Wear-resistant coating and preparation method thereof

A wear-resistant coating with modified resin and specific filler components addresses poor oil and wear resistance by enhancing lubrication and mechanical properties through chemical cross-linking, achieving improved durability and resistance to oil seepage.

CN119060600AActive Publication Date: 2024-12-03ANQING LINGHU PAINT
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411330556.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

Existing wear-resistant coatings exhibit poor oil resistance and wear resistance, prone to oil seepage, and require improved anti-penetration performance.

Method used

A wear-resistant coating comprising specific ratios of modified resin, filler, dispersant, defoamer, and curing agent, with components like modified graphite, silicon carbide, molybdenum sulfide, and ferric oxide, along with a hardener containing pentaerythritol tetrakis(3-mercaptopropionic acid) grafted with 1H,1H,2H,2H-heptadecafluorodecyl acrylate, enhancing lubrication, drag reduction, and mechanical properties.

Benefits of technology

The coating demonstrates improved oil resistance, wear resistance, and mechanical properties due to the specific formulation and chemical cross-linking, providing long-lasting lubrication and reduced adhesion of pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005056751010000141
    Figure BDA0005056751010000141
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, in particular to a wear-resistant coating and a preparation method thereof.The wear-resistant coating is prepared from a solvent, modified resin, filler, a dispersing agent, a defoaming agent, a hardening agent and a curing agent; the modified resin is prepared from oleophobic particles, B resin and a silane coupling agent; the oleophobic particles are prepared from silicon dioxide, tetraethyl orthosilicate, heptadecafluorodecyl trichlorosilane and diatomite, and can improve the oil resistance of the coating; the filler is obtained by mixing modified graphite, silicon carbide, silicon dioxide, molybdenum sulfide and ferric oxide according to a specific proportion and can improve the self-lubricating property, the mechanical property and the oil resistance of the coating; the hardening agent is tetrakis (3-thiohydracrylic acid) pentaerythritol ester grafted by acrylic acid 1H, 1H, 2H, 2H-heptadecafluorodecyl ester, and can be chemically crosslinked with other components, so that the wear resistance of the coating is improved; therefore, the wear-resistant coating disclosed by the invention has better oil resistance, wear resistance and wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a wear-resistant coating and a preparation method thereof. Background Art

[0002] As a protective functional coating, wear-resistant coating has the characteristics of low friction coefficient on the coating surface, large load bearing capacity, and strong resistance to mechanical force. Therefore, when subjected to external force, it can effectively reduce the friction between interfaces, reduce the intensity of wear and the strength of resistance to wear, and play a role in protecting the substrate and extending its service life. It is widely used in aerospace, vehicles, ships, instruments, machine tool industries and other fields. With the rapid growth of demand for wear-resistant coatings in the energy field, it has also been widely used in wind turbine blades, nuclear reactor containment, dam structures, turbines, etc. A large number of literature shows that wear-resistant coatings at home and abroad currently achieve their wear-resistant effects mainly in two ways:

[0003] One is to add lubricants such as polytetrafluoroethylene powder, graphite, molybdenum disulfide, graphene and its derivatives to the coating to make the coating have good lubrication conditions, and transfer the friction pair to the internal friction of the lubricant during interface contact, thereby reducing the friction between the contact surfaces and achieving lubrication and friction reduction; the other is to add wear-resistant aggregates such as aluminum oxide, silicon carbide, and silicon dioxide to the coating to improve the strength of the coating, which can effectively resist frequent wear, high-speed erosion, and violent collisions from the outside world; in addition, the matrix resin also plays a decisive role in the wear resistance of the coating. Patent technical document CN118126602A discloses a wear-resistant epoxy resin coating and a preparation method thereof, comprising the following components in parts by mass: 25-30 parts of modified epoxy resin, 13-18 parts of water-based saturated polyester modified silicone resin, 1-5 parts of expanded graphite, 2-7 parts of polyimide, 5-9 parts of modified mica powder, 4-7 parts of modified silicon dioxide, 1-4 parts of nano titanium nitride, 0.5-2.5 parts of molybdenum disulfide, 1-2 parts of curing agent, 1-3 parts of dispersant, 1-2 parts of thickener and 40-45 parts of deionized water; the patent takes various methods into consideration.

[0004] However, these existing technologies still do not solve the problems that the wear-resistant coating has poor anti-penetration performance, is prone to oil seepage, and the wear resistance still needs to be improved.

[0005] Therefore, according to the above-mentioned related technologies, it is urgent to develop a wear-resistant coating and a preparation method thereof. Summary of the invention

[0006] In view of this, the purpose of the present invention is to provide a wear-resistant coating and a preparation method thereof, so as to solve the problem that the wear-resistant coating in the prior art has relatively poor oil resistance and wear resistance.

[0007] Based on the above purpose, the present invention provides a wear-resistant coating and a preparation method thereof.

