Preparation method of anti-radiation and wave-absorbing functional structure integrated ceramic matrix composite material

By using the coating and laying method and CVI process to deposit the interface and matrix in the ceramic-based composite material, the SiCf/Si3N4-WBS composite material is formed, which solves the problem of insufficient performance of ceramic-based radiation shielding materials in high temperature environments and achieves high efficiency Radiation shielding and electromagnetic wave absorption effects.

CN119059825AInactive Publication Date: 2024-12-03RES & DEV INST OF NORTHWESTERN POLYTECHNICAL UNIV IN SHENZHEN
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411250602.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The shielding performance of ceramic-based radiation shielding materials is limited, especially in high-energy zones and complex environments, and the prior art is difficult to effectively serve in high-temperature environments.

Method used

The coating layering method was used to introduce functional component particles and CVI process to deposit interfaces and substrates, and prepare a ceramic matrix composite material with radiation-resistant and wave-absorbing functional structures. By depositing boron nitride BN interface and silicon nitride Si3N4 protective layer, And the mixed slurry is applied on the SiC fiber cloth to form a SiCf/Si3N4-WBS composite material to improve the density and wave absorption performance.

Benefits of technology

The multifunctional radiation shielding and electromagnetic wave absorption of ceramic matrix composite materials in high temperature environments have been realized. The linear attenuation coefficient and mass attenuation coefficient reach 0.263cm-1 and 0.105cm2/g respectively, the shielding effect reaches more than 70%, and the electromagnetic wave absorption rate is approximately 80%, effective absorbance bandwidth is 2.7GHz.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059825A_ABST
    Figure CN119059825A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of an anti-radiation and wave-absorbing functional structure integrated ceramic matrix composite material. The preparation method comprises the following steps: firstly, preparing silicon carbide (SiC) prefabricated cloth and coating slurry; secondly, uniformly coating the slurry on the surface of the SiC prefabricated cloth, and laminating and fixing; and finally, performing chemical vapor infiltration (CVI) process on the laminated and fixed preform to deposit a silicon nitride (Si3N4) matrix for densification. According to the preparation method provided by the invention, the integration of anti-radiation and wave-absorbing functional structures of the ceramic-based composite material is realized, so that the radiation shielding material serves in a higher-temperature environment, and the overall comprehensive performance and high-temperature environment applicability of the ceramic-based composite material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of radiation shielding materials and relates to a method for preparing a ceramic-based composite material with an integrated radiation-resistant and wave-absorbing functional structure. Background Art

[0002] With the development of nuclear technology and the increasing application of nuclear energy in aerospace, military, industry, medical and other fields, while it promotes social development and brings huge benefits, it will also face the problem of increasing radiation sources and the risk of radiation exposure to personnel and equipment increasing accordingly.

[0003] Therefore, mankind has placed nuclear safety in an increasingly important position. Radiation shielding materials (RSMs) are an important part of achieving nuclear safety. In order to ensure the safety of personnel and equipment in a radiation environment and to actively and effectively use nuclear energy, the development of efficient radiation shielding materials is an inevitable trend and an important issue that cannot be ignored.

[0004] At present, in the field of radiation shielding and protection, the research and application of ceramic-based shielding materials are relatively small compared with metal-based shielding materials, polymer-based shielding materials, concrete, and glass shielding materials. In recent years, research on new ceramic radiation shielding materials has gradually increased, especially spinel ferrites (MFe2O4 (M=Co, Cu, Mn, Zn, Ni, etc.)), barium titanate (BaTiO3, referred to as BTO) and some high-temperature superconductor materials (REBCO, BSCCO, YBCO). Studies have shown that ZnFe2O4 has the best shielding parameters among many spinel ferrites; the performance of BTO in radiation protection depends on the nature of the dopant. For example, adding zinc and tungsten oxides to BaTiO3 can improve its radiation shielding performance, while adding silicon dioxide weakens its shielding ability. Therefore, it is very important to select a suitable dopant to improve its radiation shielding performance. However, the shielding performance of ceramic radiation shielding materials is limited, mainly reflected in the relatively good shielding performance in the low-energy zone, but there is still a large gap compared with other materials. As a potential alternative material in the field of radiation shielding, there is still a lot of room for improvement in performance.

