Composite lithium supplement material and preparation method thereof, positive plate and battery
By setting a multi-layer coating structure on the surface of lithium-rich materials, including porous carbide or nitride and carbon material layers, the problems of easy collapse of the positive electrode lithium replenishment structure and insufficient conductivity are solved, thereby improving the energy density and cycle performance of the battery.
Patent Information
- Application Number
- CN202410961592.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-29
AI Technical Summary
Existing positive electrode lithium replenishment agents are prone to structural collapse and insufficient conductivity after charging, which leads to increased battery impedance and affects electrochemical performance.
The structure employs a multi-layer coating, including a first coating layer and a second coating layer on the surface of the lithium-rich material. The first coating layer is a porous carbide or nitride layer, and the second coating layer is a carbon material layer, which improves the structural strength and conductivity.
It enhances the structural stability and conductivity of the composite lithium replenishment material, thereby improving the energy density and cycle performance of the battery.
Smart Images

Figure CN119050354A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a composite lithium supplement material and a preparation method thereof, a positive electrode sheet and a battery. Background Art
[0002] During the first charge and discharge process of lithium-ion batteries, a large amount of solid electrolyte interface film (SEI) will be generated on the surface of the negative electrode of the battery, which consumes the limited lithium ions and electrolyte in the battery, causing irreversible capacity loss and reducing the cycle performance and energy density of lithium-ion batteries. In order to improve the energy density of lithium batteries, reducing the consumption of lithium ions during the first charge and discharge process of lithium batteries has become one of the important solutions. In the related art, by adding positive electrode lithium replenishers to the positive electrode material, the first irreversible capacity loss of the lithium battery can be effectively compensated, and the positive electrode lithium replenisher can be directly applied to the slurry, which can save costs and is practical and convenient. However, due to the one-time use characteristics of the current positive electrode lithium replenisher, lithium ions are irreversible, the structure is inactivated after charging, it is easy to collapse and the conductivity is insufficient, which deteriorates the impedance and power performance of the battery. Therefore, how to solve this problem has become one of the key issues of concern.
[0003] In the related art, a lot of research has been conducted to alleviate the above problems. For example, the patent with publication number CN117219761A discloses a synthesis method for improving the stability of positive electrode lithium supplement agents. A layer of lithium carbonate is coated on the outside of the lithium supplement agent to improve a certain structural strength. However, the lithium carbonate component is unstable and is easily decomposed and gasified at high temperatures, which destroys its structural stability and affects the structural strength of the positive electrode lithium supplement agent. For another example, the patent with publication number CN113471554A discloses a synthesis method for improving the stability of positive electrode lithium supplement agents. By coating a layer of carbon layer on the outside of the lithium supplement agent, the strength of the lithium supplement agent is improved to a certain extent. However, due to the low structural strength of the carbon coating, the degree of improvement in the structural strength of the positive electrode lithium supplement agent is not large. Ultimately, after the lithium supplement is completed, the positive electrode material is easily broken, resulting in an increase in the battery impedance and deterioration of the electrochemical performance. Therefore, how to effectively improve the structural strength of the positive electrode lithium supplement agent is crucial for the application of the lithium supplement agent. Summary of the invention
[0004] In view of this, the present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention provides a composite lithium supplement material and a preparation method thereof, a positive electrode sheet and a battery, which can improve the structural strength of the lithium supplement material, have a certain conductivity, can optimize the conductivity of the material, and is conducive to improving the energy density and cycle performance of the battery.
[0005] In order to solve the above technical problems, this application is implemented as follows:
[0006] According to one aspect of the present application, an embodiment of the present application provides a composite lithium supplement material, the composite lithium supplement material comprising:
[0007] Lithium-rich materials;
[0008] A first coating layer, coating at least a portion of the surface of the lithium-rich material, wherein the first coating layer comprises a carbide or nitride layer having a porous structure; and
[0009] The second coating layer is coated on at least a portion of the surface of the first coating layer, and the second coating layer includes a carbon material layer.
[0010] In addition, the composite lithium supplement material according to the present application may also have the following additional technical features:
[0011] In some embodiments, the lithium-rich material includes at least one of lithium-rich nickel oxide, lithium-rich lithium iron oxide, lithium-rich lithium cobalt oxide, lithium oxide, lithium fluoride, lithium nitride or lithium sulfide.
[0012] In some embodiments, the average particle size of the lithium-rich material is 0.5 μm to 5 μm.
[0013] In some embodiments, the thickness of the first coating layer is 0.1 μm to 1 μm.
[0014] In some embodiments, the pore size of the porous structure ranges from 100 nm to 500 nm.
[0015] In some embodiments, the carbide includes at least one of titanium carbide, tungsten carbide, or zirconium carbide.
[0016] In some of the embodiments, the nitride includes titanium nitride.
[0017] In some embodiments, the second coating layer has a thickness of 0.1 μm to 0.5 μm.
[0018] In some embodiments, the second coating layer includes at least one of an activated carbon layer, a graphene layer, a porous carbon layer or an amorphous carbon layer.
[0019] According to another aspect of the present application, an embodiment of the present application provides a method for preparing a composite lithium supplement material, which comprises the following steps:
[0020] The pore-forming agent solution is attached to the lithium-rich material by spray drying to obtain an intermediate;
[0021] The intermediate and the first coating layer precursor are ball-milled and dried, and a reactive gas is introduced under a protective atmosphere to perform a first heat treatment to obtain a lithium-rich material coated with a first coating layer, wherein the first coating layer includes a carbide or nitride layer with a porous structure;
[0022] The lithium-rich material coated by the first coating layer is mixed with a second coating layer precursor, and subjected to a second heat treatment, and the second coating layer is coated on the surface of the first coating layer, wherein the second coating layer includes a carbon material layer, to obtain the composite lithium supplement material.
[0023] In some embodiments, the step of obtaining the intermediate satisfies at least one of the following characteristics (1) to (3): (1) the pore-forming agent solution is composed of a pore-forming agent and a solvent, the pore-forming agent includes at least one of ammonium carbonate, ammonium bicarbonate or ammonium chloride, and / or the solvent includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, polyethylene oxide or ethylene oxide; optionally, the mass ratio of the pore-forming agent to the lithium-rich material is (0.1 to 1): (99 to 99.9); (2) the average particle size of the intermediate is 0.5 μm to 3 μm; (3) the lithium-rich material includes at least one of lithium nickel-rich lithium oxide, lithium iron-rich lithium oxide, lithium cobalt-rich lithium oxide, lithium oxide, lithium fluoride, lithium nitride or lithium sulfide.
[0024] In some embodiments, the step of obtaining the lithium-rich material coated by the first coating layer satisfies at least one of the following characteristics (1) to (6): (1) the first coating layer precursor includes at least one of a titanium tetrachloride solution, a tungsten tetrachloride solution or a zirconium chloride solution; optionally, the concentration of the first coating layer precursor is 0.01 to 0.5 mol / L; (2) the rotation speed of the ball mill is 800 to 2000 r / min, and the ball milling time is 2 to 10 h; (3) the drying is vacuum drying, and the temperature of the vacuum drying is The temperature is 60℃~120℃, and the vacuum drying time is 2h~24h; (4) the mass ratio of the first coating layer precursor to the intermediate is (0.1~1):(99~99.9); (5) the reactive gas is suitable for reacting with the first coating layer precursor, and the reactive gas includes at least one of alkane gas or ammonia; optionally, the alkane gas includes at least one of methane, ethane, propane or butane; (6) the temperature of the first heat treatment is 800℃~1400℃, and the time is 2h~6h.
[0025] In some embodiments, the step of obtaining the composite lithium-supplementing material satisfies at least one of the following characteristics (1) to (5): (1) the second coating layer precursor includes at least one of an organic carbon source selected from the group consisting of glucose solution, sucrose solution, soluble starch solution, cellulose solution and polyvinyl alcohol solution; optionally, the concentration of the second coating layer precursor is 10 to 50 g / L; (2) the mass ratio of the lithium-rich material to the carbon material layer is (92 to 98): (2 to 5); (3) the lithium-rich material coated by the first coating layer and the second coating layer precursor are immersed and mixed for 2 h to 6 h; (4) during the second heat treatment, an alkane gas is introduced under a protective atmosphere; optionally, the alkane gas includes at least one of methane, ethane, propane and butane; (5) the temperature of the second heat treatment is 600°C to 1000°C, and the time is 2 h to 4 h.
[0026] According to another aspect of the present application, an embodiment of the present application provides a positive electrode sheet, which includes a current collector and a positive electrode active material layer arranged on the surface of the current collector; the positive electrode active material layer includes the aforementioned composite lithium supplement material or the composite lithium supplement material prepared by the aforementioned method, as well as a positive electrode active material, a conductive agent and a binder.
[0027] In some of the embodiments, in the positive electrode active material layer, the mass ratio of the positive electrode active material, the composite lithium supplement material, the conductive agent and the binder is (85-95): (1-10): (0.1-5): (1-5).
