Preparation method of low-temperature curing polyimide binder for lithium ion battery, binder prepared by preparation method and electrode plate

Through the coordinated effect of polyimide molecular structure design and catalyst, the imidation temperature of polyamic acid is reduced, the stability and energy consumption problems of traditional adhesives at high temperatures are solved, and the high thermal stability of lithium-ion batteries is achieved It has a stronger bonding performance, supporting the application of batteries under more stringent conditions.

CN119050279AActive Publication Date: 2024-11-29HANGZHOU INST OF ADVANCED MATERIAL BEIJING UNIV OF CHEM TECH

Patent Information

Application Number
CN202411150177.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The poor stability and weak bonding performance of traditional lithium-ion battery adhesives in high temperature environments lead to shortening battery safety and cycle life. The high imidation temperature of existing polyimide adhesives leads to high energy consumption. The cost is high, limiting its industrial application.

Method used

By designing the molecular structure of polyimide and synergistically with the catalyst, the imidation temperature of polyamic acid is reduced, and the condensation polymerization reaction under nitrogen atmosphere and ice water bath conditions is prepared by combining the capping agent and the catalyst to prepare low-temperature curing Polyimide binder reduces energy consumption and improves bonding performance.

Benefits of technology

It achieves high thermal stability and stronger bonding performance of lithium-ion batteries, reduces energy consumption and production costs, supports the application of batteries under more stringent conditions, and improves the electrochemical performance and cycle life of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a preparation method of a low-temperature curing polyimide binder for a lithium ion battery, the binder prepared by the preparation method and an electrode plate. The preparation method comprises the following steps: carrying out condensation polymerization on dianhydride, a diamine monomer and a monomer containing a special functional group in a solvent to obtain copolymerized polyamide acid; adding an end-capping reagent, and fully and uniformly stirring to obtain end-capped polyamide acid; adding a catalyst and fully and uniformly stirring to obtain a precursor solution of polyimide; and uniformly mixing the polyimide with an active substance and a conductive agent to prepare slurry, coating the surface of a current collector with the slurry, and performing heat treatment at 100-150 DEG C to prepare the lithium ion battery pole piece taking the low-temperature cured polyimide as the adhesive. According to the method, the process use temperature of the polyimide binder can be greatly reduced, energy is saved, cost is reduced, and meanwhile the influence of high-temperature treatment of traditional thermal imidization on the performance of an electrode material is avoided. The lithium ion battery assembled by adopting the electrode plate prepared by the invention has excellent electrical properties such as higher specific capacity and capacity retention rate and safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode materials, and in particular to a method for preparing a low-temperature curing polyimide adhesive for lithium-ion batteries, and the prepared adhesive and electrode pole piece. Background Art

[0002] Lithium-ion batteries have developed into one of the most promising new generation energy sources today due to their high specific energy, low self-discharge, no memory effect and environmental protection. However, with the continuous improvement of their energy density and capacity, the resulting battery safety issues have become increasingly prominent. As an important component of lithium-ion battery electrodes, although the binder accounts for a relatively low proportion of the mass in the electrode material, its function cannot be ignored. The binder is not only responsible for tightly combining the active material, the conductive agent and the current collector, but also plays a key role in the electrode performance and stability. Specifically, the binder can inhibit the volume expansion of the electrode during the charge and discharge process and effectively reduce the side reactions between the active material and the electrolyte, thereby improving the cycle life and safety of the battery. At present, although traditional binders have a low cost, they have poor stability in high temperature environments. During the long-term use of lithium-ion batteries, the increase in the internal temperature of the battery may cause thermal degradation of the binder, which not only affects the mechanical integrity of the battery, but may also cause serious safety hazards. In addition, the bonding performance of existing binders will weaken after multiple charge and discharge cycles, resulting in failure of the interface connection between the active material and the current collector, and thus failing to effectively inhibit the volume expansion of the electrode. These problems ultimately lead to a shortened cycle life of lithium-ion batteries and increased capacity decay, limiting their application in high-performance applications. Therefore, in view of the shortcomings of existing binders in terms of heat resistance and bonding performance, the development of new binder materials with higher thermal stability and stronger bonding force has become a key research direction for improving the performance of lithium-ion batteries. This not only helps to improve the safety and cycle life of the battery, but also supports the application of lithium-ion batteries under more stringent working conditions.

