Method for improving carbonization performance of high-magnesium low-carbon clinker

By mixing high-magnesium and low-carbon clinker with phosphogypsum and MgSO4 and carbonized under specific conditions, the problems of high-magnesium and low-carbon clinker are solved, and the carbonization strength and carbon sequestration rate are significantly improved. The efficient utilization of high-magnesium limestone has been achieved.

CN119059748AActive Publication Date: 2024-12-03HUAXIN CEMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411188302.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The calcination temperature of high magnesium and low carbon clinker is high during firing, and the active hydration of effective hydration is reduced. MgO exists in the form of low-active overfired, making it difficult to meet production and product standards, and MgO enters the calcium silicate mineral with low activity. The carbonization activity of the obtained low-carbon clinker is reduced.

Method used

Mix high-magnesium low-carbon clinker with acidic exciters phosphogypsum and MgSO4, dry after pressing and molding, and carbonize under specific conditions. The dissolution and carbonization of Ca2+ and Mg2+ are promoted through reactions 1 to 4, thereby improving carbonization activity and carbon sequestration rate. .

Benefits of technology

The carbonization strength and carbon sedimentation ratio of high-magnesium and low-carbon clinker have been significantly improved, and the high value-added resource utilization of high-magnesium limestone has been achieved, with the carbonization strength increased by 30-80% and the carbon sedimentation ratio increased by 30-50%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014207370000031
    Figure BDA0005014207370000031
  • Figure BDA0005014207370000041
    Figure BDA0005014207370000041
  • Figure HDA0005014207380000011
    Figure HDA0005014207380000011
Patent Text Reader

Abstract

The invention discloses a method for improving carbonization performance of high-magnesium low-carbon clinker, which comprises the following steps: (1) mixing the high-magnesium low-carbon clinker, an acid activator and water, and carrying out compression molding; wherein the acid exciting agent is prepared from phosphogypsum and MgSO4; and (2) drying the molded sample, regulating the water content, and carbonizing to obtain a carbonized product. According to the present invention, the gypsum and the MgSO4 are adopted as the main raw materials to prepare the acid activator, and the acid activator is applied to the high-magnesium low-carbon clinker carbonization process, such that the carbonization strength and the carbon sequestration rate of the high-magnesium low-carbon clinker can be significant, and the high value-added resource utilization of the low-carbon clinker prepared from the high-magnesium limestone can be achieved; and the related preparation method is relatively simple and convenient to operate, has good economic and environmental benefits, and is suitable for popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a method for improving the carbonization performance of high-magnesium low-carbon clinker. Background Art

[0002] CO2 emissions from cement manufacturing mainly come from the CO2 decomposed from limestone during cement production. Compared with silicate cement clinker, low-carbon cement clinker (low-calcium cement clinker) requires less limestone and lower calcination temperature during burning, which can reduce CO2 emissions by about 20% during the production process, and the subsequent carbonization process can absorb CO2, which has significant environmental benefits.

[0003] High-magnesium limestone has low CaO content and high MgO and SiO2 content, making it difficult to be used. When high-magnesium limestone is used to produce silicate cement clinker, the calcination temperature of the clinker will be high, the effective hydration active components will be reduced, and MgO will usually exist in the form of low-activity overburned MgO, which is difficult to meet the requirements of production and product standards. When high-magnesium limestone is used to produce low-carbon cement clinker, MgO will enter the highly active low-calcium-silicon ratio calcium silicate minerals C2S, C3S2, and CS to form less active C7MS4, C3MS2, and C2MS2 phases. Since the relative molecular mass of MgO is significantly smaller than that of Al2O3, MgO can combine with more CaO and SiO2 to form less active C7MS4, C3MS2, and C2MS2 phases, thereby significantly reducing the carbonization activity of the resulting low-carbon clinker.

[0004] How to improve and enhance the carbonization performance of high-magnesium low-carbon clinker, so as to achieve the effective utilization of low-carbon clinker made from high-magnesium limestone, has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] The main purpose of the present invention is to provide a method for improving the carbonization performance of high-magnesium low-carbon clinker, which can improve the carbonization activity of high-magnesium low-carbon clinker, significantly improve the carbonization strength and carbon fixation rate of high-magnesium low-carbon clinker, and realize high value-added resource utilization of low-carbon clinker made from high-magnesium limestone.

