Method for producing hardened steel components
By using local heating and cooling measures to control temperature inhomogeneity in the production process of hardened steel parts, the problem of dimensional deviation in the indirect method is solved, and the accuracy and production efficiency of hardened parts are improved.
Patent Information
- Application Number
- CN202380011651.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-29
AI Technical Summary
When producing hardened steel parts in the indirect method, temperature unevenness leads to dimensional deviations, and it is difficult for existing methods to adjust the dimensional accuracy of components in batches separately, affecting production efficiency and quality.
By applying local heating and cooling measures in furnaces, transfer processes and molding hardening presses, the temperature of the component blank is controlled to meet specific maximum temperature differences and component positioning conditions to reduce inhomogeneity within batches and increase the size of hardened components Accuracy.
It effectively reduces temperature inhomogeneity in batches, improves the dimensional accuracy and production efficiency of hardened parts, reduces tolerance deviations, and achieves more economical multi-process production.
Smart Images

Figure CN119053445A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing a hardened steel component.
[0002] In particular, the present invention relates to a method for producing hardened sheet steel parts using the so-called indirect process, for which the applicant has coined the term "form hardening". Background Art
[0003] It is known that high-strength components made of sheet steel, for example for automobile construction, are produced by hardening, in particular by quench hardening or transformation hardening from the austenitic state.
[0004] Quench hardening means heating an item made of a hardenable steel material to a temperature at which its structure is mostly or completely in the form of austenite or gamma-iron, i.e., heating to a temperature above the so-called Ac3 point of the corresponding steel material. Austenite is then transformed into martensite by cooling faster than the so-called critical cooling rate, thereby obtaining high tensile strength.
[0005] Therefore, the steel used in this case is a steel that can be hardened by quenching, such as boron manganese steel of 22MnB5 or 34MnB5 alloy.
[0006] To produce this hardenable steel sheet material, the hardenable steel alloy is melted and usually cast into a sheet ingot using a continuous casting process, which is then hot rolled on a hot strip mill and cold rolled on a cold rolling mill to produce steel strip. The steel strip is usually several hundred meters to more than a thousand meters long, a few millimeters or less than a millimeter thick, and is rolled into so-called coils.
[0007] During hot and cold rolling, the thickness of the plate ingot is greatly reduced, resulting in a corresponding increase in length. However, by appropriate measures, the width is largely maintained. For the purposes of this disclosure, thickness reduction is not considered a forming process.
[0008] It is common practice to galvanize such cold coils in a galvanizing line; for this purpose, the steel strip is unwound from the coil and then rewound up again at the end. The galvanizing can be carried out by hot-dip galvanizing, electrolytic coating or PVD coating. For the purposes of the present invention, galvanized or alloy-galvanized steel strips or sheets are steel strips or sheets with a coating containing zinc or a zinc-based alloy. "Zinc-based" means that zinc is the largest alloy component in the coating, in particular more than 50% of the coating weight. Such cold coils can also be provided with an aluminum-silicon coating or can be further processed without a coating.
[0009] To produce sheet steel components, a steel strip is unwound from a coil and components are cut from the strip, which are called slabs. These slabs are therefore flat steel sheets of limited dimensions. To produce hardened sheet steel components, these slabs can be further processed in two ways.
[0010] In the so-called direct method (also called press hardening process or press hardening), the blank is usually austenitized by heating in a furnace and then hot formed into a sheet metal component in a relatively cold tool (press hardening tool), usually in just one step. As soon as the hot forming has taken place and the tool is completely closed, the tool surface comes into contact with the sheet metal component. This causes heat to be dissipated into the usually cooled tool at a rate above the critical hardening rate, so that the above-mentioned hardening is achieved by transformation into a martensitic structure. In press hardening, steel strips with aluminum silicon coatings, galvanized or alloy galvanized steel strips or uncoated steel strips are usually used. Since in pressing only one tool can be used for forming and hardening, the final finishing (i.e. final finishing of the outer edges and hole edges) can only be carried out after the formed and hardened component has been removed from the tool. This is usually carried out in an additional process step with the aid of laser cutting. In principle, the dimensional accuracy of the final trimming is decoupled from that of the geometry after hardening. However, laser cutting makes it difficult to pick up the components correctly and evenly in terms of dimensional accuracy, and is time-consuming and costly, especially in the case of large trimming lengths, a large number of holes, short cycle times or high output, multi-step production and large batch sizes.
[0011] In the so-called indirect method, also called form hardening method or form hardening (FH), a cold sheet blank is formed into a component blank in a typical multi-step forming and finishing process, usually mainly by a combination of deep drawing, finishing and / or post-forming, collectively referred to herein as cold forming (CF), in a cold forming tool set, for example, comprising three to five individual tools, collectively referred to herein as cold forming tools. The component blank is then usually austenitized in a furnace and, while still hot, inserted into a usually cooled tool (form hardening tool), which is usually placed on a usually spring-loaded support device (also called lifting device) that is located in the form hardening tool and displaced by the upper part of the press to prevent uncontrolled cooling of the component blank from the time of insertion into the form hardening tool to the time of closing the form hardening tool. Normally, the form hardening tool no longer performs any actual forming during the closing process, but this is possible to a small extent in the case of spring-loaded component blanks and / or final forming procedures. As soon as the tool is completely closed, the tool surface contacts the surface of the component blank and dissipates heat from the blank surface at a rate above the critical hardening rate, causing the component blank to harden and form the component. Form hardening usually uses galvanized steel strips, but in principle uncoated steel strips can also be used. However, steel strips with an aluminum silicon coating cannot be form hardened, because the aluminum silicon layer is very brittle at room temperature and the coating will peel off during the cold forming process. During form hardening, (laser) trimming in the hardened state is usually no longer necessary, because the final trimming is usually already completed as part of the cold forming; of course, (laser) trimming in the hardened state is also feasible to a small extent, for example, for individual holes with particularly high precision requirements, which will incur corresponding additional costs.