[0003] Polyimide (PI) has many monomer types and a highly designable molecular structure. It is considered the first choice for lithium-ion battery binders because of its high and low temperature resistance, high bonding strength, chemical stability, and self-extinguishing flame retardant properties. Its excellent heat resistance can maintain the structural stability of electrode materials under high temperature and high pressure, and improve the capacity of electrodes under high-pressure cycles. Good chemical stability makes polyimide adhesives less likely to be oxidized or reduced, and does not react with other materials, thus ensuring the electrochemical stability of the electrode. In addition, the molecular structure of polyimide gives it higher tensile strength and elastic recovery ability, which can effectively adapt to the contraction and expansion of the electrode, ensuring the structural integrity and stability of the electrode during the cycle. However, the imidization process of polyimide usually requires high-temperature treatment above 300°C, which is not conducive to reducing energy consumption. At the same time, high-temperature treatment may also affect the performance of the electrode material itself. Therefore, there is an urgent need for a low-temperature curing technology to reduce the imidization temperature of polyimide, so that it has more potential for industrial application. Summary of the invention

[0004] The purpose of the present invention is to overcome the poor safety performance of traditional adhesives in high specific capacity lithium-ion batteries, and the high imidization temperature of existing polyimide adhesives, which leads to high energy consumption, high cost, and is not conducive to industrial application. Provided are a preparation method of a low-temperature curing polyimide adhesive for lithium-ion batteries and an adhesive and an electrode plate prepared thereby. The preparation method can significantly reduce the thermal imidization temperature of the polyimide adhesive in the later stage through special design of the molecular structure of polyimide and the synergistic effect of the later stage and the catalyst, thereby reducing energy consumption and having more excellent electrical properties than traditional adhesives.

[0005] To achieve the above-mentioned purpose, the present invention provides a method for preparing a low-temperature curing polyimide binder for lithium-ion batteries and an electrode plate prepared therefrom, comprising the following steps.

[0006] (1) Under nitrogen atmosphere and ice-water bath conditions, an excess of dianhydride monomer, a diamine monomer and a third monomer containing a special functional group are subjected to condensation polymerization in a reaction solvent to obtain a copolymerized polyamic acid solution. The molecular weight of the polyimide can be adjusted by the relative amount of the dianhydride monomer added.

[0007] (2) adding a blocking agent to the polyamic acid solution obtained by the above copolymerization and stirring the mixture to obtain a blocked polyamic acid solution;

[0008] (3) adding a catalyst to the polyamic acid solution obtained in step (2) and stirring the mixture to obtain a precursor solution of a low-temperature curable polyimide;

[0009] (4) The active material, the conductive agent and the precursor solution obtained in step (3) are uniformly mixed to obtain a slurry, which is coated on the surface of the current collector and then subjected to thermal imidization treatment to obtain an electrode plate with a low-temperature curing polyimide as a binder.

[0010] Preferably, the solid content of the polyamic acid solution in step (1) is 0.5-40wt%; the molar ratio of the dianhydride monomer to the diamine monomer is 1.01:1-1.3:1; the molar ratio of the dianhydride monomer to the diamine monomer containing a special functional group is 9-25:1; the reaction time is 0.5-12h;

[0011] Preferably, the dianhydride monomer in step (1) is a mixture of one or more of pyromellitic dianhydride (PMDA), 4,4'-diphenyl ether dianhydride (ODPA), biphenyl dianhydride (BPDA), 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride (DSDA), hexafluoro dianhydride (6FDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 4,4'-(4,4'-isopropylidene diphenyloxy) diphthalic anhydride (BPADA), and p-phenylene-triphenylene dianhydride (TAHQ) in any proportion;

[0012] Preferably, the diamine monomer in step (1) is a mixture of one or more of p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), 4,4'-diaminodiphenyl ether (ODA), 3,4'-diaminodiphenyl ether (3,4'-ODA), 4,4'-diaminodiphenyl sulfone (DDS), 3,3'-diaminodiphenyl sulfone (MSDS), 2,2'-dimethyl-4,4'-diaminobiphenyl (MTB), 4,4'-diaminodiphenylmethane (MDA), and 1,3-bis(4'-aminophenoxy)benzene (TPE) in any proportion;

