Machining method of slender rod type part and slender rod type part
Through the steps of tempering treatment, vehicle appearance, straightening and stress removal treatment, combined with special fixtures, the problems of low efficiency, difficulty in controlling accuracy and deformation prevention in the processing of slender rod parts are solved, and high precision and stable fineness are achieved Production of long rod parts.
Patent Information
- Application Number
- CN202411210902.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing processing methods for slender rod parts have problems such as low production efficiency, difficulty in controlling accuracy, insufficient deformation prevention and straightening stability, resulting in unstable product structure and difficult to meet high-precision requirements.
Adopt the steps of tempering treatment, car shape, straightening and stress removal, grinding and groove milling, and drilling, combined with special stress removal fixtures and shaping fixtures to ensure the stress release and accuracy control of the bar material in each process. , and finally obtain high-precision slender rod parts through straightening and heat setting treatment.
It improves turning efficiency, reduces deformation, reduces grinding margin, ensures the accuracy and stability of parts, solves the problems of production efficiency and precision control, and realizes the feasibility of mass production.
Smart Images

Figure CN119057393A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of processing slender rod parts, and in particular to a processing method of a slender rod part and the slender rod part. Background Art
[0002] In the technical field of new diesel engine multi-cylinder combined injection pumps, slender rod parts, as core components, undertake the key task of accurately adjusting the fuel supply. Its accuracy is not only directly related to the overall performance and stability of the diesel engine, but also an important consideration for technological innovation and optimization.
[0003] The aspect ratio of slender rod parts is as high as 44. There are 12 groups of tooth grooves on the outer circle, with 2 teeth in each group, as well as a plane and 3 keyways. The slender rod parts in the existing technology face multiple challenges and shortcomings in the processing and production process, resulting in unstable part structure and easy deformation. The straightness of the outer circle required by the product is difficult to reach the required 0.1. The specific performance is as follows: 1) Low turning process efficiency and significant deformation: The traditional turning solution is divided into three independent steps. During the process, due to the excessive overhang of the parts, the turning stability is poor, and vibration and taper processing problems are prone to occur, resulting in increased abnormal processing time and low turning efficiency. At the same time, the error caused by the two clamping of the center hole causes the tailstock center to apply additional stress when correcting the center deviation, causing the parts to be in a stressed state, which in turn causes the parts to rebound and deform after processing, making it difficult to meet high-precision requirements.
[0004] 2) Redundant external cylindrical grinding allowance affects processing efficiency: Due to the slenderness of the parts and the significant deformation during the turning process, the external cylindrical runout increases significantly after the turning process is completed, generally between 0.4mm and 0.6mm, forcing the grinding allowance to be set to a larger value (usually more than 0.6mm) to ensure the final dimensional accuracy. Although this can barely meet the processing requirements, it greatly reduces the grinding efficiency and increases the production cost.
[0005] 3) The part structure is unstable and the deformation is difficult to control: After milling the tooth groove, plane and subsequent processing procedures, the slender rod parts gradually release the internal stress of the parts due to the large amount of material removal and the inherent characteristics of the structure, resulting in bending deformation. This process is further aggravated during subsequent processing such as milling keyways and drilling. The deformation of the final product can be as high as 0.4mm, seriously affecting the assembly accuracy and product performance.
[0006] 4) The straightening process by fitters is highly dependent on the process and the quality fluctuates greatly: To solve the problem of bending deformation, the current manual straightening method by fitters is used, and its effect is completely dependent on the operator's experience and skill level. This method is not only difficult to control the processing time and quality, but may also cause continued deformation in subsequent use due to insufficient release of internal stress, reducing product reliability and user satisfaction.
[0007] 5) Frequent deformation after assembly: According to user feedback, some fuel injection pumps have abnormally increased tensile force on parts during use. After testing, it was found that the outer circle of the parts had a certain degree of bending deformation (about 0.2mm~0.3mm). The root cause of this phenomenon is the internal stress generated during the straightening process by the fitter, which is gradually released during use, eventually leading to deformation, affecting the overall performance and service life of the product.
[0008] In summary, the existing processing methods of slender rod parts have significant deficiencies in production efficiency, precision control, deformation prevention and straightening stability. A new processing solution is urgently needed to improve product quality and production efficiency. Summary of the invention
[0009] In view of this, an object of the present invention is to provide a processing method for slender rod parts and slender rod parts, so as to solve the problem that the existing processing methods of slender rod parts have significant deficiencies in production efficiency, precision control, deformation prevention and straightening stability.
