Heat erasable microcapsule particle, preparation method and application thereof, heat erasable ink and application thereof
By preparing heat-erase microcapsule particles with particle sizes of 0.5 to 0.6 μm, combined with thermal-sensitive reaction and infrared heating, the problems of traditional ink large particle size and high energy consumption are solved, and efficient recycling and environmentally friendly printing of paper are achieved.
Patent Information
- Application Number
- CN202411337023.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
In the existing thermochromic discoloration system, the large particle size of the microcapsules causes blockage of the printing nozzle, and the traditional thermally erasable ink regeneration energy consumption and low compatibility, making it difficult to realize paper recycling.
Heat-erasable microcapsule particles are prepared using ethylenediaminetetraacetic acid, sodium hydroxide, methylvinyl ether maleic anhydride, crystal violet lactone, bisphenol AF and 4-benzyloxyphenyl ethylsanolate. , the text decolorization and paper restoration are achieved through thermal reaction and infrared heating, and the particle size is controlled between 0.5 and 0.6 μm, and is suitable for inkjet printers.
It realizes the simplicity and high recycling rate of paper recycling, reduces energy consumption for paper production and regeneration, reduces greenhouse gases and toxic substance emissions, improves the temperature change sensitivity of ink and color dispersion, and is suitable for office and study. and home print.
Smart Images

Figure CN119056357A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal sensitive inks, and in particular to thermally erasable microcapsule particles and a preparation method and application thereof, thermally erasable ink and application thereof. Background Art
[0002] Conventional waste paper recycling goes through more than 10 processes including transportation, sorting, bleaching, and papermaking, resulting in a printing paper recycling rate of less than 50% and continuing to decline. The waste paper recycling process releases a large amount of toxic waste gas, carcinogenic wastewater, and greenhouse gases, causing great harm to the ecological environment and human health.
[0003] At present, the recycling of printing paper at home and abroad can be divided into two categories: one is to improve paper, such as electronic printing paper based on charged nanoparticle coating and carbon printing paper based on organic ligand terpyridine coating. The disadvantage is that the manufacturing cost of paper improvement is high and the technology promotion is difficult; the other is to improve ink, such as methylene blue, TiO 2 The nano-crystal ink has a disappearing principle due to the catalytic reaction produced by ultraviolet irradiation. Its disadvantages are high regeneration energy consumption and low compatibility. Therefore, it is of great significance to provide a paper recycling method that reduces costs, energy consumption, carbon emissions and emissions.
[0004] Thermochromism is the process of changing the color of a system by increasing or decreasing the temperature. The color changes of existing thermochromic systems are mostly reversible, that is, the color of the system changes when the temperature is increased (or decreased) to a certain temperature, and the color of the system will immediately recover once the temperature drops below that temperature (or rises above that temperature). Using this principle to recycle printed paper has the advantages of reducing costs, energy, carbon emissions, and emissions.
[0005] For example, CN102430376A discloses a process for preparing color-changing microcapsules, comprising the following process steps: (1) mixing crystal violet lactone, dodecanol and bisphenol A uniformly to obtain a mixed solution A; adding a regulator and distilled water to the mixed solution A; homogenizing at high speed in a high-shear mixer emulsifier, and then shearing on the high-shear mixer emulsifier; then adjusting the pH value to 3.5-4 to obtain a mixed solution B; (2) stirring the obtained mixed solution B in a constant temperature water bath, and adding etherified melamine resin dropwise during the stirring process; then heating the mixed solution B to 62-66°C and keeping it warm for 4-6 minutes; (3) adjusting the pH value of the mixed solution B obtained in step (2) to 7-8 with an acetic acid solution with a concentration of 2-5 mol / L. The obtained color-changing microcapsules are all spherical, the capsule surface is not smooth, the average particle size is 15.18 μm, the particle size distribution is narrow, and the color-changing microcapsules have good solvent resistance and acid and alkali resistance, and the heat resistance can reach 198.58°C. However, the particle size of the above-mentioned color-changing microcapsule ink is large, and it is easy to clog the nozzle when used as printing ink. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a thermally erasable microcapsule particle and a preparation method and application thereof, a thermally erasable ink and application thereof. The thermally erasable microcapsule particle provided by the present invention has a small particle size and will not clog the print head. The thermally erasable ink using the thermally erasable microcapsule particle can achieve handwriting erasure and paper restoration through thermosensitive reaction and infrared heating, and the paper recycling is simple and the recycling rate is high.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing heat-erasable microcapsule particles, comprising the following steps:
[0009] first mixing ethylenediaminetetraacetic acid, sodium hydroxide, methyl vinyl ether maleic anhydride and water to obtain a mixed aqueous phase;
[0010] liquefying crystal violet lactone, bisphenol AF and 4-benzyloxyphenylethyl caprate to obtain a dye solution;
[0011] The dye solution is mixed with the mixed aqueous phase for a second time, the pH value is adjusted to 4 to 4.3, and emulsified to obtain a dye emulsion;
[0012] Dissolving formaldehyde and urea in water, adjusting the pH value of the resulting formaldehyde-urea solution to 8.2-8.8, and performing an addition condensation reaction to obtain a urea-formaldehyde resin solution;
[0013] The dye emulsion is added dropwise to the urea-formaldehyde resin solution for coating and adsorption, the pH value is adjusted to 3-3.4, the solid-liquid separation is performed, and the obtained solid phase is frozen to obtain heat-erasable microcapsule particles; the average particle size of the heat-erasable microcapsule particles is 0.5-0.6 μm.