[0006] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A method for improving the carbonization performance of high-magnesium low-carbon clinker, comprising the following steps:

[0008] (1) mixing high-magnesium low-carbon clinker, an acidic activator and water, and pressing and molding; wherein the acidic activator comprises phosphogypsum and MgSO4;

[0009] (2) Drying the molded sample and adjusting the moisture content, and carbonizing the sample to obtain a carbonized product.

[0010] According to the above scheme, the high-magnesium, low-carbon clinker in step (1) is mainly composed of one or more of the magnesium calcium silicate minerals C7MS4, C3MS2, and C2MS2.

[0011] Furthermore, in the high-magnesium low-carbon clinker, the chemical components and their mass percentages include: CaO 37-59%, SiO2 25-47%, Al2O3 0-10%, Fe2O3 0-10%, and MgO 5-15%.

[0012] Preferably, the lower the mass ratio of CaO to SiO2 in the chemical composition of the high-magnesium low-carbon clinker, the higher the content of low-carbonization active minerals C3MS2 and C2MS2, and the more obvious the effect of modification by the acidic activator.

[0013] According to the above scheme, in the acidic activator in step (1), the amount of phosphogypsum is 5-20wt% of the amount of high-magnesium low-carbon clinker, and the amount of MgSO4 is 0.5-5wt% of the amount of high-magnesium low-carbon clinker.

[0014] Furthermore, the phosphogypsum does not need to be subjected to deacidification and modification treatment, and its pH value is 1-6.

[0015] According to the above scheme, the amount of water used is 10-25wt% of the amount of high-magnesium low-carbon clinker used.

[0016] According to the above scheme, in step (2), the moisture content is adjusted to 4-20wt%.

[0017] According to the above scheme, the drying temperature used in step (2) is 20-50°C.

[0018] According to the above scheme, in step (2), the carbonization step adopts a CO2 concentration of 15-100%, a temperature of 20-50°C, a humidity of 40-80%, an air pressure of 0-0.3MPa, and a carbonization time of 6-72h.

[0019] The carbonization product prepared according to the above scheme can improve the carbonization strength by 30-80% and the carbon fixation rate by 30-50% compared with the condition without adding the acidic activator.

[0020] The principle of the present invention is:

[0021] The essence of the carbonization reaction of low-carbon clinker is that the alkaline Ca(OH)2 or alkaline calcium silicate hydrate dissolves in the low-carbon clinker and reacts with H2CO3 to produce CaCO3 by acid-base neutralization. This reaction is easy to occur and is an exothermic reaction. The addition of MgSO4 (taking MgSO4 as an example) affects the carbonization of low-carbon clinker through the following reactions 1 to 4:

[0022] Reaction 1 is that MgSO4 promotes the Ca in low carbon clinker2+ Dissolved as CaSO4·2H2O which is slightly soluble in water:

[0023] MgSO4+CaO·xSiO2+yH2O→Mg(OH)2·xSiO2·(y-3)H2O+CaSO4·2H2O

[0024] Reaction 2 is the dissolution of CO2 in water:

[0025] CO2+H2O→H2CO3

[0026] Reaction 3 is the carbonization of Mg(OH)2 to Mg(HCO3)2:

[0027] Mg(OH)2·xSiO2·(y-3)H2O+2H2CO3+H2O→Mg(HCO3)2+xSiO2·yH2O

[0028] Reaction 4 is the carbonization of CaSO4·2H2O by Mg(HCO3)2 to CaCO3 and reformation of MgSO4:

[0029] Mg(HCO3)2+CaSO4·2H2O→CaCO3+CO2+3H2O+MgSO4

[0030] High magnesium and low carbon clinker is equivalent to replacing CaO·xSiO2 with CaO·zMgO·xSiO2.

[0031] (1) The present invention adds MgSO4, which only acts as a reaction aid in carbonization. Through reaction 1, slightly soluble Mg(OH)2 silica gel complex and slightly soluble CaSO4·2H2O are generated, which can accelerate and continuously promote the Ca2+ removal in high-Mg and low-C clinker. 2+ The Mg(HCO3)2 generated can be dissolved and carbonized through reactions 2, 3, and 4, effectively increasing the carbonizable amount of high-magnesium and low-carbon clinker.