[0008] A wear-resistant coating comprises the following raw materials in parts by weight: 25-30 parts of a solvent, 50-60 parts of a modified resin, 15-20 parts of a filler, 1.5-2 parts of a dispersant, 0.3-0.5 parts of a defoamer, 13-15 parts of a hardener, and 8-10 parts of a curing agent;

[0009] The modified resin is prepared from oleophobic particles, methyl methacrylate, isooctyl methacrylate, 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate, a silane coupling agent and ethanol;

[0010] The oleophobic particles are prepared from silicon dioxide, tetraethyl orthosilicate, heptadecafluorodecyltrichlorosilane and diatomaceous earth;

[0011] The filler is obtained by mixing modified graphite, silicon carbide, silicon dioxide, molybdenum sulfide and ferric oxide in a mass ratio of 3-5:1-2:7-10:2-4:2-4;

[0012] The modified graphite is prepared from graphite, concentrated sulfuric acid, sodium nitrate, potassium permanganate, a surfactant and a wetting agent;

[0013] The hardener is pentaerythritol tetrakis(3-mercaptopropionic acid) grafted with 1H,1H,2H,2H-heptadecafluorodecyl acrylate.

[0014] Preferably, the solvent is obtained by mixing xylene, butyl acetate, ethanol and n-butanol in a mass ratio of 8-10:28-30:12-16:2-4.

[0015] Preferably, the preparation method of the modified resin is as follows:

[0016] Step A1: water, silicon dioxide and ammonia water are added to ethanol in sequence, and tetraethyl orthosilicate is added after stirring evenly. After stirring evenly again, a mixed solution of heptadecafluorodecyltrichlorosilane and n-hexane is added, and the mixture is stirred under controlled temperature to obtain resin A;

[0017] Step A2: adding resin A to diatomaceous earth, reacting at 78-80° C. for 23-25 ​​hours, then grinding and sieving with a 180-200 mesh fine sieve to obtain oleophobic particles;

[0018] Step A3: under a nitrogen atmosphere, methyl methacrylate, isooctyl methacrylate, a silane coupling agent and 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate were added to butyl acetate, and the mixture was stirred at 116-118° C., and then a mixed solution of di-tert-butyl peroxide and ethanol was added at a rate of 2-4 seconds / drop, and the mixture was reacted for 8-9 hours to obtain resin B;

[0019] Step A4: Add oleophobic particles and silane coupling agent to resin B, stir evenly and adjust the pH to 5-7, then add ethanol and stir for 60-70 minutes to obtain modified resin.

[0020] Preferably, the mass ratio of ethanol, water, silicon dioxide, ammonia water, tetraethyl orthosilicate, heptadecafluorodecyltrichlorosilane and n-hexane in step A1 is 80-85:8-10:8-10:4-5:0.5-0.6:5-6:20-25; the speed during the temperature-controlled stirring is 1000-1100 rpm, the time is 23-25 ​​h, and the temperature is 65-70 ° C.

[0021] Preferably, the mass ratio of diatomaceous earth to resin A in step A2 is 10-12:8-10; the mass ratio of butyl acetate, methyl methacrylate, isooctyl methacrylate, silane coupling agent, 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate, di-tert-butyl peroxide, and ethanol in step A3 is 45-50:10-12:7.3-7.5:1.8-2:28-30:0.3-0.5:8-10; the mass ratio of resin B, oleophobic particles, silane coupling agent, and ethanol in step A4 is 30-32:8-10:2-3:10-15.

[0022] Preferably, the preparation method of the modified graphite is as follows:

[0023] Step B1: After mixing concentrated sulfuric acid and sodium nitrate evenly, add graphite, then add potassium permanganate at 58-60° C. at a rate of 2-4 seconds / drop and react for 6-8 hours to obtain graphite oxide;

[0024] Step B2: The surfactant and the wetting agent are mixed evenly, and then graphite oxide is added, stirred at 58-60° C. for 4-5 hours, filtered, and dried to obtain modified graphite.

[0025] Preferably, the mass ratio of concentrated sulfuric acid, sodium nitrate and potassium permanganate added to the graphite in step B1 is 5-5.5:4.8-5:10-12:4.8-5; the mass ratio of the surfactant, modifier and graphite oxide in step B2 is 2-2.5:2-2.5:20-25.

[0026] Preferably, the preparation method of the hardener is as follows:

[0027] Pentaerythritol tetrakis(3-mercaptopropionic acid), dibutylamine and acetone were mixed evenly, and then a mixed solution of 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate and acetone was added at 2-4 seconds / drop, and stirred at 1000-1100 rpm for 15-17 hours, and acetone was removed to obtain a hardener.

[0028] Preferably, the mass ratio of pentaerythritol tetrakis(3-mercaptopropionate), dibutylamine, acetone, 1H,1H,2H,2H-heptadecafluorodecyl acrylate and acetone is 4.8-5:0.013-0.015:5-5.2:5.1-5.3:5-5.2.

[0029] A method for preparing a wear-resistant coating, the preparation method is as follows:

[0030] Add modified resin to the solvent, stir for 10-15 minutes, then add filler, continue stirring for 5-10 minutes, then add dispersant, defoamer, hardener and curing agent in sequence, and stir for another 10-15 minutes to obtain a wear-resistant coating.