[0012] In both cases, i.e. in the direct method and in the indirect method, the product is a hardened, finally trimmed steel sheet component, wherein in the direct method the final trimming is carried out after hot forming and hardening, i.e. on the hardened component, while in the indirect method the trimming is carried out as part of the cold forming of the component blank and therefore before hardening.
[0013] In both cases, the steel undergoes several changes in volume or length in all spatial directions, starting from the state before heating until the insertion of the corresponding tool, a situation that is particularly important for the component blank in the indirect method. In principle, these changes in length can be described on the basis of dilatometer curves, i.e. on the basis of the temperature-elongation curve of the steel sample used, e.g. Figure 1As shown: In the furnace, thermal expansion (a) occurs first until the onset of austenitization, followed by contraction (b) during the structural transformation to austenite, and then thermal expansion (c) occurs again before further heating out of the furnace, after which, during the transfer from the furnace to the forming hardening tool, corresponding contraction (d) occurs and cooling to the corresponding insertion temperature occurs. For the purposes of the present invention, the insertion temperature in the indirect method is the average temperature of the component blank after insertion into the tool and shortly before reaching the bottom dead center of the tool or press, calculated weighted according to its surface proportion. The transfer between furnace and tool usually takes place in ambient air, and the cooling to the corresponding insertion temperature depends in particular on the radiative heat losses and the heat losses due to forced and free convection. The above-mentioned heat losses in turn depend in particular on the transfer time, the sheet thickness, the surface emissivity, the geometry (due to self-radiation effects) and the air flow during the transfer. Based on the ratio between the length at the insertion temperature and the length before the start of heating, in the indirect method it is possible to at least approximately determine the extent to which the cold forming tool for producing the component blank must be reduced, i.e. made smaller in all spatial directions, so that the component blank produced by the cold forming tool can fit onto the form-hardening tool when the press is closed after heating in the furnace and subsequent cooling during transfer from the furnace to the form-hardening tool.
[0014] Since in the above-mentioned indirect method no final trimming is performed after hardening, in order to ensure the dimensional accuracy of the component in the indirect method, the austenitized component blank must be inserted into the form-hardening tool at the correct temperature and thus at the correct size, i.e. it must fit, and then hardened when the press is closed. If the insertion temperature is too high and the component blank is therefore too large, the outer trim of the hardened component will generally be too large and the hole shape will be correspondingly deformed. If the insertion temperature is too low and the component blank is therefore too small, the outer trim of the hardened component will generally be too small and the hole shape will be correspondingly deformed. In addition, inserting a component blank that is too large or too small into the form-hardening tool can lead to further problems. For example, if the component blank tilts on the centering pin or if unwanted post-forming occurs in susceptible areas of the component blank (usually the side wall area), this can lead to so-called component misalignment, which can lead to production interruptions or even tool damage.
[0015] In the case of zinc-coated steel sheets, component blanks that are too large or especially too small when inserted into the form-hardening tool can also cause undesirable microcracks to appear in the steel substrate due to so-called liquid metal embrittlement (LME) as a result of post-forming when the form-hardening tool is closed.
[0016] In addition, when the component blank is inserted at an inappropriate insertion temperature, further dimensional deviations, especially the side wall angles, may occur due to changes in local cooling conditions of the tool, especially in the positive and negative radius areas, as well as the result of torsion.
[0017] For reasons of economy, form-hardened components are usually not hardened individually in a form-hardening press, which is very large. Instead, as part of so-called multi-step production, a number of components are usually form-hardened together as a so-called "batch" in order to produce as many components as possible per stroke and thus per unit time and to make maximum use of the size of the press table. Figure 2 The sequence of the method described above is shown in a highly simplified form and how, for example, a batch of four CF parts can be heated to a temperature above Ac3 in a continuous furnace, in which case these parts are adjacent to each other in the direction of movement and are inserted together as a batch of austenitized parts via a transfer device into a form-hardening tool in a form-hardening press and subsequently form-hardened together.
[0018] For the sake of clarity, it should be stated that in continuous furnaces, the expressions "adjacent to one another in the direction of movement" and "one after another in the direction of movement" refer only to the arrangement of the components within a batch. Furthermore, "adjacent to one another in the direction of movement" means that no components in the batch are one after another in the direction of movement. An adjacent arrangement of components in the direction of movement usually occurs in components whose longitudinal axes are essentially parallel to the direction of movement, i.e. the longest axis determining the direction of movement of the components is essentially parallel to the direction of movement. For furnaces without a direction of movement, such as multi-layer chamber furnaces, the statements about the arrangement of components refer accordingly to the conveying direction, i.e. the loading and unloading direction.
[0019] In the multi-step production of form-hardened tools, there are several variants, sometimes with great differences, e.g. Figure 3 shown.
[0020] In the case of multi-step production, on the one hand, there are considerable differences depending on whether the form-hardened tools carry out so-called identical component production, which is particularly relevant with regard to the usual quality requirements, especially in vehicle construction.
[0021] The production of identical parts in a form-hardening tool occurs when more than one form-hardening tool cavity is used for the same hardened part, i.e. two or more identical parts are hardened in each stroke of the form-hardening tool.
[0022] If there is only one form-hardening tool cavity per hardened part in the form-hardening tool, for example one part of the first type and one part of the second type, such as the B-pillar on the left and the B-pillar on the right of the vehicle, then in this example, multi-step production (i.e. double production) actually occurs. If there is only one part of the first type, i.e. the B-pillar on the left (FH-L), and one part of the second type, i.e. the B-pillar on the right (FH-R), then there is indeed multi-step production, but not production of identical parts. This is usually the case for space reasons for relatively large and bulky parts, such as the B-pillars on the left and right sides of the car.