[0013] Preferably, the third monomer containing a special functional group in step (1) is a mixture of one or more of 2,3-diaminopyridine, 2,4-diaminopyridine, 2,5-diaminopyridine, 3,4-diaminopyridine, 5,6-diaminobenzimidazolone, 2,4-diamino-6-[2-methyl-(-imidazolyl)ethyl]-1,3,5-quinoline, and 5-amino-2-(4-aminophenyl)benzimidazole in any proportion;

[0014] Preferably, the solvent in step (1) is a mixture of one or more of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-ethylpyrrolidone (NEP), dimethyl sulfoxide (DMSO), and hexamethylphosphoramide (HMPA) in any proportion;

[0015] Preferably, in step (2), the molar ratio of the end-capping agent to the dianhydride monomer is 0.01:1-5:1; the reaction time is 0.5-12h;

[0016] Preferably, the end-capping agent in step (2) is a mixture of one or more of 5-aminobenzimidazole (ABZ), 2-aminoimidazole, 2-aminopyridine, and aminopyrazine in any proportion;

[0017] Preferably, in step (3), the molar ratio of the catalyst to the dianhydride monomer is 0.01:1-5:1; the reaction time is 0.5-12h;

[0018] Preferably, the catalyst in step (3) is a mixture of one or more of N-N'carbonyldiimidazole (CDI), 6-aminoquinoline (AQL), ​​benzotriazole (BTA) and 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) in any proportion;

[0019] Preferably, the solid content of the electrode slurry in step (4) is 20-90wt%; the non-solvent part of the electrode slurry contains 80-99wt% of active material, 0.5-10wt% of conductive agent, and 0.5-10wt% of precursor solution;

[0020] Preferably, the positive electrode active material in step (4) is a mixture of one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt aluminum oxide and lithium nickel cobalt manganese oxide ternary materials in any proportion;

[0021] Preferably, the negative electrode active material in step (4) is a mixture of one or more of carbon materials, silicon and its oxides, tin and its oxides, silicon-carbon composite materials, silicon-oxygen-carbon composite materials and tin-carbon composite materials in any proportion;

[0022] Preferably, the conductive agent in step (4) is a mixture of one or more of conductive carbon black, conductive graphite, graphene and carbon nanotubes in any proportion.

[0023] Preferably, the current collector in step (4) is a carbon-containing aluminum foil or a carbon-containing copper foil;

[0024] Preferably, the electrode slurry coating thickness in step (4) is 75-200 μm; the thermal imidization temperature is 100-150° C., and the time is 0.5-2 h;

[0025] Another object of the present invention is to provide a low-temperature curing polyimide adhesive for lithium-ion batteries prepared by the method and an electrode plate prepared therefrom.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The method of the present invention can significantly reduce the imidization temperature of polyamic acid by designing the molecular structure of polyimide and the synergistic effect with an external catalyst, avoiding the occurrence of side reactions in the electrode material during the high-temperature imidization process, while reducing energy consumption and saving production costs. The lithium-ion battery assembled by the method has more excellent electrical properties. The method of the present invention does not need to change the original production and process flow, is simple to operate, and is convenient for continuous production.

[0028] 2. The end-capping agent and catalyst used in the method of the present invention are more environmentally friendly than traditional chemical imidization agents, improve the operating environment, and are conducive to green production. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The following is further explained in conjunction with specific embodiments. It should be noted that the following embodiments are only used to illustrate but not limit the technical solutions described in the present invention, and all equivalent exchanges made on the basis of the technical solutions of this application fall within the protection scope of the present invention.

[0031] The present invention provides a low-temperature curing polyimide binder for lithium-ion batteries and an electrode plate prepared therefrom. The electrochemical properties and applications thereof are investigated by assembling a button cell for charge and discharge testing using a conventional method in the art. The button cell assembly process and technology are as follows:

[0032] After drying the electrode, place it in the glove box, and assemble the button battery using a 2032-type button battery shell: the negative electrode shell, negative electrode sheet, diaphragm, electrolyte drop, positive electrode sheet, gasket, and spring are placed in order, covered with the positive electrode shell, sealed with a sealing machine, tested with a current of 0.1C, and the voltage range is 2.5 to 4.3V. This electrode preparation and battery assembly are applicable to all the following embodiments and comparative examples.

