Fuel cell module integrated gluing process based on self-gluing membrane electrode

Through the integrated glue process of self-glued membrane electrodes, the hot melt adhesive layer and hot press forming technology are used to solve the problem of difficult airtightness between the membrane electrode and the bipolar plate in the fuel cell stack, and high-strength connection is achieved and stable sealing improve the performance and production efficiency of the stack.

CN119050403APending Publication Date: 2024-11-29CHANGSHU LIANHUA NEW ENERGY TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411546885.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During the fuel cell stack manufacturing process, the airtightness between the membrane electrode and the bipolar plate is difficult to control, resulting in the risk of hydrogen or oxygen leakage. The prior art such as dispensing process and preset sealing gasket method have limitations. Impacts the yield and safety of the stack.

Method used

Using an integrated glue process based on self-glued film electrodes, the high-strength connection between graphite anode plate, self-glued film electrode and graphite cathode plate is achieved through uniform coverage and hot pressing of the hot melt adhesive layer, forming a large-area stable interface. Ensure sealability.

Benefits of technology

It improves the sealing performance and stability of the stack, simplifies the production process, reduces technical thresholds and costs, and enhances the overall operating reliability and service life of the fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050403A_ABST
    Figure CN119050403A_ABST
Patent Text Reader

Abstract

The invention particularly relates to a fuel cell module integrated gluing process based on a self-gluing membrane electrode, which comprises a manufacturing process of a membrane electrode, and comprises the following steps: step S101, selecting a whole roll of polymer plastic material as a base material, and uniformly covering two sides of the base material with a hot melt adhesive layer; and step S102, cutting the base material into a plurality of qualified frames, and simultaneously selecting a plurality of qualified catalyst coating proton exchange membranes and gas diffusion layers matched with the frames. According to the invention, the self-glued membrane electrode, the graphite cathode plate and the graphite anode plate are integrally glued and molded, so that the hot melt adhesive layer forms a firm and lasting glued interface after chemical bonding, the connection between the self-glued membrane electrode and the graphite partition plate is ensured, and the problem of poor sealing property caused by accumulative errors is effectively avoided; therefore, the overall stability and durability of the stack are enhanced, and a key technical support is provided for improving the performance and quality control of the fuel cell stack.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fuel cells, and in particular to an integrated gluing process for fuel cell modules based on self-gluing membrane electrodes. Background Art

[0002] Hydrogen fuel cells, as one of the most promising clean energy technologies, are increasingly receiving high attention from scientific research institutions and industries around the world. In order to achieve the ideal voltage level and power level, the manufacturing process of fuel cell stacks usually requires hundreds of bipolar plates and membrane electrodes to be precisely stacked and assembled in a specific order to form a highly integrated and complex three-dimensional structure. This three-dimensional structure places extremely high demands on the refinement of large-scale stack production, but "how to accurately position the bipolar plates and membrane electrodes and ensure excellent airtightness between the two" has always been a problem that has plagued the industry.

[0003] According to the domestic patent numbers: CN112186216A, CN212303729U, CN114243075A, CN115064723B, CN114388862A, it can be seen that the most widely used glue dispensing process in China is to solve the problem of achieving efficient sealing between the membrane electrode and the bipolar plate. However, this technology has great limitations. For example, due to the complex structure, there are often multiple glue dispensing lines crossing at the junction of the membrane electrode and the bipolar plate. The thickness of the glue layer at these intersections is difficult to control as accurately as other single coating areas. In the large-scale stacking process, the accumulation of tiny unevenness will cause the problem of reduced airtightness at the intersection of the glue dispensing lines, which may cause the risk of hydrogen or oxygen leakage, which poses a challenge to the yield and safety of fuel cells. And in summary of the above-mentioned public patents, in order to overcome this shortcoming of the dispensing process, the industry has also developed another technical solution of pre-setting the sealing gasket. During the bipolar plate production stage, the customized sealing gasket is pre-embedded into the bipolar plate, which can solve the leakage problem caused by the uneven thickness of the dispensing intersection to a certain extent. However, this method has more stringent requirements on production equipment and technology. Specifically, it is necessary to accurately fix the soft and elastic sealing gasket in the corresponding position of the bipolar plate while ensuring accuracy. This not only requires the equipment to have high-precision positioning function, but also tests the rationality of material and structural design and the degree of refinement of the production process. Otherwise, any slight uneven sealing may lead to local gas leakage or coolant leakage, which will seriously affect the overall performance and life of the battery stack.

