Preparation method and application of polyester / nano lignin-ZnO composite film
By preparing nanolignin coated ZnO hybrid nanoparticles and combining with surfactant modification, the problem of poor dispersion of degradable polyester materials in the food and drug packaging fields is solved, and polyester/nanolignin is realized -The high-efficiency antibacterial, antioxidant and anti-ultraviolet properties of -ZnO composite membranes have broadened the application fields of ZnO.
Patent Information
- Application Number
- CN202411272647.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-03
AI Technical Summary
The application of existing degradable polyester materials in food, drug packaging and other fields is limited by their single function, sensitivity to bacteria, active free radicals, ultraviolet rays, poor dispersion of lignin in composite materials and ZnO in photothermal Free radicals under conditions have adverse health effects.
The nanolignin-coated ZnO hybrid nanoparticles were prepared by hydrothermal method, and polyester/nanolignin-ZnO composite film was prepared by surfactant modification, combined with melt casting or solution casting to enhance its mechanical strength and antibacterial , antioxidant and anti-ultraviolet aging properties.
The excellent antibacterial, antioxidant and ultraviolet properties of the composite film are achieved, the application field of ZnO is broadened, the antibacterial activity of lignin is improved, and the breathability, hydrophobicity and degradability of the material are maintained.
Smart Images

Figure CN119060378A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer composite materials, and in particular to a preparation method of a polyester / nano-lignin-ZnO composite film and application thereof. Background Art
[0002] Among synthetic biodegradable plastics, degradable polyester materials have a broad development prospect. Most degradable polyester materials have good processing properties, mechanical properties, ductility and heat resistance. However, like many traditional materials, most degradable polyester materials have a single function and cannot resist the invasion of bacteria, active free radicals and ultraviolet rays, which greatly limits their application in food and drug packaging, medical devices and other fields.
[0003] As the second most abundant natural polymer in the world, lignin has rich phenolic hydroxyl, methoxyl and other functional groups, which give it good biological activity, such as antioxidant, antibacterial, and anti-ultraviolet properties. This makes lignin a biological additive in the fields of composite materials and has broad application prospects, but the antibacterial and antioxidant properties of single lignin are still slightly insufficient when applied. The literature (Pharmaceutics, 2019, 11, 165) reported that when unmodified lignin was applied to polyester materials as a single additive, the residual DPPH content of the composite material decreased significantly with the increase of lignin dosage and time. The residual amount of DPPH in the composite material with 3% lignin content after 5h antioxidant test was only about 20%. However, no matter how much lignin was added, no matter how long the antibacterial effect lasted, the bacterial adhesion of the composite material hardly changed. It can be seen that it is difficult for pure lignin to have good antibacterial properties while having high antioxidant properties. At the same time, the various intermolecular coupling effects of lignin, hydrogen bonds between hydroxyl molecules and within molecules, intermolecular and intramolecular interactions, and the formation of cross-linked networks at high temperatures all make the dispersion of lignin in biodegradable polyesters poor. ZnO is a widely used inorganic antibacterial metal oxide with high photocatalytic activity, biocompatibility, and safety and non-toxicity. It produces antibacterial ions Zn 2+, destroying cell membranes and inducing oxidative stress to achieve the purpose of antibacterial and bactericidal effects. However, the literature (The Journal of Physical Chemistry C 2024, 128, 5179-5188) mentioned that the large amount of free radicals produced by ZnO under photothermal conditions can have adverse effects on human and animal health, causing cardiovascular and respiratory dysfunction, asthma, reduced blood supply and influenza infection. In addition, the large number of unstable free radicals produced by ZnO will further trigger and propagate lipid oxidation reactions, thereby leading to a decline in food quality and a serious shortening of the shelf life. The oxidized lipids produced by lipid oxidation reactions can directly lead to major human diseases, such as cancer, heart disease, etc., which also limits the application of ZnO in food and drug packaging.
[0004] In view of this, it is necessary to design an improved preparation method of polyester / nano-lignin-ZnO composite film and its application to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation method of a polyester / nano-lignin-ZnO composite film and its application.
[0006] To achieve the above-mentioned object of the invention, the present invention provides a method for preparing a polyester / nano-lignin-ZnO composite film, comprising the following steps:
[0007] S1, hydrothermally reacting a mixture of a nano-lignin suspension and a zinc acetate solution at 50-140° C. for 6-24 hours to obtain LNP-ZnO hybrid nanoparticles; slowly adding the suspension of the LNP-ZnO hybrid nanoparticles into a surfactant solution to obtain modified nano-lignin;
[0008] S2. Using the modified nano-lignin and polyester obtained in step S1 as raw materials, a polyester / nano-lignin-ZnO composite film is prepared by a melt casting method or a solution casting method.
[0009] Preferably, in step S1, the mass ratio of nano-lignin to zinc acetate in the mixed solution is 5:1-1:1.
[0010] Preferably, in step S2, the added amount of the modified nano-lignin is 0.5-5 wt % of the total mass of the modified nano-lignin and the polyester.
[0011] Preferably, in step S1, the nano-lignin suspension is prepared by dissolving nano-lignin in a NaOH solution with a concentration of 0.01-0.1 g / mL, and the concentration of the NaOH solution is 0.01-1 mol / L; the nano-lignin is one of alkali lignin, lignin sulfonate, sulfate lignin, and organic solvent lignin.
[0012] Preferably, the surfactant solution is obtained by dispersing a surfactant in a first organic solvent, and its concentration is 0.5-40 g / L; the surfactant is one or more of dodecyltrimethylammonium bromide, didodecyldimethylammonium bromide, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, and hexadecylpyridinium chloride, and the first organic solvent is one or more of ethanol, isopropanol, methanol, and acetone.