[0005] The development of radiation shielding materials requires not only the optimization of traditional shielding materials, but also the development of new shielding materials to meet the needs of complex application environments. The design of shielding materials needs to meet the requirements of low cost, rapid preparation, multi-function, safety, and comprehensiveness as much as possible. Ceramic-based composite materials have excellent properties such as strong designability, high temperature resistance, high strength, and light weight. From the perspective of materials, the development of lightweight, high-strength, high-efficiency, and multifunctional new shielding materials is an important direction for current and future research in this field. Summary of the invention

[0006] Technical issues to be solved

[0007] In order to avoid the shortcomings of the prior art, the present invention proposes a method for preparing a ceramic matrix composite material with integrated radiation-absorbing functional structure to meet the multifunctional requirements of radiation shielding materials in complex and harsh environments. The ceramic matrix composite material with integrated radiation-absorbing functional structure can be prepared by introducing functional component particles by coating and layering method and depositing interface and matrix by CVI process.

[0008] Technical Solution

[0009] A method for preparing a ceramic-based composite material with an integrated radiation-resistant and wave-absorbing functional structure, characterized by the following steps:

[0010] Step 1: using CVI process to deposit boron nitride BN interface and silicon nitride Si3N4 protective layer on SiC fiber cloth in sequence; the SiC fiber cloth is a plurality of layers stacked and fixed; the deposited boron nitride BN interface has a thickness of 450-500nm; the thickness of silicon nitride Si3N4 protective layer has a thickness of 2.5-4.5μm;

[0011] When the CVI process is used to deposit the boron nitride BN interface, the precursor gas sources are boron trichloride BCl3 and ammonia NH3, wherein BCl3 is a boron source, NH3 is a nitrogen source, the carrier gas is argon Ar, and the dilution gas is hydrogen H2;

[0012] When the CVI process is used to deposit the silicon nitride Si3N4 protective layer, the precursor gas sources are silicon tetrachloride SiCl4 and ammonia NH3, wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon Ar, and the diluent gas is hydrogen H2;

[0013] Step 2: Applying the mixed slurry on the SiC fiber cloth with a protective layer;

[0014] The mixed slurry is a mixture of mixed powder and ultrapure water; wherein the mixed powder includes 50% to 60% by volume of W powder, 30% to 40% of B4C powder and 10% to 20% of Sm2O3 powder;

[0015] Step 3: After the SiC fiber cloth coated with the mixed slurry is stacked, the Si3N4 matrix is ​​deposited using the CVI process to densify the SiC prefabricated cloth. During the deposition, the precursor gas sources are silicon tetrachloride SiCl4 and ammonia NH3, wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon Ar, and the dilution gas is hydrogen H2.

[0016] When the CVI process is used to deposit the boron nitride BN interface, the deposition time is 160 to 260 hours, the deposition temperature is 650 to 850° C., and the gas flow ratio is: silicon source SiCl4 is 20 to 30 ml / min, nitrogen source NH3 is 60 to 70 ml / min, carrier gas argon Ar is 100 to 120 ml / min, and dilution gas hydrogen H2 is 100 to 120 ml / min.

[0017] When the CVI process is used to deposit the silicon nitride Si3N4 protective layer, the deposition time is 120 to 220 hours, the deposition temperature is 800 to 1000°C, and the gas flow ratio is: silicon source SiCl4 is 100 to 110 ml / min, nitrogen source NH3 is 60 to 70 ml / min, carrier gas argon Ar is 100 to 120 ml / min, and dilution gas hydrogen H2 is 100 to 120 ml / min.

[0018] The mixed powder is prepared by ball milling, with a ball-to-material ratio of 7:1 to 8:1 and a ball milling time of 24 to 28 hours.

[0019] The mixed powder and ultrapure water are mixed in a mass ratio of 4:1 to 6:1.

[0020] When the mixed powder is mixed with ultrapure water, the mixture is evenly mixed in an electric stirrer at a rotation speed of 200 to 400 rpm for a time of 10 to 20 minutes.

[0021] When the Si3N4 substrate is deposited by the CVI process in step 3, the deposition temperature is 800-1000, and the gas flow ratio is: silicon source SiCl4 is 100-110 ml / min, nitrogen source NH3 is 60-70 ml / min, carrier gas argon Ar is 100-120 ml / min, and dilution gas hydrogen H2 is 100-120 ml / min.

[0022] The SiC fiber cloth is a 2D SiC fiber cloth, and the number of the multiple layers is 10 to 14.

[0023] A ceramic matrix composite material with integrated radiation-resistant and wave-absorbing functional structure prepared by the preparation method, characterized in that: the composite structure is SiC f / SiC-W-B4C-Sm2O3, including SiC fiber cloth, a boron nitride BN interface with a thickness of 450-500nm on the SiC fiber cloth; a silicon nitride Si3N4 with a thickness of 2.5-4.5μm on the BN interface; functional component particles are introduced into the SiC fiber cloth by a coating and layering method to form a WBS (W-B4C-Sm2O3) functional filling material, and the overall structure is obtained by CVI process deposition and densification. The obtained SiC f / Si3N4-WBS composite material has a densification degree of no less than 85%, and the linear attenuation coefficient and mass attenuation coefficient are 0.263cm -1 and 0.105cm 2 / g, the shielding effect is over 70%; the RL value reaches full-frequency absorption below -7dB, the electromagnetic wave absorption rate is about over 80%, and the effective absorbing bandwidth is 2.7GHz.