[0004] Therefore, whether it is the dispensing process or the pre-set sealing gasket method, the fuel cell stack sealing process faces its own technical challenges, and manufacturers still have room for further improvement in this technology. Summary of the invention

[0005] The present invention provides a fuel cell module integrated bonding process based on a self-bonding membrane electrode to solve the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: A membrane electrode manufacturing process comprises the following steps: Step S101, selecting a whole roll of polymer plastic material as a base material, and evenly covering both sides of the base material with a layer of hot melt adhesive; Step S102, cutting the base material into a plurality of qualified frames, and selecting a plurality of qualified catalyst-coated proton exchange membranes and gas diffusion layers that are compatible with the frames; Step S103, evenly apply hot melt adhesive to the areas where the outer edges of the catalyst-coated proton exchange membranes contact the frame, and accurately align the catalyst-coated proton exchange membranes with the frame after the application of glue, so that the catalyst-coated proton exchange membranes are tightly pressed on the frame; Step S104, uniformly dispensing hot melt adhesive on the area where the outer edge of the gas diffusion layer contacts the catalyst-coated proton exchange membrane; Step S105 , drying the surface of the gas diffusion layer after dispensing, and attaching and fixing a plurality of gas diffusion layers in groups of two on both sides of the catalyst-coated proton exchange membrane.

[0007] Preferably, the base material in step S101 is made of polyimide, polyethylene terephthalate, polyethylene naphthalate, polypropylene or polyphenylene sulfide, and the thickness of the base material is 150-350 μm.

[0008] Preferably, the hot melt adhesive used in step S101, step S103 and step S104 is made of EPDM rubber, silicone rubber, fluororubber, polyolefin rubber, nitrile rubber or chloroprene rubber.

[0009] Preferably, the hot melt adhesive layer in step S101 is covered by screen printing, spraying or pasting a hot melt adhesive sheet, and the thickness of the hot melt adhesive layer is 10-50 μm.

[0010] A self-bonding membrane electrode is prepared by adopting the above-mentioned membrane electrode manufacturing process.

[0011] A fuel cell module integrated bonding process based on self-bonding membrane electrode comprises the following steps: Step S201, selecting some of the processed graphite separators as graphite anode plates, and selecting some as graphite cathode plates; Step S202, opening a water seal groove on the upper surface of the graphite anode plate or the lower surface of the graphite cathode plate; Step S203, cleaning and drying the surfaces of the graphite anode plate and the graphite cathode plate; Step S204, filling and fixing hot melt adhesive in the water seal groove of the graphite anode plate or the graphite cathode plate; Step S205, disposing at least one of the self-bonding membrane electrodes between the graphite anode plate and the graphite cathode plate, and disposing a fixed hot melt adhesive between the graphite anode plate and the graphite cathode plate between every two adjacent self-bonding membrane electrodes; Step S206, setting the time, pressure and temperature for the hot pressing equipment so that after the hot pressing operation is set, at least one graphite anode plate, the self-bonding membrane electrode and the graphite cathode plate are integrated and bonded.

[0012] Preferably, the surface cleaning process of the graphite anode plate and the graphite cathode plate in step S203 is water washing to initially remove impurities, ultrasonic deep cleaning and plasma technology fine cleaning.

[0013] Preferably, in step S203, the graphite anode plate and the graphite cathode plate are dried by natural air drying or by using a drying device.

[0014] Preferably, in step S206, the bonding time of the graphite anode plate, the self-bonding membrane electrode and the graphite cathode plate is 5-20 min, the bonding temperature is 100-190° C., and the bonding pressure is 30 KN.

[0015] Preferably, in step S206, the hot melt adhesive is fixed in the water seal groove through a hot pressing process to form a sealing ring.

[0016] Preferably, first of all, the present invention has radically abandoned the complicated and time-consuming steps of manufacturing sealing rings between graphite cathode and anode plates and membrane electrodes in the traditional battery stack assembly process, and instead uses a frame material with a self-bonding function to package the battery stack. The frame material with a self-bonding function has the characteristics of simple preparation process and low cost. Thus, this improvement greatly simplifies the production process, greatly reduces time and resource consumption, and at the same time reduces the process difficulty and technical threshold.