[0028] According to another aspect of the present application, an embodiment of the present application provides a battery, which includes the aforementioned positive electrode sheet and negative electrode sheet.
[0029] Implementing the technical solution of the present invention has at least the following beneficial effects:
[0030] In an embodiment of the present application, the provided composite lithium-replenishing material has a first coating layer arranged on the surface of the lithium-rich material, and a second coating layer arranged on the surface of the first coating layer, that is, a multi-layer coating structure is adopted. The first coating layer includes a carbide or nitride layer with a porous structure. The structural strength of the composite lithium-replenishing material can be improved by setting the carbide or nitride layer with a porous structure, and the carbide or nitride has a certain conductivity, which can optimize the conductivity of the composite lithium-replenishing material, and the porous structure of the first coating layer is conducive to the deintercalation of lithium ions in the composite lithium-replenishing material. The second coating layer includes a carbon material layer. The contact between the composite lithium-replenishing material and the positive electrode active material can be reduced by setting the carbon material layer, improving the contact impedance, and the carbon material layer has good conductivity, which can further improve the conductivity of the composite lithium-replenishing material.
[0031] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Shown is a schematic structural diagram of a composite lithium supplement material provided in an embodiment of the present invention.
[0033] Description of reference numerals:
[0034] 10-lithium-rich materials;
[0035] 20-a first coating layer;
[0036] 201-porous structure;
[0037] 30-Second coating layer. DETAILED DESCRIPTION
[0038] The present application is further described below in conjunction with specific embodiments. It should be understood that these embodiments of the present application are only used to illustrate the present application and are not used to limit the scope of the present application.
[0039] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0040] Hereinafter, the embodiments of the composite lithium supplement material, the method for preparing the composite lithium supplement material, the battery, etc. of the present application will be specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0041] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0042] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0043] As analyzed in the background technology of this application, by adding a certain amount of lithium-rich material as a positive electrode lithium supplement to the traditional positive electrode material, it is beneficial to improve the energy density and cycle performance of the lithium battery. However, the existing lithium-rich materials and other positive electrode lithium supplements still have certain shortcomings, such as the structure is easy to collapse after charging is completed, that is, the structural strength is low, resulting in poor structural stability, and poor conductivity. Therefore, it is necessary to fully consider the characteristics of the existing lithium-rich materials, and improve the structural strength of the materials or the conductivity of the materials by modification to alleviate the above problems. In view of this, the present application provides a composite lithium supplement material and its preparation method, a positive electrode sheet and a battery, and the present application is described in detail below.
[0044] [Composite lithium supplement materials]
[0045] See also Figure 1 As shown, in some embodiments, the present application provides a composite lithium supplement material, the composite lithium supplement material comprising:
[0046] Lithium-rich materials 10;
[0047] A first coating layer 20 is coated on at least a portion of the surface of the lithium-rich material 10, and the first coating layer 20 includes a carbide or nitride layer having a porous structure 201; and,
[0048] The second coating layer 30 is coated on at least a portion of the surface of the first coating layer 20 , and the second coating layer 30 includes a carbon material layer.
[0049] It should be pointed out that in the present application, the "coating" is not limited to direct coating, but also includes indirect coating. For example, the first coating layer 20 coats the lithium-rich material 10, and there may be no other structure between the first coating layer 20 and the outer surface of the lithium-rich material 10, or there may be one or more layers of other structures between the first coating layer 20 and the outer surface of the lithium-rich material 10. Preferably, there is no other structure between the first coating layer 20 and the outer surface of the lithium-rich material 10. Similarly, the second coating layer 30 coats the first coating layer 20, and there may be no other structure between the second coating layer 30 and the outer surface of the first coating layer 20, or there may be one or more layers of other structures between the second coating layer 30 and the outer surface of the first coating layer 20.
[0050] The first coating layer 20 is formed or coated on at least part of the surface of the lithium-rich material 10, which can protect and improve the lithium-rich material 10, can be used to improve the structural stability of the composite lithium-supplementing material, and can also optimize the conductivity of the composite lithium-supplementing material. The first coating layer 20 is formed on at least part of the surface of the lithium-rich material 10, which means that the first coating layer 20 can completely encapsulate the lithium-rich material 10 in the first coating layer 20, or the first coating layer 20 can only coat a part of the outer surface of the lithium-rich material 10; that is, the first coating layer 20 can completely coat the lithium-rich material 10, or can coat part of the surface of the lithium-rich material 10, preferably completely coating.
[0051] The second coating layer 30 is formed or coated on at least part of the surface of the first coating layer 20, which can protect the lithium-rich material 10 and the first coating layer 20, and can be used to improve the contact impedance with the positive electrode active material, and can also be used to improve the conductivity of the composite lithium-supplementing material and enhance the electrochemical performance of the composite lithium-supplementing material. The second coating layer 30 is formed on at least part of the surface of the first coating layer 20, which means that the second coating layer 30 can completely encapsulate the first coating layer 20 in the second coating layer 30, or the second coating layer 30 can only coat a part of the outer surface of the first coating layer 20; that is, the second coating layer 30 can completely coat the first coating layer 20, or can coat part of the surface of the first coating layer 20, preferably completely.
[0052] The composite lithium supplement material provided is a core-shell structure, in which the core adopts the traditional lithium-rich material 10, and the shell or shell layer includes a first coating layer 20 and a second coating layer 30, wherein the first coating layer 20 can be a coating with rigidity, and the second coating layer 30 can be a carbon layer (carbon material layer) with toughness or flexibility. In this embodiment, the first coating layer 20 includes a carbide or nitride layer with a porous structure 201, that is, the first coating layer 20 can be a carbide layer, and the carbide layer has a porous structure 201, or the first coating layer 20 can be a nitride layer, and the nitride layer has a porous structure 201, which can play an excellent protective or improvement role on the core material of the lithium-rich material 10, especially can be used to improve the structural strength of the composite lithium supplement material, or for optimizing the conductivity of the composite lithium supplement material. The second coating layer 30 includes a carbon material layer, which can protect the lithium-rich material 10 and the first coating layer 20, especially can be used to improve the contact impedance between the material and the positive electrode active material, and can also be used to improve the conductivity of the composite lithium supplement material.
[0053] Therefore, by sequentially setting the first coating layer 20 and the second coating layer 30 on the surface of the lithium-rich material 10, that is, adopting a multi-layer coating structure, it is possible to effectively play an excellent protective or modifying role on the lithium-rich material 10, improve the structural stability of the composite lithium-supplementing material, improve the conductivity of the composite lithium-supplementing material, and effectively improve the electrochemical performance. Among them, the lithium-rich material 10 is a core material that can provide a supplementary source of lithium ions; the first coating layer 20 is a rigid coating, and a carbide or nitride layer with a porous structure 201 is used. The structural strength of the composite lithium-supplementing material can be improved by setting the carbide or nitride layer, and the collapse or breakage of the composite lithium-supplementing material can be reduced or avoided. The carbide or nitride has a certain conductivity, which can optimize the conductivity of the composite lithium-supplementing material, and the porous structure 201 of the first coating layer 20 is conducive to the deintercalation of lithium ions in the composite lithium-supplementing material. The second coating layer 30 is a tough or flexible carbon layer. The carbon material layer can reduce the contact between the composite lithium supplement material and the positive electrode active material and improve the contact impedance. The carbon material layer has good conductivity and can further improve the conductivity of the composite lithium supplement material.
[0054] The inventors have found through in-depth research that when the composite lithium supplement material of the present application satisfies the above-mentioned design conditions and optionally satisfies one or more of the following conditions, the performance of the composite lithium supplement material can be further improved.
[0055] In an embodiment of the present invention, the composite lithium replenishing material is a positive electrode lithium replenishing material with high stability, which can be composed of a lithium-rich material 10, a first coating layer 20 arranged on the surface of the lithium-rich material 10, that is, a rigid coating, and a second coating layer 30 arranged on the surface of the first coating layer 20, that is, a flexible carbon layer.
[0056] In some embodiments, the lithium-rich material 10 includes, but is not limited to, at least one of lithium-rich nickel oxide (Li2NiO2), lithium-rich lithium iron oxide (Li5FeO4), lithium-rich lithium cobalt oxide (LiCoO2), lithium oxide (Li2O), lithium fluoride, lithium nitride or lithium sulfide.
[0057] Preferably, the lithium-rich material 10 is selected from one or more combinations of lithium-rich nickel oxide (Li2NiO2), lithium-rich lithium iron oxide (Li5FeO4) or lithium oxide (Li2O).
[0058] The selected lithium-rich material 10 has a high theoretical charge capacity (e.g., the theoretical capacity of some of the lithium-rich materials can be above 400 mAh / g), and the composite lithium-supplementing material containing the material can actually provide a high lithium-supplementing capacity, which helps to better improve the capacity of the battery. In addition, the selected lithium-rich materials can play a good role in lithium-supplementing, which is beneficial to improving the cycle performance, energy density, etc. of the battery.