[0024] An application of the anti-radiation-wave absorbing functional structure integrated ceramic-based composite material is characterized by being used in a high-temperature irradiation complex environment with a temperature not higher than 800°C, a radiation source energy and an electromagnetic wave frequency of 0.662MeV and 12.4GHz respectively, and the shielding effect and electromagnetic wave absorption rate can reach 70% and 80% or more respectively.

[0025] Beneficial Effects

[0026] The present invention proposes a method for preparing a ceramic matrix composite material with an integrated radiation-resistant and wave-absorbing functional structure. First, a silicon carbide (SiC) prefabricated cloth and a coating slurry are prepared; secondly, the slurry is evenly coated on the surface of the SiC prefabricated cloth and laminated and fixed; finally, the laminated and fixed prefabricated body is subjected to a chemical vapor infiltration (CVI) process to deposit a silicon nitride (Si3N4) matrix for densification. The preparation method provided by the present invention realizes the integration of the radiation-resistant and wave-absorbing functional structure of the ceramic matrix composite material, enables the radiation shielding material to serve in a higher temperature environment, and improves the overall comprehensive performance and high temperature environment applicability of the ceramic matrix composite material.

[0027] In terms of densification, SiC f / The densification degree of Si3N4-WBS composite material is not less than 85%;

[0028] The radiation resistance of the composite material is good at 137Cs source with higher energy (not less than 0.662MeV), SiC f The linear attenuation coefficient and mass attenuation coefficient of the / Si3N4-WBS composite material are 0.263 cm -1 and 0.105cm 2 / g, the half-value layer is about 2.64cm, and when the thickness of the composite material is greater than 0.47cm, the shielding effect can reach more than 70%;

[0029] In terms of the microwave absorption performance of this composite material, under the X-band conditions of 8.2 to 12.4 GHz, SiC f The real part, imaginary part and dielectric loss tangent of the average dielectric constant of the / Si3N4-WBS composite material are approximately 10.94, 5.01 and 0.46, respectively. When the thickness of the composite material is 2.3mm, the RL value can reach full-frequency absorption below -7dB, the electromagnetic wave absorption rate is approximately more than 80%, and the effective absorption bandwidth is 2.7GHz.

[0030] By adopting the technical solution of the present invention, the advantages and beneficial effects are as follows: after the BN interface and Si3N4 protective layer are deposited on the surface of the SiC fiber cloth, W, B4C, Sm2O3 (WBS) functional component particles are introduced into the SiC preform by using the coating and laying method, wherein W is used as a gamma-ray shielding component, B4C is used as a neutron radiation shielding component, and Sm2O3 is used as a coordination component, which makes up for the insufficient performance of W and B4C in radiation shielding, and at the same time improves the wave absorption performance of the overall material. In the process of depositing the matrix using the CVI process, the functional component particle WBS mixture reacts with the deposited Si3N4 matrix during the high-temperature CVI process, and a Si-Sm-ON glass phase is formed at the interface between the Si3N4 matrix and the WBS, and a transition layer is formed on both sides of the glass phase, which improves the problem of weak interlayer bonding to a certain extent. As the glass phase layer thickens, the glass phase grows toward the direction of high gas concentration in the pores and is accompanied by the deposition and wrapping of the Si3N4 matrix, eventually forming a rod-shaped core-shell structure, which fills the pores between some fiber bundles and improves the densification of the composite material. The process changed by the present invention cannot be simply determined.

[0031] The present invention introduces functional component particles through a coating layer method and deposits interfaces and substrates through a CVI process, thereby preparing a ceramic-based composite material with integrated radiation-resistant and wave-absorbing functional structures, allowing the radiation shielding material to serve in a higher temperature environment while meeting the multifunctional requirements of the radiation shielding material in complex and harsh environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Preparation of SiC for the embodiment of the present invention f / Process flow chart of SiC-W-B4C-Sm2O3 composite material;