[0010] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for processing a slender rod-like part comprises the following steps: Quenching and tempering treatment: the bar is subjected to heat treatment, quenching treatment, tempering treatment, first straightening treatment and first stress relief treatment; Turning the shape: turning the reference outer circle in the middle of the bar after quenching and tempering, and then turning the remaining outer circle of the bar on one side of the reference outer circle, turning the two end faces of the bar and turning the remaining outer circle of the bar on the other side of the reference outer circle; Straightening and stress relief treatment: The bar material after contouring is subjected to a second straightening treatment and a second stress relief treatment; Grinding the outer circle: The straightened and stress-relieved bar is subjected to outer circle grinding; Milling grooves, milling surfaces and drilling holes; milling tooth grooves and planes, milling keyways and flat surfaces, and drilling holes on the bar after grinding the outer circle; Straightening and heat setting treatment: The bar material after milling grooves, milling surfaces and drilling is straightened and heat set for the third time to obtain the finished slender rod parts.
[0011] According to the above technical means, firstly, the bar is subjected to quenching and tempering treatment, which effectively ensures the hardness and straightness of the bar and fully removes the stress. Secondly, the turning method adopted realizes the equal division of the turning length, reduces the turning difficulty and improves the turning efficiency. At the same time, the center hole is punched and the tailstock top is supported against the center hole, and the turning of the shape is completed in one clamping, which ensures that the center hole is on the center of the spindle, and no bending stress is generated when the tailstock top is supported against the center hole, which effectively reduces the turning deformation. Thirdly, after turning, the bar is straightened and stress-relieved, so that the straightness of the bar before external cylindrical grinding is greatly improved, the grinding allowance is greatly reduced, the grinding efficiency is significantly improved, and the stress of the bar is effectively removed, so that the deformation after milling the tooth groove and plane and milling the keyway is reduced. Fourthly, the milling of the tooth groove and plane after grinding effectively ensures the accuracy of the bar in the clamped state, and provides the prerequisite for subsequent straightening and heat setting treatment. Finally, straightening and heat setting treatment are adopted to ensure the accuracy requirements of slender rod parts. The invention solves the problem that the existing processing methods of slender rod parts have significant deficiencies in production efficiency, precision control, deformation prevention and straightening stability.
[0012] Preferably, the heat treatment is: subjecting the rod material to heat treatment at a temperature of 840° C. to 860° C. for 80 min to 100 min.
[0013] Preferably, the quenching treatment is: quenching treatment is performed in quenching oil.
[0014] Preferably, the tempering treatment is: heat preservation treatment at a temperature of 540° C. to 580° C. for 125 min to 145 min.
[0015] The quenched bar is tempered so that the hardness of the tempered bar is 28HRC~32HRC.
[0016] Preferably, the first straightening process is: tapping the bar until the straightness is 1 mm.
[0017] Preferably, the first stress relief treatment is: heat preservation treatment at a temperature of 430° C. to 510° C. for 60 min to 80 min.
[0018] The straightened bars are subjected to heat preservation treatment to fully remove the stress caused by straightening.
[0019] Preferably, the turning shape is: turning a reference outer circle with a length of about 40 mm in the middle of the bar after quenching and tempering, and then turning the remaining outer circle of the bar on one side of the reference outer circle, turning one end face of the bar, turning the remaining outer circle of the bar on the other side of the reference outer circle and turning the other end face of the bar, so that the outer circle tolerance is within 0.1 mm, the turning allowance of the outer circle is 3 mm~4 mm, and the turning allowance of the two end faces is 1 mm~2 mm.
[0020] Preferably, the straightening and stress relief treatment is: fixing the rod after contouring on a stress relief fixture and placing it at a temperature of 400°C to 440°C for a heat preservation treatment for 110min to 130min, so as to simultaneously achieve straightening and stress relief of the rod.
[0021] Preferably, the outer circle grinding is: subjecting the straightened and stress-relieved bar to outer circle grinding so that the outer circle tolerance is within 0.03 mm, the cylindricity is within 0.02 mm, and the outer circle grinding allowance is 0.3 mm to 0.4 mm.
[0022] The bar material after turning is subjected to a second straightening treatment and a second stress relief treatment to fully remove the stress generated during the turning process and ensure that the outer circle straightness after the stress relief treatment is within 0.2mm.