[0033] The following is further explained in conjunction with specific embodiments. It should be noted that the following embodiments are only used to illustrate but not limit the technical solutions described in the present invention, and all equivalent exchanges made on the basis of the technical solutions of this application fall within the protection scope of the present invention.

[0034] Example 1

[0035] (1) 3.273 g of 4,4'-diaminodiphenyl ether and 0.198 g of 2,3-diaminopyridine were dissolved in 50 ml of N-methylpyrrolidone solvent, and 5.75 g of 4,4'-biphenyl ether dianhydride was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a homogeneous polyamic acid solution;

[0036] (2) adding 2% by molar mass of 4,4'-biphenyl ether dianhydride capping agent 5-aminobenzimidazole to the polyamic acid solution and stirring the mixture thoroughly to obtain a capped polyamic acid solution;

[0037] (3) adding a catalyst N-N'-carbonyldiimidazole having a molar mass of 10% of 4,4'-biphenyl ether dianhydride to the blocked polyamic acid solution obtained in step (2), and stirring the mixture thoroughly to obtain a precursor solution of a low-temperature curing polyimide adhesive;

[0038] (4) The above precursor solution was diluted to a solution with a solid content of 5wt%, and mixed with the positive electrode active material NCM811, conductive carbon black, and the diluted precursor solution in a mass fraction of 92:5:3, and N-methylpyrrolidone solvent was added to dissolve the mixture, and the positive electrode slurry was prepared by fully stirring. The above slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12h, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150°C, and kept warm for 2h, and the pole piece was taken out and weighed.

[0039] (5) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 198.32 mAh / g, the first coulombic efficiency is 86.9%, and the capacity retention rate is 87.03% after 100 cycles at 0.1C.

[0040] Example 2

[0041] (1) 3.444 g of 4,4'-diaminodiphenyl ether and 0.113 g of 5,6-diaminobenzimidazolone were dissolved in 50 ml of N-methylpyrrolidone solvent, and 5.723 g of 4,4'-biphenyl ether dianhydride was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a homogeneous polyamic acid solution;

[0042] (2) Adding 2% of the molar mass of 4,4'-biphenyl ether dianhydride as a blocking agent 5-aminobenzimidazole to the above polyamic acid solution and stirring thoroughly to obtain a blocked polyamic acid solution.

[0043] (3) Adding N-N'-carbonyldiimidazole containing 10% of the molar mass of 4,4'-biphenyl ether dianhydride to the blocked polyamic acid solution obtained in step (2), stirring thoroughly, and obtaining a precursor solution of a low-temperature curing polyimide adhesive.

[0044] (4) The above precursor solution was diluted to a solution with a solid content of 5wt%, and mixed with the positive electrode active material NCM811, conductive carbon black, and the diluted precursor solution in a mass fraction of 92:5:3, and N-methylpyrrolidone solvent was added to dissolve the mixture, and the positive electrode slurry was prepared by fully stirring. The above slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12h, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150°C, and kept warm for 2h, and the pole piece was taken out and weighed.

[0045] (5) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 195.01mAh / g, the first efficiency is 85.43%, and the capacity retention rate is 85.37% after 100 cycles at 0.1C.

[0046] Example 3

[0047] (1) 3.199 g of 4,4'-diaminodiphenyl ether and 3.199 g of 5-amino-2-(4-aminophenyl)benzimidazole were dissolved in 50 ml of N-methylpyrrolidone solvent, and 5.682 g of 4,4'-biphenyl ether dianhydride was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a homogeneous polyamic acid solution;

[0048] (2) Add 5-aminobenzimidazole as a capping agent with a molar mass of 2% of 4,4'-biphenyl ether dianhydride to the above polyamic acid solution and stir thoroughly to obtain a capped polyamic acid solution.

[0049] (3) adding N-N'-carbonyldiimidazole containing 10% of the molar mass of 4,4'-biphenyl ether dianhydride to the blocked polyamic acid solution obtained in step (2), and stirring thoroughly to obtain a precursor solution of a low-temperature curing polyimide adhesive;

[0050] (4) The above precursor solution was diluted to a solution with a solid content of 5wt%, and mixed with the positive electrode active material NCM811, conductive carbon black, and the diluted precursor solution in a mass fraction of 92:5:3, and N-methylpyrrolidone solvent was added to dissolve the mixture, and the positive electrode slurry was prepared by fully stirring. The above slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12h, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150°C, and kept warm for 2h, and the pole piece was taken out and weighed.