[0014] Preferably, the raw materials for preparing the mixed aqueous phase include, by weight: 0.5 to 1 part of ethylenediaminetetraacetic acid, 5 to 8 parts of sodium hydroxide, 10 to 30 parts of methyl vinyl ether maleic anhydride, and 150 to 250 parts of water;
[0015] The temperature of the first mixing is 80-110°C.
[0016] Preferably, the raw materials for preparing the dye solution include, by weight: 2 to 6 parts of crystal violet lactone, 5 to 10 parts of bisphenol AF, and 40 to 80 parts of 4-benzyloxyphenylethyl caprate;
[0017] The liquefaction temperature is 100-150°C.
[0018] Preferably, the mass ratio of the mixed water phase to the dye solution is 165.5-289:47-96;
[0019] The emulsification temperature is 75-95° C., the emulsification is high-speed emulsification, and the stirring speed of the high-speed emulsification is 2000-3000 r / min.
[0020] Preferably, the raw materials for preparing the formaldehyde-urea solution include, by weight: 10 to 20 parts of formaldehyde, 5 to 10 parts of urea, and 20 to 30 parts of water;
[0021] The temperature of the addition condensation reaction is 65-85° C., and the time is 1-3 hours.
[0022] Preferably, the ratio of the total mass of the dye solution and the mixed water phase in the dye emulsion to the mass of the formaldehyde-urea solution is 212.5-358:35-60;
[0023] The coating-adsorption temperature is 65-90°C and the time is 4.5-6h;
[0024] The freezing temperature is -30 to -20°C.
[0025] The present invention also provides heat-erasable microcapsule particles prepared by the preparation method described in the above technical solution, with an average particle size of 0.5 to 0.6 μm.
[0026] The present invention also provides application of the heat-erasable microcapsule particles described in the above technical solution in ink.
[0027] The present invention also provides a heat-erasable ink, and the preparation raw materials include, by weight: 10 to 20 parts of the heat-erasable microcapsule particles described in the above technical solution, 0 to 60 parts of a water-soluble resin, 0 to 3 parts of a dispersant, 0 to 8 parts of a viscosity regulator, 0 to 1 part of a humectant, and 50 to 100 parts of water.
[0028] The present invention also provides the application of the thermally erasable ink described in the above technical solution in printing.
[0029] The heat-erasable microcapsule particles prepared by the present invention have an average particle size of 0.5 to 0.6 μm, and the particle size is small, so the nozzle will not be blocked when used for printing. The heat-erasable microcapsule particles prepared by the present invention use crystal violet lactone as a pigment and bisphenol AF as a developer; at the same time, in order to improve the temperature sensitivity of the ink and quickly change color after reaching the specified temperature, 4-benzyloxyphenylethyl caprylate is used as a sensitizer, which has the characteristics of being colorless at high temperature (60 to 70°C) and blue at low temperature (below -10°C), thereby improving the temperature sensitivity of the ink and quickly changing color after reaching the specified temperature. Moreover, the present invention uses urea-formaldehyde resin as the wall material to form microcapsules, creating a stable thermal sensitive reaction environment, so that the heat-erasable microcapsule particles provided by the present invention can be used to prepare thermal sensitive inks.
[0030] The average particle size of the thermally erasable microcapsule particles in the thermally erasable ink provided by the present invention is 0.5-0.6 μm, and the small particle size makes it suitable for the printing process and nozzle caliber of the inkjet printer, effectively solving the problem that the particle size of the traditional thermally erasable ink is too large and easy to clog the nozzle. The present invention uses water as a solvent, which is green and environmentally friendly. The main principle of the thermally erasable ink provided by the present invention is thermal reaction and infrared heating, which cooperate to achieve the decolorization of handwriting and the restoration of paper, and the paper cycle is simple and the recycling rate is high. The present invention creatively integrates thermal ink and home printers, shortens the traditional paper recycling process, realizes the instant recycling of paper in daily printing, and there is no greenhouse gas and toxic substance emission in the recycling process. And the thermally erasable ink provided by the present invention has the characteristics of clear printing handwriting, bright colors, and low pollution. It is used in daily printing scenes such as office, study, and home, effectively solving the problems of difficulty in recycling printing paper and serious waste of paper resources, and realizing cost reduction, energy saving, carbon reduction and emission reduction.