[0013] Preferably, in step S2, the method for preparing the polyester / nano-lignin-ZnO composite film by melt casting is as follows: the modified nano-lignin and the polyester are added to a device for melt processing and mixed evenly, and then reacted at 120-180° C. for 5-10 minutes to obtain the polyester / nano-lignin-ZnO composite film by melt casting.
[0014] Preferably, in step S2, the method for preparing the polyester / nano-lignin-ZnO composite film by solution casting is as follows: the polyester and the modified nano-lignin are respectively dissolved in a second organic solvent to obtain a polyester solution and a modified nano-lignin dispersion; under mechanical stirring, the modified nano-lignin dispersion is slowly added to the polyester solution, and stirred for 15-45 minutes to obtain a mixed solution; the mixed solution is poured into a flat dish to form a film, and then subjected to hot pressing treatment to obtain the polyester / nano-lignin-ZnO composite film.
[0015] Preferably, the temperature of the hot pressing treatment is 120-200° C., and the hot pressing time is 3-10 min.
[0016] Preferably, the polyester is one of polybutylene adipate / terephthalate, polylactic acid, polybutylene succinate, polyglycolic acid, polycaprolactone, and polyhydroxybutyrate, and the weight average molecular weight of the polyester is ≥5×10 4 , optical purity ≥95%.
[0017] In particular, the polyester / nano-lignin-ZnO composite film prepared by the preparation method proposed in the present invention can be applied to the fields of food, medical equipment and pharmaceutical packaging.
[0018] The beneficial effects of the present invention are:
[0019] 1. The present invention provides a method for preparing a polyester / nano-lignin-ZnO composite film. The method first adopts a hydrothermal method to prepare hybrid nanoparticles of nano-lignin-coated ZnO, and then utilizes the hydrogen bonding and electrostatic effects between the hybrid nanoparticles and a surfactant to self-assemble long-chain alkanes on the surface of the hybrid nanoparticles to obtain modified nano-lignin. Finally, the modified nano-lignin is combined with a degradable polyester to prepare a composite film with excellent mechanical strength, ultraviolet shielding, anti-ultraviolet aging, antioxidant and antibacterial properties.
[0020] 2. The preparation method of the polyester / nano-lignin-ZnO composite film provided by the present invention first coats ZnO with nano-lignin, and then uses a surfactant to perform surface hydrophobic modification on the coated ZnO. The nano-lignin can be used to adsorb free radicals generated by ZnO under light conditions to avoid the harm caused by free radicals. At the same time, the composite film is endowed with excellent antioxidant and antibacterial properties (when the addition amount of lignin hybrid nanoparticles is 0.5-5wt%, the antibacterial rate against Escherichia coli can reach 100%, and the antioxidant RSA can reach 35.3%), which broadens the application field of ZnO; secondly, by grinding the lignin and directly applying it, the lignin can be well retained. The skeleton and multiple active group structures of the present invention are conducive to the realization of the process of lignin coating ZnO. At the same time, the degree of complexation between lignin and zinc acetate can be changed by adjusting the ratio of lignin and zinc acetate, thereby adjusting the morphology and performance of hybrid nanoparticles. Furthermore, by using long-chain alkane cationic surfactants to modify the hydrophobicity of lignin hybrid nanoparticles, it can not only improve its interfacial compatibility with degradable polyester, but also make the composite film use hydrophobic long-chain alkanes to attack the lipid layer of the cell membrane when it contacts the surface of bacterial cells. The cations can adsorb negatively charged bacteria and destroy the membrane structure of the cells, thereby achieving more excellent antibacterial properties and further realizing the antibacterial activity enhancement of lignin. In addition, the polyester composite film prepared by the present invention also has the characteristics of air permeability, hydrophobicity, degradability, and environmental friendliness, and can be used as food and drug packaging materials. In the above manner, a preparation method of a polyester / nano lignin-ZnO composite film with cheap and easy-to-obtain raw materials, simple process, and high yield is provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The SEM images of LNP-ZnO hybrid nanoparticles prepared in Examples 1-6 of the present invention. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0023] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.
[0024] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0025] The method for preparing the polyester / nano-lignin-ZnO composite film provided by the present invention comprises the following steps:
[0026] S1. Preparation of modified nano-lignin: a mixture of a nano-lignin (LNP) suspension and a zinc acetate solution is subjected to a hydrothermal reaction at 50-140° C. for 6-24 hours to obtain LNP-ZnO hybrid nanoparticles; the suspension of LNP-ZnO hybrid nanoparticles is slowly added to a surfactant solution to introduce long-chain alkanes into the LNP-ZnO hybrid nanoparticles, and then the mixture is subjected to centrifugation and freeze-drying to obtain modified nano-lignin;
[0027] S2. Preparation of polyester / nano-lignin-ZnO composite film: using the modified nano-lignin and polyester prepared in step S1 as raw materials, a polyester / nano-lignin-ZnO composite film is prepared by melt casting or solution casting.
