Graphite negative electrode binder, slurry mixing method, negative electrode pole piece and lithium ion battery
By using polyacrylic binder in graphite negative electrode batteries to improve the solid content and viscosity of the slurry, the problems of curling, cracking and rolling caused by low solid content are solved, and the cycle life and low-temperature discharge performance of lithium-ion batteries are improved.
Patent Information
- Application Number
- CN202411160878.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing graphite negative electrode slurry combination process, low-solid content slurry leads to problems such as curling edges, cracking, rolling pressure and easy rolling and powder loss, which affects the processing performance and cycle life of lithium-ion batteries.
The slurry combination method of graphite negative electrode containing polyacrylic binder is adopted. By adding polyacrylic binder, the solid content and viscosity of the slurry are improved, the stability and processing performance of graphite materials are improved, and the electrode sheet and foil are enhanced. Adhesion force reduces the sticking and material dropping during roll pressure slitting.
It improves the solid content and viscosity stability of the slurry, improves the processing performance of the electrode sheet, extends the cycle life of the lithium-ion battery, and improves the discharge efficiency in a low-temperature environment, reducing the risk of shedding and fracture of the electrode sheet.
Smart Images

Figure CN119050270A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery preparation, and in particular to a graphite negative electrode binder, a slurry mixing method, a negative electrode sheet and a lithium ion battery. Background Art
[0002] With the rise of lithium-ion batteries, graphite materials, as the most widely used negative electrode materials, have attracted the attention of various lithium battery manufacturers. Graphite is abundant in sources, cheap and has excellent rate performance, making it the most commercialized negative electrode material for lithium batteries. However, if the slurry obtained by the widely used graphite negative electrode slurry process is to meet the viscosity of 1500-4500mpa.s, its solid content must be reduced to 45%-52% to ensure that the slurry can pass through a 150-mesh sieve normally. Conventional low-solid content slurry coating process is prone to curling and cracking, easy to stick to the roller during rolling, and easy to lose powder during slitting, which affects the yield of the winding process and even self-discharge in the later process.
[0003] In order to solve the above problems, the present invention is proposed. Summary of the invention
[0004] In order to solve the above-mentioned problems of low solid content of slurry and powder falling of pole pieces, the present invention provides a method for slurrying of graphite negative electrode containing polyacrylic acid binder (PAA), and also provides the improvement of binder under different ratios. When polyacrylic acid binder is added during homogenization, the solid content of slurry can be increased while stabilizing the viscosity of slurry, so that pole pieces have better processing performance, improve battery self-discharge, and are also beneficial to the stability of graphite materials, so that the battery cycle life is better.
[0005] The above purpose is achieved by the following technical solutions:
[0006] The object of the present invention is achieved in that:
[0007] In the first aspect, the raw material components included in the graphite negative electrode binder are graphite material, carbon black conductive agent, sodium carboxymethyl cellulose, polyacrylic acid binder, styrene-butadiene rubber binder, and deionized water, and the mass ratio of the raw material components is set to 90-98, 0.5-3, 0.5-2, 0.5-5, 1-5, and 10-100.
[0008] In a second aspect, the present invention provides a method for preparing a slurry of a graphite negative electrode binder, the method comprising the following steps:
[0009] (1) preparing raw material components for preparing graphite negative electrode slurry, the raw material components including graphite material, carbon black conductive agent, sodium carboxymethyl cellulose, polyacrylic acid binder, styrene-butadiene rubber binder, and deionized water, wherein the mass ratio of the raw material components is set to 90-98, 0.5-3, 0.5-2, 0.5-5, 1-5, and 10-100;
[0010] (2) adding graphite material, carbon black conductive agent and sodium carboxymethyl cellulose into a planetary mixer and mixing for 0.5 to 1.5 hours to obtain a uniform powder;
[0011] (3) adding 55-80% deionized water to the uniform powder obtained in step (2) and stirring for 2-4 hours;
[0012] (4) adding a polyacrylic acid binder to the slurry obtained in step (3) and stirring for 1 to 3 hours;
[0013] (5) adding the remaining deionized water to the slurry obtained in step (4) and continuing stirring for 0.5 to 1.5 hours to adjust the viscosity to 1500 to 4500 mPa.s;
[0014] (6) Add the styrene-butadiene rubber binder to the slurry with the viscosity adjusted in step (5) and stir for 0.5 to 1 hour; reverse the stirring blade of the planetary mixer, vacuumize to remove small bubbles in the slurry, and then sieve the material through the sieve plate from the discharge port of the planetary mixer to obtain the slurry of the graphite negative electrode binder to be prepared.