[0031] The present invention can improve the dispersion of colorants in thermal erasable ink and adjust the viscosity of thermal erasable ink by adding a dispersant. The present invention prolongs the shelf life of thermal erasable ink by adding a humectant. The present invention can better disperse components that are difficult to dissolve in water by adding a dispersant, and can prevent the sedimentation and aggregation of particles. The present invention can adjust the viscosity of ink by adding a viscosity modifier so that the viscosity is within the working range of the inkjet printer. The solvent of the thermal erasable ink provided by the present invention is water, which is more environmentally friendly than oily thermal erasable ink. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A specific use flow chart of the invention for printing on recycled paper using thermally erasable ink;
[0033] Figure 2 A schematic diagram of the application principle of the thermal erasable ink provided by the present invention;
[0034] Figure 3 A particle size distribution diagram of the thermally erasable ink provided by the present invention;
[0035] Figure 4 This is a particle size distribution diagram of commercially available heat-erasable ink for gel pens;
[0036] Figure 5 This is a color-erasable diagram of the heat-erasable ink provided by the present invention. DETAILED DESCRIPTION
[0037] The present invention provides a method for preparing heat-erasable microcapsule particles, comprising the following steps:
[0038] first mixing ethylenediaminetetraacetic acid, sodium hydroxide, methyl vinyl ether maleic anhydride and water to obtain a mixed aqueous phase;
[0039] liquefying crystal violet lactone, bisphenol AF and 4-benzyloxyphenylethyl caprate to obtain a dye solution;
[0040] The dye solution is mixed with the mixed aqueous phase for a second time, the pH value is adjusted to 4 to 4.3, and emulsified to obtain a dye emulsion;
[0041] Dissolving formaldehyde and urea in water, adjusting the pH value of the resulting formaldehyde-urea solution to 8.2-8.8, and performing an addition condensation reaction to obtain a urea-formaldehyde resin solution;
[0042] The dye emulsion is added dropwise to the urea-formaldehyde resin solution for coating and adsorption, the pH value is adjusted to 3-3.4, the solid-liquid separation is performed, and the obtained solid phase is frozen to obtain heat-erasable microcapsule particles; the average particle size of the heat-erasable microcapsule particles is 0.5-0.6 μm.
[0043] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.
[0044] The present invention first mixes ethylenediaminetetraacetic acid, sodium hydroxide, methyl vinyl ether maleic anhydride and water to obtain a mixed water phase.
[0045] In the present invention, the raw materials for preparing the mixed aqueous phase preferably include, by mass: 0.5 to 1 part of ethylenediaminetetraacetic acid, more preferably 0.6 to 0.9 parts, specifically preferably 0.5 parts, 0.55 parts, 0.6 parts, 0.65 parts, 0.7 parts, 0.75 parts, 0.8 parts, 0.85 parts, 0.9 parts, 0.95 parts or 1 parts; 5 to 8 parts of sodium hydroxide, more preferably 6 to 7 parts, specifically preferably 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts or 8 parts; 10 to 30 parts of methyl vinyl ether maleic anhydride, more preferably 15 to 25 parts, specifically preferably 10 parts, 11 parts, 12 parts, 13 parts , 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29 or 30 parts; 150-250 parts of water, more preferably 180-220 parts, specifically preferably 150, 155, 160, 165, 170, 175, 180, 185, 190, 195, 200, 205, 210, 215, 220, 225, 230, 235, 240, 245 or 250 parts; the water preferably includes deionized water.
[0046] In the present invention, the temperature of the first mixing is preferably 80-110°C, more preferably 90-105°C, and further preferably 100-105°C; the mixing is preferably stirring mixing, and the stirring mixing speed is preferably 400-600r / min, more preferably 450-550r / min, and further preferably 500r / min; the present invention has no special limitation on the time of the first mixing, as long as the solid can be completely dissolved in water, specifically 3-5min, and more preferably 4min; during the first mixing process, methyl vinyl ether maleic anhydride can be completely dissolved in the system of ethylenediaminetetraacetic acid, sodium hydroxide and water.
[0047] The invention liquefies crystal violet lactone, bisphenol AF and 4-benzyloxyphenylethyl caproate to obtain a dye solution.