[0023] Preferably, the milling grooves, milling surfaces and drilling holes are as follows: the bar material after grinding the outer circle is clamped on the vertical machining center with a milling fixture, and the tooth grooves and plane processing are performed, and then the outer circle of the bar material is clamped with a chuck on the dividing head, the circumferential direction is determined by a plane, the center hole is supported by the tailstock top, and the keyway, flat surface and hole at one end are processed, and then the keyway, flat surface and hole at the other end are turned around to process, so that the parallelism of the processed plane to the lower generatrix of the outer circle is within 0.02mm.
[0024] Preferably, before the straightening and heat setting treatments, the process also includes removing the process pads.
[0025] Preferably, the stress relief fixture comprises: a first positioning plate, a first pressure plate, a first screw, a first spring washer and a first lifting ring; The first positioning plate is formed with a first positioning groove for positioning the bar; The first pressing plate is arranged on the first positioning groove; The first spring washer is provided between the first pressing plate and the first screw; The first positioning plate is also provided with the first lifting ring.
[0026] By designing a special stress relief fixture, the deformation of the bar during the stress release process is controlled.
[0027] Preferably, the milling fixture comprises: a clamp body, a second positioning plate, a second pressing plate, a T-shaped nut and a second screw; The second positioning plates are arranged at both ends of the clamp body. A second positioning groove for positioning the bar is formed on the clamp body; The second pressing plate is arranged on the second positioning groove; The second pressing plate is assembled and fixed to the clamp body by a second screw; The clamp body is assembled and fixed to the machine tool via a T-shaped nut and a second screw.
[0028] By designing a special milling fixture, the parallelism of the plane to the lower generatrix of the outer circle after milling is ensured to be within 0.02mm.
[0029] Preferably, the third straightening process is to fix the bar material after the milling groove, milling surface and drilling on a shaping fixture for straightening.
[0030] Preferably, the heat setting treatment is: placing the rod material that has undergone the third straightening treatment at a temperature of 330°C to 370°C for insulation treatment for 170min to 190min, and after heat setting, the outer circle straightness is within 0.1mm, and a finished slender rod part is obtained.
[0031] Preferably, the shaping fixture comprises: a third positioning plate, a positioning block, a positioning pressure block, a third pressure plate, a third screw, a second spring washer and a second lifting ring; The positioning block is pressed and installed on the third positioning plate by a third screw to form a third positioning groove for positioning the bar; The positioning block has a certain amount of moving space on the third positioning plate, so that the width of the formed third positioning groove can be adjusted according to needs; The positioning pressing block is arranged on the third positioning groove; The lower end of the positioning block adopts a V-shaped structure, i.e. a V-shaped structure, so as to provide better support when pressing the bar material, and the upper end adopts a cylindrical structure, i.e. a cylindrical structure, and the upper end is assembled with the third pressing plate by interference fit; The third pressing plate is assembled and fixed with the positioning block by a third screw; A second spring washer is provided between the third screw and the third pressing plate, so that the third pressing plate and the positioning pressing block are floatingly pressed on the bar material; The third positioning plate is also provided with a second lifting ring; By setting up a special shaping fixture, the deformation of the bar during the heat shaping process is controlled.
[0032] Preferably, the bar is a 40Cr hot-rolled bar.
[0033] The present invention also provides a slender rod-like part, which is processed by the processing method of the present invention.
[0034] Beneficial effects of the present invention: The processing method of the slender rod parts of the present invention first performs a tempering treatment on the bar material, which effectively ensures the hardness and straightness of the bar material and fully removes the stress. Secondly, the turning method adopted realizes the equal distribution of the turning length, reduces the turning difficulty, and improves the turning efficiency; at the same time, the center hole is drilled and the tailstock top supports the center hole, and the shape is turned in one clamping, which ensures that the center hole is on the center of the spindle, and no bending stress is generated when the tailstock top supports the center hole, which effectively reduces the turning deformation; thirdly, the bar material is straightened and stress is relieved after turning, so that the straightness of the bar material before the outer cylindrical grinding is greatly improved, so that The grinding allowance is greatly reduced, the grinding efficiency is significantly improved, and the stress of the bar is effectively removed, so that the deformation after milling the tooth groove and plane and milling the keyway is reduced; fourthly, the milling of the tooth groove and plane after grinding effectively ensures the accuracy of the bar in the compressed state, and provides the prerequisite for subsequent straightening and heat setting treatment; finally, the straightening and heat setting treatment is adopted to effectively ensure the accuracy requirements of slender rod