[0017] Secondly, the present invention innovatively uses simple and efficient hot pressing molding technology to ensure that a large-area, high-strength and stable connection interface can be formed between the graphite anode plate and the graphite cathode plate and the self-bonding membrane electrode, meeting the stringent requirements of the fuel cell for high sealing performance during long-term operation. This reliable sealing can improve the overall operating reliability of the fuel cell and extend its service life.

[0018] Finally, by applying hot-melt adhesive integrated molding technology to produce single or multiple battery cell modules, the traditional battery stack assembly process has been greatly simplified, which not only reduces the complexity of the process links, but also significantly improves production speed and flexibility.

[0019] By adopting the above technical solution, the beneficial effects achieved by the present invention are: In the present invention, by selecting the same kind of hot melt adhesive for hot-pressing bonding of catalyst-coated proton exchange membrane, gas diffusion layer and frame material, as well as hot-pressing bonding of graphite anode plate, self-bonding membrane electrode and graphite cathode plate, the self-bonding membrane electrode and graphite cathode and anode plates are integrally bonded and formed, successfully solving the problem of difficult-to-control airtightness, greatly improving the precision control level and product qualification rate of battery cell modules in a large-scale production environment, abandoning the piece-by-piece stacking method and adopting an integrated packaging structure, effectively avoiding the problem of poor sealing due to cumulative errors, thereby enhancing the overall stability and durability of the battery stack.

[0020] In the present invention, a hot melt adhesive layer is pre-arranged in the contact area with the graphite anode plate and the graphite cathode plate by the frame material, so that during the hot pressing process of the graphite anode plate, the self-bonding membrane electrode and the graphite cathode plate, the hot melt adhesive layer can undergo chemical bonding due to the action of specific temperature and pressure to form a strong and durable bonding interface, thereby ensuring a stable mechanical connection between the self-bonding membrane electrode and the graphite separator, effectively preventing unexpected leakage or cross-flow of gas within the three-layer structure, improving the sealing efficiency between the components within the fuel cell stack, and simplifying the complex steps in the traditional packaging process, effectively saving production time and labor costs.

[0021] In summary, the technology of integrated molding of graphite cathode and anode plates and self-bonding membrane electrode frame materials in the present invention not only provides key technical support for improving the performance and quality control of fuel cell stacks, but also lays a solid foundation for promoting the scale-up of the hydrogen energy industry, lowering the technical threshold, standardization and high-quality development of fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the self-bonding membrane electrode of the present invention.

[0023] Figure 2 It is a schematic diagram of the integrated bonding process of a single self-bonded membrane electrode and a graphite separator of the present invention.

[0024] Figure 3 It is a schematic diagram of the integrated bonding process of the multi-self-bonded membrane electrode and the graphite separator of the present invention.

[0025] In the figure: 1. frame; 2. catalyst coated proton exchange membrane; 3. gas diffusion layer; 4. hot melt adhesive layer; 5. self-bonding membrane electrode; 6. graphite anode plate; 7. graphite cathode plate; 8. fixing hot melt adhesive. DETAILED DESCRIPTION

[0026] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described below in conjunction with the accompanying drawings and embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0027] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways than those described herein. Therefore, the present invention is not limited to the specific embodiments of the following disclosure. Embodiment 1

[0028] like Figure 1 As shown, the present invention provides a membrane electrode manufacturing process, comprising the following steps: Step S101, selecting a whole roll of polymer plastic material as a base material, and evenly covering both sides of the base material with a layer of hot melt adhesive 4; As a further feature, the frame 1 materials used in this solution are diverse, and a series of advanced polymer materials are carefully selected. For example, the base material in step S101 is made of polyimide (PI), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polypropylene (PP) or polyphenylene sulfide (PPS) and other films. With their excellent mechanical properties, chemical stability and thermal stability, they ensure the long-term reliable operation of the frame 1 under complex working conditions and increase its service life.

[0029] As a further feature, the thickness of the base material is 150-350 μm, so that the cut frame 1 material can resist various chemical corrosions that may be encountered during the electrolysis process, while having good thermal stability and electrical insulation properties.

[0030] Furthermore, in step S101, the hot melt adhesive layer 4 is covered by screen printing, spraying or pasting a hot melt adhesive sheet. The hot melt adhesive layer 4 on the surface of the frame 1 material is pre-prepared on the surface and can be achieved by technical means such as screen printing, spraying technology, or pasting a hot melt adhesive sheet.