[0031] Beneficial effects of the present invention:

[0032] The invention provides a wear-resistant coating and a preparation method thereof. The invention improves the lubrication and drag reduction capability, the ability of long-lasting and stable lubrication, the mechanical properties and the oil resistance of the coating to the greatest extent by mixing modified graphite with silicon carbide, silicon dioxide, molybdenum sulfide and ferric oxide in a specific ratio; the hardener and the modified resin can reduce the surface rearrangement caused by the adhesion of oil stains, so that the fluorine-containing polymer has a very low adhesion tendency and gives the coating excellent hydrophobicity and oleophobicity; the siloxane monomers in each component can improve the mechanical properties of the coating; the Si-O bonds in the organosilicon polymer make the coating have low surface energy and low elastic modulus, which can further reduce the adhesion of pollutants; and the oleophobic units of the oleophobic particles are closely arranged to prevent the hydrophilic units from being attracted back to the outer surface by other polar groups, thereby improving the oil resistance and water resistance of the coating; the hardener also contains a thiol group, which can be chemically cross-linked with other components containing carbon-carbon double bonds through a thiol-ene click reaction, thereby improving the wear resistance of the coating.

[0033] Therefore, compared with the prior art, the wear-resistant coating prepared by the present invention has better oil resistance, wear resistance and broad application prospects. DETAILED DESCRIPTION

[0034] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0035] The sources and properties of some of the raw materials used in the present invention are as follows:

[0036] Graphite (particle size 10 nm) was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.; surfactant was purchased from Hubei Jusheng Technology Co., Ltd., CAS: 85854-32-6; wetting agent was purchased from Linyi Guoli Chemical Co., Ltd., CAS: 577-11-7; pentaerythritol tetrakis(3-mercaptopropionic acid) ester was purchased from Shanghai Yuanye Biotechnology Co., Ltd., CAS: 7575-23-7; 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate was purchased from Shanghai Aladdin Biotechnology Co., Ltd., CAS: 27905-45-9; heptadecafluorodecyl trichlorosilane was purchased from Hubei Jusheng Technology Co., Ltd., CAS: 78560-44-8; methyl methacrylate Ester was purchased from Shandong Jinyueyuan New Materials Co., Ltd., CAS: 80-62-6; isooctyl methacrylate was purchased from Shandong Yonglida New Materials Technology Co., Ltd., CAS: 28675-80-1; silane coupling agent was purchased from Shanghai Yuanye Biotechnology Co., Ltd., CAS: 2530-85-0; di-tert-butyl peroxide was purchased from Jinan Hongteng Weiye New Materials Co., Ltd., CAS: 110-05-4; dispersant was purchased from Anhui Shengyuan Chemical Co., Ltd., CAS: 36290-04-7; defoamer was purchased from Linyi Guoli Chemical Co., Ltd., CAS: 993-11-6; curing agent was purchased from Shandong Zhengxing New Materials Co., Ltd., CAS: 85-44-9.

[0037] Embodiment 1: A method for preparing a wear-resistant coating, comprising the following steps:

[0038] S1: 5 g of 98% concentrated sulfuric acid and 4.8 g of sodium nitrate were mixed, 10 g of graphite was added, and 4.8 g of potassium permanganate was added at 58°C at a rate of 2 seconds per drop and reacted for 6 hours to obtain graphite oxide;

[0039] S2: 2 g of surfactant and 2 g of wetting agent were mixed evenly, and then 20 g of graphite oxide was added, stirred at 58 °C for 4 h, filtered and dried to obtain modified graphite;

[0040] S3: 3 g of modified graphene, 1 g of silicon carbide, 7 g of silicon dioxide, 2 g of molybdenum sulfide and 2 g of ferric oxide are mixed uniformly to obtain a filler;

[0041] S4: 4.8 g of pentaerythritol tetrakis(3-mercaptopropionic acid), 0.013 g of dibutylamine and 5 g of acetone were mixed evenly, and then a mixed solution of 5.1 g of 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate and 5 g of acetone was added at a rate of 2 seconds / drop, and the mixture was stirred at 1000 rpm for 15 hours, and the acetone was removed to obtain a hardener;

[0042] S5: 8 g of water, 8 g of silicon dioxide and 4 g of ammonia water were added to 80 g of ethanol in sequence, and 0.5 g of tetraethyl orthosilicate was added after stirring evenly. After stirring evenly again, a mixed solution of 5 g of heptadecafluorodecyltrichlorosilane and 20 g of n-hexane was added, and the mixture was stirred at 1000 rpm at 65° C. for 23 h to obtain resin A;

[0043] S6: adding 8 g of A resin to 10 g of diatomaceous earth, reacting at 78° C. for 23 h, then grinding and sieving through a 180-mesh fine sieve to obtain oleophobic particles;

[0044] S7: Under nitrogen atmosphere, 10 g of methyl methacrylate, 7.3 g of isooctyl methacrylate, 1.8 g of silane coupling agent and 28 g of 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate were added to 45 g of butyl acetate, and the mixture was stirred evenly at 116° C. Then, a mixed solution of 0.3 g of di-tert-butyl peroxide and 8 g of ethanol was added at a rate of 2 seconds / drop, and the mixture was reacted for 8 hours to obtain resin B;

[0045] S8: Add 8 g of oleophobic particles and 2 g of silane coupling agent to 30 g of B resin, stir evenly and adjust the pH to 5, then add 10 g of ethanol and stir for 60 min to obtain a modified resin;

[0046] S9: Add 50g of modified resin to 25g of solvent, stir for 10min, then add 15g of filler, continue stirring for 5min, then add 1.5g of dispersant, 0.3g of defoamer, 13g of hardener and 8g of curing agent in sequence, and stir for another 10min to obtain a wear-resistant coating.