[0023] If there are two tool cavities for each hardened part in the form-hardening tool, for example one part of the first type and one part of the second type, such as a rocker panel on the left side of the vehicle and a rocker panel on the right side, this is quadruple production, with two identical parts of the first type, in this case the two rocker panels on the left side (FH-L1 and FH-L2), and two identical parts of the second type, in this case the two rocker panels on the right side (FH-R1 and FH-R2). This is usually the case for relatively large parts with narrow shapes, such as rocker panels, or for smaller parts of any suitable geometry on the left and right side of the vehicle. For reasons of symmetry, force flux and tool deflection, the left and right parts are usually mirror-symmetrical to a large extent, so L1-R1 and L2-R2 are usually placed next to each other.
[0024] For automotive parts without left-right variations, such as center tunnels, in order to maximize the use of the press table size, it is theoretically also possible to produce them in quadruplicate with four identical parts (FH-1, FH-2, FH-3 and FH-4), or in sextuple with six identical parts, etc. However, this can lead to tolerance problems due to the high dimensional accuracy requirements of identical parts.
[0025] There is usually no visual difference between identical parts and they are usually not sorted by cavity in the loader for subsequent vehicle construction, i.e. identical parts in the loader are mixed together and transported to vehicle construction for further processing without being sorted.
[0026] Similar to cold-formed parts, hardened parts for vehicle construction are also important, mainly for reasons of connection and dimensional accuracy. The parts must not only be within the specified dimensional tolerances, but also show a certain consistency within the specified tolerances. Ensuring this is even more demanding for identical parts, because in addition to the deviations within a single cavity, the maximum deviations between cavities are also relevant.
[0027] from Figure 4 This relationship can be seen in , which shows the deviation of the same part within a single cavity as well as all the deviations between cavities.
[0028] In principle, as the number of identical parts in multi-step production increases, the requirements for dimensional accuracy of the produced parts also increase, leading to additional tolerance restrictions and problems.
[0029] As mentioned at the beginning, in the indirect method, the austenitized component blank must be inserted into the form-hardening tool at the optimum temperature to achieve the optimum dimensions. If the temperature is too high, resulting in an inserted component blank that is too large, this can usually be corrected by increasing the transfer time between the furnace and the press, thereby reducing the insertion temperature.
[0030] If the temperature is too low and the inserted component blanks are therefore too small, the transfer time between the furnace and the press is usually shortened accordingly. It should be noted here that extending or shortening the transfer time between the furnace and the press always affects the entire batch. Therefore, a change in the transfer time cannot be used to correct the dimensional accuracy of a single component in the respective batch, because all components in the batch will be affected.
[0031] On the other hand, another significant difference in multi-step production depends on whether each cavity of the form-hardening tool receives its component blank from a cavity specifically assigned to the cold-forming tool, or whether multiple form-hardening tool cavities share one cold-forming tool cavity, which is particularly relevant for the influence of (trimming) corrections in the cold-forming tool cavity on the hardened part coming from the form-hardening tool cavity. Figure 3 Some production combinations of CF and FH are illustrated.
[0032] If each cavity of the form-hardening tool receives its component blank from a specially designated cavity of the cold-forming tool, for example, component blanks for the left and right B-pillars are produced in each stroke of the cold-forming and the left and right B-pillars are introduced into the furnace as a batch, transferred to the form-hardening tool and then hardened together there, then any dimensional deviations of the individual hardened components of each batch (for example the left B-pillar) can be corrected by adjusting the specially designated cavity of the cold-forming tool.
[0033] If several form-hardening tool cavities share one cold-forming tool cavity, for example if component blanks for a left and a right rocker panel are produced in each cold-forming stroke, but two left and two right rocker panels are passed through the furnace as a batch, transferred to the form-hardening tool and hardened together there, then it should be noted that an adjustment of the cold-forming tool cavity affects all components in the relevant form-hardening cavity, which means that it is not possible to carry out targeted corrections only for the individual hardened components in the respective batch.
[0034] Although in theory each form-hardening tool cavity can receive its component blank from a specially assigned cavity in the cold forming tool when producing the same component, when producing the same component in a form-hardening tool, for logistical and cost reasons, several form-hardening tool cavities usually share one cold forming tool cavity, i.e. for economic reasons and to prevent confusion, more than one form-hardening tool cavity is usually used in each cold forming tool cavity to achieve multi-step production of the same component.
[0035] In practice it has been found that temperature non-uniformities within a batch when the press is closed, due to furnace heating, transfers between furnace and press or other reasons, can lead to dimensional deviations between batches of parts. Therefore, for tolerance reasons, especially in the case of production of identical parts, economical multi-step production is not implemented, although it is feasible due to the existing press table dimensions and press pressures. Summary of the invention
[0036] The object of the present invention is to provide a method for producing hardened steel components which method allows the dimensional accuracy of the produced components to be increased and the production to be more economical.
[0037] This object is achieved by a method having the features of claim 1 .
[0038] Further advantageous embodiments are disclosed in the dependent claims.
[0039] The inventors have found that temperature non-uniformity within a batch and within a part can lead to undesirable dimensional deviations. The inventors have also found that, for the reasons mentioned above, varying the transfer time between the oven and the press cannot be used to influence individual parts within a batch.
[0040] Furthermore, the inventors have found that the inhomogeneities are generated by the process itself and that overlapping effects also occur in this respect. According to the invention, the inventors have also found that exerting influence by changing the cold forming tool is not advantageous in all cases from a practical point of view, since this is the most expensive means and is not always sufficient.
[0041] The solution of the present invention is to reduce or even eliminate the inhomogeneities within the batch, which can be achieved in at least three determined influence areas, namely firstly in the furnace, secondly during the transfer from the furnace to the form-hardening tool, and thirdly in the form-hardening press, from the insertion of the form-hardening tool to the closing of the press or the form-hardening tool.
[0042] In this case, the inhomogeneities of each affected area can be treated in the respective affected area, or alternatively or additionally, the inhomogeneities that first appear in the subsequent area can be treated. For example, during furnace heating, the temperature of the component blank can be deliberately set locally higher to compensate for the local cooling that occurs during the subsequent transfer process until the press is closed.