[0059] In some embodiments, the average particle size of the lithium-rich material 10 (granular) is 0.5 μm to 5 μm. Preferably, in some embodiments, the average particle size of the lithium-rich material 10 (granular) is 0.5 μm to 2 μm. As an example, the average particle size of the lithium-rich material 10 can be any point value of 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm or any range value between two of them.
[0060] By making the particle size of the lithium-rich material 10 within the above-mentioned suitable range, the processing performance of the material can be improved, which is convenient for processing, and the comprehensive electrical performance of the composite lithium-supplementing material can also be improved.
[0061] In the present application, the carbide or nitride with a porous structure 201 is coated on the surface of the lithium-rich material 10 to form a first coating layer 20 of a certain thickness; when the carbide or nitride with a porous structure 201 is in a coating relationship with the lithium-rich material 10, the modification effect of the carbide or nitride with a porous structure 201 can be exerted to a greater extent, thereby improving the structural strength of the material.
[0062] In some embodiments, the thickness of the first coating layer 20 is 0.1 μm to 1 μm. Preferably, in some embodiments, the thickness of the first coating layer 20 is 0.2 μm to 0.8 μm. As an example, the thickness of the first coating layer 20 can be any one of 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, or a range between any two of them.
[0063] The thickness of the first coating layer 20 can be adjusted according to the size of the core of the lithium-rich material 10. The appropriate thickness of the first coating layer 20 can not only ensure that the composite lithium supplement material has good processing performance, but also avoid excessive thickness and excessive first coating material affecting the timely release of active lithium, increasing battery impedance or affecting the cycle performance of the battery cell, or avoid excessive thickness that is insufficient to effectively exert the modification effect of the first coating layer 20, that is, avoid excessively thin thickness that reduces the effect of the first coating layer 20 in improving the structural strength of the material.
[0064] In some embodiments, the pore size of the porous structure 201 ranges from 100 nm to 500 nm. As an example, the pore size of the porous structure 201 can be any point value of 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or a range value between any two of them. By controlling the pore size of the porous structure 201 within the above-mentioned appropriate range, it helps to improve the structural strength of the material; if the pore size of the porous structure 201 is too large, such as exceeding 500 nm, it will affect the stability of the first coating layer 20, and thus affect the structural strength of the material; if the pore size of the porous structure 201 is too small, such as less than 100 nm, it is not conducive to the deintercalation of lithium ions in the main material of the lithium supplement.
[0065] In the present application, the first coating layer 20 is provided with a porous structure 201, and the porous structure 201 may not be the porous structure 201 of the nitride or carbide itself. The porous structure 201 may be a pore-forming agent added when preparing the first coating layer 20, and a large number of pores are formed by thermal decomposition of the pore-forming agent itself at high temperature, that is, a porous structure 201 is formed; the gas production stage is in the material synthesis stage, and basically does not affect the subsequent use of the battery. For example, in the preparation process, by first directly coating a layer of pore-forming agent such as sodium bicarbonate material on the surface of the lithium-rich material 10, and then in the heating process of preparing the first coating layer 20, the modified porous structure 201 can be prepared by thermal decomposition of the pore-forming agent such as sodium bicarbonate material at high temperature, that is, a rigid coating with a porous structure 201 is prepared.
[0066] Therefore, the present application provides the first coating layer 20 , ie, the rigid coating layer, with a porous structure 201 , which is beneficial to the deintercalation of lithium ions in the main material of the lithium supplement agent.
[0067] It should be pointed out that the present application does not limit the specific shape of the porous structure 201 , which may be a conventional shape such as a circle, or an ellipse or other regular or irregular shapes, without limitation thereto.
[0068] In some embodiments, the carbide includes, but is not limited to, at least one of titanium carbide, tungsten carbide, or zirconium carbide.
[0069] In some embodiments, the nitride includes, but is not limited to, titanium nitride.
[0070] In the present application, the carbide or nitride in the first coating layer 20 can be a rigid conductive material, such as titanium carbide, tungsten carbide, zirconium carbide, titanium nitride and the like. These materials not only have a certain rigidity, but also have a certain conductivity, which is not only beneficial to improving the structural strength of the composite lithium supplement material, but also can optimize the conductivity of the composite lithium supplement material.
[0071] It should be noted that carbides and nitrides are not limited to the substances listed above. Other rigid conductive materials that can be used to improve the structural strength of the material and optimize the conductivity of the material do not limit the purpose of the present invention. Other similar carbides and nitrides can also be used in the present invention.
[0072] In some embodiments, the thickness of the second coating layer 30 is 0.1 μm to 0.5 μm. As an example, the thickness of the second coating layer 30 can be any one of 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, and 0.5 μm, or a range of any two thereof.
[0073] The thickness of the second coating layer 30 can be adjusted according to the size of the core of the lithium-rich material 10. The appropriate thickness of the second coating layer 30 can not only ensure that the composite lithium supplement material has good processing performance, but also avoid the thickness being too thick and the second coating material being too much, which may affect the timely release of active lithium, increase battery impedance or affect the cycle performance of the battery cell, or avoid the thickness being too thin to effectively exert the modification effect of the second coating layer 30.
[0074] In some embodiments, the second coating layer 30 includes, but is not limited to, at least one of an activated carbon layer, a graphene layer, a porous carbon layer, or an amorphous carbon layer. The second coating layer 30 may be a carbon material layer, and the carbon material may be selected from a combination of one or more of activated carbon, graphene, porous carbon, amorphous carbon, etc.
[0075] It should be noted that the specific types of carbon materials are not limited to the substances listed above. Other carbon materials with certain toughness and capable of being used to optimize the conductivity of the material do not limit the purpose of the present invention. Other similar carbon materials can also be used in the present invention.
[0076] The above-mentioned composite lithium supplement material provided in the embodiment of the present application has high structural strength, good structural stability, good conductivity, and high lithium supplement capacity, which is beneficial to improving the cycle performance, conductivity and energy density of the battery.
[0077] [Preparation method of composite lithium supplement material]
[0078] According to another aspect of the present application, an embodiment of the present application provides a method for preparing a composite lithium supplement material, which comprises the following steps:
[0079] The pore-forming agent solution is attached to the lithium-rich material 10 by spray drying to obtain an intermediate;
[0080] The intermediate and the first coating layer precursor are ball-milled and dried, and a reactive gas is introduced under a protective atmosphere to perform a first heat treatment to obtain a lithium-rich material 10 coated with a first coating layer 20, wherein the first coating layer 20 includes a carbide or nitride layer having a porous structure 201;
[0081] The lithium-rich material 10 coated by the first coating layer 20 is mixed with the precursor of the second coating layer 30 and subjected to a second heat treatment to coat the surface of the first coating layer 20 with the second coating layer 30 , wherein the second coating layer 30 includes a carbon material layer, to obtain a composite lithium supplement material.
[0082] The preparation method of the composite lithium-replenishing material provided by the present invention can first attach or coat the pore-forming agent on the surface of the lithium-rich material 10, and then mix the lithium-rich material 10 with the pore-forming agent attached to the surface with the first coating layer precursor. After ball milling and drying, a first coating layer precursor including the pore-forming agent and the first coating layer precursor (such as a carbide or nitride precursor) can be formed on the surface of the lithium-rich material 10. After heating treatment, the pore-forming agent in the first coating layer precursor can be thermally decomposed to form a first coating layer 20 with a porous structure 201. That is, in the preparation process of the composite lithium-replenishing material of the present application, the porous structure 201 is formed by thermal decomposition of the pore-forming agent itself at high temperature. The porous structure 201 is not obtained by the reaction of the first coating layer precursor with the pore-forming agent, nor is it a porous structure 201 of a nitride or carbide, and the final composite lithium-replenishing material cannot contain a pore-forming agent component; and the gas production stage is in the synthesis stage of the composite lithium-replenishing material, which will not affect the subsequent use in the battery. Furthermore, a composite lithium-replenishing material with a core-shell structure can be obtained by forming a second coating layer 30 on the surface of the first coating layer 20 , that is, a composite lithium-replenishing material with a multi-layer coating structure can be obtained.
[0083] The preparation method provided by the embodiment of the present invention has simple process, convenient operation, strong feasibility, and is easy to realize industrialization; by this method, a composite lithium supplement material with a multi-layer coated structure can be prepared, which has high structural strength, good structural stability, good conductivity, and high lithium supplement capacity, which is conducive to the use of lithium supplement agents.
[0084] It should be understood that all the features and advantages described above for the “composite lithium supplement material” are also applicable to the “method for preparing the composite lithium supplement material” and will not be described in detail here.
[0085] In some specific embodiments, the method for preparing the composite lithium supplement material specifically comprises the following steps (a) to (c):
[0086] (a) Preparation of intermediates.
[0087] In step (a), preparing the intermediate includes: attaching the pore-forming agent solution to the lithium-rich material 10 by spray drying to obtain the intermediate.