[0015] As a further improvement of the present technology, in step (2), the revolution speed of the planetary mixer is 15 to 35 rpm, and the rotation speed is 100 to 500 rpm.
[0016] As a further improvement of the present technology, in step (3), the revolution speed of the planetary mixer is 25 to 40 rpm, and the rotation speed is 300 to 1000 rpm.
[0017] As a further improvement of the present technology, in step (4), the revolution speed of the planetary mixer is 25 to 40 rpm, and the rotation speed is 500 to 1500 rpm.
[0018] As a further improvement of the present technology, in step (5), the revolution speed of the planetary mixer is 25 to 45 rpm, and the rotation speed is 1000 to 2000 rpm.
[0019] As a further improvement of the present technology, in step (6), the revolution speed of the planetary mixer is 25 to 40 rpm, and the rotation speed is 300 to 1200 rpm.
[0020] As a further improvement of the present technology, the mesh size of the sieve plate through which the slurry is screened in step (6) is set to 150.
[0021] In a second aspect, the present invention provides a negative electrode plate, comprising the negative electrode slurry obtained by the above method; the preparation method thereof is: the negative electrode slurry is uniformly applied on a copper foil according to a set surface density, and the solvent in the slurry is removed by baking to obtain an unrolled negative electrode plate.
[0022] As a further improvement of the present technology, the thickness of the copper foil is 8-12 μm.
[0023] In a third aspect, the present invention provides a lithium-ion battery comprising the above-mentioned negative electrode plate.
[0024] Compared with the prior art, the beneficial technical effects of the present invention are:
[0025] ① The present invention adds a polyacrylic acid binder, which is beneficial to increasing the solid content of the slurry, while ensuring the stability of the slurry viscosity, facilitating slurry homogenization and screening, and avoiding the problem of screen clogging caused by graphite particle agglomeration.
[0026] ② At the same time, it greatly improves the curling and cracking problems in the coating process; it also greatly improves the adhesion between the graphite material and the foil, so that the electrode has better processing performance, and reduces the occurrence of roller sticking and material falling during electrode rolling and slitting; it further improves the stability of the graphite material and makes the battery cycle life better.
[0027] ③ The present invention adds a polyacrylic acid binder, which can improve the discharge efficiency of the battery in a low temperature environment and help improve the low temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The present invention will be further described below in conjunction with the accompanying drawings.
[0029] Figure 1 It is a schematic diagram of the capacity retention rate of the cylindrical 18650 lithium-ion battery cycle test curve of the present invention.
[0030] Figure 2 It is a schematic diagram of the discharge efficiency of the cylindrical 18650 lithium battery of the present invention at a low temperature of -20°C. DETAILED DESCRIPTION
[0031] Embodiment 1: A method for preparing a slurry of a graphite negative electrode containing a polyacrylic acid binder, comprising the following steps:
[0032] (1) preparing raw material components for preparing graphite negative electrode slurry, the raw material components comprising graphite material, carbon black conductive agent, sodium carboxymethyl cellulose, polyacrylic acid binder, styrene-butadiene rubber binder, and deionized water, wherein the mass ratio of the raw material components is set to 96.5:0.5:1.0:1.0:1.0:75;
[0033] (2) adding graphite material, carbon black conductive agent and sodium carboxymethyl cellulose to a planetary mixer and mixing them for 0.5 h to obtain a uniform powder. The revolution speed of the planetary mixer is 20 rpm and the rotation speed is 200 rpm.
[0034] (3) adding 55% deionized water to the uniform powder obtained in step (2) and stirring for 3.5 hours, the revolution speed of the planetary mixer is 35 rpm and the rotation speed is 400 rpm;
[0035] (4) adding a polyacrylic acid binder to the slurry obtained in step (3) and stirring for 1 hour, the planetary mixer has an orbital speed of 35 rpm and an autorotational speed of 1500 rpm;
[0036] (5) Add the remaining deionized water to the slurry obtained in step (4) and continue stirring for 0.5 h, adjust the viscosity to 1500-5000 mPa.s, and the revolution speed of the planetary mixer is 35 rpm and the rotation speed is 2000 rpm;
[0037] (6) Add styrene-butadiene rubber binder to the slurry with the viscosity adjusted in step (5) and stir for 0.5 h. The planetary mixer has an orbital speed of 35 rpm and an autorotational speed of 1000 rpm. Reverse the stirring paddle of the planetary mixer to remove small bubbles in the slurry, and then sieve the slurry through a sieve plate from the outlet of the planetary mixer to obtain the graphite negative electrode slurry to be prepared.