[0048] In the present invention, the raw materials for preparing the dye solution preferably include, by mass: 2 to 6 parts of crystal violet lactone, more preferably 3 to 5 parts, specifically preferably 3.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts; 5 to 10 parts of bisphenol AF, preferably 6 to 8 parts, specifically preferably 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts or 10 parts; 40 to 80 parts of 4-benzyloxyphenylethyl caprate, preferably 50 to 70 parts, specifically preferably 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts or 80 parts.
[0049] In the present invention, the liquefaction temperature is preferably 100-150°C, more preferably 100-130°C, and further preferably 100-110°C; the liquefaction is preferably carried out under stirring conditions, and the stirring speed is preferably 200-500r / min, more preferably 250-450r / min, and further preferably 300-400r / min; the present invention has no special limitation on the liquefaction time, as long as each raw material can be completely liquefied. In the present invention, 4-benzyloxyphenylethyl caprylate is also used as a solvent, so that crystal violet lactone and bisphenol AF with a melting point higher than 150°C can be dissolved and / or liquefied. In the present invention, crystal violet lactone is a pigment, bisphenol AF is a color developer, and 4-benzyloxyphenylethyl caprylate is a sensitizer.
[0050] After obtaining the dye solution and the mixed aqueous phase, the present invention secondly mixes the dye solution and the mixed aqueous phase, adjusts the pH value to 4-4.3, and emulsifies to obtain the dye emulsion.
[0051] In the present invention, the mass ratio of the mixed aqueous phase to the dye solution is preferably 165.5-289:47-96, more preferably 180-270:50-90, and further preferably 200-250:60-80.
[0052] In the present invention, the second mixing is preferably adding the dye solution into the mixed aqueous phase under stirring; the dye solution is preferably added for 1 to 3 minutes, more preferably 2 minutes.
[0053] In the present invention, the acid used to adjust the pH value to 4-4.3 preferably includes dilute acetic acid and / or dilute sulfuric acid, and the concentration of the dilute acetic acid is preferably 0.5-2 mol / L, more preferably 1-1.5 mol / L; the concentration of the dilute sulfuric acid is preferably 0.3-0.5 mol / L, more preferably 0.4 mol / L; the present invention has no special limitation on the amount of the acid, and the pH value can be adjusted to 4-4.3, and the pH value is preferably 4.1-4.2. The present invention uses dilute acetic acid and / or dilute sulfuric acid as a pH adjustment buffer to ensure the stability of the pH in the reaction environment.
[0054] In the present invention, the emulsification temperature is preferably 75-95°C, more preferably 80-90°C, and further preferably 85°C; the emulsification is high-speed emulsification, and the stirring speed of the high-speed emulsification is preferably 2000-3000r / min, more preferably 2500-2600r / min; the emulsification time is preferably 3-6h, and further preferably 3-4h.
[0055] The invention dissolves formaldehyde and urea in water, adjusts the pH value of the obtained formaldehyde-urea solution to 8.2-8.8, performs addition condensation reaction, and obtains urea-formaldehyde resin liquid.
[0056] In the present invention, the raw materials for preparing the formaldehyde-urea solution preferably include, by mass: 10 to 20 parts of formaldehyde, more preferably 15 parts, specifically preferably 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts; 5 to 10 parts of urea, preferably 6 to 8 parts, specifically preferably 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts or 10 parts; 20 to 30 parts of water, more preferably 25 parts, specifically preferably 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts; the water preferably includes deionized water.
[0057] In the present invention, the dissolution temperature is preferably 60-90°C, more preferably 60-70°C; the dissolution is preferably carried out under stirring conditions, and the stirring speed is preferably 100-200 r / min, more preferably 150-200 r / min.
[0058] In the present invention, the base used to adjust the pH value to 8.2-8.8 preferably includes triethanolamine. The present invention has no special limitation on the amount of the base used, and the pH value can be adjusted to 8.2-8.8. The pH value is more preferably 8.4-8.6, and more preferably 8.5. After the pH value of the obtained formaldehyde-urea solution is adjusted to 8.2-8.8, the solution is clear and transparent. The present invention uses triethanolamine as a pH adjustment buffer to ensure the stability of the acidity and alkalinity in the reaction environment.
[0059] In the present invention, the temperature of the addition condensation reaction is preferably 65-85°C, more preferably 70-80°C, and further preferably 75°C; the time of the addition condensation reaction is preferably 1-3h, more preferably 1.5-2.5h, and further preferably 2h; the addition condensation reaction is preferably carried out under stirring conditions.