parts, solve the problems of low production efficiency, difficult precision control and unstable quality in the existing processing of slender rod parts, and realize mass production, which has the value of promotion and application in the field of slender rod parts processing technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic diagram of the first turning process of the bar in S2; Figure 2 It is a schematic diagram of the second turning process of the bar in S2; Figure 3 It is a schematic diagram of the third turning process of the bar in S2; Figure 4 It is a schematic structural diagram of the stress relief fixture of the present invention; Figure 5 for Figure 4 Left view of Figure 6 It is a structural schematic diagram of the milling fixture of the present invention; Figure 7 for Figure 6 Sectional view along AA; Figure 8 A schematic diagram of the structure of the slender rod part processed by the present invention; Fig. 9 for Figure 8 A top view of Fig.10 It is a structural schematic diagram of the shaping fixture of the present invention; Fig.11 for Fig.10 Left view of Fig.12 It is a structural schematic diagram of the positioning block; Among them, 1-bar, 11-reference outer circle, 12-first outer circle, 13-second outer circle, 14-first end face, 15-second end face, 16-plane, 17-tooth groove, 18-keyway, 19-flat surface; 2-stress relief fixture, 21-first positioning plate, 211-first positioning groove, 22-first pressure plate, 23-first screw, 24-first spring washer, 25-first lifting ring; 3-milling fixture, 31-clamp body, 311-second positioning groove, 32-second positioning plate, 33-second pressure plate 3, 34-T-nut, 35-second screw; 4-forming fixture, 41-third positioning plate, 42-positioning block, 43-positioning pressure block, 431-V-shaped structure, 432-cylindrical structure, 44-third pressure plate, 45-third screw, 46-second spring washer, 47-second lifting ring. DETAILED DESCRIPTION
[0036] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.
[0037] It should be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present invention, and thus the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0038] The present invention intends to disclose a processing method of a slender rod-like part and a slender rod-like part, so as to solve the problem that the existing processing method of slender rod-like parts has significant deficiencies in production efficiency, precision control, deformation prevention and straightening stability.
[0039] Among them, a processing method of slender rod parts is suitable for processing high-precision slender rod parts, comprising the following steps: S1. The quenching and tempering treatment is as follows: subjecting the 40Cr hot-rolled bar to heat treatment, quenching treatment, tempering treatment, first straightening treatment and first stress relief treatment; S2, turning the shape: turning the reference outer circle in the middle of the bar after quenching and tempering, and then turning the remaining outer circle of the bar on one side of the reference outer circle, turning the two end faces of the bar and turning the remaining outer circle of the bar on the other side of the reference outer circle; S3, straightening and stress relief treatment: the bar material after the shape turning is subjected to the second straightening treatment and the second stress relief treatment; S4, external grinding: the straightened and stress-relieved bar is subjected to external grinding; S5, Milling tooth groove and plane: S6, milling keyway, flat face and drilling: S7, remove the process: S8, straightening and heat setting treatment: the bar material after milling grooves, milling surfaces and drilling holes is straightened and heat set for the third time to obtain the finished slender rod parts.
[0040] Milling grooves, milling surfaces and drilling holes; milling tooth grooves and planes, milling keyways and flat surfaces, and drilling holes on the bar after grinding the outer circle; Straightening and heat setting treatment: The bar material after milling grooves, milling surfaces and drilling is straightened and heat set for the third time to obtain the finished slender rod parts.
[0041] The slender rod-like parts are racks.
[0042] In some embodiments, the conditioning process includes: Heat treatment: keep the bar at 840℃~860℃ for 80min~100min; The quenching treatment is as follows: quenching treatment is carried out in quenching oil; Tempering treatment: keep the temperature at 540℃~580℃ for 125min~145min, and the hardness after tempering is 28HRC~32HRC; The first straightening process is: tap the bar until the straightness is 1mm; The first stress relief treatment is: heat preservation treatment at a temperature of 430℃~510℃ for 60min~80min to fully remove the stress caused by straightening.
[0043] Exemplarily, the heat treatment is: subjecting the rod to a heat treatment at a temperature of 850° C. for 90 minutes.
[0044] Exemplarily, the tempering treatment is: heat preservation treatment at a temperature of 560° C. for 135 minutes.
[0045] Exemplarily, the first straightening process is: using a hammer to hit the high point of the bar until the straightness is 1 mm.
[0046] Exemplarily, the first stress relief treatment is: heat preservation treatment at a temperature of 470° C. for 70 minutes.
[0047] In some embodiments, the turning shape is as follows: a reference outer circle with a length of about 40 mm is turned in the middle of the bar after the quenching and tempering treatment, and then the remaining outer circle of the bar on one side of the reference outer circle, one end face of the bar, the remaining outer circle of the bar on the other side of the reference outer circle and the other end face of the bar are turned in sequence, so that the outer circle tolerance is within 0.1 mm and the grinding allowance of the outer circle is 0.3 mm~0.4 mm.