[0051] (5) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 190.87 mAh / g, the first efficiency is 83.34%, and the capacity retention rate is 86.22% after 100 cycles at 0.1C.

[0052] Example 4

[0053] (1) 3.273 g of 4,4'-diaminodiphenyl ether and 0.198 g of 2,3-diaminopyridine were dissolved in 50 ml of N-methylpyrrolidone solvent, and 5.75 g of 4,4'-biphenyl ether dianhydride was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a homogeneous polyamic acid solution;

[0054] (2) adding 2-aminopyridine, a capping agent, in an amount of 2% by molar weight of 4,4'-biphenyl ether dianhydride to the polyamic acid solution and stirring the mixture thoroughly to obtain a capped polyamic acid solution;

[0055] (3) Adding 10% of the molar mass of 4,4'-biphenyl ether dianhydride catalyst N-N' to the blocked polyamic acid solution obtained in step (2)

[0056] carbonyldiimidazole, and fully stirring to obtain a precursor solution of a low-temperature curing polyimide adhesive;

[0057] (4) The above precursor solution was diluted to a solution with a solid content of 5wt%, and mixed with the positive electrode active material NCM811, conductive carbon black, and the diluted precursor solution in a mass fraction of 92:5:3, and N-methylpyrrolidone solvent was added to dissolve the mixture, and the positive electrode slurry was prepared by fully stirring. The above slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12h, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150°C, and kept warm for 2h, and the pole piece was taken out and weighed.

[0058] (5) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 193.23 mAh / g, the first efficiency is 86.43%, and the capacity retention rate is 85.68% after 100 cycles at 0.1C.

[0059] Example 5

[0060] (1) 3.273 g of 4,4'-diaminodiphenyl ether and 0.198 g of 2,3-diaminopyridine were dissolved in 50 ml of N-methylpyrrolidone solvent, and 5.75 g of 4,4'-biphenyl ether dianhydride was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a homogeneous polyamic acid solution;

[0061] (2) adding 2-aminoimidazole, a capping agent having a molar weight of 2% of 4,4'-biphenyl ether dianhydride, to the polyamic acid solution and stirring the mixture thoroughly to obtain a capped polyamic acid solution;

[0062] (3) adding N-N'-carbonyldiimidazole containing 10% of the molar mass of 4,4'-biphenyl ether dianhydride to the blocked polyamic acid solution obtained in step (2), and stirring thoroughly to obtain a precursor solution of a low-temperature curing polyimide adhesive;

[0063] (4) The above precursor solution was diluted to a solution with a solid content of 5wt%, and mixed with the positive electrode active material NCM811, conductive carbon black, and the diluted precursor solution in a mass fraction of 92:5:3, and N-methylpyrrolidone solvent was added to dissolve the mixture, and the positive electrode slurry was prepared by fully stirring. The above slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12h, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150°C, and kept warm for 2h, and the pole piece was taken out and weighed.

[0064] (5) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 193.47 mAh / g, the first coulombic efficiency is 86.28%, and the capacity retention rate is 85.58% after 100 cycles at 0.1C.

[0065] Example 6

[0066] (1) 3.273 g of 4,4'-diaminodiphenyl ether and 0.198 g of 2,3-diaminopyridine were dissolved in 50 ml of N-methylpyrrolidone solvent, and 5.75 g of 4,4'-biphenyl ether dianhydride was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a homogeneous polyamic acid solution;

[0067] (2) adding 2% by molar mass of 4,4'-biphenyl ether dianhydride capping agent 5-aminobenzimidazole to the polyamic acid solution and stirring the mixture thoroughly to obtain a capped polyamic acid solution;

[0068] (3) adding a catalyst 6-aminoquinoline having a molar mass of 80% of 4,4'-biphenyl ether dianhydride to the blocked polyamic acid solution obtained in step (2), and stirring the mixture thoroughly to obtain a precursor solution of a low-temperature curing polyimide adhesive;

[0069] (4) The above precursor solution was diluted to a solution with a solid content of 5wt%, and mixed with the positive electrode active material NCM811, conductive carbon black, and the diluted precursor solution in a mass fraction of 92:5:3, and N-methylpyrrolidone solvent was added to dissolve the mixture, and the positive electrode slurry was prepared by fully stirring. The above slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12h, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150°C, and kept warm for 2h, and the pole piece was taken out and weighed.