[0060] After obtaining the dye emulsion and the urea-formaldehyde resin liquid, the present invention drips the dye emulsion into the urea-formaldehyde resin liquid for coating-adsorption, adjusts the pH value to 3-3.4, separates the solid and the liquid, freezes the obtained solid phase, and obtains heat-erasable microcapsule particles; the average particle size of the heat-erasable microcapsule particles is 0.5-0.6 μm.
[0061] In the present invention, the mass ratio of the total mass of the dye solution and the mixed water phase in the dye emulsion to the mass of the formaldehyde-urea solution is preferably 212.5-358:35-60, more preferably 250-350:40-55, further preferably 300-320:45-50.
[0062] In the present invention, the dye emulsion is preferably added dropwise for 1 to 3 minutes, more preferably 2 minutes.
[0063] In the present invention, the coating-adsorption preferably includes the first coating-adsorption and the second coating-adsorption in sequence. In the present invention, the temperature of the first coating-adsorption is preferably 65-90°C, more preferably 70-85°C, and further preferably 75-85°C; the time of the first coating-adsorption is preferably 30-60min, and more preferably 50-60min; the first coating-adsorption is preferably carried out under stirring conditions, and the stirring speed is preferably 300-400r / min, and more preferably 350-400r / min. In the present invention, the temperature of the second coating-adsorption is preferably 60-95°C, more preferably 75-90°C, and further preferably 80-85°C; the time of the second coating-adsorption is preferably 4-5h, and more preferably 4.5h; the second coating-adsorption is preferably carried out under stirring conditions, and the stirring speed is preferably 100-200r / min, and more preferably 150-200r / min. In the present invention, in the coating-adsorption process, part of the dye emulsion is coated by the urea-formaldehyde resin as a core material, and the remaining dye emulsion is adsorbed onto the surface of the urea-formaldehyde resin.
[0064] In the present invention, the acid used to adjust the pH value to 3-3.4 preferably includes dilute acetic acid and / or dilute sulfuric acid, and the concentration of the dilute acetic acid is preferably 0.5-2 mol / L, more preferably 1-1.5 mol / L; the concentration of the dilute sulfuric acid is preferably 0.3-0.5 mol / L, more preferably 0.4 mol / L; the present invention has no special limitation on the amount of the acid, and the pH value can be adjusted to 3-3.4, and the pH value is preferably 3.1-3.3, more preferably 3.2. The present invention uses dilute acetic acid and / or dilute sulfuric acid as a pH adjustment buffer to ensure the stability of the pH in the reaction environment.
[0065] In the present invention, it is preferred that the system with the pH value adjusted to 3 to 3.4 is allowed to stand before solid-liquid separation. In the present invention, the temperature of the standing is preferably room temperature, and the standing time is preferably 20 to 26 hours, more preferably 22 to 24 hours; the purpose of the standing is to initially separate the particle phase (solid phase) and the aqueous phase. In the present invention, the solid-liquid separation preferably includes centrifugal separation.
[0066] In the present invention, the freezing temperature is preferably -30 to -20°C, more preferably -30 to -25°C. The present invention has no particular limitation on the freezing time, and the freezing may be performed until the capsule particles are completely colored.
[0067] The present invention provides heat-erasable microcapsule particles prepared by the preparation method described in the above technical scheme, wherein the average particle size of the heat-erasable microcapsule particles is 0.5-0.6 μm, preferably 0.55-0.6 μm; the particle size of the heat-erasable microcapsule particles is preferably 0.2-0.1 μm, more preferably 0.2-0.6 μm.
[0068] The present invention also provides application of the heat-erasable microcapsule particles described in the above technical solution in ink.
[0069] The present invention also provides a heat-erasable ink, and the preparation raw materials include, by weight: 10 to 20 parts of the heat-erasable microcapsule particles described in the above technical solution, 0 to 60 parts of a water-soluble resin, 0 to 3 parts of a dispersant, 0 to 8 parts of a viscosity regulator, 0 to 1 part of a humectant, and 50 to 100 parts of water.
[0070] In parts by mass, the raw materials for preparing the thermally erasable ink provided by the present invention include 10 to 20 parts of the thermally erasable microcapsule particles described in the above technical scheme, preferably 15 parts, and specifically preferably 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts.
[0071] Based on the mass fraction of the heat-erasable microcapsule particles, the raw materials for preparing the heat-erasable ink provided by the present invention include 0 to 60 parts of a water-soluble resin, preferably 10 to 60 parts, more preferably 20 to 60 parts, and further preferably 30 to 60 parts, and specifically preferably 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55 or 60 parts. In the present invention, the water-soluble resin preferably includes methyl hexadecanoate and / or ethyl formate. The present invention can improve the dispersion of the colorant in the heat-erasable ink and adjust the viscosity of the heat-erasable ink by adding a dispersant.