[0028] As an embodiment of the present invention, in step S1, lignin is one of alkali lignin, lignin sulfonate, sulfate lignin, and organic solvent lignin; the nano-lignin suspension is prepared by dissolving nano-lignin in a NaOH solution, and its concentration is 0.01-0.1g / mL, and the concentration of the NaOH solution is 0.01-1mol / L; the zinc acetate solution is obtained by dissolving zinc acetate in water, and its concentration is 0.01-0.3g / mL, and the mass ratio of nano-lignin to zinc acetate in the mixed solution is 1:5-15:1. In the above process, the hydrogen bonds and surface hydroxyls between nano-lignin and zinc acetate react under hydrothermal conditions to make the nano-lignin coat ZnO, so that the nano-lignin is used to adsorb the free radicals generated by ZnO under light conditions, reduce the harm caused by the presence of free radicals to ZnO, and at the same time give ZnO excellent antibacterial and antioxidant properties. When the mass ratio of nano-lignin and zinc acetate is not controlled within the above given range, the obtained composite film has poor performance.
[0029] As an embodiment of the present invention, in step S1, the particle size of the LNP-ZnO hybrid nanoparticles is 140-200 nm.
[0030] As an embodiment of the present invention, in step S1, the surfactant solution is obtained by dispersing the surfactant in the first organic solvent, and the concentration thereof is 0.5-40 g / L, and the content of the surfactant in the surfactant solution is 10-40% of the sum of the mass of nano-lignin and zinc acetate; specifically, the surfactant is one or more of dodecyltrimethylammonium bromide (DTAB), didodecyldimethylammonium bromide (DDAB), tetradecyltrimethylammonium bromide (TTAB), hexadecyltrimethylammonium chloride (CTAC), and hexadecylpyridinium chloride (CPC), and the first organic solvent is one or more of ethanol, isopropanol, methanol, and acetone.
[0031] As an embodiment of the present invention, in step S2, the added amount of the modified nano-lignin is 0.5-5wt% of the total mass of the modified nano-lignin and the polyester.
[0032] As an embodiment of the present invention, in step S2, the polyester is degradable, and is specifically one of polybutylene adipate / terephthalate (PBAT), polylactic acid (PLA), polybutylene succinate (PBS), polyglycolic acid (PGA), polycaprolactone (PCL), and polyhydroxybutyrate (PHB), and the weight average molecular weight of the polyester is ≥5×10 4 , optical purity ≥95%.
[0033] As an embodiment of the present invention, in step S2, the method for preparing a polyester / nano-lignin-ZnO composite film by melt casting is as follows: modified nano-lignin and polyester particles are added to a device for melt processing and mixed evenly, and then reacted at 120-180°C for 5-10 minutes to obtain a polyester / nano-lignin-ZnO composite film by melt casting.
[0034] As an embodiment of the present invention, in step S2, the method for preparing a polyester / nano-lignin-ZnO composite film by solution casting is as follows: dissolving polyester particles and modified nano-lignin in a second organic solvent respectively to obtain a polyester solution and a modified nano-lignin dispersion; slowly adding the modified nano-lignin dispersion to the polyester solution under mechanical stirring, stirring for 15-45 minutes to obtain a mixed solution; pouring the mixed solution into a flat dish to form a film, and then hot pressing at 120-200°C for 3-10 minutes to obtain a polyester / nano-lignin-ZnO composite film. Wherein, the second organic solvent is one or both of chloroform and dichloromethane. It should be noted that the melt casting method and solution casting method in this article are both conventional methods in the art, so they are not described in detail here.
[0035] In particular, the polyester / nano-lignin-ZnO composite film prepared by the method proposed in the present invention can be applied to the fields of food, medical equipment, and pharmaceutical packaging.
[0036] The preparation method of the polyester / nano-lignin-ZnO composite film proposed by the present invention is further described below in conjunction with specific examples:
[0037] The lignin used in the embodiments of the present invention was purchased from Sigma with a CAS number of 8068-05-1. The other reagents and raw materials can be obtained from the market unless otherwise specified.
[0038] Example 1
[0039] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0040] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 3 g of micron lignin to 150 mL of a 0.05 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a DTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. The DTAB solution is 1.8 g The DTAB powder was dissolved in 150 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 3 g of zinc acetate in 30 mL of water;
[0041] The formation mechanism of LNP-ZnO hybrid nanoparticles formed by coating ZnO with nano-lignin in the above steps is as follows: under hydrothermal reaction conditions, dehydration condensation occurs between nano-lignin and ZnO through surface hydroxyl groups to generate hydrogen bonding. During the self-assembly process, the positive charge of the surfactant interacts with the negative charge of lignin to generate electrostatic effects. The interaction between hydrogen bonding and electrostatic effects coats nano-ZnO in nano-lignin to form LNP-ZnO hybrid nanoparticles.
[0042] S2. Dissolve 12 g of PBAT in 100 mL of chloroform to obtain a PBAT solution; disperse 0.06 g of modified nano-lignin in 80 mL of chloroform to obtain a modified nano-lignin dispersion; slowly add the modified nano-lignin dispersion to the PBAT solution under mechanical stirring conditions, stir for 30 minutes, and obtain a mixed solution; pour the mixed solution into a flat dish to form a film, and then hot-press at 150° C. for 3 minutes on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm.
[0043] Example 2
[0044] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0045] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 3 g of micron lignin to 150 mL of a 0.05 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a DTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. The DTAB solution is 1.8 g The DTAB powder was dissolved in 150 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 3 g of zinc acetate in 30 mL of water;
[0046] S2. Dissolve 12 g of PBAT in 100 mL of chloroform to obtain a PBAT solution; disperse 0.31 g of modified nano-lignin in 80 mL of chloroform to obtain a modified nano-lignin dispersion; slowly add the modified nano-lignin dispersion to the PBAT solution under mechanical stirring conditions and stir for 30 minutes to obtain a mixed solution; pour the mixed solution into a flat dish to form a film, and then hot-press at 150° C. for 3 minutes on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm.