[0088] In the present application, the pore-forming agent solution can be completely coated on the surface of the lithium-rich material 10 by spray drying, and the spray drying method is simple to operate and easy to control. The specific operating conditions of spray drying can be selected and adjusted according to actual conditions, and there is no limitation on this.
[0089] Optionally, the pore-forming agent solution is composed of a pore-forming agent and a solvent. For example, the pore-forming agent solution can be obtained by dispersing the pore-forming agent in a solvent and uniformly mixing the solvents.
[0090] Exemplarily, step (a) specifically includes: uniformly dispersing the pore former in the solvent, uniformly mixing to obtain a pore former solution, spraying the pore former solution onto the lithium-rich material 10 by spray drying to obtain an intermediate. Optionally, before mixing, the pore former can be ball-milled to obtain pore former particles of a suitable particle size, and then dispersed in the solvent. Optionally, before spray drying, the lithium-rich material 10 can be ball-milled to obtain lithium-rich material 10 particles of a preset particle size.
[0091] In some embodiments, the pore-forming agent may be an ammonium bicarbonate-based substance, for example, the pore-forming agent includes, but is not limited to, at least one of ammonium carbonate, ammonium bicarbonate or ammonium chloride.
[0092] In the present application, a substance that can completely decompose into gas by thermal decomposition is used as a pore-forming agent to prepare the first coating layer 20, i.e., the rigid coating. For example, ammonium carbonate, ammonium bicarbonate, ammonium chloride and other ammonium bicarbonate-type substances are used as pore-forming agents. These substances can completely decompose into gas by thermal decomposition at high temperatures, and do not need to undergo subsequent impurity removal and other treatments, which simplifies the process and does not introduce some unnecessary substances into the product, thereby ensuring the performance of the product.
[0093] It should be noted that the pore-forming agent is not limited to the substances listed above, and can be used to provide the porous structure 201 and completely thermally decompose into gas at high temperature, which does not limit the purpose of the present invention. Other similar pore-forming agents can also be used in the present invention.
[0094] In some embodiments, the solvent includes, but is not limited to, at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, polyethylene oxide (PEO), or ethylene oxide (EO).
[0095] In the present application, the solvent in the pore-forming agent solution may be a binder, preferably a binder commonly used in the positive electrode of a battery, for example, PVDF, PEO, EO, PTFE and other binders may be used as the solvent.
[0096] It should be noted that the solvent is not limited to the substances listed above, and can be used to dissolve or disperse the above-mentioned pore-forming agent, which does not limit the purpose of the present invention. Other similar organic solvents such as binders can also be used in the present invention.
[0097] In some embodiments, the mass ratio of the pore former to the lithium-rich material 10 is (0.1-1):(99-99.9). As an example, the mass ratio of the pore former to the lithium-rich material 10 is 0.1:99.9, 0.2:99.8, 0.3:99.7, 0.4:99.6, 0.5:99.5, 0.6:99.4, 0.7:99.3, 0.8:99.2, 0.9:99.1, 1:99, etc.
[0098] By controlling the mass ratio of the pore-forming agent to the lithium-rich material 10 within the above range, the strength of the first coating layer 20 can be ensured, which is beneficial to the deintercalation of lithium ions in the main material of the lithium supplement agent. The amount of the pore-forming agent added should not be too much. If the content of the pore-forming agent is too much, there will be too many holes in the first coating layer 20, which will deteriorate the connectivity of the first coating layer 20 and affect the structural strength of the first coating layer 20.
[0099] In some embodiments, the average particle size of the intermediate is 0.5 μm to 3 μm. In step (a) of the present application, the obtained intermediate can be ball-milled into particles of a preset particle size, such as particles with a particle size of about 0.5 μm to 3 μm. Preferably, in some embodiments, the average particle size of the intermediate is 0.5 μm to 2 μm. As an example, the average particle size of the intermediate can be any one of 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, or a range value between any two of them.
[0100] By making the particle size of the intermediate within the above-mentioned suitable range, the processing performance of the material can be improved, which is convenient for processing, and the comprehensive electrical properties of the obtained composite lithium supplement material can also be better.
[0101] In some embodiments, the lithium-rich material 10 includes, but is not limited to, at least one of lithium-rich nickel oxide, lithium-rich iron oxide, lithium-rich cobalt oxide, lithium oxide, lithium fluoride, lithium nitride, or lithium sulfide. Optionally, the average particle size of the lithium-rich material 10 (granular) is 0.5 μm to 5 μm, preferably 0.5 μm to 2 μm.
[0102] (b) Preparing a first coating layer.
[0103] In step (b), preparing the first coating layer 20 includes: ball milling and drying the intermediate obtained in step (a) and the first coating layer precursor, introducing a reactive gas under a protective atmosphere, and performing a first heat treatment to obtain a lithium-rich material 10 coated by the first coating layer. The first coating layer 20 includes a carbide or nitride layer having a porous structure 201.
[0104] In the present application, the prepared intermediate, that is, the lithium-rich material 10 with a pore-forming agent attached to the surface, is mixed with the first coating layer precursor. After ball milling and drying, a first coating layer precursor including a pore-forming agent and a first coating layer precursor (such as a carbide or nitride precursor) can be formed on the surface of the lithium-rich material 10. The first coating layer precursor contains a pore-forming agent and a carbide or nitride precursor. Further, under a protective atmosphere, a reactive gas is introduced, and the first coating layer precursor is heat-treated to obtain a first coating layer 20. During the heating treatment process, a pore-forming agent such as ammonium bicarbonate can be first used at a relatively low temperature to obtain a large number of pores by thermal decomposition. Subsequently, at a higher temperature, the first coating layer precursor adsorbed on the surface and inside of the pore, that is, the carbide or nitride precursor, reacts with the reactive gas to obtain a carbide or nitride, and then a carbide or nitride layer having a porous structure 201 is obtained.
[0105] As an example, when the pore-forming agent is ammonium bicarbonate (NH4HCO3), the equation for its decomposition upon heating is as follows:
[0106] NH4HCO3→NH3+H2O+CO2;
[0107] It can be seen that the ammonium bicarbonate-based substances are used as pore-forming agents, and the decomposition products obtained by heating and decomposing at high temperatures can all be gases, so that the first coating layer 20 can form a porous structure 201.
[0108] In some embodiments, in step (b), the first coating layer precursor includes, but is not limited to, at least one of a titanium tetrachloride solution, a tungsten tetrachloride solution, or a zirconium chloride solution.
[0109] In the present application, the first coating layer precursor may be a titanium tetrachloride solution, a tungsten tetrachloride solution, a zirconium chloride solution, etc. Thus, at high temperature, titanium tetrachloride may react with a reactive gas such as an alkane gas to generate titanium carbide, tungsten tetrachloride may react with a reactive gas such as an alkane gas to generate tungsten carbide, zirconium chloride may react with an alkane gas to generate zirconium carbide, and titanium tetrachloride may also react with a reactive gas such as ammonia (NH3) to generate titanium nitride.
[0110] Optionally, the concentration of the first coating layer precursor is 0.01-0.5 mol / L; for example, the concentration of the titanium tetrachloride solution, the tungsten tetrachloride solution or the zirconium chloride solution can be 0.01-0.5 mol / L. As an example, the concentration of the first coating layer precursor can be any one of 0.01 mol / L, 0.02 mol / L, 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L or a range between any two of them.
[0111] In some embodiments, in step (b), the mass ratio of the first coating layer precursor to the intermediate is (0.1-1): (99-99.9). It should be noted that the mass ratio of the first coating layer precursor to the intermediate here mainly refers to the mass ratio of the solute in the first coating layer precursor, such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride, to the intermediate. By limiting the ratio range of the first coating layer precursor to the intermediate, it is beneficial to obtain a first coating layer of suitable thickness, which is beneficial to improve the structural strength of the composite lithium supplement material and reduce costs. As an example, the mass ratio of the first coating layer precursor to the intermediate can be 0.1:99.9, 0.2:99.8, 0.3:99.7, 0.4:99.6, 0.5:99.5, 0.6:99.4, 0.7:99.3, 0.8:99.2, 0.9:99.1, 1:99, etc.
[0112] In some embodiments, in step (b), the ball milling of the intermediate and the first coating layer precursor can be performed by agate ball high-speed ball milling, and optionally, the ball milling speed is 800-2000 r / min, and the ball milling time is 2-10 hours. As an example, the ball milling speed can be 800 r / min, 1000 r / min, 1200 r / min, 1500 r / min, 1800 r / min, 2000 r / min, etc., and the ball milling time can be 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, etc.
[0113] Optionally, during ball milling, the mass ratio of each material can be 1:3:(4-6) of the raw material (intermediate and first coating layer precursor), dispersant and ball. The mass ratio of the raw material, dispersant and ball can be adjusted according to actual conditions, and this embodiment does not limit this.