[0048] For example, Figures 1 to 3 As shown, the turning of the shape includes three steps. The first step is to turn a reference outer circle 11 with a length of about 40 mm in the middle of the bar 1 after quenching and tempering. The second step is to hold the second outer circle 13 of the bar 1 on the other side of the reference outer circle 11 with a center frame. At this time, the spindle and the bar 1 do not rotate, and the power head is rotated to punch the center hole of the first end face 14, and then the center hole of the first end face 14 is supported by the tailstock top, the center frame is released, the spindle is started to rotate, and the first outer circle 12 on one side of the reference outer circle 11 is started to be turned. After turning, the spindle is stopped, the center frame is started to hold the second outer circle 13 on the other side of the reference outer circle 11, and the tailstock is retracted. Start the spindle again to turn the first end face 14 on one side of the bar; the third step: use the center frame to hold the first outer circle 12 (that is, the outer circle that has been turned) of the bar located on the side of the reference outer circle 11. At this time, the spindle and the bar do not rotate, and the power head is rotated to drill the center hole of the second end face 15, and then the center hole of the second end face 15 is supported by the tailstock top, the center frame is released, the spindle is started to rotate, and the second outer circle 13 located on the other side of the reference outer circle 11 is started to be turned. After turning, the spindle rotation is stopped, the center frame is started to hold the first outer circle 12 located on the side of the reference outer circle 11, the tailstock is retracted, and the spindle is started again to turn the second end face 15 on the other side of the bar.
[0049] Among them, the requirements for the turning shape are that the outer circle tolerance is within 0.1mm, the corresponding outer circle turning allowance is 3mm~4mm, the two end surface turning allowance is 1mm~2mm and the two end surface process center hole allowance is 5mm~7mm.
[0050] Exemplarily, the turning allowance of both end faces is 1.5 mm and the process center hole allowance of both end faces is 6 mm.
[0051] In some embodiments, the straightening and stress relief treatment is as follows: the rod after the shape turning is fixed on a stress relief fixture and placed in a temperature of 400°C~440°C for insulation treatment for 110min~130min, so as to simultaneously achieve straightening and stress relief of the rod, and the outer circle straightness after stress relief is within 0.2mm.
[0052] Exemplarily, the straightening and stress relief treatment is as follows: after the bar is fixed with a special stress relief fixture, it is placed in a vacuum furnace at a temperature of 420°C for insulation treatment for 120 minutes to simultaneously remove stress and straighten, and ensure that the outer circle straightness after the stress relief treatment is within 0.2 mm.
[0053] In some embodiments, the outer circle grinding includes: subjecting the straightened and stress-relieved bar to outer circle grinding so that the outer circle tolerance is within 0.03 mm and the cylindricity is within 0.02 mm.
[0054] For example, grinding the outer circle is: the straightened and stress-relieved bar is ground on the outer circle grinder using two top clamps, and the two tops are used to support the center holes at both ends of the bar for grinding. In order to increase rigidity, an adjustable center support part is added to the middle of the bar. After grinding the outer circle, the outer circle tolerance is controlled within 0.03mm, the cylindricity is controlled within 0.02mm, and the outer circle grinding allowance is 0.3mm~0.4mm.
[0055] For example, the milling of grooves, milling of faces and drilling of holes are as follows: the bar material after grinding the outer circle is clamped and fixed on the vertical machining center with a special milling fixture to mill the tooth grooves and planes; then on the vertical machining center, the outer circle of the bar material is clamped with a chuck on the indexing head, the circumferential direction is determined by a plane, the center hole is supported by the tailstock top, and then the keyway, flat surface and hole at one end are processed. After processing one end, turn around and process the keyway, flat surface and hole at the other end. After processing, the parallelism of the plane to the lower generatrix of the outer circle is within 0.02mm.
[0056] In some embodiments, Figure 4 and Figure 5 As shown, in order to ensure that the deformation of the bar material during the stress release process is controllable, a special stress relief fixture 2 is designed. The stress relief fixture 2 includes: a first positioning plate 21, a first pressure plate 22, a first screw 23, a first spring washer 24 and a first lifting ring 25; A first positioning groove 211 is formed on the first positioning plate 21 for positioning the bar 1. The first positioning groove 211 is finely processed after high-temperature aging, which can effectively reduce the deformation in subsequent use. The design gap of the first positioning groove 211 is 0.1mm~0.15mm; The first pressing plate 22 is disposed on the first positioning groove 211 of the first positioning plate 21; one first pressing plate 22 can be used to simultaneously press the bars 1 in the two first positioning grooves 211; A first spring washer 24 is provided between the first pressing plate 22 and the first screw 23 to ensure that the pressing plate is pressed on the bar material in a floating manner, so that there is a certain amount of deformation space in the heat treatment furnace; The first positioning plate 21 is further provided with a first hanging ring 25 .