[0072] The raw materials for preparing the thermally erasable ink provided by the present invention include 0 to 3 parts of dispersant, preferably 1 to 3 parts, more preferably 2 to 3 parts, and specifically preferably 0 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts or 3 parts, based on the mass fraction of the thermally erasable microcapsule particles. In the present invention, the dispersant preferably includes polyacrylamide and / or polyvinyl chloride alkylamine. By adding a dispersant, the present invention can better disperse the components that are difficult to dissolve in water, and at the same time prevent the sedimentation and agglomeration of the particles.
[0073] The raw materials for preparing the thermally erasable ink provided by the present invention include 0 to 8 parts of viscosity modifier, preferably 2 to 8 parts, more preferably 5 to 8 parts, and specifically preferably 0, 1, 2, 3, 4, 5, 6, 7 or 8 parts, based on the mass fraction of the thermally erasable microcapsule particles. In the present invention, the viscosity modifier preferably includes one or more of xanthan gum, polyvinyl alcohol and hydroxypropyl cellulose. By adding a viscosity modifier, the viscosity of the ink can be adjusted so that the viscosity is within the working range of the inkjet printer.
[0074] The raw materials for preparing the heat-erasable ink provided by the present invention include 0 to 1 part of a moisturizer, preferably 0.2 to 1 part, more preferably 0.5 to 1 part, and specifically preferably 0 part, 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part or 1 part, based on the mass fraction of the heat-erasable microcapsule particles. In the present invention, the moisturizer preferably includes one or more of ethylene glycol, 1,2-propylene glycol and 1,3-butylene glycol. The present invention prolongs the shelf life of the heat-erasable ink by adding a moisturizer.
[0075] The raw materials for preparing the thermal erasable ink provided by the present invention include 50 to 100 parts of water, preferably 60 to 90 parts, more preferably 70 to 80 parts, and specifically preferably 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts or 100 parts, based on the mass fraction of the thermal erasable microcapsule particles. In the present invention, the water preferably includes deionized water. The solvent of the thermal erasable ink provided by the present invention is water, which is more environmentally friendly than oily thermal erasable ink.
[0076] In the present invention, the preparation method of the thermally erasable ink preferably includes the following steps: adding thermally erasable microcapsule particles to a water-soluble resin, adding water for a third mixing, and then adding a dispersant, a viscosity modifier and a humectant for a fourth mixing. In the present invention, the temperature of the third mixing is preferably room temperature; the third mixing is preferably stirring and mixing, and the present invention has no special restrictions on the third mixing, as long as the raw materials can be mixed evenly. In the present invention, the temperature of the fourth mixing is preferably room temperature; the fourth mixing is preferably stirring and mixing, and the stirring and mixing speed is preferably 200 to 300 r / min, more preferably 250 to 300 r / min; the time of the fourth mixing is preferably 20 to 40 min, more preferably 30 min. In the present invention, when the raw materials for preparing the thermally erasable ink do not contain one or more of the water-soluble resin, dispersant, viscosity modifier and humectant, the step of adding the corresponding raw materials is omitted.
[0077] The present invention also provides the application of the thermally erasable ink described in the above technical solution in printing.
[0078] The specific use process of using the thermal erasable ink provided by the present invention for printing on recycled paper is shown in Figure 1 , application principle see Figure 2. The main principle of the thermally erasable ink provided by the present invention is thermal sensitive reaction and infrared heating, and the two cooperate to achieve the decolorization of writing and the restoration of paper. The paper is printed with thermally erasable ink, the paper is restored (the writing disappears when the temperature rises to 60-70°C, the writing disappears when the temperature drops to below -10°C, and then returns to room temperature), and the paper is printed again with thermally erasable ink. The paper can be recycled 8 times by printing with the thermally erasable ink provided by the invention. (1) Printing with thermally erasable ink: the writing has the characteristic of decolorization upon heating (60-70°C), and the process is pollution-free. The present invention optimizes the physicochemical properties of the thermally erasable microcapsule particles, such as the particle size and solvent, to make them compatible with the printing process and nozzle diameter of the inkjet printer. (2) Infrared heating: the discarded printing paper is placed in the infrared heating erasing equipment, and the infrared heating tube is used to heat the paper so that the writing temperature rises to the decolorization threshold (60-70°C), and the process has low energy consumption. (3) Secondary printing: After the discarded paper cools down and the writing disappears, the paper is left to cool down. After returning to normal temperature, secondary printing can be performed. The process is convenient and paper recycling can be achieved immediately. Figure 5 .