[0031] Furthermore, the thickness of the hot melt adhesive layer 4 is 10-50 μm. In order to ensure good bonding between the hot melt adhesive layer 4 and the membrane electrode and the stability and airtightness of the entire fuel cell assembly, the coating thickness of the hot melt adhesive layer 4 is precisely controlled between 10 and 50 μm according to the specific thickness requirements of the actual membrane electrode to be packaged. The technical steps of this method significantly enhance the stability and sealing performance of the electrochemical reaction area.

[0032] It should be noted that the technology of pre-coating the hot melt adhesive layer 4 on both sides of the entire roll of base material before the base material is formally cut into frame 1 material draws on the mature manufacturing process of transparent tape on the market. It is a well-known and open technology and will not be described in detail herein.

[0033] Step S102, cutting the base material into a plurality of qualified frames 1, and selecting a plurality of qualified catalyst-coated proton exchange membranes 2 and gas diffusion layers 3 that are compatible with the frames 1; Among them, a large opening area is provided in the center of the main part of the frame 1, and the area is reserved for embedding and fixing the catalyst-coated proton exchange membrane 2, and the left and right sides of the area are symmetrically distributed with opening channels, three on each side, a total of six, these openings correspond to the inlet and outlet paths of hydrogen, cooling water and air inside the fuel cell, ensuring efficient gas transmission and smooth heat management, and the position layout and size of each opening strictly match the corresponding interfaces on the graphite anode plate 6 and the graphite cathode plate 7 to achieve seamless connection between components in the fuel cell stack, ensuring the functionality and efficient sealing performance of the overall structure, and this technology is already well known in the art and is well known to those skilled in the art, so this article will not elaborate on this.

[0034] Step S103, evenly apply hot melt adhesive to the areas where the outer edges of the catalyst coated proton exchange membranes 2 contact the frame 1, and accurately align the catalyst coated proton exchange membranes 2 and the frame 1 after the application of adhesive, so that the catalyst coated proton exchange membrane 2 is tightly pressed on the frame 1. It should be emphasized that this process requires that the hot melt adhesive of a preset thickness is evenly applied to the edge of the catalyst coated proton exchange membrane 2 (CCM) and the frame 1 material under precisely controlled temperature. After appropriate pressure and cooling and curing steps, the two can be tightly and durably combined together, which not only enhances the stability of the overall structure, but also ensures the sealing performance required for the operation of the fuel cell; Step S104, uniformly dispensing hot melt adhesive on the area where the outer edge of the gas diffusion layer 3 contacts the catalyst-coated proton exchange membrane 2; Step S105 , drying the surface of the gas diffusion layer 3 after glue application, and attaching and fixing a plurality of gas diffusion layers 3 in a group of two on both sides of the catalyst-coated proton exchange membrane 2 .

[0035] As a further step, an advanced hot-melt adhesive bonding process is used to ensure that the gas diffusion layer 3 (GDL) can be attached to the catalyst-coated proton exchange membrane 2 (CCM) without gaps or wrinkles, forming excellent mechanical strength and a good gas transmission path, avoiding local overpotential losses caused by uneven gas flow, and effectively improving the working efficiency and life of the battery.

[0036] Among them, the outer edge of the catalyst-coated proton exchange membrane 2 and the outer edge of the gas diffusion layer 3 are glued in the area such as Figure 1 Glue dispensing lines shown.

[0037] As a further example, the hot melt adhesive used in step S101, step S103 and step S104 is EPDM rubber, silicone rubber, fluororubber, polyolefin rubber, nitrile rubber or chloroprene rubber.

[0038] Specifically, the use of the same hot melt adhesive can ensure that the catalyst coated proton exchange membrane 2 (CCM), the gas diffusion layer 3 (GDL) and the frame 1 material are integrally glued together during hot pressing.

[0039] In summary, a self-bonding membrane electrode 5 is prepared by adopting the above-mentioned membrane electrode manufacturing process.

[0040] As a further feature, the core components of the self-bonded membrane electrode 5 group include a catalyst-coated proton exchange membrane 2, a frame 1, and two gas diffusion layers 3, wherein the two gas diffusion layers 3 are an anode end gas diffusion layer and a cathode end gas diffusion layer, respectively.