[0114] In some embodiments, in step (b), the drying after ball milling can be vacuum drying, the vacuum drying temperature is 60°C to 120°C, and the vacuum drying time is 2h to 24h. As an example, the drying temperature can be any point value of 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, or a range value between any two thereof; the drying time can be any point value of 2h, 4h, 6h, 8h, 10h, 12h, 16h, 18h, 20h, 24h, or a range value between any two thereof.
[0115] In some embodiments, in step (b), the protective atmosphere gas may be nitrogen (N2), or may be a rare gas such as helium or argon; preferably, the protective atmosphere gas is nitrogen.
[0116] In some embodiments, in step (b), the reactive gas is suitable for reacting with the first coating layer precursor such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride, for example, the reactive gas includes at least one of alkane gas or ammonia gas.
[0117] In the present application, a reactive gas that can react with titanium tetrachloride, tungsten tetrachloride or zirconium chloride at high temperature is selected, such as alkane gas, ammonia gas and the like. At high temperature, a rigid conductive material such as titanium carbide, titanium nitride, tungsten carbide, zirconium carbide and the like can be generated by reacting alkane gas, ammonia gas and the like with a precursor such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride to obtain a carbide or nitride layer.
[0118] Optionally, the alkane gas includes, but is not limited to, at least one of methane, ethane, propane or butane.
[0119] It should be noted that the alkane gas is not limited to the substances listed above, and can be used to react with precursors such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride, which does not limit the purpose of the present invention. Other similar alkane gases can also be used in the present invention.
[0120] In some embodiments, in step (b), the temperature of the first heating treatment is 800°C to 1400°C, and the time is 2h to 6h. As an example, the first heating temperature can be any one of 50°C, 52°C, 54°C, 55°C, 58°C, and 60°C, or a range between any two thereof; the time can be any one of 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, and 6h, or a range between any two thereof.
[0121] In the above-mentioned first heating treatment temperature range, precursors such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride can react with reactive gases such as alkane gases and ammonia to generate rigid conductive materials such as titanium carbide, titanium nitride, tungsten carbide, and zirconium carbide. In addition, during the first heating treatment process, the temperature can be first raised to a relatively low temperature, which is the temperature at which the pore-forming agent decomposes under heat. The pore-forming agent such as ammonium bicarbonate can be heated and decomposed into gas. The temperature can be determined according to the decomposition temperature of the pore-forming agent and is not limited to this; then, the temperature is raised to the above-mentioned first heating treatment temperature to allow the precursors such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride to react with the reactive gas.
[0122] Exemplarily, the above step (b) specifically includes: ball milling and drying the intermediate obtained in step (a) and the first coating layer precursor, wherein the first coating layer precursor can be a titanium tetrachloride solution, a tungsten tetrachloride solution or a zirconium chloride solution, the concentration of the first coating layer precursor is 0.01-0.5 mol / L, the mass ratio of the first coating layer precursor to the intermediate is (0.1-1): (99-99.9), the ball milling speed can be 800-2000 r / min, the ball milling time is 2-10 h, the drying can be vacuum drying, the vacuum drying temperature is 60°C-120°C, and the vacuum drying time is 2h-24h; then, under a protective atmosphere such as nitrogen, a reactive gas, such as at least one of an alkane gas or ammonia gas, is introduced to perform a first heat treatment, that is, react at 800°C-1400°C for 2h-6h. A lithium-rich material 10 coated by the first coating layer 20 can be obtained. The first coating layer 20 includes a carbide or nitride layer having a porous structure 201 .
[0123] (c) Preparing a second coating layer.
[0124] In step (c), preparing the second coating layer 30 includes: mixing the material obtained in step (b) with the second coating layer precursor, performing a second heat treatment, coating the surface of the first coating layer 20 with the second coating layer 30, the second coating layer 30 including a carbon material layer, to obtain a composite lithium supplement material.
[0125] In the present application, by forming the second coating layer 30 on the surface of the first coating layer 20 , a composite lithium supplement material having a multi-layer coating structure can be obtained.
[0126] Specifically, step (c) may include: grinding the material obtained in step (b) and evenly immersing it in a second coating layer precursor, taking out the material after immersion for a certain period of time, and then introducing an alkane gas into a protective gas in a tubular furnace, and reacting at a second heating temperature for a certain period of time, so that a carbon coating layer, i.e., the second coating layer 30, can be deposited on the surface of the first coating layer 20.
[0127] In some embodiments, in step (c), the second coating layer precursor includes at least one of an organic carbon source glucose solution, a sucrose solution, a soluble starch solution, a cellulose solution or a polyvinyl alcohol solution. As an example, the second coating layer precursor can be obtained by uniformly dissolving at least one of an organic carbon source glucose, sucrose, a soluble starch, a cellulose, a polyvinyl alcohol, etc. into a solvent water.
[0128] Optionally, the concentration of the second coating layer precursor is 10-50 g / L; that is, the concentration of the organic carbon source glucose solution, sucrose solution, soluble starch solution, cellulose solution or polyvinyl alcohol solution is 10-50 g / L. As an example, the concentration can be any one of 10 g / h, 20 g / h, 30 g / h, 40 g / h, 50 g / h or a range between any two of them.
[0129] In some embodiments, in step (c), the mass ratio of the lithium-rich material 10 to the carbon material layer is (92-98):(2-5). As an example, the mass ratio of the lithium-rich material 10 to the carbon material layer is 92:2, 92:3, 92:4, 92:5, 94:5, 95:2, 95:5, 98:2, etc.
[0130] In some embodiments, in step (c), the lithium-rich material 10 coated by the first coating layer 20, i.e., the material obtained in step (b), is immersed and mixed with the second coating layer precursor for 2 to 6 hours. As an example, the time can be any one of 2 hours, 3 hours, 4 hours, 5 hours, and 6 hours, or a range between any two of them.
[0131] In some embodiments, in step (c), an alkane gas is introduced into a protective gas in a tubular furnace, and the reaction is treated at a second heating temperature for a certain period of time, wherein the protective gas can be a protective gas such as nitrogen, and the alkane gas includes but is not limited to at least one of methane, ethane, propane or butane.
[0132] A carbon material layer can be generated by reacting the alkane gas with the organic carbon source molecules adsorbed on the surface of the main material (such as the organic carbon source molecules such as glucose and sucrose adsorbed on the surface of the material obtained in step (b)) at high temperature. The carbon material layer can improve the toughness and conductivity of the surface of the composite lithium supplement material.
[0133] In some embodiments, in step (c), the temperature of the second heat treatment is 600°C to 1000°C, and the time is 2h to 4h. As an example, the temperature of the second heat treatment can be any one of 600°C, 700°C, 800°C, 900°C, and 1000°C, or a range between any two of them; the first time can be any one of 2h, 2.5h, 3h, 3.5h, and 4h, or a range between any two of them.
[0134] The preparation method of the composite lithium supplement material provided in the embodiment of the present application has simple process, strong feasibility, high efficiency and environmental protection, and is easy to realize large-scale production.
[0135] [Positive electrode]
[0136] In some embodiments, the embodiments of the present application provide a positive electrode sheet, which includes a current collector and a positive electrode active material layer arranged on the surface of the current collector; the positive electrode active material layer includes the aforementioned composite lithium replenishing material or the composite lithium replenishing material prepared by the aforementioned method, as well as a positive electrode active material, a conductive agent and a binder.
[0137] The positive electrode sheet includes the above-mentioned composite lithium supplement material provided in the embodiment of the present application, and therefore, the positive electrode sheet also has the characteristic of excellent electrochemical performance.
[0138] In some embodiments, in the positive electrode active material layer, the mass ratio of the positive electrode active material, the composite lithium supplement material, the conductive agent and the binder is (85-95): (1-10): (0.1-5): (1-5).
[0139] In some embodiments, the mass proportion of the composite lithium supplement material in the positive electrode active material layer is 1% to 10%. As an example, the mass proportion of the composite lithium supplement material in the positive electrode active material layer can be any one of 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 5%, 6%, 8%, 10%, or a range between any two of them.
[0140] The present application has no particular restrictions on the material of the current collector in the positive electrode sheet, as long as the purpose of the present application can be achieved, and it can be selected according to actual needs. For example, in some embodiments, the positive electrode current collector may include aluminum foil, aluminum alloy foil, etc. Of course, in other embodiments, a composite current collector (such as an aluminum-carbon composite current collector) may also be used.
[0141] The embodiments of the present application are not particularly limited to the types of positive active materials, conductive agents and binders in the positive active material layer, as long as the purpose of the present application can be achieved. For example, in some embodiments, the positive active material may include but is not limited to one or more of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium cobalt acid, lithium manganate, lithium nickel manganate, lithium nickel cobalt manganate, and lithium nickel cobalt aluminum acid. The binder may include but is not limited to one or more of polyacrylate, polyimide, polyvinyl alcohol, polyamide, polyamide-imide, polyvinylidene fluoride, polystyrene butadiene copolymer (styrene butadiene rubber), polytetrafluoroethylene, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose or sodium hydroxymethyl cellulose. The conductive agent may include but is not limited to at least one of conductive carbon black (such as acetylene black, Ketjen black), carbon nanotubes (CNTs), carbon fibers, graphene, etc. The above-mentioned carbon nanotubes may be single-walled carbon nanotubes and / or multi-walled carbon nanotubes.