[0033] Figure 2 SiC prepared in the embodiment of the present invention f Scanning electron microscope (SEM) image and EDS spectrum of the cross section of the SiC-W-B4C-Sm2O3 composite material, (a) morphology distribution characteristics of each component at low magnification, (b) rods generated in the pores, (c) growth morphology of rods at high magnification, (d) internal morphology of rods and surface scanning images of Si, N, Sm, and O elements, (e) white glass phase and distribution of each component and surface scanning images of W, B, Sm, Si, C, and N elements;

[0034] Figure 3 SiC prepared in the embodiment of the present invention f SiC / SiC-W-B4C-Sm2O3 composites at 0.662MeV energy f / The radiation shielding performance of Si3N4-W-B4C-Sm2O3 composite material and its comparison with the shielding performance of reported typical radiation shielding materials;

[0035] Figure 4 SiC prepared in the embodiment of the present invention f Three-dimensional RL diagram of the microwave absorption performance of / SiC-W-B4C-Sm2O3 composite material varying with frequency and thickness. DETAILED DESCRIPTION

[0036] The present invention will now be further described with reference to the embodiments and the accompanying drawings:

[0037] A method for preparing a ceramic-based composite material with an integrated radiation-resistant and wave-absorbing functional structure, characterized in that it comprises the following steps:

[0038] Step 1: Preparation of SiC prefabricated cloth: Use a steel ruler to measure a certain size of fiber cloth on the SiC fiber cloth, use a knife to cut a certain number of pieces according to the size, and fix it with a splint. Use the CVI process to deposit boron nitride (BN) interface and silicon nitride (Si3N4) protective layer on the fixed SiC fiber cloth in sequence;

[0039] Furthermore, the SiC fiber cloth described in step 1 is a 2D SiC fiber cloth having a length of 250 mm and a width of 150 mm, and a total number of 10 to 14 sheets.

[0040] Furthermore, the precursor gas sources used for depositing the BN interface in the CVI process described in step 1 are boron trichloride (BCl3) and ammonia (NH3), wherein BCl3 is a boron source, NH3 is a nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 20-30 ml / min, 60-70 ml / min, 100-120 ml / min, and 100-120 ml / min, respectively. The deposition time is 160-260 h, the deposition temperature is 650-850 ° C, and the thickness is about 450-500 nm.

[0041] Furthermore, the precursor gas sources used for depositing the Si3N4 protective layer by the CVI process described in step 1 are silicon tetrachloride (SiCl4) and ammonia (NH3), wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 100-110 ml / min, 60-70 ml / min, 100-120 ml / min, and 100-120 ml / min, respectively. The deposition time is 120-220 h, the deposition temperature is 800-1000°C, and the thickness is about 2.5-4.5 μm.

[0042] Step 2: Preparation of mixed slurry: W powder, B4C powder and Sm2O3 powder are mixed in a certain proportion to form a mixed powder, which is then mixed with ultrapure water and stirred evenly to form a mixed slurry;

[0043] Furthermore, the mixed powder described in step 2 contains tungsten (W) powder, boron carbide (B4C) powder and samarium oxide (Sm2O3) powder, wherein the volume fraction of tungsten (W) powder is 50% to 60%, boron carbide (B4C) powder is 30% to 40%, and samarium oxide (Sm2O3) powder is 10% to 20%. In the ball milling process, the ball-to-material ratio is 7:1 to 8:1, and the ball milling time is 24 to 28 hours.

[0044] Furthermore, the mixed slurry described in step 2 is mixed with ultrapure water in a mass ratio of 4:1 to 6:1, and is mixed evenly in an electric stirrer at a speed of 200 to 400 rpm for 10 to 20 minutes.

[0045] Step 3: Matrix densification: Use a brush to evenly apply the mixed slurry prepared in step (2) to the surface of the SiC prefabricated cloth prepared in step (1) and laminate and fix them, then use the CVI process to deposit the Si3N4 matrix to densify the SiC prefabricated cloth.

[0046] Furthermore, the precursor gas sources used for densifying the substrate by the CVI process described in step 3 are silicon tetrachloride (SiCl4) and ammonia (NH3), wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 100-120 ml / min, 60-70 ml / min, 100-120 ml / min, and 100-120 ml / min, respectively, and the deposition temperature is 800-1000°C.

[0047] Embodiment 1:

[0048] In this embodiment, the SiC prepared by the coating layer method f The volume fraction ratio of the functional component particles in the / SiC-W-B4C-Sm2O3 composite material is 5:3:2, and the thickness is 2.77 mm.