[0041] As a further feature, the overall thickness of the self-bonded membrane electrode 5 is designed to be 200-500 μm. Taking into account factors such as gas diffusion performance, electrochemical reaction rate, mechanical stability and manufacturing process, the size design is such that the anode end gas diffusion layer and the cathode end gas diffusion layer are both larger than the size of their corresponding catalyst coated proton exchange membrane 2 (CCM) to ensure sufficient and efficient gas diffusion and to provide mechanical protection for the catalyst coated proton exchange membrane 2 (CCM) with weaker mechanical strength. Embodiment 2

[0042] like Figure 2 As shown, a fuel cell module integrated bonding process based on a self-bonding membrane electrode, using the self-bonding membrane electrode 5 prepared in Example 1, the specific process of the bonding process is as follows: Step S201, selecting some of the processed graphite separators as graphite anode plates 6, and selecting some as graphite cathode plates 7; Among them, the graphite separator is mainly made of graphite material and a flexible graphite composite material formed by a hot pressing process. The material has a porous structure, which is conducive to being closely connected with the bonding material during the hot pressing process; Step S202, opening a water seal groove on the upper surface of the graphite anode plate 6 or the lower surface of the graphite cathode plate 7; Step S203, cleaning and drying the surfaces of the graphite anode plate 6 and the graphite cathode plate 7; As a further step, the surface cleaning process of the graphite anode plate 6 and the graphite cathode plate 7 is water washing to initially remove impurities, ultrasonic deep cleaning and plasma technology fine cleaning, and the drying treatment of the graphite anode plate 6 and the graphite cathode plate 7 is natural air drying or drying treatment using a drying device; It should be noted that the specific cleaning can be flexibly set according to the characteristics and cleaning requirements of the graphite anode plate 6 and the graphite cathode plate 7. The specific operation method is well known to those skilled in the art and will not be described in detail herein. Step S204, filling and fixing hot melt adhesive 8 in the water seal groove of the graphite anode plate 6 or the graphite cathode plate 7; Among them, the front side of the graphite anode plate 6 is provided with an anode reaction area, and the front side of the graphite cathode plate 7 is provided with a cathode reaction area, and the two reaction areas are arranged correspondingly so as to realize an effective chemical reaction in the battery. In order to ensure the normal operation and safety of the battery, the back side of the graphite anode plate 6 and the back side of the graphite cathode plate 7 are glued together by a fixed hot melt adhesive 8. The fixed hot melt adhesive 8 forms a sealing ring in the water seal groove after a hot pressing process, which effectively prevents the leakage of the coolant and provides stable structural support. Furthermore, when the fixed hot melt adhesive 8 is filled in the water seal groove, its end surface part protrudes from the water seal groove, and this design ensures that the fixed hot melt adhesive 8 can effectively prevent the leakage of the coolant, and the depth of the water seal groove can be adjusted according to actual needs, generally set in the range of 0.3-1.0mm, and the thickness of the fixed hot melt adhesive 8 can be selected in the range of 0.3-10mm to meet the sealing and cooling requirements under different working conditions; It should be noted that, in this solution, a water seal groove is provided on the upper surface of the graphite anode plate 6 , and the hot melt adhesive 8 is fixed inside the water seal groove of the graphite anode plate 6 .

[0043] Step S205, placing a self-bonding membrane electrode 5 between the graphite anode plate 6 and the graphite cathode plate 7; Step S206, setting the time, pressure and temperature for the hot pressing equipment so that after the hot pressing operation is set, at least one graphite anode plate 6, the self-bonding membrane electrode 5 and the graphite cathode plate 7 are integrated and bonded.

[0044] As a further feature, in step S206, the bonding time of the graphite anode plate 6, the self-bonding membrane electrode 5 and the graphite cathode plate 7 is 5-20 min, the bonding temperature is 100-190° C., and the bonding pressure is 30 KN.

[0045] Specifically, when a single self-bonding membrane electrode 5 is placed between a graphite anode plate 6 and a graphite cathode plate 7, it forms a single battery cell module after hot pressing. When forming a single battery cell module, one side of the self-bonding membrane electrode 5 is bonded to the graphite anode plate 6 through a hot melt adhesive layer 4, and the other side of the self-bonding membrane electrode 5 is bonded to the graphite cathode plate 7 through a hot melt adhesive layer 4, so that the graphite anode plate 6, the self-bonding membrane electrode 5 and the graphite cathode plate 7 are integrated and bonded by hot pressing. This process not only ensures the close fit and efficient conductivity between the component materials, but also enhances the stability and durability of the overall structure, successfully solves the problem of airtightness control between the self-bonding membrane electrode 5 and the graphite separator, and greatly improves the precision control level and product qualification rate in a large-scale production environment.