[0047] Example 3
[0048] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0049] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 3 g of micron lignin to 150 mL of a 0.05 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a DTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. The DTAB solution is 1.8 g The DTAB powder was dissolved in 150 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 1 g of zinc acetate in 30 mL of water;
[0050] S2. Dissolve 12 g of PBAT in 100 mL of chloroform to obtain a PBAT solution; disperse 0.63 g of modified nano-lignin in 80 mL of chloroform to obtain a modified nano-lignin dispersion; slowly add the modified nano-lignin dispersion to the PBAT solution under mechanical stirring conditions and stir for 30 minutes to obtain a mixed solution; pour the mixed solution into a flat dish to form a film, and then hot-press at 150° C. for 3 minutes on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm.
[0051] Example 4
[0052] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0053] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 3 g of micron lignin to 150 mL of a 0.05 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a DTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. The DTAB solution is 0.6 g The DTAB powder was dissolved in 150 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 3 g of zinc acetate in 30 mL of water;
[0054] S2. Dissolve 12 g of PBAT in 100 mL of chloroform to obtain a PBAT solution; disperse 0.31 g of modified nano-lignin in 80 mL of chloroform to obtain a modified nano-lignin dispersion; slowly add the modified nano-lignin dispersion to the PBAT solution under mechanical stirring conditions, stir for 30 minutes, and obtain a mixed solution; pour the mixed solution into a flat dish to form a film, and then hot-press at 120° C. for 5 minutes on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm.
[0055] Example 5
[0056] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0057] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 3 g of micron lignin into 150 mL of 0.05 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, and use 1 mol / L After adjusting the pH of the mixed solution to 10 with NaOH, the solution was transferred to a flask and reacted for 12 hours under a nitrogen atmosphere at 90°C. After the reaction was completed, the precipitated product was collected by centrifugation at 11000 rpm. The supernatant was replaced with distilled water during the centrifugation process. The centrifugation operation was repeated three times to obtain a water-LZn suspension; under magnetic stirring conditions, the water-LZn suspension was slowly dripped into the CPC solution, stirred for 3 hours, centrifuged 3 times, and freeze-dried to obtain modified nano-lignin; wherein the CPC solution was obtained by dissolving 2.4 g CPC powder in 150 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 3 g zinc acetate in 30 mL of water;
[0058] S2. Dissolve 12 g of PBAT in 100 mL of chloroform to obtain a PBAT solution; disperse 0.31 g of modified nano-lignin in 80 mL of chloroform to obtain a modified nano-lignin dispersion; slowly add the modified nano-lignin dispersion to the PBAT solution under mechanical stirring conditions, stir for 30 minutes, and obtain a mixed solution; pour the mixed solution into a flat dish to form a film, and then hot-press at 150° C. for 5 minutes on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm.
[0059] Example 6
[0060] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0061] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 3 g of micron lignin to 150 mL of a 0.05 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a TTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. Among them, the TTAB solution is 1.8 g The TTAB powder was dissolved in 150 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 0.6 g of zinc acetate in 30 mL of water; the SEM images of the LNP-ZnO hybrid nanoparticles formed by coating ZnO with nano-lignin in Examples 1-6 are shown in FIG. Figure 1 As shown, it can be seen from the figure that the particle size of the hybrid nanoparticles is 50-160nm;
[0062] S2. Dissolve 12 g of PBAT in 100 mL of chloroform to obtain a PBAT solution; disperse 0.31 g of modified nano-lignin in 80 mL of chloroform to obtain a modified nano-lignin dispersion; slowly add the modified nano-lignin dispersion to the PBAT solution under mechanical stirring conditions and stir for 30 minutes to obtain a mixed solution; pour the mixed solution into a flat dish to form a film, and then hot-press at 180° C. for 3 minutes on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm.
[0063] Example 7
[0064] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0065] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 18 g of micron lignin into 250 mL of a 0.2 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a DTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. The DTAB solution is 10.8 g The DTAB powder is dissolved in 500 mL of 10% ethanol solution, and the zinc acetate solution is dissolved in 90 mL of water.
[0066] S2. Add 2.52 g of the modified nano-lignin prepared in step S1 and 500 g of PBAT particles into a twin-screw extruder at the same time. The processing temperature is 160° C., the screw speed is 100 rpm, and the extrusion time of the polyester / lignin blend is maintained at 5 min. A polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm is prepared by melt casting.
[0067] Example 8
[0068] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0069] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 18 g of micron lignin into 250 mL of a 0.2 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a DTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. The DTAB solution is 10.8 g The DTAB powder was dissolved in 500 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 18 g of zinc acetate in 90 mL of water;
[0070] S2. 12.82 g of the modified nano-lignin prepared in step S1 and 500 g of PBAT particles were added into a twin-screw extruder at the same time. The processing temperature was 160° C., the screw speed was 100 rpm, and the extrusion time of the polyester / lignin blend was maintained at 5 min. A polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm was prepared by melt casting.
[0071] Example 9
[0072] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0073] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 18 g of micron lignin into 250 mL of a 0.2 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a DTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. The DTAB solution is 10.8 g DTAB powder is dissolved in 500 mL of 10% ethanol solution, and zinc acetate solution is obtained by dissolving 6.0 g of zinc acetate in 90 mL of water;
[0074] S2. Add 26.32 g of the modified nano-lignin prepared in step S1 and 500 g of PBAT particles into a twin-screw extruder at the same time. The processing temperature is 160° C., the screw speed is 100 rpm, and the extrusion time of the polyester / lignin blend is maintained at 5 min. A polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm is prepared by melt casting.