[0047] Embodiment 2: A method for preparing a wear-resistant coating, comprising the following steps:

[0048] S1: 5.3 g of 98% concentrated sulfuric acid and 4.9 g of sodium nitrate were mixed, and then 11 g of graphite was added. 4.9 g of potassium permanganate was added at 59°C at a rate of 3 seconds per drop and reacted for 7 hours to obtain graphite oxide;

[0049] S2: 2.3 g of surfactant and 2.3 g of wetting agent were mixed evenly, and then 23 g of graphite oxide was added, stirred at 59 °C for 4.5 h, filtered and dried to obtain modified graphite;

[0050] S3: 4 g of modified graphene, 1.5 g of silicon carbide, 9 g of silicon dioxide, 3 g of molybdenum sulfide and 3 g of ferric oxide are mixed uniformly to obtain a filler;

[0051] S4: 4.9 g of pentaerythritol tetrakis(3-mercaptopropionic acid), 0.014 g of dibutylamine and 5.1 g of acetone were mixed evenly, and then a mixed solution of 5.2 g of 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate and 5.1 g of acetone was added at a rate of 3 seconds / drop, and the mixture was stirred at 1050 rpm for 16 hours, and the acetone was removed to obtain a hardener;

[0052] S5: 9 g of water, 9 g of silicon dioxide and 4.5 g of ammonia water were added to 83 g of ethanol in sequence, and 0.55 g of tetraethyl orthosilicate was added after stirring evenly. After stirring evenly again, a mixed solution of 5.5 g of heptadecafluorodecyltrichlorosilane and 23 g of n-hexane was added, and the mixture was stirred at 1050 rpm at 68° C. for 24 h to obtain resin A;

[0053] S6: Add 9 g of A resin to 11 g of diatomaceous earth, react at 79° C. for 24 h, then grind and sieve through a 190-mesh fine sieve to obtain oleophobic particles;

[0054] S7: Under nitrogen atmosphere, 11 g of methyl methacrylate, 7.4 g of isooctyl methacrylate, 1.9 g of silane coupling agent and 29 g of 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate were added to 48 g of butyl acetate, and the mixture was stirred evenly at 117° C. Then, a mixed solution of 0.4 g of di-tert-butyl peroxide and 9 g of ethanol was added at a rate of 3 seconds / drop, and the mixture was reacted for 8.5 hours to obtain resin B;

[0055] S8: Add 9 g of oleophobic particles and 2.5 g of silane coupling agent to 31 g of B resin, stir evenly and adjust the pH to 6, then add 13 g of ethanol and stir for 65 min to obtain a modified resin;

[0056] S9: Add 55g of modified resin to 28g of solvent, stir for 13min, then add 18g of filler, continue stirring for 8min, then add 1.8g of dispersant, 0.4g of defoamer, 14g of hardener and 9g of curing agent in sequence, and stir for another 13min to obtain a wear-resistant coating.

[0057] Embodiment 3: A method for preparing a wear-resistant coating, comprising the following steps:

[0058] S1: 5.5 g of 98% concentrated sulfuric acid and 5 g of sodium nitrate were mixed, 12 g of graphite was added, and 5 g of potassium permanganate was added at 60°C at a rate of 4 seconds per drop and reacted for 8 hours to obtain graphite oxide;

[0059] S2: 2.5 g of surfactant and 2.5 g of wetting agent were mixed evenly, and then 25 g of graphite oxide was added, stirred at 60 ° C for 5 h, filtered and dried to obtain modified graphite;

[0060] S3: 5 g of modified graphene, 2 g of silicon carbide, 10 g of silicon dioxide, 4 g of molybdenum sulfide and 4 g of ferric oxide are mixed uniformly to obtain a filler;

[0061] S4: 5 g of pentaerythritol tetrakis(3-mercaptopropionic acid), 0.015 g of dibutylamine and 5.2 g of acetone were mixed evenly, and then a mixed solution of 5.3 g of 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate and 5.2 g of acetone was added at 4 seconds / drop, and stirred at 1100 rpm for 17 hours, and the acetone was removed to obtain a hardener;

[0062] S5: 10 g of water, 10 g of silicon dioxide and 5 g of ammonia water were added to 85 g of ethanol in sequence, and after stirring evenly, 0.6 g of tetraethyl orthosilicate was added, and after stirring evenly again, a mixed solution of 6 g of heptadecafluorodecyltrichlorosilane and 25 g of n-hexane was added, and the mixture was stirred at 70° C. and 1100 rpm for 25 h to obtain resin A;

[0063] S6: adding 10 g of A resin to 12 g of diatomaceous earth, reacting at 80° C. for 25 h, then grinding and sieving with a 200-mesh fine sieve to obtain oleophobic particles;