[0043] In furnaces, this can be influenced on the one hand by the nature of the component arrangement and on the other hand by local heating, in particular in the last furnace zone of a continuous furnace or in the furnace of a chamber furnace.
[0044] Furthermore, during the transfer from the furnace to the form-hardening tool, influences can be exerted using devices mounted on the manipulator or the transfer tool, such as preventing cooling of certain areas by means of wind shields and / or local reflectors and / or cooling of certain areas by means of local blowing devices. Furthermore, a tempering station with local blowing devices can be provided, in front of which the batch is placed during the transfer from the furnace to the form-hardening tool. When taking cooling measures, care must be taken to ensure that the component blank does not develop an undesirable external structure.
[0045] It is also possible to exert influence in the press, for example by means of localized blowing, from the time the form-hardening tool is inserted until the press is closed, ie until the closing of the form-hardening press is complete.
[0046] The invention therefore relates in particular to a method for producing a hardened steel component, wherein a flat steel sheet blank is cut from a flat steel strip made of a quench-hardenable steel alloy, the steel sheet blank is formed into a component blank in a cold forming process and subjected to complete or substantial final trimming, the resulting component blank is then heated in a heating device to a temperature at which the steel material partially or completely transforms into austenite, the component blank is then transferred from the heating device to a form-hardening press and inserted into a form-hardening tool, cooled at a rate above the critical hardening rate and thus hardened, wherein, in order to improve the dimensional accuracy of the hardened component, in particular the dimensional accuracy of the outer trimming and the hole shape, at least one of the conditions a) to c) is met:
[0047] a) The maximum temperature difference of the component blanks in the batch, taking into account each component blank individually and all component blanks in relation to each other, before the closing of the form hardening press is completed is Δθ, where:
[0048]
[0049] in, is the shape constant in K*m, L max is the maximum dimension of the largest blank in the batch measured in m. The following values apply depending on L max The shape constant
[0050] From L max Starting from greater than 1m: in particular Best Especially preferred
[0051] From L max Starting from 0.5m: Best Especially preferred
[0052] b) component blanks in a batch, including components of a first type and components of a second type, are positioned in the furnace in such a way that at least a portion of the first type of component is positioned directly next to at least one second portion of the first type of component and a portion of the second type of component is positioned directly next to at least one second portion of the second type of component, respectively;
[0053] c) in a batch of component blanks consisting of a first type of components and a second type of components, the cold-formed dimensions or three-dimensional shapes of the first type of components and the second type of components are different due to differences in thermal expansion, and / or the cold-formed dimensions or three-dimensional shapes of at least one type of components are different, so that any dimensional differences are substantially compensated when the form-hardening press is closed.
[0054] The maximum temperature difference Δθ for condition a) depends on the dimensions of the component blank and is therefore expressed in a formula. Depending on customer requirements, smaller or larger tolerance ranges are permitted for the hardened component; this can be achieved by selecting the shape constants The shape constant D is considered as a function of the maximum dimension of the component blank. In this case, the shape constant D applies only to component blanks with a maximum dimension greater than 1000 mm. The other shape constants are used for component blanks with a maximum dimension greater than 500 mm.
[0055] The following is a calculation example: For a component blank with a maximum size of 1100 mm, When the maximum allowable temperature difference or the maximum allowable temperature difference is 106.7K; when When the maximum temperature difference is 59.3K; when When the maximum temperature difference is 39.5K; when The narrowest tolerance, which produces the best results, has a maximum temperature difference of 19.8K.
[0056] Generally speaking, it should be noted that in condition a), the temperature of the component blank within the batch refers to both the temperature of the entire surface of the component blank and the temperature of the entire surface of all component blanks within the batch. The maximum temperature difference, i.e. the maximum difference in the temperature of the component blanks in the batch, is the difference between the highest temperature and the lowest temperature.
[0057] According to another embodiment, under a), the component blank or the component blank region which is cooler when the form hardening press is closed is additionally heated in the furnace. The heating is preferably carried out using locally controllable heating elements such as electric radiant heaters. In this case, the temperature of the cooler region in the furnace can reach the temperature of other regions and, if necessary, even exceed the temperature of other regions in order to compensate for inhomogeneities resulting from the subsequent transfer. Advantageously, the adjustment of the additional heating can be carried out simply, flexibly and reproducibly.
[0058] According to another embodiment, under a), the component blank or the component blank region which is at a higher temperature when the form hardening press is closed is actively cooled during the transfer process. Advantageously, the active cooling can be adjusted simply, flexibly and reproducibly.
[0059] According to another embodiment, under condition a), the component blank or the region of the component blank which is cooler when the hardening press is closed is largely protected from cooling during the transfer process, in particular heat losses due to forced convection and / or heat radiation, preferably by using draft shields and / or reflective panels. Advantageously, the work of preventing cooling can be carried out simply and reproducibly.
[0060] According to another embodiment, under a), before the hardening press is closed, the component blank or the component blank region which is hotter when the hardening press is closed is actively cooled in the press. Advantageously, the active cooling can be adjusted simply, flexibly and reproducibly.
[0061] According to another embodiment, under condition b), in a batch consisting of components of the first and second types, the components of the first and second types are positioned adjacent to and successively to each other in a direction of travel or conveyance through the furnace, respectively.
[0062] According to another embodiment, the component blanks within a batch are located adjacent to each other in the furnace in the direction of travel or conveying of the furnace.
[0063] According to a further embodiment, the component blank or a region of the component blank close to the exit door is additionally heated in a heating device.
[0064] According to another embodiment, the component blank from one cold forming cavity is hardened in at least two different forming hardening tool cavities. This has the advantage of improving the economy of the method and eliminating the risk of confusion when selecting the component blank.