[0038] (7) Slurry viscosity test results: 3166mpa.s, slurry solid content test results: 55.11%;
[0039] Example 2: The same as Example 1, except that the mass ratio of the raw material components in step (1) is set to 96.5:0.5:1.5:0.7:0.8:71.42; the slurry viscosity test result: 2065mpa.s, the slurry solid content test result: 54.23%;
[0040] Comparative Example 1: A conventional graphite negative electrode slurry mixing method, comprising the following steps:
[0041] (1) preparing raw material components for preparing graphite negative electrode slurry, the raw material components comprising graphite material, carbon black conductive agent, sodium carboxymethyl cellulose, styrene-butadiene rubber binder, and deionized water, wherein the mass ratio of the raw material components is set to 96.0:0.5:1.5:2.0:98;
[0042] (2) adding graphite material, carbon black conductive agent and sodium carboxymethyl cellulose to a planetary mixer and mixing them for 0.5 h to obtain a uniform powder. The revolution speed of the planetary mixer is 20 rpm and the rotation speed is 100 rpm.
[0043] (3) adding 80% deionized water to the uniform powder obtained in step (2) and stirring for 2.5 hours, the revolution speed of the planetary mixer is 35 rpm and the rotation speed is 400 rpm;
[0044] (4) adding the remaining deionized water to the slurry obtained in step (3) and continuing stirring, adjusting the viscosity to 1500-5000 mPa.s, the revolution speed of the planetary mixer to 35 rpm, and the rotation speed to 2000 rpm;
[0045] (5) Add styrene-butadiene rubber binder to the slurry with the viscosity adjusted in step (4) and stir for 0.5 h. The planetary mixer has an orbital speed of 35 rpm and an autorotational speed of 1000 rpm. Reverse the stirring paddle of the planetary mixer to remove small bubbles in the slurry, and then sieve the slurry through a sieve plate from the outlet of the planetary mixer to obtain the graphite negative electrode slurry to be prepared.
[0046] (6) Slurry viscosity test results: 2178mpa.s, slurry solid content test results: 50.11%;
[0047] Comparative Example 2: The same as Comparative Example 1, except that the mass ratio of the raw material components in step (1) is set to 95.0:1.0:1.5:2.5:98; the slurry viscosity test result: 2578mpa.s, the slurry solid content test result: 48.89%;
[0048] Preparation of negative electrode graphite slurry: The graphite negative electrode slurry obtained in Examples 1 and 2 and Comparative Examples 1 and 2 was used for viscosity testing using a digital viscometer. The viscosity of the slurry after adjustment was basically maintained at 1500-5000 mPa.s when the discharge screening was met. The solid content of the slurry was tested using a sampling and drying method. The solid content data showed that the solid content of Comparative Examples 1 and 2 was obviously low, as shown in Table 1.
[0049] Table 1 Comparative performance table of negative electrode slurry viscosity of embodiment and comparative example (unit: mpa.s)
[0050] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Viscosity 3166 2065 2178 2578 Solid content 55.11% 54.23% 50.11% 48.89%
[0051] It can be seen from Table 1 that the solid content of the slurries prepared in Examples 1 and 2 is significantly higher than that in Comparative Examples 1 and 2, wherein the polyacrylic acid binder has a significant effect on increasing the solid content of the slurry.
[0052] Slurry stability test: The graphite negative electrode slurry obtained in Examples 1 and 2 and Comparative Examples 1 and 2 was allowed to stand under the same environment, and samples were taken at different times to test the viscosity and solid content thereof, as shown in Tables 2 and 3.
[0053] Table 2 Comparative performance table of viscosity stability of negative electrode slurry of embodiment and comparative example (unit: mpa.s)
[0054] Standing time 10min 4h 8h 24h Example 1 1653 3374 4410 5142 Example 2 1591 3703 4467 5201 Comparative Example 1 1865 3578 4963 6088 Comparative Example 2 2016 4215 5212 6436
[0055] It can be seen from Table 2 that the graphite negative electrode slurries obtained in Examples 1 and 2 and Comparative Examples 1 and 2 are relatively more stable in viscosity and change less under the same environment and the same standing time, while the viscosity of the slurries in Comparative Examples 1 and 2 changes greatly.