[0046] Furthermore, during the hot pressing process of the graphite anode plate 6, the self-bonded membrane electrode 5 and the graphite cathode plate 7, in order to ensure good sealing performance in the flow field area and prevent cooling water leakage, it is necessary to design and prefabricate a circle of special water seals on the side of the graphite anode plate 6 or the graphite cathode plate 7 with the water flow field, such as Figure 2 The fixed hot melt adhesive 8 is shown. In specific implementation, after the initial hot pressing bonding between the graphite anode plate 6, the self-bonding membrane electrode 5 and the graphite cathode plate 7 is completed, this circle of sealing member can be attached to the corresponding position.

[0047] It is worth noting that in the present invention, the sealing member is made of a fixed hot melt adhesive 8 material that matches the properties of the hot melt adhesive layer 4. When the subsequent hot pressing molding operation is performed, the fixed hot melt adhesive 8 material will undergo a vulcanization reaction under the temperature and pressure of the hot pressing, and then be transformed into a sealing ring with high elasticity, forming a circle of tight water seal structure.

[0048] Furthermore, when assembling a fuel cell stack based on the two-in-one glued single-cell module, it is first necessary to conduct a strict airtightness test on the glued single-cell module. Only qualified modules that pass the test can enter the stack assembly stage. This rigorous quality control method eliminates potential defective products, greatly improves the yield rate of the stack assembly, meets the urgent needs of large-scale production for high quality and high yield rate, and provides strong support for efficient mass production and market promotion.

[0049] Furthermore, when these single-cell modules are arranged to form a battery stack, they are in contact with each other through the water flow field. This innovative design structure allows for quick and efficient replacement of a single-cell module if a fault occurs during the later operation of the battery stack and repair or replacement is required. At the same time, during the disassembly and assembly process, this design effectively avoids physical damage to the self-bonded membrane electrode 5, facilitating the maintenance of the battery stack. Embodiment 3

[0050] like Figure 3 As shown, a fuel cell module integrated bonding process based on a self-bonding membrane electrode, using the self-bonding membrane electrode 5 prepared in Example 1, the specific process of the bonding process is as follows: Step S201, selecting some of the processed graphite separators as graphite anode plates 6, and selecting some as graphite cathode plates 7; Step S202, opening a water seal groove on the upper surface of the graphite anode plate 6 or the lower surface of the graphite cathode plate 7; Step S203, cleaning and drying the surfaces of the graphite anode plate 6 and the graphite cathode plate 7; Step S204, filling and fixing hot melt adhesive 8 in the water seal groove of the graphite anode plate 6 or the graphite cathode plate 7; Among them, steps S201 to S204 in the second embodiment are the same as steps S201 to S204 in the first embodiment. For details, please refer to the first embodiment, and this embodiment will not be described again.

[0051] Step S205, disposing at least two self-bonding membrane electrodes 5 between the graphite anode plate 6 and the graphite cathode plate 7, disposing a graphite anode plate 6 and a graphite cathode plate 7 between every two adjacent self-bonding membrane electrodes 5, and fixing hot melt adhesive 8 between the graphite anode plate 6 and the graphite cathode plate 7 between every two adjacent self-bonding membrane electrodes 5; Step S206, setting the time, pressure and temperature for the hot pressing equipment so that after the hot pressing operation is set, at least one graphite anode plate 6, the self-bonding membrane electrode 5 and the graphite cathode plate 7 are integrated and bonded.

[0052] Specifically, according to the above step S205, the graphite anode plate 6, the self-bonding membrane electrode 5, the graphite cathode plate 7 and the fixing hot melt adhesive 8 which are fully prepared in advance are stacked layer by layer in sequence. Figure 3In the arrangement shown, the stacked multi-cell module will be placed inside the mold and then undergo the critical hot pressing molding process to ensure that the set time, pressure and temperature allow the hot melt adhesive in each area of ​​the multi-cell module to fully melt and bond the components, thereby obtaining a multi-cell module assembly made using integrated gluing and packaging technology. The multi-cell module assembly has excellent structural strength and airtightness, greatly improving the precision control level and product qualification rate in a large-scale production environment.