[0142] The present application has no particular restrictions on the preparation method of the positive electrode sheet, and a preparation method known in the art can be selected as long as the purpose of the present application can be achieved. For example, the preparation method of the positive electrode sheet includes but is not limited to the following steps: dispersing the positive electrode active material, the composite lithium supplement material, the positive electrode conductive agent, and the positive electrode binder in N-methylpyrrolidone (NMP) solvent and mixing to form a uniform positive electrode slurry, coating the positive electrode slurry on the positive electrode collector, and drying, cold pressing, slitting, etc. to obtain the positive electrode sheet.
[0143] [Battery]
[0144] In some embodiments, the present application provides a battery, which includes the aforementioned positive electrode sheet and a negative electrode sheet.
[0145] The battery includes the above-mentioned composite lithium supplement material provided in the embodiment of the present application. Therefore, the battery, such as a lithium-ion secondary battery, also has the characteristics of excellent electrochemical performance, such as the battery has the characteristics of long cycle life, good conductivity and high energy density.
[0146] The electrochemical cell may be a secondary battery having high cycle performance and high safety. Specifically, the secondary battery may be a lithium secondary battery.
[0147] The battery may be a secondary battery or a primary battery, preferably a secondary battery. For example, the battery may be a lithium ion secondary battery, a lithium primary battery, etc., but is not limited thereto. The battery structure of the present application includes but is not limited to a soft-pack lithium ion battery, a square hard-shell battery, or a cylindrical hard-shell battery, etc.
[0148] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode material. As an example, the negative electrode current collector has two surfaces opposite to each other in its own thickness direction, and the negative electrode active material layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0149] In this embodiment, the specific materials and structures of the negative electrode current collector and the negative electrode active material layer in the negative electrode sheet are not limited, and the negative electrode sheet structure and components known in the art that can be used in secondary batteries can be selected.
[0150] In some embodiments, the battery further includes an electrolyte and a separator.
[0151] The electrolyte may be an electrolyte, and the electrolyte that can be used in the embodiments of the present application may be an electrolyte known in the prior art. The specific type and structure of the electrolyte may be an electrolyte type that can be used in a secondary battery and is well known in the art, such as an ester electrolyte or an ether electrolyte, etc., which is not limited and will not be described in detail here.
[0152] The present application has no particular restrictions on the type of isolation membrane, and any known porous isolation membrane with good chemical stability and mechanical stability can be selected. As an example, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride.
[0153] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in this area or the product instructions are used. If the manufacturer of the reagents, materials or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0154] Example 1
[0155] 1. Preparation of composite lithium supplement materials
[0156] (a) A lithium-rich material (Li2NiO2, with an average particle size of 1.5 μm) and a pore-forming agent (ammonium bicarbonate) are mixed in a mass ratio of 99.5%:0.5%, and the ammonium bicarbonate particles are evenly dispersed in a PVDF solvent, and then the dispersion is stirred in a vacuum, and then the pore-forming agent solution is sprayed onto the surface of the lithium-rich material by spray drying to obtain an intermediate.
[0157] (b) ball milling and drying the intermediate obtained in step (a) and 0.2 mol / L titanium tetrachloride solution, wherein the ball milling speed is 1000 r / min, the ball milling time is 4 hours, and the drying is vacuum drying, the vacuum drying temperature is 85°C, and the vacuum drying time is 6 hours; then, in an atmosphere of protective gas nitrogen, a reactive gas alkane gas is introduced, and the reaction is carried out at 1000°C for 4 hours to obtain a lithium-rich material coated with a 0.5 μm first coating layer, wherein the first coating layer includes a titanium carbide layer with a porous structure.
[0158] (c) dissolving the organic carbon source glucose in water to prepare a solution with a concentration of 20 g / L to obtain a second coating layer precursor, grinding the material obtained in step (b) and evenly immersing it in the second coating layer precursor. After immersion for 2 hours, the material is taken out, and then an alkane gas methane is introduced into a protective gas nitrogen in a tubular furnace, and the reaction is carried out at a temperature of 800° C. for 3 hours, so that a 0.2 μm carbon coating layer (the thickness of the carbon coating layer can be determined by the number of carbon depositions) can be deposited on the surface of the first coating layer, i.e., the second coating layer, to obtain a composite lithium supplement material.
[0159] 2. Preparation of lithium batteries
[0160] 1) Preparation of positive electrode sheet: The positive electrode active material ternary material (NCM), the prepared composite lithium supplement material, the conductive agent acetylene black and the binder PVDF are mixed in a mass ratio of 92:5:1.5:1.5, and the solvent NMP is added and stirred to form a uniform and stable positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the coating surface density is 195g / m 2 After drying and cold pressing, the positive electrode sheet is obtained, and the compaction density is 3.4g / cm 3 .
[0161] 2) Preparation of negative electrode sheet: Mix the negative electrode active material graphite, conductive agent SP, binder CMC and SBR in a mass ratio of 96.5:1:1:1.5, add solvent deionized water and stir to form a mixed and stable negative electrode slurry; evenly coat the negative electrode slurry on the negative electrode current collector copper foil (thickness of 6 μm), with a coating surface density of 156 g / m 2 After drying and cold pressing, the negative electrode sheet is obtained, and the compaction density is 1.5g / cm 3 .
[0162] 3) Prepare an electrolyte: mix ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) in a volume ratio of 1:1:1 to obtain an organic solvent, then add solute LiPF6 to the organic solvent to dissolve and mix evenly to obtain an electrolyte; wherein the concentration of LiPF6 is 1.2 mol / L.
[0163] 4) Selection of isolation membrane: The isolation membrane uses polypropylene film as the base membrane with a thickness of 9 μm, a PVDF layer with a thickness of 3 μm is coated on both sides, and an aluminum oxide layer with a thickness of 3 μm is coated on the positive electrode side.
[0164] 5) Battery assembly
[0165] Arrange the positive electrode sheet, isolation film and negative electrode sheet in order, and select the assembly method of lamination. Inject the electrolyte into the dry battery cell, soak for 24 hours, and then form it at 45℃. The formation process is: charge at 0.05C to 3.4V, and then charge at 0.2C to 3.75V; after aging at room temperature for 24 hours, the battery cell is completed.
[0166] Example 2
[0167] Embodiment 2 is substantially the same as Embodiment 1, except that:
[0168] In <Preparation of composite lithium-supplementing material>, in step (a), the average particle size of the lithium-rich material (Li2NiO2) is 2μm.
[0169] The rest are the same as in Example 1.
[0170] Example 3
[0171] Embodiment 3 is substantially the same as Embodiment 1, except that:
[0172] In <Preparation of composite lithium-supplementing material>, in step (a), the average particle size of the lithium-rich material (Li2NiO2) is 1 μm.
[0173] The rest are the same as in Example 1.
[0174] Example 4
[0175] Embodiment 4 is substantially the same as Embodiment 1, except that:
[0176] In <Preparation of composite lithium supplementing material>, in step (a), the lithium-rich material and the pore-forming agent (ammonium bicarbonate) are mixed in a mass ratio of 99.9%:0.1%.
[0177] The rest are the same as in Example 1.
[0178] Example 5
[0179] Example 5 is substantially the same as Example 1, except that:
[0180] In <Preparation of composite lithium supplementing material>, in step (a), the lithium-rich material and the pore-forming agent (ammonium carbonate) are mixed in a mass ratio of 99%:1%.
[0181] The rest are the same as in Example 1.
[0182] Example 6
[0183] Embodiment 6 is substantially the same as Embodiment 1, except that:
[0184] In <Preparation of composite lithium supplementing material>, in step (a), the lithium-rich material and the pore-forming agent (ammonium bicarbonate) are mixed in a mass ratio of 98%:2%.
[0185] The rest are the same as in Example 1.
[0186] Example 7
[0187] Example 7 is substantially the same as Example 1, except that:
[0188] In <Preparation of composite lithium supplement material>, in step (b), the reaction is carried out at 1200° C. for 4 hours.
[0189] The rest are the same as in Example 1.
[0190] Example 8
[0191] Example 8 is substantially the same as Example 1, except that:
[0192] In <Preparation of composite lithium supplement material>, in step (b), the reaction is carried out at 800° C. for 6 hours.
[0193] The rest are the same as in Example 1.
[0194] Example 9
[0195] Example 9 is substantially the same as Example 1, except that:
[0196] In <Preparation of composite lithium supplement material>, in step (b), the intermediate obtained in step (a) is ball-milled with 0.4 mol / L titanium tetrachloride solution and dried.
[0197] The titanium carbide layer obtained in Example 9 was 0.7 μm.
[0198] The rest are the same as in Example 1.