[0056] Table 3 Comparative performance table of solid content stability of negative electrode slurry of embodiment and comparative example (unit: mpa.s)
[0057] Standing time 10min 4h 8h 24h Example 1 54.18% 54.21% 54.15% 53.12% Example 2 53.15% 53.27% 53.26% 53.20% Comparative Example 1 48.97% 48.70% 48.36% 48.07% Comparative Example 2 48.89% 48.58% 48.26% 47.92%
[0058] It can be seen from Table 3 that the graphite negative electrode slurries obtained in Examples 1 and 2 and Comparative Examples 1 and 2 are stable in the same environment and for the same standing time. The solid content of the slurries in Examples 1 and 2 is stable, and 24 hours of standing has basically no effect on them. The solid content of the slurries in Comparative Examples 1 and 2 gradually decreases with time, indicating that the slurries are unstable and have a certain stratification phenomenon.
[0059] Preparation of negative electrode sheet: The graphite negative electrode slurry obtained in Examples 1 and 2 and Comparative Examples 1 and 2 was uniformly coated on the surface of the copper foil, and finally formed into a negative electrode sheet after processes such as rolling and slicing. During coating, it can be clearly observed that the electrode sheets of Comparative Examples 1 and 2 have curling and cracking, and in the subsequent rolling process, the roller sticking is prone to occur, and in the slicing stage, the edge parts are prone to material falling.
[0060] Performance test: The negative electrode sheet prepared above was prepared into a 18650-2600mAh lithium-ion battery. The negative electrode sheet was subjected to a peeling force test using a micro-controlled electronic universal testing machine. The test data is shown in Table 4. The lithium-ion battery was subjected to a cycle performance test, such as Figure 1 shown.
[0061] Table 4: Comparative performance table of negative electrode sheet peeling force of examples and comparative examples (unit: N)
[0062] plan average value Test value 1 Test value 2 Test value 3 Test value 4 Test value 5 Test value 6 Example 1 0.1650 0.1616 0.1556 0.1731 0.1718 0.1668 0.1613 Example 2 0.1355 0.1275 0.1348 0.1377 0.1482 0.1318 0.1330 Comparative Example 1 0.0334 0.0502 0.0414 0.0233 0.0208 0.0249 0.0397 Comparative Example 2 0.0442 0.0333 0.0570 0.0396 0.0347 0.0481 0.0527
[0063] It can be seen from Table 4 that the negative electrode sheets prepared in Examples 1 and 2 have significantly better peeling force than Comparative Examples 1 and 2, wherein the polyacrylic acid binder has a significant effect on improving the peeling force, greatly improving the adhesion between the graphite material and the foil, making the sheet have better processing performance, and reducing the occurrence of roller sticking and material falling during the rolling and slitting of the sheet; further improving the stability of the graphite material, and making the battery cycle life better.
[0064] Improvement of low-temperature discharge performance: The addition of polyacrylic acid binder can not only greatly improve the adhesion of the negative electrode, but also help reduce the polarization impedance of the electrode. Low temperature environment will increase the brittleness of the material. The adhesion of PAA can effectively prevent the electrode from falling off or breaking during the charge and discharge process, help maintain the integrity of the electrode, and prevent structural damage caused by temperature changes. Although the carboxyl terminal group in PAA has a certain effect on the performance of the binder, through appropriate chemical modification, such as the use of PAALi and PAANa, it can be more evenly distributed through the electrostatic repulsion between the -COO- groups, which is conducive to building a uniform and stable conductive network, thereby blocking the electrolyte to a certain extent, inhibiting the decomposition of the electrolyte, and further improving battery performance.
[0065] from Figure 1 It can be seen that the cylindrical 18650 lithium-ion battery cycle test curves prepared in Example 1 and Example 2 have higher capacity retention rates, and have better cycle performance than the lithium-ion batteries in Comparative Example 1 and Comparative Example 2. This shows that the binder ratio and slurry mixing method of the present invention can not only effectively improve the processing performance of the graphite negative electrode sheet, but also improve the cycle stability of the lithium-ion battery.
[0066] from Figure 2 It can be seen that the discharge efficiency of the cylindrical 18650 lithium-ion batteries prepared in Example 1 and Example 2 at a low temperature of -20°C is higher than that of Comparative Example 1 and Comparative Example 2. This shows that the binder ratio and slurry mixing method of the present invention can not only effectively improve the processing performance of the graphite negative electrode sheet and enhance the cycle stability of the lithium-ion battery, but also improve the low-temperature discharge performance.
