High-strength aluminum alloy and preparation method thereof

By regulating the Si/Mg ratio and adding nanotitanium dioxide-graphene-copper-aluminum alloy, combined with a special preparation process, the performance and cost challenges of existing aluminum alloys in automotive lightweight design are solved, and high-strength, good plasticity aluminum is prepared. The alloy is suitable for anti-collision beams for new energy vehicles, achieving higher lightweight and performance improvements.

CN119061296AInactive Publication Date: 2024-12-03SHENZHEN XINSHEN NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411242307.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing aluminum alloys are difficult to meet higher performance and cost requirements in automotive lightweight design, especially in the field of new energy vehicles. How to develop new aluminum alloys with high strength, good plasticity and lightweight characteristics to meet market demands? challenge.

Method used

By adjusting the Si/Mg ratio and Y/Sr ratio, and adding nanotitanium dioxide-graphene-copper-aluminum alloy, the particle size and second phase type characteristics in the alloy structure are changed, and combined with a special preparation process, a high resistance is prepared High-strength aluminum alloy with tensile strength, yield strength and elongation is suitable for anti-collision beams of new energy vehicles.

Benefits of technology

It achieves high strength and good plasticity of aluminum alloy, has better lightweight properties and stronger rigidity and toughness, and can perform well in higher demand automotive collision tests, and the lightweight weight reduction effect can reach more than 20%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloys, in particular to a high-strength aluminum alloy and a preparation method thereof. The invention relates to a high-strength aluminum alloy, which is prepared from the following preparation raw materials in percentage by mass: 0.16 to 0.25 percent of Fe, 0.65 to 0.9 percent of Mn, 0.8 to 1.20 percent of Si, 0.80 to 1.0 percent of Mg, 0.15 to 0.22 percent of Cr, 0.13 to 0.20 percent of Y, 0.01 to 0.02 percent of Sr, 8.8 to 9.7 percent of nano titanium dioxide-graphene-copper aluminum alloy and the balance of Al. By regulating and controlling the Si / Mg ratio and the Y / Sr ratio, adding the nano titanium dioxide-graphene-copper aluminum alloy and combining with special setting of a preparation process, the particle size and the second phase type characteristics in an alloy structure can be effectively changed, so that the mechanical property of the aluminum alloy is improved, the plasticity of the aluminum alloy is still good on the premise that the aluminum alloy has high strength, and the service life of the aluminum alloy is prolonged. And the material can be prepared through extrusion molding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aluminum alloys, and in particular to a high-strength aluminum alloy and a preparation method thereof. Background Art

[0002] With the progress of society and the rapid development of technology, aluminum alloys are used more and more widely in production and life, and higher and higher requirements are placed on the performance of aluminum alloys, resulting in the inability of existing aluminum alloys to meet new demands.

[0003] Taking the automobile industry as an example, the transformation and upgrading of the automobile industry is gradually developing in the direction of new energy, lightweight, intelligent and networked. Due to its many excellent properties, aluminum alloy has become a representative material for lightweighting automobiles, especially new energy vehicles. The application of lightweight aluminum alloy structural parts has played an increasingly important role in improving the performance and competitiveness of automobile products.

[0004] In recent years, with the gradual acceleration of the process of automobile lightweighting, the amount of aluminum used in structural parts and covering parts of domestically produced automobiles has begun to increase.

[0005] However, after the aluminum content of the vehicle body approaches or even reaches its limit, how to continue to achieve lightweighting of the vehicle has become an urgent problem to be solved. At the same time, the automotive industry has been under great pressure to reduce prices in the past two years, which requires that costs should be reduced as much as possible while lightweighting, but the vehicle's requirements for safety and other performance must also be met. Therefore, how to develop new aluminum alloys to meet the design requirements of lightweight vehicles and market price pressure has become an important task for the aluminum alloy industry. Summary of the invention

[0006] The purpose of this application is to provide a high-strength aluminum alloy and its preparation method in view of the shortcomings of the current technology. This application can effectively change the particle size and second phase characteristics in the alloy structure by adjusting the Si / Mg ratio, Y / Sr ratio and adding nano-titanium dioxide-graphene-copper aluminum alloy, and at the same time combine the special setting of the preparation process, so as to improve the mechanical properties of the aluminum alloy, so that the aluminum alloy has good plasticity under the premise of high strength, and can be prepared by extrusion molding. The aluminum alloy prepared in this application has good mechanical properties, its tensile strength ≥390MPa, yield strength ≥350MPa, elongation ≥12.0%, and the bending angle can be maintained above 60°; the aluminum alloy of this application has better lightweight characteristics, as well as stronger rigidity and toughness, which can ensure that the whole vehicle collision, head-on collision and offset collision reach a better level. The product can be used in SUV new energy vehicles with higher requirements as anti-collision beams, while maintaining a good lightweight effect, and the lightweight weight reduction effect can reach more than 20%.