[0049] (1) Preparation of SiC prefabricated cloth: Use a steel ruler to measure the size of 250mm×150mm on the 2D SiC fiber cloth, and use a knife to cut it according to the size. A total of 10 sheets are cut, and they are soaked in anhydrous ethanol for ultrasonic cleaning. After removing surface impurities and drying, they are aligned and stacked. Use a graphite splint to fix the arranged SiC fiber cloth, and fix it around with graphite bolts to ensure the flatness of the SiC fiber cloth; then use the CVI process to deposit the BN interface. The precursor gas sources used are boron trichloride (BCl3) and ammonia (NH3), where BCl3 is the boron source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 20ml / min, 60ml / min, 100ml / min, and 100ml / min, respectively. The deposition time is 160h, and the deposition time is 160h. The deposition temperature is 650℃ and the thickness is about 450nm; then the CVI process is used to deposit the Si3N4 protective layer. The precursor gas sources used are silicon tetrachloride (SiCl4) and ammonia (NH3), among which SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 100ml / min, 60ml / min, 100ml / min, and 100ml / min respectively. The deposition time is 120h, the deposition temperature is 800℃, and the thickness is about 2.5μm.

[0050] (2) Preparation of mixed slurry: W powder, B4C powder and Sm2O3 powder were mixed in a volume fraction ratio of 5:3:2, and the mixed powder was placed in a ball mill and ball milled for 24 hours at a ball-to-material ratio of 7:1 to form a mixed powder. Then, the uniformly mixed powder was ground and sieved to obtain a filler powder mixture. The filler powder mixture and the solution carrier (water and xylene) were placed in a beaker at a mass ratio of 4:1, and mixed evenly using an electric stirrer at a speed of 200 rpm and a stirring time of 10 min to obtain a non-fluid coating slurry.

[0051] (3) Matrix densification: The slurry prepared in step (2) is then evenly applied to the surface of the SiC fiber prefabricated fabric prepared in step (1) with a brush, and then multiple layers of prefabricated fabrics coated with the slurry are stacked and fixed with a graphite clamp. Finally, the Si3N4 matrix is ​​densified using the CVI process. The precursor gas sources used are silicon tetrachloride (SiCl4) and ammonia (NH3), wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 100 ml / min, 60 ml / min, 100 ml / min, and 100 ml / min, respectively, and the deposition temperature is 800°C.

[0052] Embodiment 2:

[0053] In this embodiment, the SiC prepared by the coating layer method f The volume fraction ratio of the functional component particles in the / SiC-W-B4C-Sm2O3 composite material is 5:4:1, and the thickness is 3.32 mm.

[0054] (1) Preparation of SiC prefabricated cloth: Use a steel ruler to measure the size of 250mm×150mm on the 2D SiC fiber cloth, and use a knife to cut it according to the size. A total of 12 sheets are cut, and they are soaked in anhydrous ethanol for ultrasonic cleaning. After removing surface impurities and drying, they are aligned and stacked. Use a graphite splint to fix the arranged SiC fiber cloth, and fix it around with graphite bolts to ensure the flatness of the SiC fiber cloth; then use the CVI process to deposit the BN interface. The precursor gas sources used are boron trichloride (BCl3) and ammonia (NH3), where BCl3 is the boron source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 25ml / min, 65ml / min, 110ml / min, and 110ml / min, respectively. The deposition time is 210h, and the deposition time is 210h. The deposition temperature is 750℃ and the thickness is about 470nm; then the CVI process is used to deposit the Si3N4 protective layer. The precursor gas sources used are silicon tetrachloride (SiCl4) and ammonia (NH3), among which SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 105ml / min, 65ml / min, 110ml / min, and 110ml / min respectively. The deposition time is 170h, the deposition temperature is 900℃, and the thickness is about 3.5μm.

[0055] (2) Preparation of mixed slurry: W powder, B4C powder and Sm2O3 powder were mixed in a volume fraction ratio of 5:4:1, and the mixed powder was placed in a ball mill and ball milled for 26 hours at a ball-to-material ratio of 7:1 to form a mixed powder. Then, the mixed powder was ground and sieved to obtain a filler powder mixture. The filler powder mixture and the solution carrier (water and xylene) were placed in a beaker at a mass ratio of 5:1 and mixed evenly using an electric stirrer at a speed of 300 rpm for 15 min to obtain a non-fluid coating slurry. The SiC f / SiC-W-B4C-Sm2O3 composite material functional component particles Figure 2 .

[0056] (3) Matrix densification: The slurry prepared in step (2) is then evenly applied to the surface of the SiC fiber prefabricated fabric prepared in step (1) with a brush, and then multiple layers of prefabricated fabrics coated with the slurry are stacked and fixed with a graphite clamp. Finally, the Si3N4 matrix is ​​densified using the CVI process. The precursor gas sources used are silicon tetrachloride (SiCl4) and ammonia (NH3), wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 110 ml / min, 65 ml / min, 110 ml / min, and 110 ml / min, respectively. The deposition temperature is 900 °C. The SiC prepared by the coating layer method f The shielding performance of SiC-W-B4C-Sm2O3 composites is compared with other shielding materials. Figure 3 And the variation of its wave absorption performance with frequency and thickness can be seen in Figure 4 .