[0067] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. Graphite negative electrode binder, It is characterized in that The raw material components include graphite material, carbon black conductive agent, sodium carboxymethyl cellulose, polyacrylic acid binder, styrene-butadiene rubber binder and deionized water, and the mass ratios of the raw material components are set to 90-98, 0.5-3, 0.5-2, 0.5-5, 1-5 and 10-100.
2. Graphite negative electrode binder slurry mixing method, Features: The method comprises the following steps: (1) preparing raw material components for preparing graphite negative electrode slurry, the raw material components including graphite material, carbon black conductive agent, sodium carboxymethyl cellulose, polyacrylic acid binder, styrene-butadiene rubber binder, and deionized water, wherein the mass ratio of the raw material components is set to 90-98, 0.5-3, 0.5-2, 0.5-5, 1-5, and 10-100; (2) adding graphite material, carbon black conductive agent and sodium carboxymethyl cellulose into a planetary mixer and mixing for 0.5 to 1.5 hours to obtain a uniform powder; (3) adding 55-80% deionized water to the uniform powder obtained in step (2) and stirring for 2-4 hours; (4) adding a polyacrylic acid binder to the slurry obtained in step (3) and stirring for 1 to 3 hours; (5) adding the remaining deionized water to the slurry obtained in step (4) and continuing stirring for 0.5 to 1.5 hours to adjust the viscosity to 1500 to 4500 mPa.s; (6) Add the styrene-butadiene rubber binder to the slurry with the viscosity adjusted in step (5) and stir for 0.5 to 1 hour; reverse the stirring blade of the planetary mixer, vacuumize to remove small bubbles in the slurry, and then sieve the material through the sieve plate from the discharge port of the planetary mixer to obtain the slurry of the graphite negative electrode binder to be prepared.
3. The method for preparing a slurry of a graphite negative electrode binder according to claim 2, Features: In the step (2), the planetary mixer has a revolution speed of 15 to 35 rpm and a rotation speed of 100 to 500 rpm.
4. The method for preparing a slurry of a graphite negative electrode binder according to claim 2, Features: In the step (3), the planetary mixer has an orbital speed of 25 to 40 rpm and an autorotational speed of 300 to 1000 rpm.
5. The method for preparing a slurry of a graphite negative electrode binder according to claim 2, Features: In the step (4), the planetary mixer has an orbital speed of 25 to 40 rpm and an autorotational speed of 500 to 1500 rpm.
6. The method for preparing a slurry of a graphite negative electrode binder according to claim 2, Features: In the step (5), the planetary mixer has an orbital speed of 25 to 45 rpm and an autorotational speed of 1000 to 2000 rpm.
7. The method for preparing a slurry of a graphite negative electrode binder according to claim 2, Features: In the step (6), the revolution speed of the planetary mixer is 25-40 rpm, and the rotation speed is 300-1200 rpm; the mesh number of the sieve plate for screening the slurry discharge in the step (6) is set to 150.
8. Negative electrode, Features: The invention relates to a negative electrode slurry obtained by the method described in any one of claims 1 to 7; the preparation method thereof is as follows: the negative electrode slurry is uniformly coated on a copper foil according to a set surface density, and the solvent in the slurry is removed by baking to obtain an unrolled negative electrode sheet.
9. The negative electrode sheet according to claim 8, Features: The copper foil has a thickness of 8-12 μm.
10. Lithium-ion battery, Features: A negative electrode sheet comprising the negative electrode sheet as described in any one of claims 8 or 9.
Citation Information
Patent Citations
Preparation method of lithium battery negative electrode slurry
CN107240674A
Silicon-carbon negative electrode slurry mixing method
CN111313005A
Negative electrode slurry and preparation method thereof
CN115663106A
Lithium battery negative electrode slurry and preparation method thereof
CN117317222A
Cited By
Secondary battery and preparation method thereof, energy storage device and electric equipment
CN119994215A
Secondary battery, method for preparing same, energy storage device, and electrical equipment
CN119994215B
Slurry auxiliary agent and method for preparing aqueous hard carbon negative pole piece of sodium ion battery by using slurry auxiliary agent
CN120169022A
Negative electrode slurry for lithium ion battery, preparation method of negative electrode slurry, negative electrode and lithium ion battery
CN120527351A