[0075] Example 10
[0076] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0077] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 18 g of micron lignin into 250 mL of a 0.2 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a DTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. The DTAB solution is 3.6 g The DTAB powder was dissolved in 500 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 18 g of zinc acetate in 90 mL of water;
[0078] S2. 12.82 g of the modified nano-lignin prepared in step S1 and 500 g of PBAT particles were added into a twin-screw extruder at the same time. The processing temperature was 120° C., the screw speed was 100 rpm, and the extrusion time of the polyester / lignin blend was maintained at 5 min. A polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm was prepared by melt casting.
[0079] Embodiment 11
[0080] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0081] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 18 g of micron lignin into 250 mL of 0.2 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly dropwise add zinc acetate solution into the nano lignin suspension, and use 1 mol / L After adjusting the pH of the mixed solution to 10 with NaOH, the solution was transferred to a flask and reacted for 12 hours under a nitrogen atmosphere at 90°C. After the reaction was completed, the precipitated product was collected by centrifugation at 11000 rpm. The supernatant was replaced with distilled water during the centrifugation process. The centrifugation operation was repeated three times to obtain a water-LZn suspension. Under magnetic stirring conditions, the water-LZn suspension was slowly dripped into the CPC solution, stirred for 3 hours, centrifuged 3 times, and freeze-dried to obtain modified nano-lignin. Among them, the CPC solution was obtained by dissolving 14.4 g CPC powder in 500 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 18 g zinc acetate in 90 mL water.
[0082] S2. 12.82 g of the modified nano-lignin prepared in step S1 and 500 g of PBAT particles were added into a twin-screw extruder at the same time. The processing temperature was 140° C., the screw speed was 100 rpm, and the extrusion time of the polyester / lignin blend was maintained at 10 min. A polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm was prepared by melt casting.
[0083] Example 12
[0084] This embodiment prepares a polyester / nano-lignin-ZnO composite film, and the preparation method thereof comprises the following steps:
[0085] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin. Under stirring conditions, slowly add 18 g of micron lignin into 250 mL of a 0.2 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension. Under stirring conditions, slowly drop zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times, and obtain a water-LZn suspension. Under magnetic stirring conditions, slowly drop the water-LZn suspension into a TTAB solution, stir for 3 h, centrifuge for 3 times, and freeze-dry to obtain modified nano lignin. Among them, the TTAB solution is 10.8 g TTAB powder was dissolved in 300 mL of 10% ethanol solution, and zinc acetate solution was obtained by dissolving 3.6 g of zinc acetate in 90 mL of water;
[0086] S2. 12.82 g of the modified nano-lignin prepared in step S1 and 500 g of PBAT particles were added into a twin-screw extruder at the same time. The processing temperature was 160° C., the screw speed was 100 rpm, and the extrusion time of the polyester / lignin blend was maintained at 5 min. A polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm was prepared by melt casting.
[0087] Comparative Example 1
[0088] The main difference between Comparative Example 1 and Example 2 is that the nano-lignin is not modified. The specific preparation method is as follows:
[0089] S1, grinding the purchased lignin and sieving it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin;
[0090] S2, dispersing 0.31g of the micron lignin obtained in step S1 in 80mL of chloroform to obtain a nano-lignin dispersion; dissolving 12g of PBAT in 100mL of chloroform to obtain a PBAT solution; slowly adding the nano-lignin dispersion to the PBAT solution under mechanical stirring, and continuing to stir for 30min to obtain a mixed solution; pouring the above mixed solution into a flat dish to form a film, and then hot pressing it at 150°C for 3min on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1mm.
[0091] Comparative Example 2
[0092] The main difference between Comparative Example 2 and Example 2 is that no surfactant is added during the modification of nano-lignin. The specific preparation method is as follows:
[0093] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin; under stirring conditions, slowly add 3 g of micron lignin to 150 mL of a 0.05 mol / L NaOH solution to fully dissolve it to obtain a nano lignin suspension; under stirring conditions, slowly drop a zinc acetate solution into the nano lignin suspension, adjust the pH of the mixed solution to 10 with 1 mol / L NaOH, transfer the solution to a flask, and react for 12 h under a nitrogen atmosphere at 90°C. After the reaction is completed, collect the precipitated product by centrifugation at 11000 rpm, replace the supernatant with distilled water during the centrifugation process, repeat the centrifugation operation three times to obtain a water-LZn suspension, centrifuge it three times, and freeze-dry it to obtain a powdered solid; wherein the zinc acetate solution is obtained by dissolving 3 g of zinc acetate in 30 mL of water;
[0094] S2, dispersing 0.31g of the powdered solid obtained in step S1 in 80mL of chloroform to obtain a modified nano-lignin dispersion; dispersing 12g of PBAT in 100mL of chloroform to obtain a PBAT solution; slowly adding the modified nano-lignin dispersion to the PBAT solution under mechanical stirring, and continuing to stir for 30min to obtain a mixed solution; pouring the mixed solution into a flat dish to form a film, and then hot pressing it at 150°C for 3min on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1mm.