[0064] S7: Under nitrogen atmosphere, 12 g of methyl methacrylate, 7.5 g of isooctyl methacrylate, 2 g of silane coupling agent and 30 g of 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate were added to 50 g of butyl acetate, and the mixture was stirred evenly at 118° C. Then, a mixed solution of 0.5 g of di-tert-butyl peroxide and 10 g of ethanol was added at a rate of 4 seconds / drop, and the mixture was reacted for 9 hours to obtain resin B;

[0065] S8: Add 10 g of oleophobic particles and 3 g of silane coupling agent to 32 g of B resin, stir well and adjust the pH to 7, then add 15 g of ethanol and stir for 70 min to obtain a modified resin;

[0066] S9: Add 60g of modified resin to 30g of solvent, stir for 15min, then add 20g of filler, continue stirring for 10min, then add 2g of dispersant, 0.5g of defoamer, 15g of hardener and 10g of curing agent in sequence, and stir for another 15min to obtain a wear-resistant coating.

[0067] Comparative Example 1:

[0068] Compared with Example 1, this comparative example only replaces "modified graphite" with "graphite", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a wear-resistant coating is obtained.

[0069] Comparative Example 2:

[0070] Compared with Example 1, this comparative example does not add ferric oxide, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a wear-resistant coating is obtained.

[0071] Comparative Example 3:

[0072] Compared with Example 1, this comparative example does not add molybdenum sulfide during the preparation of the filler, and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, a wear-resistant coating is obtained.

[0073] Comparative Example 4:

[0074] Compared with Example 1, this comparative example only replaces "3g modified graphene, 1g silicon carbide, 7g silicon dioxide, 2 molybdenum sulfide and 2g ferric oxide" with "3g modified graphene, 1g silicon carbide, 7g silicon dioxide, 0.5g molybdenum sulfide and 3.5g ferric oxide", and the remaining steps and parameters are the same and will not be repeated in this comparative example. Finally, a wear-resistant coating is obtained.

[0075] Comparative Example 5:

[0076] Compared with Example 1, this comparative example does not add oleophobic particles during the preparation of the modified coating, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a wear-resistant coating is obtained.

[0077] Comparative Example 6:

[0078] Compared with Example 1, this comparative example only replaces the "modified resin" with "acrylic resin", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a wear-resistant coating is obtained.

[0079] Comparative Example 7:

[0080] Compared with Example 1, no hardener was added in this comparative example, and the remaining steps and parameters were the same, which will not be repeated in this comparative example, and finally a wear-resistant coating was obtained.

[0081] Performance Test:

[0082] Take 10 groups of steel plates with a size of 120 mm × 50 mm and use 1200 mesh sandpaper to remove the rust on the surface, then use anhydrous ethanol to ultrasonically clean the steel plates, and blow dry them with a hair dryer for use; place the treated steel plates on the test bench, and use a wire rod coater with a specification of 100 μm (Oshiji Precision Tools Co., Ltd.) to apply the wear-resistant coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 7 on each group of steel plates, respectively, with a wet film thickness of 100 μm; after coating, place the sample flat on the test bench, dry it at 125 ° C for 10 hours, and obtain a wear-resistant coating sample, and perform performance tests on the prepared wear-resistant coating sample:

[0083] Determination of adhesion:

[0084] Referring to the test standard of GB / T9286-2021 "Paint and varnish - scratch test", place the wear-resistant coating sample on a flat and hard operating table, and use a hundred-grid blade to evenly scratch in two perpendicular directions. Pay attention to even force and smooth scratching without shaking, and the scratching should penetrate the coating and touch the metal plate. After scratching, use a soft brush to gently wipe along the diagonal direction of the grid, and then stick the special 3M tape on the entire grid formed by the scratching. Press hard with your fingers to ensure that the tape is in good contact with the coating. When tearing off the tape, the tape should be at a 60° angle to the coating and tear off smoothly and quickly within 1s. The coating adhesion level is evaluated by observing the size of the tearing area, which is divided into 0-5 levels. The adhesion is strongest at level 0 and the worst at level 5. According to this test standard, the adhesion (level) test is performed on the samples prepared with the wear-resistant coatings prepared in Example 1-Example 3 and Comparative Example 1-Comparative Example 7;

[0085] Determination of adhesion after oil immersion:

[0086] With reference to the test standard of GB / T9286-2021 "Paints and varnishes - Cross-cut test", according to the above-mentioned adhesion determination method, the adhesion (grade) test was performed on the samples prepared by the wear-resistant coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 7 after being immersed in a mixture of soybean oil and hexadecane with a volume ratio of 3:1 for 90 days at 25°C;

[0087] Determination of corrosion resistance:

[0088] Referring to the test standard of GB / T10125-2021 "Artificial Atmosphere Corrosion Test-Salt Spray Test", the wear-resistant coating sample was edge-sealed with epoxy putty, and then placed in a salt spray test box (JAY-1127, Zhuhai Jiayi Testing Equipment Co., Ltd.), at 35 ° C, pH = 6.5-7.2, 5% sodium chloride solution was used for 24h salt spray and 24h drying cycle test, and sampling was observed every 48h, and the test time for the appearance of red rust on each sample was recorded. When the last sample appeared red rust, the neutral salt spray test was terminated; according to this test standard, the samples prepared with the wear-resistant coatings prepared in Example 1-Example 3 and Comparative Example 1-Comparative Example 7 were tested for corrosion resistance (h);