[0057] Embodiment 3:

[0058] In this embodiment, the SiC prepared by the coating layer method f The volume fraction ratio of the functional component particles in the / SiC-W-B4C-Sm2O3 composite material is 6:3:1, and the thickness is 3.88 mm.

[0059] (1) Preparation of SiC prefabricated cloth: Use a steel ruler to measure the size of 250mm×150mm on the 2D SiC fiber cloth, and use a knife to cut it according to the size. A total of 14 sheets are cut, and they are soaked in anhydrous ethanol for ultrasonic cleaning. After removing surface impurities and drying, they are aligned and stacked. Use a graphite splint to fix the arranged SiC fiber cloth, and fix it around with graphite bolts to ensure the flatness of the SiC fiber cloth; then use the CVI process to deposit the BN interface. The precursor gas sources used are boron trichloride (BCl3) and ammonia (NH3), where BCl3 is the boron source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 30ml / min, 70ml / min, 120ml / min, and 120ml / min, respectively. The deposition time is 260h, and the deposition time is 260h. The deposition temperature is 850℃ and the thickness is about 500nm; then the CVI process is used to deposit the Si3N4 protective layer. The precursor gas sources used are silicon tetrachloride (SiCl4) and ammonia (NH3), among which SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 110ml / min, 70ml / min, 120ml / min, and 120ml / min respectively. The deposition time is 220h, the deposition temperature is 1000℃, and the thickness is about 4.5μm.

[0060] (2) Preparation of mixed slurry: W powder, B4C powder and Sm2O3 powder were mixed in a volume fraction ratio of 6:3:1, and the mixed powder was placed in a ball mill and ball milled for 28 hours at a ball-to-material ratio of 8:1 to form a mixed powder. Then, the uniformly mixed powder was ground and sieved to obtain a filler powder mixture. The filler powder mixture and the solution carrier (water and xylene) were placed in a beaker at a mass ratio of 6:1, and mixed evenly using an electric stirrer at a speed of 400 rpm for 20 min to obtain a non-fluid coating slurry.

[0061] (3) Matrix densification: The slurry prepared in step (2) is then evenly applied to the surface of the SiC fiber prefabricated fabric prepared in step (1) with a brush, and then multiple layers of prefabricated fabrics coated with the slurry are stacked and fixed with a graphite clamp. Finally, the Si3N4 matrix is ​​densified using the CVI process. The precursor gas sources used are silicon tetrachloride (SiCl4) and ammonia (NH3), wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon (Ar), and the dilution gas is hydrogen (H2). The gas flow rates are 120 ml / min, 70 ml / min, 120 ml / min, and 120 ml / min, respectively, and the deposition temperature is 1000°C.

[0062] With reference to Examples 1-3 of the present invention, other components, proportions and specific preparation process parameters can be selected according to actual needs, and the technical effects recorded in the present invention can all be achieved. Therefore, the present invention will no longer list and explain them one by one.

[0063] The beneficial effects of the method and the prepared materials shown in the embodiments and drawings are as follows:

[0064] Figure 2 .SiC f SEM images and EDS energy spectrum surface scanning results of the internal microstructure of the / Si3N4-W-B4C-Sm2O3 composite material: (a) morphology distribution characteristics of each component at low magnification, (b) rods generated in the pores, (c) growth morphology of rods at high magnification, (d) internal morphology of rods and surface scanning images of Si, N, Sm, and O elements, (e) surface scanning images of the white glass phase and the distribution of each component and W, B, Sm, Si, C, and N elements.

[0065] Figure 2 It is shown that the composite material consists of the gray area (SiC fiber bundles and Si3N4 matrix) and the WBS mixed functional phase, such as Figure 2(a) shows that the fiber, the interface layer and the protective layer are tightly bonded and have a complete morphology. Only a small number of fibers at the outer edge of the fiber bundle have circumferential fractures in the interface layer and radial cracks in the Si3N4 matrix protective layer. A small amount of functional fillers flow into the interior along the crack channel. WBS is distributed in the inter-bundle pores on the inside and outside of the composite material. The Si3N4 matrix is ​​mainly wrapped around the outside of the WBS mixed phase, and the rest is dispersed inside the WBS mixed phase. Prepared SiC f In some inter-bundle holes of the Si3N4-WBS composite material, a large number of rod-like substances grow crosswise into the holes to fill the holes, such as Figure 2 (b) As shown in the EDS spectrum scan results, Figure 2 (d), the rod-like substance is Si-N phase. Its cross section shows that the rod-like substance grows with the gray-white substance as the core. The gray-white substance is enriched with Sm and O elements. In addition, it is observed that there is a large amount of gray-white phase at the junction of the Si3N4 matrix (gray phase) around the pores and the WBS mixed phase, such as Figure 2 As shown in (c), its elemental composition is basically the same as the gray-white phase in the rod-like substance.