[0095] Comparative Example 3
[0096] The main difference between Comparative Example 3 and Example 2 is that zinc acetate is not added during the modification of nano-lignin. The specific preparation method is as follows:
[0097] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin; slowly add 6 g of micron lignin into 500 mL of water under stirring and fully disperse it to obtain a nano lignin suspension; slowly dropwise add the nano lignin suspension into the DTAB solution under stirring, continue stirring for 3 hours, and centrifuge three times. During the centrifugation process, replace the supernatant with distilled water, and freeze-dry to obtain modified nano lignin powder; wherein the DTAB solution is obtained by dissolving 1.8 g of DTAB powder in 150 mL of ethanol solution;
[0098] S2, dispersing 0.31g of the modified nano-lignin powder obtained in step S1 in 80mL of chloroform to obtain a modified nano-lignin dispersion; dispersing 12g of PBAT in 100mL of chloroform to obtain a PBAT solution; slowly adding the modified nano-lignin dispersion to the PBAT solution under mechanical stirring, and continuing to stir for 30min to obtain a mixed solution; pouring the mixed solution into a flat dish to form a film, and then hot pressing it at 150°C for 3min on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1mm.
[0099] Comparative Example 4
[0100] The main difference between Comparative Example 4 and Example 2 is that the nano-lignin is not modified by using ZnO and a surfactant, but a composite film is directly prepared by directly using a mixture of ZnO and nano-lignin and polyester. The specific preparation method is as follows:
[0101] S1. Grind the purchased lignin and screen it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin; under stirring conditions, dissolve 3 g of zinc acetate in 30 mL of water, adjust the solution pH to 10 with NaOH, transfer it to a flask, and react at 90 ° C for 12 h under a nitrogen atmosphere. After the reaction is completed, use a centrifuge to collect the precipitated product at a speed of 11000 rpm, replace the supernatant with distilled water, repeat the centrifugation operation three times to obtain a suspension, centrifuge it three times, and freeze-dry it to obtain a ZnO powder solid;
[0102] S2, dispersing 0.155g of the micron lignin powder obtained in step S1 and 0.155g of ZnO powdered solid in 30mL of chloroform to obtain a nano-lignin-ZnO dispersion; dispersing 12g of PBAT in 100mL of chloroform to obtain a PBAT solution; slowly adding the nano-lignin-ZnO dispersion to the PBAT solution under mechanical stirring, and continuing to stir for 30min to obtain a mixed solution; pouring the mixed solution into a flat dish to form a film, and then hot pressing it at 150°C for 3min on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1mm.
[0103] Comparative Example 5
[0104] The main difference between Comparative Example 5 and Example 2 is that the ZnO is not coated with nano-lignin, but the ZnO and the surfactant are directly modified and prepared together with the polyester to form a composite film. The specific preparation method is as follows:
[0105] S1. Under stirring conditions, 3 g of zinc acetate was dissolved in water, and the pH of the solution was adjusted to 10 with NaOH, and the solution was transferred to a flask. The solution was reacted at 90°C for 12 h under a nitrogen atmosphere. After the reaction was completed, the precipitated product was collected by centrifugation at a speed of 11000 rpm, and the supernatant was replaced with distilled water. The centrifugation operation was repeated three times to obtain a suspension, and the suspension was centrifuged three times to obtain a water-ZnO suspension. Under magnetic stirring conditions, the water-ZnO suspension was slowly dripped into the DTAB solution, stirred for 3 h, centrifuged three times, and freeze-dried to obtain modified ZnO. The DTAB solution was obtained by dissolving 1.8 g of DTAB powder in 150 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 3 g of zinc acetate in 30 mL of water.
[0106] S2. Dissolve 12 g of PBAT in 100 mL of chloroform to obtain a PBAT solution; disperse 0.31 g of modified ZnO powdered solid in 80 mL of chloroform to obtain a ZnO dispersion; slowly add the ZnO dispersion to the PBAT solution under mechanical stirring conditions and stir for 30 minutes to obtain a mixed solution; pour the mixed solution into a flat dish to form a film, and then hot-press at 150° C. for 3 minutes on a flat vulcanizer to obtain a polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm.
[0107] Comparative Example 6
[0108] The main difference between Comparative Example 6 and Example 8 is that zinc acetate is not added during the modification of nano-lignin. The specific preparation method is as follows:
[0109] S1. Grind the purchased lignin and filter it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin; slowly add 36 g of micron lignin into 3 L of water under stirring to fully disperse it to obtain a nano lignin suspension; slowly drop the nano lignin suspension into the DTAB solution under stirring, continue stirring for 3 hours, and centrifuge three times. During the centrifugation process, replace the supernatant with distilled water, and freeze-dry to obtain modified nano lignin powder; wherein the DTAB solution is obtained by dissolving 10.8 g of DTAB powder in 300 mL of 10% ethanol solution;
[0110] S2. 12.82 g of the modified nano-lignin powder obtained in step S1 and 500 g of PBAT particles were added to a twin-screw extruder at the same time. The processing temperature was 160° C., the screw speed was 100 rpm, and the extrusion time of the polyester / lignin blend was maintained at 5 min. A polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm was obtained by melt casting.
[0111] Comparative Example 7
[0112] The main difference between Comparative Example 7 and Example 8 is that the nano-lignin is not modified by using ZnO and a surfactant, but a composite film is directly prepared by directly using a mixture of ZnO and nano-lignin and polyester. The specific preparation method is as follows:
[0113] S1. Grind the purchased lignin and screen it through a sieve with a mesh size of 140 mesh (aperture 109 μm) to obtain micron lignin; under stirring conditions, dissolve 18 g of zinc acetate in water, adjust the solution pH to 10 with NaOH, transfer it to a flask, and react at 90° C. for 12 h under a nitrogen atmosphere. After the reaction is completed, use a centrifuge to collect the precipitated product at a speed of 11000 rpm, replace the supernatant with distilled water, repeat the centrifugation operation three times to obtain a suspension, centrifuge it three times, and freeze-dry it to obtain a ZnO powder solid;
[0114] S2, 6.41g of the micron lignin powder obtained in step S1, 6.41g of ZnO powdered solid and 500g of PBAT particles were added to the twin-screw extruder at the same time, the processing temperature was 160°C, the screw speed was 100rpm, the extrusion time of the polyester / lignin blend was maintained at 5min, and a polyester / nano-lignin-ZnO composite film with a thickness of 0.1mm was obtained by melt casting.