[0089] Determination of hardness:

[0090] Referring to GB / T6739-2006 "Paints and varnishes - Determination of film hardness by pencil method", use a cylindrical lead with a length of about 3mm, a load of 750g, and push the experimental instrument forward and downward for 10mm at a speed of 1mm / s and 45°, and repeat five scratches; after each scratch, place the lead vertically on 400# water sandpaper to draw a circle, and re-grind the tip of the pencil lead until the tip of the pencil is ground into a flat surface with a sharp edge. In the five-stroke scratch test, the pencil hardness of the coating is expressed by the hardest pencil hardness that does not scratch or only scratches the bottom coating film. The hardness is divided into 20 levels from soft to hard, including 9B, 8B, 7B, 6B, 5B, 4B, 3B, 2B, B, BH, F, H, 2H, 3H, 4H, 5H, 6H, 7H, 8H, and 9H. According to this test standard, the hardness of the samples prepared with the wear-resistant coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 7 is tested;

[0091] Determination of wear resistance:

[0092] Referring to the test standard of ASTM-D4060-19 "Standard Test Method for Wear Resistance of Organic Coatings Using Taber Abrasion Tester", a grinder was used to measure the wear resistance of the coating when the turntable speed was 60r / min, the rubber grinding wheel model was CS-10, the load was 1kg, and the number of rotations was 5000r. Before the test and every 500r of wear, the rubber grinding wheel was trimmed with No.S-11 sand sheet for 50r to maintain the roughness of the grinding wheel surface; before the test, the coating was worn for 50r and then the sample was weighed as the initial count; the cumulative wear was 5000r, and the wear resistance was determined by the weight difference before and after the coating was worn; according to this test standard, the wear resistance test was performed on the sample prepared by the wear-resistant coating prepared by Example 1-Example 3 and Comparative Example 1-Comparative Example 7;

[0093] Determination of oil resistance after wear:

[0094] Referring to the determination standard of QJ990.1-1986 "Coating Inspection Method - Coating Oil Resistance Inspection Method", at 25°C, 2 / 3 of the coating is immersed in a mixture of soybean oil and hexadecane in a volume ratio of 3:1, and the mixture is replaced every 30 days. Take out the coating every 10 days to observe the area of ​​oil stains adhered to the surface of the coating and whether the coating has bubbling and other phenomena, and test the wettability of water droplets and oil droplets in the non-adherent area. When the oil stain adhesion area in the immersion area is greater than 1 / 2, the coating is considered to have failed, and the number of days required is recorded as the coating oil resistance; according to this test standard, the wear resistance is measured for the wear-resistant coatings prepared in Example 1-Example 3 and Comparative Example 1-Comparative Example 7 after wear and tear. The oil resistance (days) after wear is measured;

[0095] Determination of friction coefficient:

[0096] Referring to the test standard of GB / T10006-1988 "Method for Determination of Friction Coefficient of Plastic Film and Sheet", the cured sample was placed in a friction and wear tester (M-2000, Zhangjiakou Xuanhua Kehua Testing Machine Manufacturing Co., Ltd.), and the specific speed, load, test temperature and time were set on the computer to start the experiment. The result obtained from the experiment was the average friction coefficient; according to this test standard, the friction coefficient of the sample prepared by the wear-resistant coating prepared by Example 1 to Example 3 and Comparative Example 1 to Comparative Example 7 was measured;

[0097] Determination of impact resistance:

[0098] Referring to the test standard of GB / T20624.2-2006 "Paints and varnishes - Rapid impact (impact resistance) test, Part II: Drop hammer test (small area punch)", a paint film impact tester with a weight of 1 kg (TCJ-Ⅱ, Shanghai Leao Testing Instrument Co., Ltd.) was used to test the impact resistance (kg·m) of the samples prepared by the wear-resistant coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 7; the test results are shown in Table 1;

[0099] Table 1

[0100]

[0101] Data Analysis:

[0102] It can be seen from Table 1 that the wear-resistant coating prepared by the present invention has stronger adhesion, corrosion resistance, wear resistance, oil resistance, higher hardness and smaller friction coefficient, that is, the wear-resistant coating prepared by the present invention has better wear resistance, corrosion resistance, oil resistance and mechanical properties;