[0066] Figure 3 .SiC at 0.662MeV energy f Radiation shielding properties of Si3N4-W-B4C-Sm2O3 composites and comparison with other radiation shielding materials: SiC f / Si3N4-W-B4C-Sm2O3 composite materials, SiC f Shielding effectiveness of BN / SiC composites and reported typical radiation shielding materials.

[0067] Figure 3 Demonstrated the shielding ability of different types of materials against 0.662MeV photon energy, SiC f The shielding performance of Si3N4-WBS composite materials is at a medium level among various materials. f The shielding performance of SiC / Si3N4-WBS composite materials is much lower than that of pure ceramic materials. f The shielding performance of Si3N4-WBS composite materials is slightly weaker than that of new shielding ceramic materials in recent years, but it has certain advantages over traditional ceramics and high-density ceramic-based composite materials; compared with resin-based materials, SiC f The shielding performance of the Si3N4-WBS composite material is much better than that of the resin-based material without high atomic number metal filler, and slightly better than that of the resin-based shielding material with a large amount of W filler. fThe mass attenuation coefficient of / Si3N4-WBS composite materials is close to that of some metal materials, and its radiation shielding performance is at an upper-middle level, narrowing the gap in radiation shielding between traditional ceramic materials and metal materials.

[0068] Figure 4 .SiC f / Microwave absorption properties of Si3N4-W-B4C-Sm2O3 composites: variation of three-dimensional RL values ​​with frequency and thickness.

[0069] Figure 4 Demonstrated SiC f The microwave absorption performance of Si3N4-WBS composite material changes with frequency and thickness: As the thickness increases, the reflection loss value of the material shows a trend of first decreasing and then increasing. When the material thickness is 1.86mm, the bandwidth of the material's RL value below -10d B covers the range of 10.9 to 12.4GHz. When the frequency gradually increases to 12.4GHz, the optimal electromagnetic absorption performance appears, and the minimum reflection loss is -24.1dB. When the RL value of the material is below -10dB, the electromagnetic wave absorption rate can reach more than 90%, and the frequency range at this time, namely the effective absorption bandwidth (EAB), is also an important reference for characterizing the absorption performance. When the material thickness is 2.15mm, the maximum EAB value of the material is 2.98GHz, and the bandwidth covers the range of 9.38 to 12.36GHz. When the material thickness is 2.3mm, full-frequency absorption below -7dB can be achieved in the X-band of 8.2 to 12.4GHz, and the electromagnetic wave absorption rate is approximately more than 80%. At this time, the effective absorption bandwidth of the material is 2.7GHz.

Claims

1. A method for preparing a ceramic matrix composite material with integrated radiation-resistant and wave-absorbing functional structures, characterized in that Here are the steps: Step 1: using CVI process to deposit boron nitride BN interface and silicon nitride Si3N4 protective layer on SiC fiber cloth in sequence; the SiC fiber cloth is a plurality of layers stacked and fixed; the deposited boron nitride BN interface has a thickness of 450-500nm; the thickness of silicon nitride Si3N4 protective layer has a thickness of 2.5-4.5μm; When the CVI process is used to deposit the boron nitride BN interface, the precursor gas sources are boron trichloride BCl3 and ammonia NH3, wherein BCl3 is a boron source, NH3 is a nitrogen source, the carrier gas is argon Ar, and the dilution gas is hydrogen H2; When the CVI process is used to deposit the silicon nitride Si3N4 protective layer, the precursor gas sources are silicon tetrachloride SiCl4 and ammonia NH3, wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon Ar, and the diluent gas is hydrogen H2; Step 2: Applying the mixed slurry on the SiC fiber cloth with a protective layer; The mixed slurry is a mixture of mixed powder and ultrapure water; wherein the mixed powder includes 50% to 60% by volume of W powder, 30% to 40% of B4C powder and 10% to 20% of Sm2O3 powder; Step 3: After the SiC fiber cloth coated with the mixed slurry is stacked, the Si3N4 matrix is ​​deposited using the CVI process to densify the SiC prefabricated cloth. During the deposition, the precursor gas sources are silicon tetrachloride SiCl4 and ammonia NH3, wherein SiCl4 is the silicon source, NH3 is the nitrogen source, the carrier gas is argon Ar, and the dilution gas is hydrogen H2.