[0032] (2) The present invention adds solid waste phosphogypsum, which can promote the Mg content in high-Mg low-carbon clinker. 2+ The dissolution of phosphogypsum can improve the carbonization activity; phosphogypsum is acidic, and the addition of phosphogypsum can dissolve part of Ca in high-Mg-low-C clinker before carbonization. 2+ and Mg 2+ The magnesium salt will dissolve Ca in the high-magnesium and low-carbon clinker again through reaction 1. 2+During the carbonization process, this part of Mg that once belonged to the high-Mg low-C clinker and the part of Mg that was directly introduced into the raw material as MgSO4 are carbonized into CaCO3 and MgSO4 through reactions 1 to 4, and the CaSO4·2H2O in the phosphogypsum is generated, and the MgSO4 is generated, and the recycling of the MgSO4 excitation component is realized at the same time;

[0033] In addition, CaSO4·2H2O in phosphogypsum can induce MgO in high-Mg-LC clinker to undergo reactions 3 and 4, thereby promoting the degradation of MgO in high-Mg-LC clinker. 2+ The dissolution of magnesium and low-carbon clinker increases the carbonization activity and generates MgSO4, which further promotes the reaction 1 to reaction 4.

[0034] After CaSO4·2H2O in phosphogypsum is carbonized through reaction 4, it can release water that is not used for pressing and molding. This makes it possible to gradually replenish the lost water as the carbonization proceeds, thereby extending the effective carbonization time.

[0035] (3) MgSO4 changes the carbonization from an acid-base neutralization reaction to a non-acid-base neutralization double decomposition reaction through reactions 1 to 4, which not only promotes the degradation of Ca in high-Mg and low-C clinker, but also promotes the degradation of Ca in high-Mg and low-C clinker. 2+ The dissolution of Ca 2+ The carbonization rate makes this part of Ca 2+ It can be better transported with water, so that CaCO3 is generated in the pores on the surface of non-high-magnesium low-carbon clinker. Secondly, the slow generation rate of CaCO3 and the reduction of supersaturation promote the generation of aragonite with a large aspect ratio, which plays a more effective role in filling and connecting the pores, which is conducive to the continuous carbonization of high-magnesium low-carbon clinker. Although adding only phosphogypsum can directly react with Mg in high-magnesium low-carbon clinker to generate a certain amount of MgSO4 through reaction 4, the CaSO4·2H2O activity of phosphogypsum itself is low and the reaction rate is slow. Therefore, the effect of using only phosphogypsum is poor, and additional MgSO4 needs to be added.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1) The present invention proposes for the first time to prepare an acidic activator using phosphogypsum and MgSO4 as main raw materials, and to apply the acidic activator to the carbonization process of high-magnesium low-carbon clinker, which can significantly increase the carbonization strength and carbon fixation rate of high-magnesium low-carbon clinker, and provide a new idea for the efficient resource utilization of high-magnesium low-carbon clinker;

[0038] 2) The preparation method of the present invention is relatively simple, easy to operate, has good economic and environmental benefits, and is suitable for popularization and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1SEM image of the carbonized product obtained in Example 1. DETAILED DESCRIPTION

[0040] The present invention is not limited to the above-mentioned embodiments. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

[0041] The following are the high-magnesium low-carbon clinker, phosphogypsum and MgSO4 used in the specific examples:

[0042] Different types of high-magnesium low-carbon clinkers (respectively clinker 1, clinker 2 and clinker 3) were obtained. The chemical composition and mineral composition of the high-magnesium low-carbon clinker used in the embodiment of the present invention are shown in Table 1 and Table 2, respectively, and ground to R45μm≤20%:

[0043] Table 1 Chemical composition of high magnesium low carbon clinker (%)

[0044]

[0045]

[0046] Table 2 Mineral composition of high magnesium low carbon clinker (%)

[0047] name <![CDATA[βC2S]]> <![CDATA[C7MS4]]> <![CDATA[C3MS2]]> <![CDATA[C2MS2]]> <![CDATA[C2AS]]> <h2 style=";text-align:left;direction:ltr"><![CDATA[MgFe <h2 style=";text-align:left;direction:ltr"> 0.6 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 1.4 <h2 style=";text-align:left;direction:ltr"> O4]]><h2 style=";text-align:left;direction:ltr"> MgO Clinker 1 32.4 56.5 0 0.7 0 6.0 4.3 Clinker 2 0 55.1 29.8 1.9 8.2 4.0 1.1 Clinker 3 0 41.8 41.2 7.2 9.8 0 0

[0048] In the following examples, the chemical composition of the phosphogypsum used is shown in Table 3. Before use, it was ground to R80 μm ≤ 20% and the pH value was 3.4.

[0049] Table 3 Chemical composition of phosphogypsum (%)

[0050] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08

[0051] The chemical reagent used was analytical grade MgSO4.