[0065] According to another embodiment, at least two of the conditions a) to c) are met, in particular all three conditions. Each of the three conditions a) to c) is related to improving the dimensional accuracy of the hardened component, and each condition considered alone is an improvement. However, if two of the three conditions are met, i.e. conditions a) and b) or a) and c) or b) and c), the dimensional accuracy of the hardened component can be further improved. If all three conditions are met, the best dimensional accuracy and the lowest tolerance deviation of all hardened components within a batch can be ensured.
[0066] According to another embodiment, the component blank is placed on a support device, in particular a lifting device, in the form-hardening tool to prevent uncontrolled cooling of the component blank from the insertion to the closing of the form-hardening tool before the hardening process. This can constitute a simple, robust and reproducible method to control and reduce the cooling of the component blank as much as possible when inserting the component blank into the forming tool. When the press is closed, the spring-loaded lifting device can be retracted into the forming tool, thus ensuring a safe shutdown and low temperature loss.
[0067] According to another embodiment, the steel sheet blank used is a blank with a metal anti-corrosion layer, in particular a metal anti-corrosion layer based on or made of zinc. This has the advantage that good anti-corrosion protection, in particular cathodic anti-corrosion protection, can be ensured.
[0068] According to another embodiment, the steel strip is made of a hardenable steel alloy, in particular boron manganese steel.
[0069] According to another embodiment, the steel used is a material that retards the austenite-martensite transformation during cooling, wherein the steel strip is hot rolled or cold rolled.
[0070] According to another embodiment, the steel strip used has the following composition (all figures are in wt %):
[0071]
[0072] Residual iron and impurities
[0073] According to another embodiment, the device comprises a cold forming tool, a furnace, a transfer device for transferring the component blank and a form-hardening tool, wherein a supporting device, in particular a lifting device, is provided in the form-hardening tool to prevent uncontrolled cooling of the component blank from the time of insertion into the form-hardening tool until the closing of the form-hardening tool before the hardening process. This results in a simple, robust and inexpensive device for controlling and minimizing the cooling of the component blank during its insertion into the forming tool. When the press is closed, the spring-loaded lifting device can be retracted into the forming tool, which ensures a safe shutdown and low temperature losses. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] The present invention will be described below with reference to the accompanying drawings. In the accompanying drawings:
[0075] Figure 1 : shows the dilatometer curve of a steel sample that can be hardened by quenching;
[0076] Figure 2 : is a highly schematic diagram of the form hardening method, using a continuous furnace and linear transfer for quadruple production, with four parts per batch, the parts being adjacent to each other in the direction of movement;
[0077] Figure 3 : Shows the known procedures for multi-step production in vehicle manufacturing from cold forming, form hardening to handover or delivery, as well as the corresponding component quality requirements;
[0078] Figure 4 : This graph shows the deviation of the same part within a single cavity and between all four cavities during the production of the same part;
[0079] Figure 5 : shows examples of non-uniformities identified from a furnace and the transfer between the furnace and the press according to the present invention;
[0080] Figure 6 : Shows the effect of non-uniformity due to component size and component arrangement;
[0081] Figure 7 : shows a comparison of component arrangements according to the prior art and according to the invention, and the respective effects on output and dimensional deviations within the same component;
[0082] Figure 8 : A schematic diagram showing a comparison of a component arrangement according to the prior art and according to the invention, and the respective influence on the dimensional deviations of the same component and on the deviations of the same component after adjusted cold forming;
[0083] Fig. 9 : is a highly schematic diagram of heating in a continuous furnace and a multi-layer box furnace according to the present invention;
[0084] Fig.10 : shows the measures taken during the transfer process according to the present invention;
[0085] Fig.11 : shows the local blowing performed in a press according to the present invention;
[0086] Fig.12 : shows the arrangement and treatment of the same components on a non-specific side according to the present invention;
[0087] Fig.13: shows the maximum temperature difference in a batch as a function of the largest part blank size in the batch for four different shape constants. DETAILED DESCRIPTION
[0088] Figure 1 The dilatometer curve, i.e. the temperature-elongation curve of a heated and subsequently cooled sample made of quench-hardened steel, is shown. To determine the dilatometer curve, the sample is inductively heated at a heating rate as close as possible to that used in batch production and, if necessary, cooled by blowing air over the induction coil. The resulting length change of the sample as it heats and cools is detected by a measuring needle and a displacement sensor. The temperature of the dilatometer is controlled by thermocouples on the sample surface. The result of the measurement is the temperature-length change recorded during the entire measurement, the dilatometer curve. The plotted dilatometer curve provides information on the length or volume change of the cold-formed component blank during the time in the furnace and during the subsequent transfer from the furnace to the form-hardening tool until the form-hardening tool is closed. In the furnace, thermal expansion first occurs (a) until the start of austenitization, followed by contraction during the structural transformation to austenite (b), followed by another thermal expansion during further heating until leaving the furnace (c), followed by a corresponding contraction after leaving the furnace (d), i.e. during the transfer from the furnace to the press-hardening or form-hardening tool, cooling to the corresponding insertion temperature. For the purposes of the present invention, the insertion temperature in the indirect method is the average temperature of the component blank after it has been inserted into the tool and shortly before it reaches the bottom dead center of the tool or press, weighted according to its surface proportion. Based on the ratio between the insertion length (i.e. the length at the insertion temperature) and the initial length (i.e. the length before heating), it can be determined to what extent the cold forming tool for producing the component blank must be reduced in order to transfer it to the form-hardening tool after heating in the furnace and subsequent cooling, to which they are adapted.
[0089] Figure 2 The upper part of the diagram shows a highly schematic diagram of the form hardening method, in which a flat steel strip is unwound from a coil, from which a sheet blank is cut, which is formed in a cold forming process, usually in a multi-step forming and trimming process, with the outer trimming and the hole profile being subjected to a final trimming. The component blank produced in this way is then placed in a furnace, removed from the furnace in a hot state, and placed in a form hardening tool, which is rapidly cooled by applying upper and lower tools to the formed component.