[0199] Example 10
[0200] Embodiment 10 is substantially the same as Embodiment 1, except that:
[0201] In <Preparation of composite lithium supplement material>, in step (b), the intermediate obtained in step (a) is ball-milled with 0.2 mol / L zirconium chloride solution and dried.
[0202] The zirconium carbide layer obtained in Example 10 was 0.5 μm.
[0203] The rest are the same as in Example 1.
[0204] Embodiment 11
[0205] Example 11 is substantially the same as Example 1, except that:
[0206] In <Preparation of Composite Lithium Supplementing Material>, in step (c), the thickness of the second coating layer is 0.4 μm.
[0207] The rest are the same as in Example 1.
[0208] Example 12
[0209] Example 12 is substantially the same as Example 1, except that:
[0210] In <Preparation of Composite Lithium Supplementing Material>, in step (c), the thickness of the second coating layer is 0.1 μm.
[0211] The rest are the same as in Example 1.
[0212] Embodiment 13
[0213] Example 13 is substantially the same as Example 1, except that:
[0214] In <Preparation of composite lithium supplement material>, in step (c), the reaction is carried out at a temperature of 600° C. for 4 hours.
[0215] The rest are the same as in Example 1.
[0216] Embodiment 14
[0217] Example 14 is substantially the same as Example 1, except that:
[0218] In <Preparation of composite lithium supplement material>, in step (c), the reaction is carried out at a temperature of 1000° C. for 2 hours.
[0219] The rest are the same as in Example 1.
[0220] Comparative Example 1
[0221] Comparative Example 1 is substantially the same as Example 1, except that:
[0222] In <Preparation of Composite Lithium Supplementing Material>, the first coating layer is eliminated, that is, a carbon material layer is directly formed on the surface of the lithium-rich material.
[0223] Comparative Example 2
[0224] Comparative Example 2 is substantially the same as Example 1, except that:
[0225] In <Preparation of Composite Lithium Supplementing Material>, in step (b), the temperature of the heating treatment is 600°C.
[0226] The rest are the same as in Example 1.
[0227] Comparative Example 3
[0228] Comparative Example 3 is substantially the same as Example 1, except that:
[0229] In <Preparation of composite lithium-supplementing material>, step (c) is eliminated, that is, the second coating layer is not provided, and only a lithium-rich material having a first coating layer is obtained.
[0230] The rest are the same as in Example 1.
[0231] Comparative Example 4
[0232] Comparative Example 4 is substantially the same as Example 1, except that:
[0233] In <Preparation of Composite Lithium Supplementing Material>, the addition of pore-forming agent is cancelled, that is, the processing of the porous structure of the first coating layer is cancelled, and the obtained first coating layer does not have a porous structure.
[0234] The rest are the same as in Example 1.
[0235] Comparative Example 5
[0236] Comparative Example 5 is substantially the same as Example 1, except that:
[0237] In <Preparation of Composite Lithium Supplementing Material>, the composite lithium supplementing material is an existing lithium-rich material (Li2NiO2), that is, the first coating layer and the second coating layer are not provided on the surface of the lithium-rich material.
[0238] The rest are the same as in Example 1.
[0239] Performance Testing
[0240] 1. The performance tests of the positive electrode sheets or composite lithium supplement materials prepared in the above embodiments and comparative examples are respectively carried out, specifically including:
[0241] (1) Maximum compaction density: Since the rigid coating of the present application, i.e., the first coating layer, can improve the structural stability of the composite lithium supplement material, the maximum pressure that can be borne by the positive electrode sheet without breaking the structure during the rolling process of the positive electrode sheet is increased by increasing the compaction density. The standard test method is to test the positive electrode sheet at different compaction densities, such as 3.2 g / cm 3 、3.3g / cm 3 、3.4g / cm 3 , 3.5g / cm 3 、3.6g / cm 3Under the same compaction conditions (keep using different pressure rollers to press the electrode until the composite lithium supplement material is observed to be broken), the SEM and CP of the cross section are used to determine whether the adsorption layer material is broken.
[0242] (2) Powder conductivity: The conductivity is measured by powder level resistivity test. A certain amount of composite lithium supplement material is placed in the test container of the powder resistance meter. The composite lithium supplement material of the same mass is pressed into a dense block under certain pressure conditions, such as 3-10 tons of pressure, and its resistivity is tested in this state.
[0243] (3) Electrode-level conductivity: The composite lithium supplement materials in the examples and comparative examples were uniformly mixed with the positive electrode active material in the same proportion, loaded into a powder resistance meter, extruded into cakes of the same thickness, and tested for resistivity using a four-probe resistance test.
[0244] (4) Electrode liquid absorption time: After the electrode is rolled in the same manner, the same mass of electrolyte is dripped onto the surface of the positive electrode, and the time for the electrolyte to completely penetrate is recorded.
[0245] The test results are shown in Table 1.
[0246] Table 1
[0247]
[0248] It can be seen from the data in Table 1 that by comparing Examples 1 to 14 with Comparative Examples 1 to 5, the coating of the first coating layer, i.e., the rigid coating, in the composite lithium supplement material prepared by the method described in the embodiment of the present invention improves the structural stability of the composite lithium supplement material itself and increases the structural strength of the substrate. In the subsequent practical use of lithium batteries, the compaction density can be increased, thereby improving the energy density of the battery.
[0249] Through the analysis and comparison of Example 1 and Comparative Example 1, it can be seen that Comparative Example 1 cancels the setting of the first coating layer, which reduces the compaction density and conductivity and other properties. This shows that by setting the first coating layer, i.e., the rigid coating, on the surface of the lithium-rich material, the compaction density of the material can be improved. The rigid coating has a certain conductivity and can improve the conductivity of the lithium supplement itself, so that the conductivity of the powder and the conductivity of the pole piece level can be improved. Through the analysis and comparison of Example 1 and Comparative Example 2, it can be seen that the reaction temperature of Comparative Example 2 when preparing the first coating layer is relatively low, resulting in a relatively low compaction density and a slight decrease in conductivity. This is because the generation of rigid substances such as tungsten carbide and zirconium carbide is related to temperature, wherein the bond energy or structural stability is related to temperature. If the temperature is too low, the overall structure is slightly affected, and it is easy to break, which affects the thickness of the gas adsorption, conductivity, safety performance, etc.
[0250] Through the analysis and comparison of Example 1 and Comparative Example 3, it can be seen that the outer carbon material layer is cancelled in Comparative Example 3, which reduces the conductivity of the material. This shows that by coating a carbon material layer on the outermost layer of the lithium supplement material, not only the specific surface area is improved to a certain extent, but also the conductivity of the powder and the conductivity of the pole piece level are improved. This is because the conductivity of the carbon material layer is stronger than that of the titanium carbide material. The carbon material layer may reduce the contact distance with the positive electrode active material due to its softer characteristics, which can reduce the contact impedance and improve the contact compatibility with the positive electrode material. Through the analysis and comparison of Example 1 and Comparative Example 4, it can be seen that the first coating layer in Comparative Example 4 does not have a porous structure, which greatly increases the liquid absorption time. This shows that the modified rigid coating with a porous structure, that is, the first coating layer with a porous structure, can greatly increase the diffusion rate of the electrolyte. This is mainly because the porosity of the rigid coating can provide more space and increase the diffusion rate. Through the analysis and comparison between Example 1 and Comparative Example 5, it can be seen that Comparative Example 5 uses the existing lithium-rich material, which has a lower compaction density and conductivity, indicating that the present application can increase the compaction density of the material by setting the first coating layer and the second coating layer on the surface of the lithium-rich material, and the conductivity of the powder and the conductivity of the electrode layer can be improved.
[0251] In addition, through the analysis and comparison of Example 1 and Example 6, it can be seen that the pore-forming agent content of Example 6 exceeds the preferred range specified in the present application. Although the increase in the content of the pore-forming agent will accelerate the speed of liquid infiltration, its compaction density will also decrease. This is mainly because the increase in pores leads to a decrease in the structural stability of the first coating layer. Therefore, the content of the pore-forming agent needs to be within an appropriate range to ensure the structural stability of the first coating layer.
[0252] 2. The performance tests were performed on the batteries prepared in the above embodiments and comparative examples, including:
[0253] Standard test method: In the following tests, if there is no special charge and discharge rate requirement, a unified charge and discharge system is adopted, 0.5C constant current and constant voltage charging to 4.25V, and 0.5C current discharge to 2.5V.
[0254] (1) Internal resistance: DC internal resistance ACR test: discharge the battery to 50% SOC according to the standard charge and discharge system, and use a DC internal resistance meter to test the DC internal resistance of the battery.
[0255] The specific test process of internal resistance includes: leaving the battery at 25℃ for 30 minutes, charging at 0.5C constant current to 4.25V, then charging at constant voltage to 0.05C, leaving it at rest for 30 minutes, discharging at 1C for 30 minutes (to 50% SOC), leaving it at rest for 60 minutes, then using a multimeter or voltage resistance meter to contact the positive and negative terminals with the positive and negative ears of the battery, and the reading on the display is the internal resistance of the battery at 50% SOC.