[0052] Example 1

[0053] A method for improving the carbonization performance of high-magnesium low-carbon clinker, comprising the following steps:

[0054] 1. Ratio

[0055] Weigh 1 100 parts of high-magnesium low-carbon clinker, 13 parts of phosphogypsum, 2 parts of analytically pure MgSO4, and 17 parts of water;

[0056] 2. Sample preparation

[0057] First, weighed MgSO4 is put into weighed water to completely dissolve to obtain MgSO4 solution, then high-magnesium low-carbon clinker 1 and phosphogypsum are put into a mixer and stirred for 3 minutes to form a powder, then the MgSO4 solution is added to the powder and stirred for 1 minute, and the mixed wet material is pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa;

[0058] 3. Pre-drying and carbonization

[0059] The obtained sample was dried under natural conditions to a moisture content of 13% (the moisture content with the highest carbonization strength obtained from the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0060] Example 2

[0061] A method for improving the carbonization performance of high-magnesium low-carbon clinker, comprising the following steps:

[0062] 1. Ratio

[0063] Weigh 2 100 parts of high-magnesium low-carbon clinker, 15 parts of phosphogypsum, 2 parts of analytically pure MgSO4, and 19 parts of water;

[0064] 2. Sample preparation

[0065] First, weighed MgSO4 is put into weighed water to completely dissolve to obtain MgSO4 solution, then high-magnesium low-carbon clinker 2 and phosphogypsum are put into a mixer and stirred for 3 minutes to form a powder, then the MgSO4 solution is added to the powder and stirred for 1 minute, and the mixed wet material is pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa;

[0066] 3. Pre-drying and carbonization

[0067] The obtained sample was dried under natural conditions to a moisture content of 13% (the moisture content with the highest carbonization strength obtained from the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0068] Example 3

[0069] A method for improving the carbonization performance of high-magnesium low-carbon clinker, comprising the following steps:

[0070] 1. Ratio

[0071] Weigh 3 100 parts of high-magnesium low-carbon clinker, 15 parts of phosphogypsum, 2 parts of analytically pure MgSO4, and 20 parts of water;

[0072] 2. Sample preparation

[0073] First, weighed MgSO4 is put into weighed water to completely dissolve to obtain MgSO4 solution, then high-magnesium low-carbon clinker 3 and phosphogypsum are put into a mixer and stirred for 3 minutes to form a powder, then the MgSO4 solution is added to the powder and stirred for 1 minute, and the mixed wet material is pressed into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa;

[0074] 3. Pre-drying and carbonization

[0075] The obtained sample was dried under natural conditions to a moisture content of 13% (the moisture content with the highest carbonization strength obtained from the carbonization test after drying to different moisture contents), and finally carbonized for 20 hours under the conditions of a carbon dioxide concentration of 99%, a temperature of 30°C, a humidity of 60%, and an air pressure of 0.3MPa (pressure indication 0.3MPa) to obtain a carbonized product.

[0076] Comparative Example 1

[0077] A carbonization process for high-magnesium low-carbon clinker, wherein the preparation method is substantially the same as that of Example 1, except that phosphogypsum and MgSO4 are not added.

[0078] Comparative Example 2

[0079] A carbonization process for high-magnesium low-carbon clinker, wherein the preparation method is substantially the same as that of Example 1, except that phosphogypsum is not added.

[0080] Comparative Example 3

[0081] A carbonization process for high-magnesium low-carbon clinker, wherein the preparation method is substantially the same as that of Example 1, except that MgSO4 is not added.

[0082] Comparative Example 4

[0083] A carbonization process for high-magnesium low-carbon clinker, wherein the preparation method is substantially the same as that of Example 3, except that phosphogypsum and MgSO4 are not added.

[0084] Comparative Example 5

[0085] A carbonization process for high-magnesium low-carbon clinker, wherein the preparation method is substantially the same as that of Example 3, except that phosphogypsum is not added.

[0086] Comparative Example 6

[0087] A carbonization process for high-magnesium low-carbon clinker, the preparation method of which is substantially the same as that of Example 3, except that MgSO4 is not added.

[0088] Comparative Example 7

[0089] A carbonization process for high-magnesium low-carbon clinker, wherein the preparation method is substantially the same as that of Example 2, except that phosphogypsum and MgSO4 are not added.