[0115] Comparative Example 8
[0116] The main difference between Comparative Example 8 and Example 8 is that the ZnO is not coated with nano-lignin, but the ZnO and the surfactant are directly modified and prepared together with the polyester to form a composite film. The specific preparation method is as follows:
[0117] S1. Under stirring conditions, 18 g of zinc acetate was dissolved in water, and the pH of the solution was adjusted to 10 with NaOH, and the solution was transferred to a flask. The reaction was carried out at 90° C. for 12 h under a nitrogen atmosphere. After the reaction was completed, the precipitated product was collected by centrifugation at a speed of 11000 rpm, and the supernatant was replaced with distilled water. The centrifugation operation was repeated three times to obtain a suspension, and the suspension was centrifuged three times to obtain a water-ZnO suspension; under magnetic stirring conditions, the water-ZnO suspension was slowly dripped into the DTAB solution, stirred for 3 h, centrifuged 3 times, and freeze-dried to obtain modified ZnO; wherein, the DTAB solution was obtained by dissolving 10.8 g of DTAB powder in 300 mL of 10% ethanol solution, and the zinc acetate solution was obtained by dissolving 18 g of zinc acetate in 90 mL of water;
[0118] S2. 12.82 g of modified ZnO powdered solid and 500 g of PBAT particles were added to a twin-screw extruder at the same time. The processing temperature was 160° C., the screw speed was 100 rpm, and the extrusion time of the polyester / lignin blend was maintained at 5 min. A polyester / nano-lignin-ZnO composite film with a thickness of 0.1 mm was obtained by melt casting.
[0119] The mechanical properties of the composite films prepared in Examples 1-12 and Comparative Examples 1-8 were tested using the ISO 527-1 standard. The film size was 80×10×0.1 mm. 3 The UV shielding performance was tested by UV spectrophotometer (SHIMADZU UV-3600+) with a scanning range of 900-200nm and a rate of 4nm / s. The antioxidant performance was tested by double-beam UV-visible spectrophotometer (TU-1950, Presee, China) to measure the photometric values of the blank control and the corresponding mixed solution of each sample at a wavelength of 517nm. Each sample was scanned 3 times with a medium scanning speed and a scanning range of 300-800cm -1 0.2 g of PBAT / LZn composite material was broken into pieces and immersed in 5 mL of anhydrous ethanol for 40 h to prepare the sample migration solution. 2 mL of DPPH solution and 2 mL of sample migration solution were mixed in a 5 mL test tube and kept in dark for 0.5 h to ensure complete reaction. PBAT was used as a blank control. The antibacterial rate was tested by the plate counting method. The concentration of 10 8 The bacterial solution was gradually diluted to 10 CFU / mL. 5 CFU / mL, the sample was sterilized by ultraviolet light and then fully dispersed in PBS buffer solution. Subsequently, the bacterial solution and sample solution were mixed and placed in a shaker at 37°C for 3 hours; finally, 50 μL of the cultured bacterial solution was evenly spread on the solid culture medium, and the number of colonies was counted after culturing at 37°C for 24 hours. PBS solution was used instead of sample solution as the control group, and the antibacterial rate A was calculated based on the number of colonies. The calculation formula is: Where N C and N S Represent the colony counts of the culture medium of the control group and the sample group respectively; the mechanical properties of the membrane prepared after UV aging were tested according to ISO 527-1 standard, membrane size: 80×10×0.1mm 3 The test rate is 5 mm / min. The UV aging is tested using a UV aging test box (ASR-151A). The parameters are set to 220V, 120W. The mechanical properties of the polyester composite film are tested after irradiation for 72 hours. The elongation at break after aging is calculated based on the elongation at break before and after aging. The calculation formula is: Where T e is the elongation at break after UV aging (%), T c is the elongation at break before UV aging (%).