[0057] When the stress relief fixture 2 is in use, the bar 1 is placed in the first positioning groove 211 of the first positioning plate 21, and the bending direction is placed in the vertical direction. Then, the first screw 23 is used to fix the bar 1 on the first positioning plate 21 through the first pressure plate 22 and the first spring washer 24. Finally, the stress is relieved in a heat treatment vacuum furnace with a furnace temperature of 420±20℃ and a holding time of 120±10min, so as to fully remove the stress generated during the turning process and straighten the outer circle of the bar 1.
[0058] In some embodiments, Figures 6 to 9 As shown, in order to ensure that the plane 16 of the bar 1 after processing is parallel to the lower generatrix of the outer circle within 0.02mm, a special milling fixture 3 is designed for processing on a vertical machining center. The milling fixture 3 includes a clamp body 31, a second positioning plate 32, a second pressure plate 33, a T-shaped nut 34 and a second screw 35; The second positioning plates 32 are disposed at both ends of the clamp body 31. A second positioning groove 311 is formed on the clamp body 31 for positioning the bar 1; The second pressing plate 33 is disposed on the second positioning groove 311 , and one second pressing plate 33 can be used to simultaneously press the bars 1 in the two second positioning grooves 311 ; The second pressing plate 33 is assembled and fixed to the clamp body 31 by means of second screws 35; The clamp body 31 is assembled and fixed to the machine tool by means of a T-shaped nut 34 and a second screw 35; The clamp body 31 adopts a split structure, which is composed of three sections of clamp bodies.
[0059] When the milling fixture 3 is working, the three sections of the clamp body are fixed on the machine tool workbench with T-nuts 34 and second screws 35 respectively, and the positioning surface of the clamp body 31 is made parallel to the working axis of the machine tool. Then, the bar 1 is placed on the second positioning groove 311 on the clamp body 31 and the bar 1 is fixed on the milling fixture 3 with the second screw 35 and the second pressure plate 33. Finally, the processing of the tooth groove 17 and the plane 16 of the bar 1 is started.
[0060] For example, on a vertical machining center, the outer circle of the bar 1 is clamped by a chuck on a dividing head, the circumferential direction is determined by a plane 16, the center hole is supported by a tailstock center, and then the keyway 18, flat surface 19 and hole at one end are processed. After processing one end, turn around and process the keyway 18, flat surface 19 and hole at the other end.
[0061] Exemplarily, on a vertical machining center, the bar 1 is clamped by using the milling fixture 3 used in the milling step, the flat surface 16 of the bar 1 is placed downward on the second positioning groove 311 on the clamp body 31, and the bar 1 is fixed to the milling fixture 3 using the second screw 35 and the second pressure plate 33, and the center hole stubs at both ends of the bar 1 are removed. At the same time, the keyway 18 in the middle of the bar 1 is processed.
[0062] In some embodiments, the third straightening process is to fix the bar material after the milling groove, milling surface and drilling on a shaping fixture for straightening.
[0063] In some embodiments, the heat setting treatment is: placing the rod material that has undergone the third straightening treatment at a temperature of 330°C to 370°C for 170min to 190min, and after heat setting, the outer circle straightness is within 0.1mm, and a finished slender rod part is obtained.
[0064] Exemplarily, the heat setting treatment is: placing the bar material that has undergone the third straightening treatment in a vacuum furnace at a temperature of 350° C. for heat preservation treatment for 180 minutes, and after heat setting, the outer circle straightness is within 0.1 mm, and a finished slender rod-like part is obtained.