[0090] like Figure 2 The individual components shown in the lower part do not pass through the furnace one after another, but in order to increase the output and operate the method as economically as possible, several component blanks are introduced into the furnace and Figure 2In the example shown, four components are then removed from the furnace simultaneously and inserted into the form-hardening tool (preferably in the same arrangement) in the direction of travel and hardened. As mentioned above, the contour of the entire component, i.e. the three-dimensional shape including the outer cut edges and the hole pattern, must be adapted when the heated component blank is inserted into the form-hardening tool, because corrections are no longer possible afterwards.
[0091] Figure 3 The conventional production and tool cavity combinations for cold forming (CF) and form hardening (FH) are shown, along with the quality requirements that usually result from this. As the number of identical parts in multi-step production increases, the requirements for dimensional accuracy of the produced parts also increase, which leads to additional tolerance restrictions.
[0092] In the first case, for example for relatively large and bulky components such as the two B-pillars on the left and right sides of a car, each hardened component has only one tool cavity in the form-hardening tool. In this case, form-hardening does require repeated production, but not the production of identical components. Since there is no production of identical components, standard quality requirements apply to the hardened components. In this case, each cavity of the form-hardening tool receives the component blank from a specially designated cavity of the cold forming tool, so that any necessary corrections, such as scaling and / or trimming, can be made to the finished product already after hardening in the respective CF cavity.
[0093] With two hardened parts per stroke, the output is relatively low. For further processing in vehicle construction, the hardened parts are usually divided into right-hand and left-hand parts and separated from each other in this way before being transported in a loader.
[0094] therefore, Figure 3 The top row of describes the situation of multi-step production, where the components are different depending on the side, i.e. left-specific components and right-specific components. This could be, for example, a left-hand and a right-hand B-pillar. In this case, there is one cavity per component during cold forming and one cavity per component during form hardening. In other words, strictly speaking, the cold-formed left-hand part is subsequently form hardened in the corresponding left-specific mold, and the same applies to the right-specific part.
[0095] In the multi-step production of the same part ( Figure 3), only one cavity is required per component during cold forming; two or more cavities can be required per part during form hardening. In the example shown in the figure, for example, form hardening has two or more tool cavities, one for each rocker panel on the left and right side of the vehicle; thus, at least two identical parts can be produced at least four times. This is usually the case for relatively large but narrow components, such as rocker panels, or for smaller components of any suitable geometry on the left and right side of the vehicle. For further processing in vehicle construction, these hardened parts are usually also divided into right-hand and left-hand parts only and delivered in this way separated from each other in a loader. In this case, the quality requirements increase; the quality requirements increase with the number of identical parts. On the one hand, the consistency of each component on the left and right side must be ensured, on the other hand, the requirements for identical parts are higher, because in addition to the deviations within the individual cavities, the maximum deviations between the cavities are also important. From Figure 4 This can also be seen in .
[0096] For automotive parts that do not vary left to right ( Figure 3 In order to fully utilize the dimensions of the press table, it is theoretically also possible to carry out, for example, quadruple production of four identical parts or sextuple production of six identical parts, etc. However, due to the high dimensional accuracy requirements of the identical parts, this can lead to tolerance problems.
[0097] The inventors have found that the tolerance deviation in the above method may be caused by a variety of reasons ( Figure 5 ).
[0098] About furnace and transfer ( Figure 5 ), the parts guided in the furnace and close to the furnace door have a hotter side and a cooler side, and the direction of temperature drop is toward the furnace door.
[0099] The same phenomenon also occurs during the movement outside the furnace during transfer to the form-hardening tool, i.e. due to the movement-induced airflow (air flow) and the accompanying forced convection, the area of the formed and heated component that was previously close to the furnace door and transferred out of the furnace first and is located at the front with respect to the movement direction is cooled more intensively, thereby further strengthening this effect.
[0100] also( Figure 5 lower left), such as Figure 5 As shown in the schematic diagram at the bottom left, the local cooling effect of the furnace rack where the component is located can also be observed.
[0101] Therefore, these effects may overlap with each other and apply not only to the continuous furnace and linear transfer shown in the figure, but also to the multi-layer box furnace and non-linear robot transfer not shown in the figure.
[0102] In general, the absolute length deviation at temperature deviation is proportional to the workpiece size, i.e. an incorrect deviation in the insertion temperature will have a more serious effect on large or long workpieces than on small or short workpieces. The layout of the furnace also has an influence.
[0103] superior Figure 6 It shows how relatively short parts next to each other in the direction of travel experience a temperature drop in the direction towards the furnace door. In this case, the absolute length deviation is low to medium, because the parts are only short to medium in length, and in this direction the temperature profiles and therefore the deviations are identical between the parts. If such parts are produced in large series, this length variation can even be taken into account in the cold forming tool and the cold forming tool proportions can be adjusted accordingly, so that no finishing work is required later, which is also economically feasible.
[0104] Temperature curve Figure 6 Shown at top.
[0105] The situation is completely different if the components pass through the furnace one after another in the direction of travel, for example because they are particularly long workpieces.
[0106] Figure 6 The bottom part of the diagram shows the temperature profile, i.e. the different temperatures of each component.
[0107] Due to different temperatures and the associated expansion, the parts have different lengths, so the absolute length deviations within a component group are moderate to high and increase with increasing component length. As a result, the temperatures of the components are usually different and the individual deviations are also different. Therefore, the correction of these same parts in the cold forming process is inherently problematic.
[0108] According to the invention, the components, in particular in the area of the furnace, the transfer device and the form hardening tool, are acted upon in such a way that batch inhomogeneities are eliminated or reduced, in particular temperature deviations are kept below the respective maximum temperature difference. For this purpose, a general approach is to influence the type of arrangement of the components during the heating process, if necessary by means of local heating in the last furnace zone of a continuous furnace or in the furnace chamber of a multi-layer chamber furnace.
[0109] During the transfer process, the heat can be kept in a certain area or blown locally by blocking the air flow or by partial reflectors. The partial reflectors can also be adjusted by different distances, perforations, production burrs, etc.