[0120] The performance comparison of the polyester / nano lignin-ZnO composite films obtained in Examples 1 to 12 and Comparative Examples 1-8 is shown in Table 1. It can be seen from the data in the table that with the increase in the content of nano lignin hybrid particles, the ultraviolet shielding performance, antioxidant performance and antibacterial performance of the composite film gradually improve. For example, when the amount of hybrid particles is 5wt% (Example 3), the antibacterial rate against E. coli reaches 100%, the free radical scavenging rate after 0.5h reaches 35.3%, and the ultraviolet light aging elongation at break retention rate after 72h reaches 86.2%. The principle is that lignin itself has certain antibacterial properties, and the phenolic hydroxyl groups therein form an acidic environment around the bacteria, destroying the movement of membrane protons, and ultimately causing the bacterial cell membrane to rupture and dissolve, and can also inhibit enzyme activity, and even cause the bacterial contents to flow out. The quaternary ammonium salt structure and ZnO in the added surfactant can improve the antibacterial activity of lignin. The phenolic hydroxyl groups, methoxyl groups, etc. of lignin generate phenoxy free radicals and H through hydrogen transfer. + To capture the free radicals generated by ZnO under light conditions to prevent the oxidation chain, thereby ensuring that it has relatively excellent antibacterial properties while also having good antioxidant properties and anti-ultraviolet aging properties. At the same time, when lignin is compounded with ZnO, it also shows a synergistic anti-ultraviolet effect, and the ultraviolet shielding efficiency can reach 99.9%. In addition, the long-chain alkane of the surfactant can improve the compatibility of the lignin hybrid particles with the degradable polyester, so that the performance of the composite film is more uniform, and the mechanical properties and ultraviolet shielding functions will also be improved accordingly. It can be seen from Examples 1-3 and 7-9 that with the increase in the content of lignin-based hybrid particles, the ultraviolet shielding property gradually decreases, and the antibacterial rate of E.coli bacteria gradually increases, the E.coli antibacterial rate reaches 100%, the ultraviolet shielding efficiency is greater than 99%, the free radical scavenging rate after 0.5h can be increased to 35.3% at most, and the ultraviolet light aging elongation retention rate after 72h reaches 87.3%. It can be seen from Examples 4-6 and Examples 10-12 that by changing the type and amount of surfactant, the antibacterial rate against E. coli bacteria reaches 99.9%, and the tensile strength is increased from 36.1 MPa to 39.2 MPa, indicating that the performance of the composite material has no direct relationship with the type of surfactant. The free radical scavenging rate reaches a maximum of 28.6%, the UV shielding efficiency is a maximum of 99.5%, and the retention rate of the elongation at break after UV aging after 72 hours reaches 84.5%.
[0121] Table 1 Comparison of the properties of polyester / nano-lignin-ZnO composite films prepared in Examples 1 to 12 and Comparative Examples 1 to 8
[0122]
[0123]
[0124] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a polyester / nano-lignin-ZnO composite film, characterized in that: The steps include: S1, hydrothermally reacting a mixture of a nano-lignin suspension and a zinc acetate solution at 50-140° C. for 6-24 hours to obtain LNP-ZnO hybrid nanoparticles; slowly adding the suspension of the LNP-ZnO hybrid nanoparticles into a surfactant solution to obtain modified nano-lignin; S2. Using the modified nano-lignin and polyester prepared in step S1 as raw materials, a polyester / nano-lignin-ZnO composite film is prepared by a melt casting method or a solution casting method.
2. The method for preparing the polyester / nano-lignin-ZnO composite film according to claim 1, characterized in that: In step S1, the mass ratio of nano-lignin to zinc acetate in the mixed solution is 5:1-1:
1.
3. The method for preparing the polyester / nano-lignin-ZnO composite film according to claim 1, characterized in that: In step S2, the added amount of the modified nano-lignin is 0.5-5wt% of the total mass of the modified nano-lignin and the polyester.
4. The method for preparing the polyester / nano-lignin-ZnO composite film according to claim 1, characterized in that: In step S1, the nano-lignin suspension is prepared by dissolving nano-lignin in a NaOH solution with a concentration of 0.01-0.1 g / mL, and the concentration of the NaOH solution is 0.01-1 mol / L; the nano-lignin is one of alkali lignin, lignin sulfonate, sulfate lignin, and organic solvent lignin.
5. The method for preparing the polyester / nano-lignin-ZnO composite film according to claim 1, characterized in that: The surfactant solution is obtained by dispersing the surfactant in the first organic solvent, and the concentration thereof is 0.5-40 g / L; the surfactant is one or more of dodecyltrimethylammonium bromide, didodecyldimethylammonium bromide, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, and hexadecylpyridinium chloride, and the first organic solvent is one or more of ethanol, isopropanol, methanol, and acetone.
6. The method for preparing the polyester / nano-lignin-ZnO composite film according to claim 1, characterized in that: In step S2, the method for preparing a polyester / nano-lignin-ZnO composite film by melt casting is as follows: the modified nano-lignin and the polyester are added to a device for melt processing and mixed evenly, and then reacted at 120-180° C. for 5-10 minutes to obtain a polyester / nano-lignin-ZnO composite film by melt casting.
7. The method for preparing the polyester / nano-lignin-ZnO composite film according to claim 1, characterized in that: In step S2, the method for preparing a polyester / nano-lignin-ZnO composite film by a solution casting method is as follows: the polyester and the modified nano-lignin are respectively dissolved in a second organic solvent to obtain a polyester solution and a modified nano-lignin dispersion; under mechanical stirring, the modified nano-lignin dispersion is slowly added to the polyester solution, and stirred for 15-45 minutes to obtain a mixed solution; the mixed solution is poured into a flat dish to form a film, and then subjected to hot pressing treatment to obtain a polyester / nano-lignin-ZnO composite film.
8. The method for preparing the polyester / nano-lignin-ZnO composite film according to claim 7, characterized in that: The temperature of the hot pressing treatment is 120-200° C., and the hot pressing time is 3-10 minutes.
9. The method for preparing the polyester / nano-lignin-ZnO composite film according to claim 1, characterized in that: The polyester is one of polybutylene adipate / terephthalate, polylactic acid, polybutylene succinate, polyglycolic acid, polycaprolactone, and polyhydroxybutyrate, and the weight average molecular weight of the polyester is ≥5×10 4 , optical purity ≥95%.
10. Application of a polyester / nano-lignin-ZnO composite film prepared by the preparation method described in any one of claims 1 to 9 in the field of food, medical equipment and pharmaceutical packaging.
Citation Information
Cited By
Preparation method of lignin-coated zinc oxide composite nanoparticles as well as product and application of lignin-coated zinc oxide composite nanoparticles
CN120815007A
Preparation method of lignin-coated zinc oxide composite nanoparticles, product and application thereof
CN120815007B