[0079] By using the existing infrared heating erasing equipment to heat to 60-70°C, the handwriting on the paper printed with the heat-erasable ink provided by the present invention can be made to disappear, thereby realizing the immediate and on-site recycling of paper in daily printing, bringing good ecological benefits. Each piece of printed paper does not need to go through more than 10 processes of conventional waste paper recycling, and can be recycled immediately through the decolorizing device. The number of recycling times is 8 times, the reuse rate is about 70%, saving nearly 68% of paper, reducing nearly 60% of paper production and regeneration energy consumption, and the new power consumption is only 0.002 degrees / minute, which is highly efficient and energy-saving. Moreover, compared with the traditional paper recycling with inefficient recycling and complex regeneration process, the heat-erasable ink provided by the present invention is used for printing, and then infrared heating is used for erasing, which realizes the paper recycling process without emission and pollution, reduces nearly 70% of carbon emissions, nearly 100% of noise pollution, significantly reduces the emission of toxic waste gas pollutants such as hydrogen sulfide, and carcinogenic wastewater pollutants such as dioxins, and achieves a considerable reduction in greenhouse gases and toxic substances, and achieves carbon reduction and emission reduction.
[0080] The present invention creatively integrates thermal ink and household printers, shortens the traditional paper recycling process, and realizes instant paper recycling in daily printing, without greenhouse gas and toxic substance emissions during the recycling process; the present invention innovatively improves the ink properties and uses existing infrared heating erasing equipment to improve the process flow, so that the printing system has the function of controlling the temperature change of paper and erasing the handwriting, effectively improving product performance and compatibility.
[0081] To further illustrate the present invention, the following detailed description of a thermally erasable microcapsule particle, a preparation method and application thereof, a thermally erasable ink and application thereof provided by the present invention is provided in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0082] Example 1
[0083] Prepare ingredients according to Table 1.
[0084] Ethylenediaminetetraacetic acid, sodium hydroxide, methyl vinyl ether maleic anhydride and deionized water were heated to 105° C. and stirred at 500 r / min until the solid was completely dissolved to obtain a mixed aqueous phase.
[0085] Crystal violet lactone, bisphenol AF and 4-benzyloxyphenylethyl caprate were stirred at 100° C. and 400 r / min until completely liquefied to obtain a dye solution.
[0086] The dye solution was added to the mixed aqueous phase under stirring at room temperature for 2 minutes. The pH value was adjusted to 4.2 using 1 mol / L dilute acetic acid, and then high-speed emulsification was performed at 85° C. and 2600 r / min for 3.5 hours to obtain a dye emulsion.
[0087] Formaldehyde, urea and deionized water were stirred at 60°C and 200 r / min until completely dissolved, the pH value of the resulting formaldehyde-urea solution was adjusted to 8.5 with triethanolamine, and the solution was heated to 75°C and stirred for 2 hours to obtain a urea-formaldehyde resin solution.
[0088] The dye emulsion is added dropwise to the urea-formaldehyde resin solution for 2 minutes. The mixture is stirred at 75°C and 400 r / min for 60 minutes. The stirring speed is then reduced to 200 r / min. The mixture is stirred at 85°C for 4 to 5 hours to obtain a microcapsule particle emulsion.
[0089] The pH value of the microcapsule particle emulsion is adjusted to 3.2 with 2 mol / L dilute acetic acid, and the mixture is allowed to stand for 24 hours. The mixture is centrifuged and the solid phase is frozen at -30°C until the capsule particles are completely colored, thereby obtaining heat-erasable microcapsule particles. The average particle size of the heat-erasable microcapsule particles is 0.5-0.6 μm.
[0090] Add the heat-erasable microcapsule particles to a water-soluble resin (methyl hexadecanoate,), then add deionized water and stir evenly, then add a dispersant (polyacrylamide), a viscosity regulator (xanthan gum,) and a humectant (ethylene glycol), and stir for 30 minutes at room temperature and 300 r / min to obtain a heat-erasable neutral ink (blue thermochromic).
[0091] Example 2
[0092] Thermally erasable microcapsule particles and thermally erasable neutral ink were prepared according to the method of Example 1. The amounts of the raw materials used are shown in Table 1.
[0093] Example 3
[0094] Thermally erasable microcapsule particles and thermally erasable neutral ink were prepared according to the method of Example 1. The amounts of the raw materials used are shown in Table 1. Among them, the water-soluble resin is ethyl formate, and the viscosity modifier is polyvinyl alcohol.
[0095] Example 4
[0096] Thermally erasable microcapsule particles and thermally erasable neutral ink were prepared according to the method of Example 1. The amounts of the raw materials used are shown in Table 1. Among them, the water-soluble resin is ethyl formate, and the dispersant is polyvinyl chloride alkylamine.