[0090] The compressive strength of the sample after carbonization is the carbonization strength. The carbonization strength and carbon fixation rate of each embodiment and comparative example after carbonization are shown in Table 4.

[0091] Table 4 Carbonization intensity and carbon fixation rate

[0092] project Carbonization strength / MPa Carbon fixation rate / % Example 1 136.75 21.34 Example 2 118.47 21.09 Example 3 109.64 20.33 Comparative Example 1 100.95 15.78 Comparative Example 2 119.22 19.96 Comparative Example 3 120.36 18.62 Comparative Example 4 63.21 14.82 Comparative Example 5 81.54 18.65 Comparative Example 6 84.33 18.31 Comparative Example 7 81.74 15.20

[0093] The main function of phosphogypsum is to induce Mg in high-Mg-low-C clinker. 2+ The dissolution of MgSO4, through reaction 1 to reaction 4, makes its own CaSO4·2H2O be carbonized into CaCO3 for filling the structural pores, and releases water that is not used for pressing and forming during the carbonization process to replenish water for the system and prolong the effective carbonization time; the role of MgSO4 is mainly to promote the Ca in high-magnesium low-carbon clinker 2+ The dissolution of CaCO3 is formed through reaction 1 to reaction 4, which changes the carbonization from an acid-base neutralization reaction to a double decomposition reaction without acid-base neutralization, thus reducing the alkalinity of the reaction system and the dissolved Ca 2+ The carbonization rate makes this part of Ca 2+ It can be better transported with water, so that CaCO3 is generated in the pores on the surface of non-high-magnesium low-carbon clinker. Secondly, the generation rate of CaCO3 slows down and the supersaturation decreases, which promotes the formation of aragonite with a large aspect ratio, which plays a more effective role in filling and connecting the pores, which is beneficial to the continuous carbonization of high-magnesium low-carbon clinker.

[0094] Although the addition of phosphogypsum can directly react with Mg in high-Mg-LC clinker to generate a certain amount of MgSO4 through reaction 4, the CaSO4·2H2O activity of phosphogypsum itself is low and the reaction rate is slow. Therefore, the effect of using only phosphogypsum is poor and MgSO4 needs to be added additionally.

[0095] Figure 1 This is the SEM image of the carbonization product obtained in Example 1. It can be observed that aragonite with an aspect ratio significantly larger than that of calcite is generated and can be filled into pores farther away from the high-magnesium and low-carbon clinker particles.

[0096] In summary, compared with the comparative example, the simultaneous addition of phosphogypsum and MgSO4 as acid activators for high-magnesium low-carbon clinker can more significantly improve its carbonization performance.

[0097] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A method for improving the carbonization performance of high-magnesium low-carbon clinker, characterized in that: The following steps are involved: (1) mixing high-magnesium low-carbon clinker, an acidic activator and water, and pressing and molding; wherein the acidic activator comprises phosphogypsum and MgSO4; (2) Drying the molded sample and adjusting the moisture content, and carbonizing the sample to obtain a carbonized product.

2. The method according to claim 1, characterized in that The high-magnesium, low-carbon clinker is mainly composed of one or more of magnesium calcium silicate minerals C7MS4, C3MS2, and C2MS2.

3. The method according to claim 1, characterized in that The chemical components and their mass percentages in the high-magnesium low-carbon clinker include: CaO 37-59%, SiO2 25-47%, Al2O3 0-10%, Fe2O3 0-10%, and MgO 5-15%.

4. The method according to claim 1, characterized in that In the acidic activator described in step (1), the amount of phosphogypsum is 5-20wt% of the amount of high-magnesium low-carbon clinker, and the amount of MgSO4 is 0.5-5wt% of the amount of high-magnesium low-carbon clinker.

5. The method according to claim 1, characterized in that The pH value of the phosphogypsum is 1-6.

6. The method according to claim 1, characterized in that The amount of water used is 10-25wt% of the amount of high-magnesium low-carbon clinker used.

7. The method according to claim 1, characterized in that In step (2), the moisture content is adjusted to be 4-20 wt%.

8. The method according to claim 1, characterized in that In step (2), the carbonization step adopts a CO2 concentration of 15-100%, a temperature of 20-50°C, a humidity of 40-80%, an air pressure of 0-0.3MPa, and a carbonization time of 6-72h.

Citation Information

Patent Citations

  • Carbonized plate based on low-grade low-carbon cement clinker and preparation method thereof

    CN115557756A

  • High-magnesium low-carbon cement clinker and preparation method thereof

    CN116553842A