; S4. Use a scanning transmission electron microscope to collect the electron energy loss spectra at various positions of the path strip of the transmission electron microscope sample with the generated temperature gradient, and obtain the phonon vibration spectra at different positions of the sample path strip; calculate the temperatures and temperature gradients at various positions of the sample path strip with the generated temperature gradient according to the phonon peak intensity of the Bose distribution using the obtained phonon vibration spectra; S5. According to the inverse relationship between the thermal conductivity and the temperature gradient in the one-dimensional heat conduction model, obtain the relative value of the micro-thermal conductivity of the sample path strip.
2. The method for measuring atomic-scale microscopic thermal conductivity according to claim 1, characterized in that: The specific content of S4 is as follows: Scan the sample path strip point by point continuously in space from the cold end to the hot end, collect the electron energy loss spectra, remove the background signals from the part of the electron energy loss on the right side of the zero-loss peak and the part of the electron energy gain on the left side of the zero-loss peak respectively, and obtain the loss spectrum Loss(ω) and the gain spectrum Gain(ω); The gain spectrum comes from the inelastic scattered electrons that gain energy when the transmitted electrons interact with the phonons of the sample material, corresponding to the annihilation process of phonons, which is equal to the phonon state density D(ω) multiplied by the number of excited state phonons <n>The loss spectrum comes from the inelastic scattered electrons that lose energy when the transmitted electrons interact with the phonons of the sample material. It corresponds to the phonon generation process and is the sum of the phonon state density D(ω) multiplied by the number of phonons in the excited state and the ground state. <n>+1; where <n> is the statistical average value of the number of excited-state phonons, which increases with the increase of temperature. Phonons obey the Bose distribution, and <n> can be expressed as< / n> < / n> in, is the energy of the phonon, equivalent to the energy lost or gained by the electron in the electron energy loss spectrum, k B is the Boltzmann constant, T is the temperature; For the phonon spectrum collected at any position, there is a proportional relationship between its loss spectrum Loss(ω) and gain spectrum Gain(ω), and the proportional function It is related to the temperature T at that point, that is Temperature-dependent residual spectrum Theoretically, it should be zero, and the temperature value corresponding to this point is obtained by least square fitting; The temperature is calculated by collecting the phonon spectrum of each point in the spatial range, and the temperature distribution T(x, y) within a certain spatial range is obtained, and then the temperature gradient can be calculated.
3. The method for measuring atomic-scale micro thermal conductivity according to claim 2, characterized in that: The specific content of S5 is as follows: The sample path strip is processed according to the one-dimensional heat conduction model and is applicable to the one-dimensional Fourier heat transfer law Where j is the heat flux density, which is the heat flow per unit cross-sectional area; k is the thermal conductivity, is the temperature gradient in the direction of the heat transfer path; ignoring the heat dissipation on the heat transfer path, the total heat flow is considered constant, the width of the strip path is constant, and the thickness is considered uniform. The heat flux density is approximately the same everywhere, so the microscopic thermal conductivity at each position is inversely proportional to the temperature gradient at that location. Where K is the interfacial thermal conductivity, ΔT 界面 is the temperature difference across the interface; Calculate the temperature gradient at any point based on the phonon vibration spectrum The microscopic thermal conductivity at these points is inversely proportional to the temperature gradient, and the relative value of the microscopic thermal conductivity at each location is obtained.
4. The method for measuring atomic-scale microscopic thermal conductivity according to claim 1, characterized in that: The specific content of S2 is as follows: S2.1 Select a sampling area on the pretreated sample in S1, etch pits with a depth exceeding 15 μm above and below the sampling area respectively. The upper and lower widths of the two etched areas are between 10 μm and 20 μm, and the left and right widths exceed the width of the sampling area; etch with an ion beam close to the upper and lower sides of the sampling area to make the upper and lower sides of the sampling area flat; S2.2 Insert a probe, make the tip of the probe contact the upper side of the sampling area, deposit carbon at the tip position to weld the probe to the sampling area and separate the sampling area from the sample completely; S2.3 Etch a groove slightly larger than the size of the sampling area at the electrode position of the four-electrode substrate, with a depth slightly less than the thickness of the sampling area. Embed the sampling area into the groove, deposit carbon at the four corners of the sampling area sample to connect it to the four electrodes respectively, weld the sampling area sample in the groove of the substrate, etch off the carbon deposited on the tip of the probe to separate the tip from the sampling area sample, and etch and thin the excess carbon on the upper surface to make the upper surface of the sample flat; S2.4 Select a set area and thin it up and down to make the thickness of the thin area less than 50nm, etch a path strip parallel to the heat transfer direction on the thin area, deposit a large amount of carbon at one end of the thin area to connect with the substrate base to build a heat dissipation channel, deposit thinner carbon at the other end of the thin area as a heating resistor, and additionally deposit a large amount of carbon at the electrode to concentrate the resistance in the heating circuit below the thin area.
5. The method for measuring atomic-scale micro thermal conductivity according to claim 3, characterized in that: According to the relative value of the microscopic thermal conductivity obtained by S5, the proportional relationship of the microscopic thermal conductivity at different positions of the sample path strip is obtained; by querying or measuring the absolute value of the macroscopic thermal conductivity of any component of the sample, the absolute value of the microscopic thermal conductivity at that location is calibrated as a standard value, thereby obtaining the absolute values of the microscopic thermal conductivity at all other locations.
6. The method for measuring atomic-scale micro thermal conductivity according to claim 5, characterized in that: Combined with the absolute value of the macroscopic thermal conductivity, the absolute values of the microscopic thermal conductivity and interface thermal conductivity at each location of the sample are calculated; the absolute value of the interface thermal conductivity is expressed as Where k1 is the bulk thermal conductivity of sample material one.
7. The method for measuring atomic-scale micro thermal conductivity according to claim 6, characterized in that: In view of the uneven thickness of the sample path strip, the electron energy loss spectrum is used to calculate the thickness of the sample path strip at each location, and the microscopic thermal conductivity is corrected. The corresponding formula becomes Here, t is the thickness at different locations, which is calculated by collecting the plasmon spectrum of the sample area in the electron microscope.
8. The method for measuring atomic-scale micro thermal conductivity according to claim 1, characterized in that: The sample pretreatment in S1 includes cutting the sample into small pieces that can be placed in a scanning electron microscope, wherein each size of the small pieces is less than 1 cm, grinding and polishing, and spraying carbon or gold on the surface to make it conductive.
9. The method for measuring atomic-scale micro thermal conductivity according to claim 1, characterized in that: The transmission electron microscope in the S4 is equipped with a spherical aberration corrector and a monochromator, with a spatial resolution of more than 60 pm and an energy resolution of less than 7 meV.
Citation Information
Cited By
Device and method for measuring thermal conductivity of high-thermal-conductivity material film
CN121385021A
Method for measuring atomic scale microscopic thermal conductivity
WO2026016417A1