[0097] Table 1 Preparation materials of Examples 1 to 4 (parts by mass)
[0098]
[0099] The particle size distribution of the heat-erasable neutral ink prepared in Example 1 is shown in Figure 3 and Table 2, the particle size distribution of conventional thermal erasable ink for pens (Morning AKR67K01) is shown in Figure 4 and Table 2.
[0100] Table 2 Particle size distribution of the new thermally erasable ink for printers and the thermally erasable gel pen ink for conventional pens prepared in Example 1
[0101] project Thermal Erasable Ink Heat-erasable gel pen ink for traditional pens temperature 25℃ 25℃ average value 596.7nm 1749nm Peak 796 1763
[0102] Depend on Figure 3-4 As shown in Table 2, the average particle size of commercially available thermally erasable ink for gel pens is 1746 nm, while the average particle size of the thermally erasable microcapsule particles prepared in the present invention is 596.7 nm. The thermally erasable microcapsule particles prepared in the present invention are 65.82% smaller than the average particle size of commercially available thermally erasable ink for gel pens, effectively solving the problem that the conventional thermally erasable ink capsules are large in particle size and easy to clog the nozzles.
[0103] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing heat-erasable microcapsule particles, The following steps are involved: first mixing ethylenediaminetetraacetic acid, sodium hydroxide, methyl vinyl ether maleic anhydride and water to obtain a mixed aqueous phase; liquefying crystal violet lactone, bisphenol AF and 4-benzyloxyphenylethyl caprate to obtain a dye solution; The dye solution is mixed with the mixed aqueous phase for a second time, the pH value is adjusted to 4 to 4.3, and emulsified to obtain a dye emulsion; Dissolving formaldehyde and urea in water, adjusting the pH value of the resulting formaldehyde-urea solution to 8.2-8.8, and performing an addition condensation reaction to obtain a urea-formaldehyde resin solution; The dye emulsion is added dropwise to the urea-formaldehyde resin solution for coating and adsorption, the pH value is adjusted to 3-3.4, the solid-liquid separation is performed, and the obtained solid phase is frozen to obtain heat-erasable microcapsule particles; the average particle size of the heat-erasable microcapsule particles is 0.5-0.6 μm.
2. The preparation method according to claim 1, It is characterized in that The raw materials for preparing the mixed aqueous phase include, by weight: 0.5 to 1 part of ethylenediaminetetraacetic acid, 5 to 8 parts of sodium hydroxide, 10 to 30 parts of methyl vinyl ether maleic anhydride, and 150 to 250 parts of water; The temperature of the first mixing is 80-110°C.
3. The preparation method according to claim 1, It is characterized in that The raw materials for preparing the dye solution include, by weight: 2 to 6 parts of crystal violet lactone, 5 to 10 parts of bisphenol AF, and 40 to 80 parts of 4-benzyloxyphenylethyl caprate; The liquefaction temperature is 100-150°C.
4. The preparation method according to claim 1, It is characterized in that The mass ratio of the mixed water phase to the dye solution is 165.5-289:47-96; The emulsification temperature is 75-95° C., the emulsification is high-speed emulsification, and the stirring speed of the high-speed emulsification is 2000-3000 r / min.
5. The preparation method according to claim 1, It is characterized in that The raw materials for preparing the formaldehyde-urea solution include, by weight: 10 to 20 parts of formaldehyde, 5 to 10 parts of urea, and 20 to 30 parts of water; The temperature of the addition condensation reaction is 65-85° C., and the time is 1-3 hours.
6. The preparation method according to claim 1, It is characterized in that The ratio of the total mass of the dye solution and the mixed water phase in the dye emulsion to the mass of the formaldehyde-urea solution is 212.5-358:35-60; The coating-adsorption temperature is 65-90°C and the time is 4.5-6h; The freezing temperature is -30 to -20°C.
7. The heat-erasable microcapsule particles prepared by the preparation method according to any one of claims 1 to 6, having an average particle size of 0.5 to 0.6 μm.
8. Use of the thermally erasable microcapsule particles according to claim 7 in ink.
9. A heat-erasable ink, prepared by weight of raw materials include: 10-20 parts of the heat-erasable microcapsule particles according to claim 7, 0-60 parts of a water-soluble resin, 0-3 parts of a dispersant, 0-8 parts of a viscosity regulator, 0-1 part of a moisturizer, and 50-100 parts of water.
10. Use of the thermally erasable ink according to claim 9 in printing.
Citation Information
Patent Citations
Stable discoloration ink
CN104130627A
Special microcapsule pigment particle for thermosensitive erasable pen ink and preparation method thereof
CN114196259A
Reversible thermosensitive color-changing microcapsule material as well as preparation method and application thereof
CN116393054A