[0103] This may be because after the graphite is modified, it has more active groups that can be cross-linked with other components, so that it can be well dispersed in the coating. The special structure of modified graphite and molybdenum disulfide has lower friction when sliding occurs, and molybdenum disulfide can also react with ferric oxide to form a dense composite layer of ferrous sulfide and molybdenum dioxide. Therefore, the modified graphite, molybdenum disulfide and ferric oxide in a specific ratio of the present invention can maximize the lubrication and drag reduction ability, long-term and stable lubrication ability, mechanical properties and oil resistance of the coating; the perfluoroalkyl group in the hardener and the modified resin is enriched on the surface and tightly arranged in a directional manner, and CF The 3 groups are exposed, which can reduce the surface rearrangement caused by the adhesion of oil stains, making the fluorinated polymer have a very low adhesion tendency. At the same time, the fluorocarbon chain can also work synergistically with the polymethylsiloxane segment to give the coating excellent hydrophobicity and oleophobicity; the siloxane monomers in each component can produce active silanol groups through hydrolysis, which can provide sites for chemical reactions with the substrate and can also condense into a tight network structure between them, thereby forming a tight network structure and improving the mechanical properties of the coating; the Si-O bond in the silicone polymer gives it low surface energy and low elastic modulus, which can further reduce the adhesion of pollutants. The hydrophilic unit of the oleophobic particles in the modified resin is on the inside, and the oleophobic unit is on the outside. Due to the pinning effect of the deposited fluorosilane on the surface, the oleophobic units are tightly arranged to prevent the hydrophilic units from being attracted back to the outer surface by other polar groups. Therefore, it can not only improve the oil resistance of the coating, but also improve its water resistance. The hardener also contains thiol groups, which can chemically cross-link with other components containing carbon-carbon double bonds through thiol-ene click reactions to improve the wear resistance of the coating. Because of this special arrangement from the inside out and various tightly connected arrangements, the coating has good oil resistance, and the oil resistance of the coating is still considerable after wear.

[0104] In Comparative Example 1, "modified graphite" is replaced by "graphite"; in Comparative Example 2, no ferric oxide is added; in Comparative Example 3, no molybdenum sulfide is added; in Comparative Example 4, "3g modified graphene, 1g silicon carbide, 7g silicon dioxide, 2 molybdenum sulfide and 2g ferric oxide" is replaced by "3g modified graphene, 1g silicon carbide, 7g silicon dioxide, 0.5g molybdenum sulfide and 3.5g ferric oxide". It can be seen from Table 1 that compared with Example 1, their adhesion after oil immersion, corrosion resistance, hardness, wear resistance, oil resistance after wear, friction coefficient and impact resistance are significantly improved. The friction force is relatively poor, which may be due to the fact that after the graphite is modified, it has more active groups that can be cross-linked with other components, so that it can be well dispersed in the coating. The modified graphite and molybdenum disulfide also have special lamellar structures, so they have lower friction when sliding, and molybdenum disulfide can also react with ferrous oxide to form a dense composite layer of ferrous sulfide and molybdenum dioxide. Therefore, the modified graphite, molybdenum disulfide and ferrous oxide in a specific ratio in the present invention can maximize the lubrication and drag reduction ability, long-term and stable lubrication ability, mechanical properties and oil resistance of the coating;

[0105] Comparative Example 5 did not add oleophobic particles during the preparation of the modified coating. It can be seen from Table 1 that their adhesion after oil immersion, corrosion resistance, hardness, wear resistance, oil resistance after wear, friction coefficient and impact resistance are relatively poor compared with Example 1. This may be because the hydrophilic unit of the oleophobic particles in the modified resin is inside, and the oleophobic unit is outside. Due to the pinning effect of the deposited fluorosilane on the surface, the oleophobic units are closely arranged to prevent the hydrophilic units from being attracted back to the outer surface by other polar groups. Therefore, it can not only improve the oil resistance of the coating, but also improve its corrosion resistance;

[0106] Comparative Example 6 replaces the added "modified resin" with "acrylic resin". It can be seen from Table 1 that compared with Example 1, their adhesion after oil immersion, corrosion resistance, hardness, wear resistance, oil resistance after wear, friction coefficient and impact resistance are relatively poor. This may be because the perfluoroalkyl groups in the modified resin are enriched on the surface and tightly arranged in a directional manner, and the CF3 group is exposed to the outside, which can reduce the surface rearrangement caused by the adhesion of oil stains, so that the fluorine-containing polymer has a very low adhesion tendency; the siloxane monomers therein can generate active silanol groups by hydrolysis, and these silanol groups can provide sites for chemical reaction with the substrate, and can also condense into a tight network structure between them, thereby forming a tight network structure, thereby improving the mechanical properties of the coating;

[0107] Comparative Example 7 does not add a hardener. It can be seen from Table 1 that compared with Example 1, their adhesion after oil immersion, corrosion resistance, hardness, wear resistance, oil resistance after wear, friction coefficient and impact resistance are relatively poor. This may be because the hardener has both a thiol group and a fluorocarbon chain. The thiol group can be chemically cross-linked with other components containing carbon-carbon double bonds through a thiol-ene click reaction, thereby improving the hardness, adhesion and impact resistance of the coating; the fluorocarbon chain can synergistically act with the polymethylsiloxane segment to give the coating excellent hydrophobic and oleophobic capabilities.

[0108] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0109] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A wear-resistant coating, characterized in that: The invention comprises the following raw materials in parts by weight: 25-30 parts of solvent, 50-60 parts of modified resin, 15-20 parts of filler, 1.5-2 parts of dispersant, 0.3-0.5 parts of defoamer, 13-15 parts of hardener and 8-10 parts of curing agent; The modified resin is prepared from oleophobic particles, methyl methacrylate, isooctyl methacrylate, 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate, a silane coupling agent and ethanol; The oleophobic particles are prepared from silicon dioxide, tetraethyl orthosilicate, heptadecafluorodecyltrichlorosilane and diatomaceous earth; The filler is obtained by mixing modified graphite, silicon carbide, silicon dioxide, molybdenum sulfide and ferric oxide in a mass ratio of 3-5:1-2:7-10:2-4:2-4; The modified graphite is prepared from graphite, concentrated sulfuric acid, sodium nitrate, potassium permanganate, a surfactant and a wetting agent; The hardener is pentaerythritol tetrakis(3-mercaptopropionic acid) grafted with 1H,1H,2H,2H-heptadecafluorodecyl acrylate.