[0070] (5) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 192.91 mAh / g, the first coulombic efficiency is 85.11%, and the capacity retention rate is 84.92% after 100 cycles at 0.1C.

[0071] Comparative Example 1

[0072] (1) Weigh 2.68 g of powdered PVDF and dissolve it in 30 ml of NMP to obtain a PVDF glue solution with a solid content of 5%.

[0073] (2) The positive electrode active material NCM811, conductive carbon black, and PVDF glue were mixed in the mass fractions of 94%, 3%, and 3%, and NMP solvent was added to dissolve the mixture. The mixture was stirred for 120 minutes to prepare a positive electrode slurry. The slurry containing PVDF was coated on an aluminum foil (10 cm × 12 cm) and placed in a clean bench to dry at room temperature for 12 hours. Cut into 12 mm round pieces, roll and weigh.

[0074] (3) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 160.23 mAh / g, the first efficiency is 73.2%, and the capacity retention rate is 60.23% after 100 cycles at 0.1C.

[0075] Comparative Example 2

[0076] (1) 1.962 g of ODA was dissolved in 30 ml of NMP solvent, and 3.060 g of ODPA was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a homogeneous polyamic acid solution; a precursor solution of a polyimide adhesive;

[0077] (2) The above precursor solution was diluted to a solution with a solid content of 5wt%, and mixed with the positive electrode active material NCM811, conductive carbon black, and the diluted precursor solution in a mass ratio of 92:5:3, and NMP solvent was added to dissolve the mixture, and the positive electrode slurry was prepared by stirring. The above slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12h, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150℃, and kept warm for 2h, and the pole piece was taken out and weighed.

[0078] (3) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 119 mAh / g, the first efficiency is 52.7%, and the capacity retention rate is 55.31% after 100 cycles at 0.1C.

[0079] Comparative Example 3

[0080] (1) 3.273 g of 4,4'-diaminodiphenyl ether and 0.198 g of 2,3-diaminopyridine were dissolved in 50 ml of N-methylpyrrolidone solvent, and 5.75 g of 4,4'-biphenyl ether dianhydride was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a precursor solution of a low-temperature curing polyimide adhesive;

[0081] (2) The above precursor solution was diluted to a solution with a solid content of 5wt%, and mixed with the positive electrode active material NCM811, conductive carbon black, and the diluted precursor solution in a mass ratio of 92:5:3, and N-methylpyrrolidone solvent was added to dissolve the mixture, and the positive electrode slurry was prepared by fully stirring. The above slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12h, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150℃, and kept warm for 2h, and the pole piece was taken out and weighed.

[0082] (3) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 170.46 mAh / g, the first efficiency is 84.3%, and the capacity retention rate is 64.91% after 100 cycles at 0.1C.

[0083] Comparative Example 4

[0084] (1) 3.273 g of 4,4'-diaminodiphenyl ether was dissolved in 50 ml of N-methylpyrrolidone solvent, and 5.75 g of 4,4'-biphenyl ether dianhydride was added in batches under nitrogen atmosphere and ice water bath conditions to fully react to obtain a homogeneous polyamic acid solution;

[0085] (2) Adding 2% of the molar mass of 4,4'-biphenyl ether dianhydride as a blocking agent 5-aminobenzimidazole to the above polyamic acid solution and stirring thoroughly to obtain a blocked polyamic acid solution.

[0086] (3) adding a catalyst N-N'-carbonyldiimidazole having a molar mass of 10% of 4,4'-biphenyl ether dianhydride to the blocked polyamic acid solution obtained in step (2), and stirring the mixture thoroughly to obtain a precursor solution of a low-temperature curing polyimide adhesive;

[0087] (4) obtaining a precursor solution of a low-temperature curing polyimide adhesive; diluting the precursor solution to a solution having a solid content of 5 wt %.