[0065] In some embodiments, Figures 8 to 12 As shown, in order to ensure that the outer circle straightness after heat setting is within 0.1mm, a special setting fixture 4 is designed to ensure that the deformation of the parts during the heat setting process is controllable. The setting fixture 4 includes: a third positioning plate 41, a positioning block 42, a positioning pressure block 43, a third pressure plate 44, a third screw 45, a second spring washer 46 and a second hanging ring 47; The positioning block 42 is pressed and installed on the third positioning plate 41 by a third screw 45 to form a third positioning groove for positioning the bar 1; The positioning block 42 has a certain amount of moving space on the third positioning plate 41, so that the width of the formed third positioning groove can be adjusted according to needs; The positioning pressing block 43 is arranged on the third positioning groove; The lower end of the positioning block 43 adopts a V-shaped structure, namely a V-shaped structure 431, so as to provide better support when pressing the bar 1, and the upper end adopts a cylindrical structure, namely a cylindrical structure 432, and the upper end is assembled with the third pressing plate 44 by interference fit; The third pressing plate 44 is assembled and fixed to the positioning block 42 by a third screw 45; A second spring washer 46 is provided between the third screw 45 and the third pressing plate 44, so that the third pressing plate 44 and the positioning pressing block 43 are floatingly pressed on the bar material 1, so that there is a certain amount of deformation space in the heat treatment furnace; The third positioning plate 41 is further provided with a second lifting ring 47 .
[0066] When the shaping fixture 4 is in use, the bar 1 is placed flat downward on the third positioning plate 41, and then the bar 1 is fixed to the third positioning plate 41 using the third screw 45 through the positioning block 42, the positioning pressure block 43, the third pressure plate 44 and the second spring washer 46. Finally, the bar 1 is shaped in a heat treatment vacuum furnace with a furnace temperature of 350±20℃ and a holding time of 180±10min. The outer circle of the bar 1 is straightened and the stress is fully removed, so that the part is stable and not easily deformed.
[0067] In some embodiments, a slender rod-like part is also provided which is processed by the processing method in any of the above embodiments.
[0068] In summary, the processing method of the slender rod parts of the present invention first performs a tempering treatment on the bar material, which effectively ensures the hardness and straightness of the bar material and fully removes the stress. Secondly, the turning method adopted realizes the equal distribution of the turning length, reduces the turning difficulty, and improves the turning efficiency. At the same time, the center hole is drilled and the tailstock top supports the center hole, and the shape is turned in one clamping, which ensures that the center hole is on the center of the spindle. When the tailstock top supports the center hole, no bending stress is generated, which effectively reduces the turning deformation. Thirdly, after turning, the bar material is straightened and stress is relieved, so that the straightness of the bar material before external cylindrical grinding is greatly improved. , which greatly reduces the grinding allowance, significantly improves the grinding efficiency, and effectively removes the stress of the bar, reducing the deformation after milling the tooth grooves and planes and milling the keyways; fourthly, the milling of the tooth grooves and planes after grinding effectively ensures the accuracy of the bar under the clamping state, providing the prerequisite for subsequent straightening and heat setting treatment; finally, the straightening and heat setting treatment is used to effectively ensure the accuracy requirements of slender rod parts, solves the problems of low production efficiency, difficult precision control, and unstable quality in the existing processing of slender rod parts, and realizes mass production, which has promotion and application value in the field of slender rod parts processing technology.
[0069] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.
Claims
1. A method for processing slender rod parts, characterized in that: The following steps are involved: Quenching and tempering treatment: the bar is subjected to heat treatment, quenching treatment, tempering treatment, first straightening treatment and first stress relief treatment; Turning the shape: turning the reference outer circle in the middle of the bar after quenching and tempering, and then turning the remaining outer circle of the bar on one side of the reference outer circle, turning the two end faces of the bar and turning the remaining outer circle of the bar on the other side of the reference outer circle; Straightening and stress relief treatment: The bar material after contouring is subjected to a second straightening treatment and a second stress relief treatment; Grinding the outer circle: The straightened and stress-relieved bar is subjected to outer circle grinding; Milling grooves, milling surfaces and drilling holes: milling tooth grooves and planes, milling keyways and flat surfaces, and drilling holes on the bar after grinding the outer circle; Straightening and heat setting treatment: The bar material after milling grooves, milling surfaces and drilling is straightened and heat set for the third time to obtain the finished slender rod parts.
2. The processing method of the slender rod parts according to claim 1 is characterized in that: The heat treatment comprises: subjecting the rod material to a heat preservation treatment at a temperature of 840°C to 860°C for 80min to 100min; And / or, the quenching treatment is: quenching treatment in quenching oil; And / or, the tempering treatment is: heat preservation treatment at a temperature of 540° C. to 580° C. for 125 min to 145 min; And / or, the first straightening process is: tapping the bar until the straightness is 1 mm; And / or, the first stress relief treatment is: heat preservation treatment at a temperature of 430° C. to 510° C. for 60 min to 80 min.