[0053] Further, in this embodiment, a water seal groove is selected on the upper surface of the graphite anode plate 6, and the fixing hot melt adhesive 8 is selected to be operated inside the water seal groove of the graphite anode plate 6, thereby Figure 3 In the arrangement shown, the pre-cut fixed hot melt adhesive 8 is placed in the water seal groove of the graphite anode plate 6, and then when the fixed hot melt adhesive 8 on the graphite anode plate 6 is hot-pressed to form a sealing ring, it will be tightly attached to the graphite cathode plate 7 of the next battery module connected to it, thereby realizing an effective series connection between the battery modules. At the same time, the sealing ring formed by the hot melt adhesive in the water seal groove after hot pressing will provide a tight sealing effect on this contact interface to ensure that the cooling water will not leak.

[0054] Furthermore, when assembling a fuel cell stack based on the three-in-one glued multi-cell module, it is first necessary to conduct a strict airtightness test on the glued multi-cell module. Only qualified modules that pass the test can enter the stack assembly stage. This rigorous quality control method eliminates potential defective products, greatly improves the yield rate of stack assembly, meets the urgent needs of large-scale production for high quality and high yield rate, and provides strong support for efficient mass production and market promotion.

[0055] Combining the second and third embodiments, after the graphite anode plate 6, the self-bonding membrane electrode 5 and the graphite cathode plate 7 are processed by hot pressing technology, when the self-bonding membrane electrode 5 is in contact with the mutually fitting positions of the graphite anode plate 6 and the graphite cathode plate 7 and heated, the hot melt adhesive layer 4 can quickly melt and evenly fill the tiny gap between the two, thereby achieving a firm and tight bonding effect, ensuring a stable mechanical connection between the self-bonding membrane electrode 5 and the graphite separator, and constructing a tight airtight barrier at the microscopic level, effectively preventing unexpected leakage or cross-flow of gas within the three-layer structure, thereby maintaining the effective isolation of hydrogen and oxygen inside the fuel cell and good airflow distribution in the reaction zone.

[0056] Therefore, the use of the same hot melt adhesive for hot pressing and gluing the catalyst coated proton exchange membrane 2 (CCM), the gas diffusion layer 3 (GDL) and the frame 1 material, as well as for hot pressing and gluing the graphite anode plate 6, the self-bonding membrane electrode 5 and the graphite cathode plate 7 can simplify the entire manufacturing process, improve assembly accuracy, and reduce requirements for mold and equipment specifications, thereby effectively saving production time and labor costs. At the same time, the integrated packaging technology significantly reduces the technical difficulty of stack assembly, making the entire production process more flexible and efficient.

[0057] In addition, in combination with Example 2 and Example 3, a single-cell module or a multi-cell module that has undergone strict airtightness testing in advance and is confirmed to have no leakage risks no longer needs to rely on traditional high-precision mechanical positioning equipment when entering the stacking stage. Instead, a simpler and more economical and efficient horizontal stacking process can be adopted for assembly operations. The horizontal stacking process is a technology disclosed in the art and is not elaborated in detail herein. Furthermore, the horizontal stacking process not only greatly simplifies the complex links in the battery stack assembly process and reduces the dependence on precision mechanical equipment, but also forms a dual protection mechanism with mechanical pressure, effectively improving the sealing performance, eliminating gas leakage, enhancing the operating stability and reliability of the battery unit, and effectively improving the overall product qualification rate, thereby being highly consistent with the actual needs of large-scale industrial production of battery stacks and greatly enhancing the mass production capacity.

[0058] Furthermore, when the self-bonded membrane electrode 5 and the graphite cathode and anode plates together form a battery module, they will undergo a certain degree of compression, usually compressed to 60-70% of the original thickness. This process helps to improve the contact and conductivity between the electrodes, thereby improving the overall performance of the battery.