[0088] The positive electrode slurry was prepared by mixing the positive electrode active material NCM811, conductive carbon black and the diluted precursor solution in a mass ratio of 92:5:3, adding N-methylpyrrolidone solvent to dissolve the mixture, and stirring it thoroughly to obtain the positive electrode slurry. The slurry was coated on aluminum foil (10cm×12cm) and placed in a clean bench to dry at room temperature for 12 hours, cut into discs with a diameter of 12mm, rolled, and the pole piece was placed in an oven for thermal imidization treatment, from room temperature to 150℃, and kept warm for 2 hours. The pole piece was taken out and weighed.

[0089] (5) According to the above-mentioned electrode preparation, battery assembly and testing methods, the 0.1C discharge specific capacity of NCM811 in this system is 175.22 mAh / g, the first efficiency is 82.22%, and the capacity retention rate is 61.33% after 100 cycles at 0.1C.

[0090] Figure 1 Actual picture of low-temperature cured polyimide film after being soaked in NMP and electrolyte for 7 days

[0092] Table 1 The residual weight of low-temperature cured polyimide after immersion in NMP and electrolyte for 7 days

[0093] Example 1 Example 2 Comparative Example 2 NMP 95.3% 94.6% 0% In electrolyte 99.2% 99.1% 69.2%

[0094] Table 2 Performance of positive electrode sheets prepared in Examples and Comparative Examples

[0095]

[0096] from Figure 1As can be seen from Table 1, the film obtained after low-temperature curing polyimide is cast and imidized at 150°C has no significant change in surface morphology and slight weight loss after 7 days of immersion in solvent or electrolyte. However, the polyimide cured at 150°C without special molecular structure design and catalyst synergy completely dissolved in the solvent after one day. This shows that the low-temperature curing polyimide in the present invention can be successfully imidized at 150 degrees Celsius.

[0097] From the data in Table 2, it can be seen that the battery using low-temperature curing polyimide adhesive in Comparative Example 1 has a higher capacity retention rate after 100 weeks than the capacity retention rate of lithium-ion batteries using PVDF adhesive in 0.1C discharge capacity, which further indicates that the low-temperature curing polyimide adhesive does play a role in maintaining the stability of the positive electrode material structure, effectively promoting the positive electrode capacity and improving the long cycle life of the battery. At the same time, compared with Comparative Example 2, the lithium-ion battery using low-temperature curing polyimide adhesive that has not undergone special molecular structure design and synergistic effect of catalyst will show huge attenuation in both 0.1C discharge capacity and capacity retention rate after 100 weeks. Compared with Comparative Examples 3 and 4, the lithium-ion batteries made of low-temperature curing polyimide adhesives without special functional group monomer copolymerization and catalyst addition affect the degree of imidization, thereby reducing the capacity retention rate after 100 weeks. Comparing Examples 2 and 3, it can be found that the 0.1C discharge specific capacity and the capacity retention rate after 100 weeks have no obvious changes, indicating that the listed monomers with special functional groups can effectively reduce the curing temperature of polyimide after copolymerization. Comparing Examples 4 and 6, it can be found that the listed catalysts can also effectively reduce the curing temperature of polyimide. Comparing Example 5, it can be found that the listed end-capping agents can also effectively reduce the curing temperature of polyimide.

Claims

1. A method for preparing a low-temperature curing polyimide binder for lithium-ion batteries and the binder and electrode sheet prepared thereby, characterized in that: The preparation method comprises the following steps: (1) Under nitrogen atmosphere and ice water bath conditions, an excess of dianhydride monomer, a diamine monomer and a third monomer containing a special functional group are subjected to condensation polymerization in a reaction solvent to obtain a copolymerized polyamic acid solution, wherein the molecular weight of the polyimide can be adjusted by the relative amount of the dianhydride monomer added; (2) adding a blocking agent to the polyamic acid solution obtained by the above copolymerization and stirring the mixture to obtain a blocked polyamic acid solution; (3) adding a catalyst to the blocked polyamic acid solution obtained in step (2) and stirring the mixture to obtain a low-temperature curing polyimide precursor solution; (4) The active material, the conductive agent and the precursor solution obtained in step (3) are uniformly mixed to obtain a slurry, which is coated on the surface of the current collector and then subjected to thermal imidization treatment to obtain an electrode plate with a low-temperature curing polyimide as a binder.