2. The wear-resistant coating according to claim 1, characterized in that: The solvent is obtained by mixing xylene, butyl acetate, ethanol and n-butanol in a mass ratio of 8-10:28-30:12-16:2-4.

3. The wear-resistant coating according to claim 1, characterized in that: The preparation method of the modified resin is as follows: Step A1: water, silicon dioxide and ammonia water are added to ethanol in sequence, and tetraethyl orthosilicate is added after stirring evenly. After stirring evenly again, a mixed solution of heptadecafluorodecyltrichlorosilane and n-hexane is added, and the mixture is stirred under controlled temperature to obtain resin A; Step A2: adding resin A to diatomaceous earth, reacting at 78-80° C. for 23-25 ​​hours, then grinding and sieving with a 180-200 mesh fine sieve to obtain oleophobic particles; Step A3: under a nitrogen atmosphere, methyl methacrylate, isooctyl methacrylate, a silane coupling agent and 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate were added to butyl acetate, and the mixture was stirred at 116-118° C., and then a mixed solution of di-tert-butyl peroxide and ethanol was added at a rate of 2-4 seconds / drop, and the mixture was reacted for 8-9 hours to obtain resin B; Step A4: Add oleophobic particles and silane coupling agent to resin B, stir evenly and adjust the pH to 5-7, then add ethanol and stir for 60-70 minutes to obtain modified resin.

4. The wear-resistant coating according to claim 3, characterized in that: The mass ratio of ethanol, water, silicon dioxide, ammonia water, tetraethyl orthosilicate, heptadecafluorodecyltrichlorosilane and n-hexane in step A1 is 80-85:8-10:8-10:4-5:0.5-0.6:5-6:20-25; the speed during the temperature-controlled stirring is 1000-1100 rpm, the time is 23-25 ​​hours, and the temperature is 65-70°C.

5. The wear-resistant coating according to claim 3, characterized in that: The mass ratio of diatomaceous earth to resin A in step A2 is 10-12:8-10; the mass ratio of butyl acetate, methyl methacrylate, isooctyl methacrylate, silane coupling agent, 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate, di-tert-butyl peroxide, and ethanol in step A3 is 45-50:10-12:7.3-7.5:1.8-2:28-30:0.3-0.5:8-10; the mass ratio of resin B, oleophobic particles, silane coupling agent, and ethanol in step A4 is 30-32:8-10:2-3:10-15.

6. The wear-resistant coating according to claim 1, characterized in that: The preparation method of the modified graphite is as follows: Step B1: After mixing concentrated sulfuric acid and sodium nitrate evenly, add graphite, then add potassium permanganate at 58-60° C. at a rate of 2-4 seconds / drop and react for 6-8 hours to obtain graphite oxide; Step B2: The surfactant and the wetting agent are mixed evenly, and then graphite oxide is added, stirred at 58-60° C. for 4-5 hours, filtered, and dried to obtain modified graphite.

7. The wear-resistant coating according to claim 6, characterized in that: The mass ratio of the graphite added with concentrated sulfuric acid, sodium nitrate and potassium permanganate in step B1 is 5-5.5:4.8-5:10-12:4.8-5; the mass ratio of the surfactant, modifier and graphite oxide in step B2 is 2-2.5:2-2.5:20-25.

8. The wear-resistant coating according to claim 1, characterized in that: The preparation method of the hardener is as follows: Pentaerythritol tetrakis(3-mercaptopropionic acid), dibutylamine and acetone were mixed evenly, and then a mixed solution of 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate and acetone was added at 2-4 seconds / drop, and stirred at 1000-1100 rpm for 15-17 hours, and acetone was removed to obtain a hardener.

9. The wear-resistant coating according to claim 8, characterized in that: The mass ratio of pentaerythritol tetrakis(3-mercaptopropionate), dibutylamine, acetone, 1H,1H,2H,2H-heptadecafluorodecyl acrylate and acetone is 4.8-5: 0.013-0.015: 5-5.2: 5.1-5.3: 5-5.

2.

10. A method for preparing a wear-resistant coating according to any one of claims 1 to 9, characterized in that: The preparation method is as follows: Add modified resin to the solvent, stir for 10-15 minutes, then add filler, continue stirring for 5-10 minutes, then add dispersant, defoamer, hardener and curing agent in sequence, and stir for another 10-15 minutes to obtain a wear-resistant coating.

Citation Information

Patent Citations

  • Wear-resistant epoxy resin coating and preparation method thereof

    CN118126602A

  • Fluorosilicone-modified acrylic resin hydrophobic anti-corrosion paint

    CN101928498A

  • Abrasion-resistant coating for outer casing of aluminum charger

    CN106833252A

  • Sweat-resistant water-soluble acrylic resin coating and preparation method thereof

    CN110922851A

  • Environment-friendly super-hydrophobic antifouling paint

    CN111500130A