[0110] It is also possible to influence the entire process in the press from insertion to closing by means of local air blowing or, if necessary, using infrared heaters.
[0111] Figure 7The effects of component arrangement in the prior art and the effects of component arrangement in the present invention are shown.
[0112] In the prior art, usually in a double and quadruple arrangement, one left and one right component are produced in the cold forming tool. In a double conveyor system, these left and right components also pass through a furnace and are then fed into the form hardening tool. Usually, in order to correct for left-right deviations in the finished component, different left-right scaling can be provided in the cold forming tool, for example the right side is larger than the left side. Since there are no identical parts, the overall process places relatively low demands on tolerances. However, in this case, the disadvantage is that only two components can be produced per stroke.
[0113] In the quadruple yield of the prior art ( Figure 7 Middle row), for example, two parts, i.e. left and right, are produced in a cold forming tool and then placed in the furnace in the order left one, right one, left two, right two, through which they are transferred to the form-hardening tool and then form-hardened accordingly in the form-hardening tool.
[0114] Although the output is indeed high as four parts are produced per stroke, the tolerances are very high as two identical parts are produced per stroke. As the temperature drops towards the furnace door, there are often large differences between identical parts, which often exceed the tolerance range that can still be tolerated. Figure 8 The top row shows the temperature distribution in the arrangement and the corresponding deviations of identical parts. General deviations between left and right can be adjusted by cold forming, but differences between identical parts cannot be adjusted here.
[0115] According to the quadruple production of the present invention ( Figure 7 Bottom row), the left and right parts are produced in cold forming, but instead of being placed alternately in the furnace, identical parts are placed next to each other in the furnace and correspondingly next to each other in the form-hardening tool. The advantage of this is a high output. As the temperature drops in the direction of the furnace door, the differences between identical parts also become smaller. In this case, the tolerance requirements are also very high, because there are two identical parts in each case. Overall, however, this method allows for better control, such as Figure 8 As shown in the lower middle part, the relative differences between the same parts are not high, and, as Figure 8 As shown in the lower right, the differences between identical parts can be significantly reduced by adjusted cold forming. Thus, according to the invention, this measure already allows a very large comparative uniformity to be produced.
[0116] therefore, Figure 8A comparison of the component arrangement according to the prior art and the component arrangement according to the invention is shown in the form of a schematic diagram, as well as the respective effects on the dimensional deviations of the same component and the deviations of the same component by adapted cold forming. It is clear that the length deviations when producing the same component according to the prior art are much greater than those of the method according to the invention. The component arrangement according to the invention can reduce the length deviations accordingly, which is also the case with adapted cold forming (right figure).
[0117] like Fig. 9 Another possibility according to the invention is to heat the components in the furnace, i.e. close to the furnace door, more intensively by means of corresponding additional heating elements. For example, local heating can be carried out in the last zone of a continuous furnace or in the furnace chamber of a multi-layer chamber furnace in order to eliminate or reduce batch-wide inhomogeneities that occur in the furnace or during the transfer to press closing during the form hardening process.
[0118] Specifically, this does not mean that the parts are heated differently in order to give them different properties later, as is well known; rather, the aim is to transfer the parts from the furnace with uniform heat, or to heat the parts that have cooled more during the transfer to a greater extent, so that when the press is closed, the parts are at the same temperature in the form-hardening tool.
[0119] This measure can, of course, be combined with the above-mentioned measure of arranging the components in the furnace. This would therefore also make adjusted cold forming obsolete, especially if the cold forming tool is already present and the adjustment is carried out in an ongoing process.
[0120] Alternatively or additionally, Fig.10 As shown in the top row, the parts transferred together from the furnace to the form-hardening tool can be protected from forced convection caused by "drafts" during the transfer process by corresponding partial or full covering hoods (also called wind shields). This is very useful, for example, if all parts have a very uniform temperature when they come out of the furnace.
[0121] If the parts come out of the oven at different temperatures, then Fig.10 As shown in the middle row, components or areas that usually cool more or come out of the furnace at a lower temperature can be kept warm by corresponding reflectors, which can also be adjusted by perforations or different emissivity, while components that cool less or come out of the furnace at a higher temperature can be cooled by convection.
[0122] In addition, as follows Fig.10 As shown, the parts that are more strongly heated can also be cooled by blowing air, and the blowing volume, blowing distance, etc. can be adjusted.
[0123] Alternatively or additionally, such as Fig.11As shown, the form-hardening tool or form-hardening press can also influence the temperature of the component until the tool is finally closed. For example, hotter components or areas can be cooled by blowing air. In this case, the component is still supported on the spring-loaded lifting device before the press is closed and can be cooled relatively well by blowing air. Alternatively or in addition, the component can also be heated from the outside as required by using infrared heaters (not shown in the figure), so that the temperature of the component or area is maintained, or at least cooled less.
[0124] Fig.12 The difference to the prior art is summarized again in that the components are not left-right specific but are identical from the outset, such as central channels positioned one behind the other in the direction of travel. In this case, the number of identical components is greater in order to achieve economical production and corresponding quality, and therefore the need for homogenization is also greater.
[0125] When producing four identical parts according to the prior art, the production volume is very high and the tolerance requirements are very high, because in this case there are four identical parts and corrections are not possible during the cold forming process for the reasons mentioned above. The prior art virtually excludes such a four-part production.
[0126] According to the invention, the above-mentioned furnace, transfer and form hardening tools can be influenced. Thus, high production capacities of four parts per stroke can be achieved and can only be controlled by the above-mentioned measures. Here, too, the tolerance requirements are very high and corrections in the cold forming tool are not possible.
[0127] Thus, an advantage of the present invention is that many parts can be economically produced using the same components in designated and undesignated locations.
[0128] The benefits of this are, firstly, that tolerances can be kept low, thereby reducing scrap.