2. The preparation method according to claim 1, characterized in that: The solid content of the polyamic acid solution in step (1) is 0.5-40wt%; the molar ratio of the dianhydride monomer to the diamine monomer is 1.01:1-1.3:1; the molar ratio of the dianhydride monomer to the diamine monomer containing a special functional group is 9-25:1; the reaction time is 0.5-12h; the dianhydride monomer in step (1) is pyromellitic dianhydride (PMDA), 4,4'-biphenyl ether dianhydride (ODPA), biphenyl dianhydride (BPDA), 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride (DSDA), hexafluoro The diamine monomer in step (1) is p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), 4,4'-diaminodiphenyl ether (ODA), 3,4'-diaminodiphenyl ether (3,4'-ODA), 4,4 '-diaminodiphenyl sulfone (DDS), 3,3'-diaminodiphenyl sulfone (MSDS), 2,2'-dimethyl-4,4'-diaminobiphenyl (MTB), 4,4'-diaminodiphenylmethane (MDA), 1,3-bis(4'-aminophenoxy)benzene (TPE) are mixed in any proportion; the third monomer containing a special functional group in step (1) is 2,3-diaminopyridine, 2,4-diaminopyridine, 2,5-diaminopyridine, 3,4-diaminopyridine, 5,6-diaminobenzimidazole The solvent in step (1) is a mixture of one or more of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-ethylpyrrolidone (NEP), dimethyl sulfoxide (DMSO), and hexamethylphosphoramide (HMPA) in any proportion.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the end-capping agent to the dianhydride monomer in step (2) is 0.01:1-5:1; the reaction time is 0.5-12h; the end-capping agent in step (2) is a mixture of one or more of 5-aminobenzimidazole (ABZ), 2-aminoimidazole, 2-aminopyridine, and aminopyrazine in any proportion.

4. The preparation method according to claim 1, characterized in that: The molar ratio of the catalyst to the dianhydride monomer in step (3) is 0.01:1-5:1; the reaction time is 0.5-12h; the catalyst in step (3) is a mixture of one or more of N-N'carbonyldiimidazole (CDI), 6-aminoquinoline (AQL), ​​benzotriazole (BTA) and 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) in any proportion.

5. The preparation method according to claim 1, characterized in that: The solid content of the electrode slurry in step (4) is 20-90wt%; the non-solvent part of the electrode slurry contains 80-99wt% of active material, 0.5-10wt% of conductive agent, and 0.5-10wt% of precursor solution; the positive electrode active material in step (4) is a mixture of one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt aluminum oxide and lithium nickel cobalt manganese oxide ternary materials in any proportion; the negative electrode active material in step (4) is a mixture of one or more of carbon material, silicon and its oxide, tin and its oxide, silicon-carbon composite material, silicon-oxygen-carbon composite material and tin-carbon composite material in any proportion; the conductive agent in step (4) is a mixture of one or more of conductive carbon black, conductive graphite, graphene and carbon nanotubes in any proportion; the current collector in step (4) is carbon-containing aluminum foil or carbon-containing copper foil; the thickness of the electrode slurry coating in step (4) is 75-200μm; The thermal imidization temperature is 100-150°C and the time is 0.5-2h.

6. A low-temperature curing polyimide binder for lithium-ion batteries prepared by the method according to any one of claims 1 to 16, and an electrode sheet prepared therefrom.

Citation Information

Patent Citations

  • High-temperature-resistant adhesive for lithium ion battery and battery pole piece applying the adhesive

    CN111403745A

  • Blending type polyamide acid solution, blending type polyimide adhesive, battery pole piece and preparation method of battery pole piece

    CN114752074A

  • Polyimide-coated lithium ion battery positive electrode material, preparation method and application

    CN116914101A

Cited By

  • Preparation method of polyimide composite film and polyimide composite film

    CN121449941A

  • Polyimide resin containing epoxy group on side chain, polyimide adhesive and preparation method thereof

    CN121554737A

  • Benzimidazolone polyimide electrostatic spinning lithium battery diaphragm with high cycling stability and preparation method of benzimidazolone polyimide electrostatic spinning lithium battery diaphragm