2. The method for preparing the ceramic matrix composite material with integrated radiation resistant and microwave absorbing functional structure according to claim 1, characterized in that: When the CVI process is used to deposit the boron nitride BN interface, the deposition time is 160 to 260 hours, the deposition temperature is 650 to 850° C., and the gas flow ratio is: silicon source SiCl4 is 20 to 30 ml / min, nitrogen source NH3 is 60 to 70 ml / min, carrier gas argon Ar is 100 to 120 ml / min, and dilution gas hydrogen H2 is 100 to 120 ml / min.

3. The method for preparing the ceramic matrix composite material with integrated radiation resistant and wave absorbing functional structure according to claim 1, characterized in that: When the CVI process is used to deposit the silicon nitride Si3N4 protective layer, the deposition time is 120 to 220 hours, the deposition temperature is 800 to 1000°C, and the gas flow ratio is: silicon source SiCl4 is 100 to 110 ml / min, nitrogen source NH3 is 60 to 70 ml / min, carrier gas argon Ar is 100 to 120 ml / min, and dilution gas hydrogen H2 is 100 to 120 ml / min.

4. The method for preparing the ceramic matrix composite material with integrated radiation resistant and wave absorbing functional structure according to claim 1, characterized in that: The mixed powder is prepared by ball milling, with a ball-to-material ratio of 7:1 to 8:1 and a ball milling time of 24 to 28 hours.

5. The method for preparing the ceramic matrix composite material with integrated radiation resistant and wave absorbing functional structure according to claim 1, characterized in that: The mixed powder and ultrapure water are mixed in a mass ratio of 4:1 to 6:

1.

6. The method for preparing the ceramic matrix composite material with integrated radiation resistant and wave absorbing functional structure according to claim 1, characterized in that: When the mixed powder is mixed with ultrapure water, the mixture is evenly mixed in an electric stirrer at a rotation speed of 200 to 400 rpm for a time of 10 to 20 minutes.

7. The method for preparing the ceramic matrix composite material with integrated radiation resistant and microwave absorbing functional structure according to claim 1, characterized in that: When the Si3N4 substrate is deposited by the CVI process in step 3, the deposition temperature is 800-1000, and the gas flow ratio is: silicon source SiCl4 is 100-110 ml / min, nitrogen source NH3 is 60-70 ml / min, carrier gas argon Ar is 100-120 ml / min, and dilution gas hydrogen H2 is 100-120 ml / min.

8. The method for preparing the ceramic matrix composite material with integrated radiation resistant and wave absorbing functional structure according to claim 1, characterized in that: The SiC fiber cloth is a 2D SiC fiber cloth, and the number of the multiple layers is 10 to 14.

9. A ceramic matrix composite material with integrated radiation resistant and wave absorbing functional structure prepared by the preparation method according to any one of claims 1 to 8, characterized in that: Composite structure is SiC f / SiC-W-B4C-Sm2O3, including SiC fiber cloth, a boron nitride BN interface with a thickness of 450-500nm on the SiC fiber cloth; a silicon nitride Si3N4 with a thickness of 2.5-4.5μm on the BN interface; functional component particles are introduced into the SiC fiber cloth by a coating and layering method to form a WBS (W-B4C-Sm2O3) functional filling material, and the overall structure is obtained by CVI process deposition and densification. The obtained SiC f / Si3N4-WBS composite material has a densification degree of no less than 85%, and the linear attenuation coefficient and mass attenuation coefficient are 0.263cm -1 and 0.105cm 2 / g, the shielding effect is over 70%; the RL value reaches full-frequency absorption below -7dB, the electromagnetic wave absorption rate is about over 80%, and the effective absorbing bandwidth is 2.7GHz.

10. An application of the ceramic matrix composite material with integrated radiation resistant and wave absorbing functional structure according to claim 9, characterized in that: It is used in complex high-temperature irradiation environments with temperatures not exceeding 800°C, radiation source energy and electromagnetic wave frequency of 0.662MeV and 12.4GHz respectively. The shielding effect and electromagnetic wave absorption rate can reach over 70% and 80% respectively.

Citation Information

Cited By

  • Fiber-reinforced barium titanate-polymer conversion ceramic-based composite wave-absorbing material and preparation method thereof

    CN119707517A

  • Preparation method of nitride ceramic environment sealing layer

    CN121470994A