[0059] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0060] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A process for manufacturing a membrane electrode, characterized in that: The following steps are involved: Step S101, selecting a whole roll of polymer plastic material as a base material, and evenly covering both sides of the base material with a layer of hot melt adhesive (4); Step S102, cutting the base material into a plurality of qualified frames (1), and simultaneously selecting a plurality of qualified catalyst-coated proton exchange membranes (2) and gas diffusion layers (3) that are compatible with the frames (1); Step S103, uniformly applying hot melt adhesive to the areas where the outer edges of the plurality of catalyst-coated proton exchange membranes (2) contact the frame (1), and accurately aligning the catalyst-coated proton exchange membranes (2) and the frame (1) after the adhesive application, so that the catalyst-coated proton exchange membranes (2) are tightly pressed onto the frame (1); Step S104, uniformly dispensing hot melt adhesive on the area where the outer edge of the gas diffusion layer (3) contacts the catalyst-coated proton exchange membrane (2); Step S105, drying the surface of the gas diffusion layer (3) after glue application, and attaching and fixing a plurality of gas diffusion layers (3) in groups of two on both sides of the catalyst-coated proton exchange membrane (2).

2. The process for manufacturing a membrane electrode according to claim 1, characterized in that: In the step S101 , the base material is made of polyimide, polyethylene terephthalate, polyethylene naphthalate, polypropylene or polyphenylene sulfide, and the thickness of the base material is 150-350 μm.

3. The process for manufacturing a membrane electrode according to claim 1, characterized in that: The hot melt adhesive used in step S101, step S103 and step S104 is EPDM rubber, silicone rubber, fluororubber, polyolefin rubber, nitrile rubber or chloroprene rubber.

4. The process for manufacturing a membrane electrode according to claim 1, characterized in that: The hot melt adhesive layer (4) in step S101 is covered by screen printing, spraying or pasting a hot melt adhesive sheet, and the thickness of the hot melt adhesive layer (4) is 10-50 μm.

5. A self-bonding membrane electrode, characterized in that: The membrane electrode is prepared by the manufacturing process of any one of claims 1 to 4.

6. A fuel cell module integrated bonding process based on self-bonding membrane electrode, characterized in that: The following steps are involved: Step S201, selecting a portion of the processed graphite separator plates as graphite anode plates (6), and simultaneously selecting a portion as graphite cathode plates (7); Step S202, opening a water seal groove on the upper surface of the graphite anode plate (6) or the lower surface of the graphite cathode plate (7); Step S203, cleaning the surface of the graphite anode plate (6) and the graphite cathode plate (7), and performing drying treatment; Step S204, filling the water seal groove of the graphite anode plate (6) or the graphite cathode plate (7) with a fixed hot melt adhesive (8); Step S205, disposing at least one self-bonding membrane electrode (5) as claimed in claim 5 between the graphite anode plate (6) and the graphite cathode plate (7), and disposing a fixing hot melt adhesive (8) between the graphite anode plate (6) and the graphite cathode plate (7) between every two adjacent self-bonding membrane electrodes (5); Step S206, setting the time, pressure and temperature for the hot pressing equipment so that after the hot pressing operation is set, at least one graphite anode plate (6), the self-bonding membrane electrode (5) and the graphite cathode plate (7) are integrally bonded.

7. The fuel cell module integrated gluing process according to claim 6, characterized in that: The surface cleaning process of the graphite anode plate (6) and the graphite cathode plate (7) in step S203 includes water washing to initially remove impurities, ultrasonic deep cleaning, and plasma technology fine cleaning.

8. The fuel cell module integrated gluing process according to claim 6, characterized in that: In step S203, the graphite anode plate (6) and the graphite cathode plate (7) are dried by natural air drying or by using a drying device.

9. The fuel cell module integrated gluing process according to claim 6, characterized in that: In step S206, the bonding time of the graphite anode plate (6), the self-bonding membrane electrode (5) and the graphite cathode plate (7) is 5-20 minutes, the bonding temperature is 100-190° C., and the bonding pressure is 30 KN.

10. The fuel cell module integrated gluing process according to claim 6, characterized in that: In step S206, the hot melt adhesive (8) is fixed in the water seal groove after the hot pressing process to form a sealing ring.

Citation Information

Patent Citations

  • Packaging method and membrane electrode assembly

    CN112186216A

  • Proton exchange membrane fuel cell stack full-sealing structure and assembling method thereof

    CN114243075A

  • Fuel cell short stack module, fuel cell stack and stack assembling method

    CN114388862A

  • Seals and sealing structures for fuel cells

    CN115064723B

  • A fuel cell membrane electrode assembly

    CN212303729U