3. The processing method of the slender rod parts according to claim 1, characterized in that: The turning shape is as follows: turning a reference outer circle with a length of 40mm~60mm in the middle of the bar after quenching and tempering, and then turning the remaining outer circle of the bar on one side of the reference outer circle, turning one end face of the bar, turning the remaining outer circle of the bar on the other side of the reference outer circle and turning the other end face of the bar in sequence, so that the outer circle tolerance is within 0.1mm, the outer circle turning allowance is 3mm~4mm, and the two end faces turning allowance is 1mm~2mm.
4. The processing method of the slender rod parts according to claim 1, characterized in that: The straightening and stress relief treatment is as follows: the bar material after the shape turning is fixed on the stress relief fixture and placed under the condition of 400°C to 440°C for heat preservation treatment for 110min to 130min, so as to achieve straightening and stress relief of the bar material at the same time; And / or, the outer circle grinding is: subjecting the straightened and stress-relieved bar material to outer circle grinding so that the outer circle tolerance is within 0.03 mm, the cylindricity is within 0.02 mm, and the outer circle grinding allowance is 0.3 mm to 0.4 mm; And / or, the milling, milling and drilling are as follows: the bar material after grinding the outer circle is clamped on the vertical machining center with a milling fixture, the tooth groove and plane processing are performed, and then the outer circle of the bar material is clamped with a chuck on the dividing head, the circumferential direction is determined by a plane, the center hole is supported by the tailstock top, and the keyway, flat surface and hole at one end are processed, and then the keyway, flat surface and hole at the other end are turned around and processed, so that the parallelism of the plane to the lower generatrix of the outer circle after processing is within 0.02mm; And / or, before straightening and heat setting treatment, it also includes removing process paving.
5. The processing method of the slender rod parts according to claim 4, characterized in that: The stress relief fixture comprises: a first positioning plate, a first pressing plate, a first screw, a first spring washer and a first lifting ring; The first positioning plate is formed with a first positioning groove for positioning the bar; The first pressing plate is arranged on the first positioning groove; The first spring washer is provided between the first pressing plate and the first screw; The first positioning plate is also provided with the first lifting ring.
6. The method for processing slender rod parts according to claim 4, characterized in that: The milling fixture comprises: a clamp body, a second positioning plate, a second pressing plate, a T-shaped nut and a second screw; The second positioning plates are arranged at both ends of the clamp body. A second positioning groove for positioning the bar is formed on the clamp body; The second pressing plate is arranged on the second positioning groove; The second pressing plate is assembled and fixed to the clamp body by a second screw; The clamp body is assembled and fixed to the machine tool via a T-shaped nut and a second screw.
7. The method for processing slender rod parts according to claim 1, characterized in that: The third straightening process is to fix the bar material after the milling groove, milling surface and drilling on the shaping fixture for straightening; And / or, the heat setting treatment is: placing the rod material that has undergone the third straightening treatment at a temperature of 330°C to 370°C for a heat preservation treatment for 170min to 190min, and after heat setting, the outer circle straightness is within 0.1mm, thereby obtaining a finished slender rod part.
8. The method for processing slender rod parts according to claim 7, characterized in that: The shaping fixture comprises: a third positioning plate, a positioning block, a positioning pressing block, a third pressing plate, a third screw, a second spring washer and a second lifting ring; The positioning block is pressed and installed on the third positioning plate by a third screw to form a third positioning groove for positioning the bar; The positioning block has a certain amount of moving space on the third positioning plate, so that the width of the formed third positioning groove can be adjusted according to needs; The positioning pressing block is arranged on the third positioning groove; The lower end of the positioning block adopts a V-shaped structure, i.e. a V-shaped structure, so as to provide better support when pressing the bar material, and the upper end adopts a cylindrical structure, i.e. a cylindrical structure, and the upper end is assembled with the third pressing plate by interference fit; The third pressing plate is assembled and fixed with the positioning block by a third screw; A second spring washer is provided between the third screw and the third pressing plate, so that the third pressing plate and the positioning pressing block are floatingly pressed on the bar material; The third positioning plate is also provided with a second lifting ring; And / or, the bar is a 40Cr hot-rolled bar.
9. A slender rod-like component, characterized in that: The slender rod-like parts are processed by the processing method described in any one of claims 1 to 8.
Citation Information
Patent Citations
Machining process for connecting rod
CN106271425A
Shaft core machining process
CN112792515A
Fixed-length cutting clamp and technology for batch hafnium rod corrosion samples
CN116511627A
Machining device for track pin in tracked vehicle walking system
CN214518928U
Shaft Manufacturing Process for Alternator
KR1020040038057A