[0129] Fig.13 The maximum temperature difference Δθ in a batch with four different shape constants is depicted graphically as a function of the maximum dimension of the corresponding component. For this purpose, the calculation is based on the maximum dimension of the largest component blank within the batch, for example 1800 mm. This results in four different shape constants and thus different component tolerances. In addition to the maximum dimension of the largest component blank within the batch, these maximum temperature differences also depend on the shape constant and are inversely proportional to the dimension. The function with the shape constant D, represented in the figure by ΔTHETA_D, has the highest tolerance, while the function with the inserted shape constant A, ΔTHETA_A, has the lowest tolerance and produces the most accurate component geometry. It should be noted in this regard that the shape constant D is only valid for component blanks with a maximum dimension greater than 1000 mm. The other shape constants are also valid for component blanks with a maximum dimension greater than 500 mm.
[0130] In the example with a longitudinal dimension of 1800 mm, the maximum temperature ∆ when the press is closed results in the following values for the shape constants:
[0131] Shape constant A: △θ_A_1800mm=12.1K
[0132] Shape constant B: △θ_B_1800mm=24.2K
[0133] Shape constant C: △θ_C_1800mm=36.2K
[0134] Shape constant D: △θ_D_1800mm=65.2K
[0135] This means that, according to the invention, both the individual temperatures of the component blanks and the overall temperature in a batch must be within this wide temperature range.
Claims
1. A method for producing a hardened steel component, wherein a flat steel sheet blank is cut from a flat steel strip made of a quench-hardenable steel alloy, the steel sheet blank is formed into a component blank in a cold forming process and subjected to complete or substantial final trimming, the resulting component blank is then heated in a heating device to a temperature at which the steel material partially or completely transforms into austenite, the component blank is then transferred from the heating device to a form-hardening press and inserted into a form-hardening tool, cooled at a speed above the critical hardening speed, and thereby hardened, characterized in that In order to improve the dimensional accuracy of hardened parts, especially the dimensional accuracy of external trimming and hole shapes, at least one of the conditions a) to c) must be met: a) The maximum temperature difference of the component blanks in the batch, taking into account each component blank individually and all component blanks in relation to each other, before the closing of the form hardening press is completed is in: in, is the shape constant in K*m, L max is the maximum dimension of the largest blank in the batch measured in m. The following values apply depending on L max The shape constant From L max Starting from greater than 1m: in particular Best Especially preferred From L max Starting from greater than 0.5m: Best Especially preferred b) component blanks in a batch, including components of a first type and components of a second type, are positioned in the furnace in such a way that at least a portion of the first type of component is positioned directly next to at least one second portion of the first type of component and a portion of the second type of component is positioned directly next to at least one second portion of the second type of component, respectively; c) in a batch of component blanks consisting of a first type of components and a second type of components, the cold-formed dimensions or three-dimensional shapes of the first type of components and the second type of components are different due to differences in thermal expansion, and / or the cold-formed dimensions or three-dimensional shapes of at least one type of components are different, so that any dimensional differences are substantially compensated when the form-hardening press is closed.
2. The method according to claim 1, characterized in that: In condition a), the component blank or the component blank region which is cooler when the form hardening press is closed is additionally heated in a furnace.
3. The method according to claim 1 or 2, characterized in that: In condition a), the component blank or the component blank region which is at a higher temperature when the form hardening press is closed is actively cooled during the transfer process.
4. The method according to any one of the preceding claims, characterized in that Under condition a), the cooler component blank or component blank region when the form hardening press is closed is protected to a large extent from cooling during the transfer process, in particular from heat losses due to forced convection and / or thermal radiation, preferably by using draft shields and / or reflectors.
5. The method according to claim 1, characterized in that: In condition a), the component blank or the region of the component blank which is at a higher temperature when the form-hardening press is closed is actively cooled in the press before the form-hardening press is closed.
6. The method according to claim 1, characterized in that In condition b), in a batch consisting of components of the first type and components of the second type, the components of the first type and the components of the second type are positioned adjacent to and successively to each other in the direction of travel or conveying of the furnace, respectively.
7. The method according to claims 1 to 5, characterized in that In the direction of travel or conveying of the furnace, the component blanks within a batch are adjacent to each other in the furnace.
8. The method according to claim 2, characterized in that: The component blank or the region of the component blank close to the exit door is additionally heated in a heating device.
9. The method according to any one of the preceding claims, characterized in that The component blank from one cold forming cavity is hardened in at least two different form-hardening tool cavities.
10. The method according to any of the preceding claims, characterized in that At least two of the conditions a) to c) are met, in particular all three.
11. The method according to any one of the preceding claims, characterized in that The component blank is placed in the form-hardening tool on a support device, in particular a lifting device, in order to prevent uncontrolled cooling of the component blank from the time of insertion into the form-hardening tool to the time of closing the form-hardening tool prior to the hardening process.
12. The method according to any one of the preceding claims, characterized in that The sheet steel blanks used are blanks with a metallic corrosion protection layer, in particular a metallic corrosion protection layer based on or consisting of zinc.
13. The method according to any one of the preceding claims, characterized in that The steel strip is made of a hardenable steel alloy, in particular boron manganese steel.
14. The method according to claim 13, characterized in that The steel used is a material that delays the austenite-martensite transformation during cooling, wherein the steel strip is hot rolled or cold rolled.
15. The method according to claim 13 or 14, characterized in that The steel strip used had the following composition (all figures are in wt %): Residual iron and impurities 16. An apparatus, in particular for carrying out the method according to claims 1 to 15, comprising a cold forming tool, a furnace, a transfer device for transferring the component blanks and a form hardening tool, characterized in that Supporting devices, in particular lifting devices, are provided in the form-hardening tool in order to prevent uncontrolled cooling of the component blank from the time of insertion into the form-hardening tool to the time of closing the form-hardening tool prior to the hardening process.
Citation Information
Patent Citations
Method for manufacturing super strong steel body
CN101896293A
Method for producing a hot-formed and press-hardened steel sheet part
DE102020211426A1