[0256] (2) First efficiency test: The battery is charged to 3.4V at 0.1C, 3.75V at 0.2C, and 4.25V at 0.5C. The battery is then discharged to 2.5V at 0.5C. First efficiency (%) = battery first discharge capacity / battery first charge capacity.
[0257] (3) Rate retention rate: 1. Charge at 0.5C constant current to 4.25V, then charge at 4.25V constant voltage to 0.05C; 2. Let stand for 30 minutes; 3. Discharge at 0.5C current to the lower limit voltage of 2.5V; 4. Let stand for 30 minutes; then repeat steps 1-4 in sequence, and perform 1C / 2C / 3C current discharge. 3C rate retention rate = 3C discharge capacity / 0.5C discharge capacity.
[0258] (4) 1C cycle test: Perform charge and discharge tests according to the standard test process 0.5C / 1C system until the discharge capacity of the battery is lower than 80% of the initial capacity. The test is stopped and the capacity retention rate after 500 cycles is recorded.
[0259] The specific process of the 1C cycle test includes: leaving the battery at 25°C for 30 minutes, charging at 0.5C constant current to 4.25V, then charging at 0.05C constant voltage, leaving it at 30 minutes, discharging at 1C to 2.5V, recording the discharge capacity of the first cycle as the initial capacity, and stopping the test until the discharge capacity of the battery is lower than 80% of the initial capacity, recording the capacity retention rate after 500 cycles, then the capacity retention rate of the 500th cycle = discharge capacity of the 500th cycle / discharge capacity of the first cycle.
[0260] (5) Energy density test: The battery was placed in a 25°C environment for 30 min, charged at 0.5C constant current to 4.25 V, then charged at 0.05C constant voltage, placed for 30 min, and discharged at 1C to 2.5 V. The discharge capacity and discharge voltage data of the test were collected. Then, 1C energy density = 1C discharge capacity * 1C discharge average voltage / total weight of the battery.
[0261] The test results are shown in Table 2.
[0262] Table 2
[0263]
[0264]
[0265] It can be seen from the data in Table 2 that, by comparing Examples 1 to 14 with Comparative Examples 1 to 5, the composite lithium supplement material prepared by the method described in the embodiment of the present invention improves the structural stability of the material, increases the structural strength, and can increase the compaction density and improve the energy density of the battery in practical lithium batteries; and the battery using the composite lithium supplement material provided by the embodiment of the present invention can improve conductivity, reduce internal resistance, and can also improve the first efficiency and cycle performance to a certain extent.
[0266] Parts of the present invention that are not described in detail are well known to those skilled in the art.
[0267] The basic principle of the present invention is described above in conjunction with specific embodiments. However, it should be pointed out that the advantages, strengths, effects, etc. mentioned in the present invention are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. must be possessed by each embodiment of the present invention. In addition, the specific details disclosed above are only for the purpose of illustration and facilitation of understanding, rather than limitation, and the above details do not limit the present invention to being implemented by adopting the above specific details.
[0268] It should be noted that the term "and / or" or " / " used in this document is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The singular forms of "a", "the" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0269] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0270] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite lithium supplement material, characterized in that: The composite lithium supplement material comprises: Lithium-rich materials; A first coating layer, coating at least a portion of the surface of the lithium-rich material, wherein the first coating layer comprises a carbide or nitride layer having a porous structure; and The second coating layer is coated on at least a portion of the surface of the first coating layer, and the second coating layer includes a carbon material layer.
2. The composite lithium supplement material according to claim 1, characterized in that: The lithium-rich material includes at least one of lithium-rich nickel oxide, lithium-rich iron oxide, lithium-rich cobalt oxide, lithium oxide, lithium fluoride, lithium nitride or lithium sulfide; And / or, the average particle size of the lithium-rich material is 0.5 μm to 5 μm.
3. The composite lithium supplement material according to claim 1, characterized in that: The thickness of the first coating layer is 0.1 μm to 1 μm; And / or, the pore size of the porous structure ranges from 100 nm to 500 nm; and / or, the carbide comprises at least one of titanium carbide, tungsten carbide or zirconium carbide; And / or, the nitride comprises titanium nitride.
4. The composite lithium supplement material according to any one of claims 1 to 3, characterized in that: The thickness of the second coating layer is 0.1 μm to 0.5 μm; And / or, the second coating layer includes at least one of an activated carbon layer, a graphene layer, a porous carbon layer or an amorphous carbon layer.
5. A method for preparing a composite lithium supplement material, characterized in that: The following steps are involved: The pore-forming agent solution is attached to the lithium-rich material by spray drying to obtain an intermediate; The intermediate and the first coating layer precursor are ball-milled and dried, and a reactive gas is introduced under a protective atmosphere to perform a first heat treatment to obtain a lithium-rich material coated with a first coating layer, wherein the first coating layer includes a carbide or nitride layer with a porous structure; The lithium-rich material coated by the first coating layer is mixed with a second coating layer precursor, and subjected to a second heat treatment, and the second coating layer is coated on the surface of the first coating layer, wherein the second coating layer includes a carbon material layer, to obtain the composite lithium supplement material.
6. The method for preparing the composite lithium supplement material according to claim 5, characterized in that: The step of obtaining the intermediate satisfies at least one of the following characteristics (1) to (3): (1) The pore-forming agent solution is composed of a pore-forming agent and a solvent, wherein the pore-forming agent includes at least one of ammonium carbonate, ammonium bicarbonate or ammonium chloride, and / or the solvent includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, polyethylene oxide or ethylene oxide; Optionally, the mass ratio of the pore former to the lithium-rich material is (0.1-1): (99-99.9); (2) The average particle size of the intermediate is 0.5 μm to 3 μm; (3) The lithium-rich material includes at least one of lithium-rich nickel oxide, lithium-rich lithium iron oxide, lithium-rich lithium cobalt oxide, lithium oxide, lithium fluoride, lithium nitride or lithium sulfide.
7. The method for preparing the composite lithium supplement material according to claim 5, characterized in that: The step of obtaining the lithium-rich material coated by the first coating layer satisfies at least one of the following characteristics (1) to (6): (1) The first coating layer precursor includes at least one of a titanium tetrachloride solution, a tungsten tetrachloride solution or a zirconium chloride solution; Optionally, the concentration of the first coating layer precursor is 0.01 to 0.5 mol / L; (2) The rotation speed of the ball mill is 800 to 2000 r / min, and the time of the ball mill is 2 to 10 hours; (3) The drying is vacuum drying, the vacuum drying temperature is 60° C. to 120° C., and the vacuum drying time is 2 h to 24 h; (4) The mass ratio of the first coating layer precursor to the intermediate is (0.1-1): (99-99.9); (5) The reactive gas is suitable for reacting with the first coating layer precursor, and the reactive gas includes at least one of an alkane gas or ammonia gas; Optionally, the alkane gas includes at least one of methane, ethane, propane or butane; (6) The temperature of the first heat treatment is 800°C to 1400°C, and the time is 2h to 6h.
8. The method for preparing the composite lithium supplement material according to any one of claims 5 to 7, characterized in that: The step of obtaining the composite lithium supplement material satisfies at least one of the following characteristics (1) to (5): (1) the second coating layer precursor comprises at least one of an organic carbon source selected from the group consisting of a glucose solution, a sucrose solution, a soluble starch solution, a cellulose solution, and a polyvinyl alcohol solution; Optionally, the concentration of the second coating layer precursor is 10 to 50 g / L; (2) The mass ratio of the lithium-rich material to the carbon material layer is (92-98): (2-5); (3) The lithium-rich material coated by the first coating layer and the second coating layer precursor are immersed and mixed for 2 hours to 6 hours; (4) during the second heating treatment, introducing an alkane gas under a protective atmosphere; Optionally, the alkane gas includes at least one of methane, ethane, propane or butane; (5) The temperature of the second heat treatment is 600°C to 1000°C, and the time is 2h to 4h.
9. A positive electrode sheet, characterized in that: It includes a current collector and a positive electrode active material layer arranged on the surface of the current collector; The positive electrode active material layer comprises the composite lithium supplement material according to any one of claims 1 to 4 or the composite lithium supplement material prepared by the method according to any one of claims 5 to 8, as well as a positive electrode active material, a conductive agent and a binder; Preferably, in the positive electrode active material layer, the mass ratio of the positive electrode active material, the composite lithium supplement material, the conductive agent and the binder is (85-95): (1-10): (0.1-5): (1-5).
10. A battery, characterized in that: It comprises a negative electrode sheet and the positive electrode sheet as claimed in claim 9.
Citation Information
Cited By
Double-layer coated lithium supplement material and preparation method thereof, positive pole piece and battery
CN120149594A
Double-coated lithium supplementing material, preparation method thereof, positive electrode sheet and battery
CN120149594B
Doped and coated lithium-rich compound as well as preparation method and application thereof
CN120637486A