[0007] In a first aspect, the present application provides a high-strength aluminum alloy, using the following technical solution: A high-strength aluminum alloy comprises the following raw materials, measured by mass percentage: Fe: 0.16-0.25%, Mn: 0.65-0.9%, Si: 0.8-1.20%, Mg: 0.80-1.0%, Cr: 0.15-0.22%, Y: 0.13-0.20%, Sr: 0.01-0.02%, nano titanium dioxide-graphene-copper aluminum alloy 8.8-9.7%, and the balance is Al.

[0008] By adopting the above technical scheme, Fe, Mn, Si, Mg, Cr, Y, Sr and other elements are used as the main components of the alloy. By regulating their proportions and interactions, the particle size and second phase characteristics in the alloy structure can be effectively changed, thereby improving the mechanical properties of the aluminum alloy. Nano-titanium dioxide-graphene-copper aluminum alloy is a special additive. Nano-titanium dioxide can be used as a nucleation particle to effectively refine the microstructure of the aluminum alloy; nitrogen-containing graphene uses its rich oxygen-containing functional groups to fully disperse other elements, further improving the mechanical properties of the alloy material, while achieving a lightweight effect; copper elements can increase the dispersion of the precipitated phase, play a solid solution strengthening effect, and make the aluminum alloy have good comprehensive properties. In addition to having a certain strengthening effect in the alloy, Mn can also promote the formation of material fiber structure. At the same time, Mn can effectively promote the spheroidization of the needle-shaped Fe phase into a spherical α (Fe, Mn) Al6 phase, while the needle-shaped Fe is not conducive to the improvement of the extrusion, welding, fatigue, mechanical and other properties of the material. The effects of Cr and Mn are basically the same. The composite addition of Cr and Mn can more effectively inhibit the grain nucleation and recrystallization of the material during hot working or heat treatment. At the same time, Cr will also greatly increase the quenching sensitivity of the material, so it needs to be added in combination with Mn to better balance the negative effects of the Cr element. Si and Mg elements are the main alloying elements that form strengthening phases. When both exist at the same time, aging strengthening phases such as Mg2Si will be formed. The present application improves the alloy strength and recrystallization temperature by controlling the ratio of Si and Mg, and prevents the Si phase from segregating at the grain boundaries. The Y element belongs to the core additive element of the present application, which forms an Al2Y dispersed phase in the high-strength aluminum alloy of the present application. This phase can effectively refine the alloy grains, improve the tensile strength, and improve the deformation toughness of the material during the melting and casting stage. Secondly, in the extrusion hot working process, Al2Y can effectively inhibit the recrystallization of the material, and can also become the nucleation point of the Mg2Si precipitation strengthening phase, further improving the strength of the material. The Sr element belongs to the core additive element of the present application, and its role is to refine the grains. Controlling the ratio of Y and Sr improves the strengthening effect of the MgSi phase in the alloy and the recrystallization temperature while also avoiding the decrease in the mechanical properties of the alloy. In summary, the high-strength aluminum alloy in this application achieves excellent mechanical properties through the synergistic effect of various elements and a special preparation process, so that it has good plasticity while having medium to high use strength, and can be prepared by extrusion molding.

[0009] Preferably, the mass ratio of Si to Mg is 1-1.1:1.

[0010] By adopting the above technical scheme, the mass fraction ratio of Si and Mg is controlled within the range of 1-1.1:1, because Si and Mg elements have a synergistic effect in aluminum alloys. When the ratio of Si and Mg is appropriate, they can form Mg2Si aging strengthening phase, and this precipitation phase is easy to solid dissolve, so the solid solution heat treatment is simple. By controlling the ratio of Si and Mg, the alloy strength and recrystallization temperature can be improved, and the Si phase can be prevented from segregating at the grain boundary. When Si and Mg are present in the aluminum alloy at the same time, they will form Mg2Si aging strengthening phase. This precipitation phase has high hardness and strength, which helps to improve the overall mechanical properties of the aluminum alloy. By controlling the ratio of Si and Mg, the recrystallization temperature of the alloy can be effectively increased, which helps to maintain the stability and mechanical properties of the aluminum alloy under high temperature environment. The appropriate ratio of Si and Mg can prevent the Si phase from segregating at the grain boundary, thereby avoiding grain boundary embrittlement and reducing the overall mechanical properties of the material. In summary, the present application fully utilizes the synergistic effect between Si and Mg by controlling the mass fraction ratio of Si and Mg to 1-1.1:1, and improves the mechanical properties and performance of the aluminum alloy.

[0011] Preferably, the mass ratio of Y to Sr is 8-10:1.

[0012] By adopting the above technical scheme, both Y and Sr can effectively refine the grain size of aluminum alloy, thereby improving the mechanical properties of the material. Y element forms Al2Y dispersed phase in aluminum alloy, which can effectively refine the alloy grains and improve the tensile strength and deformation toughness. Sr element improves the overall performance of the alloy by refining the grains. The ratio control of Y and Sr helps to optimize the formation of Mg2Si aging strengthening phase. By controlling the ratio of Y and Sr, the strength and recrystallization temperature of the alloy can be improved, and the Si phase can be prevented from segregating at the grain boundary. In the extrusion hot working process, Al2Y can effectively inhibit the recrystallization of the material, and can also become the nucleation point of the Mg2Si precipitation strengthening phase, further improving the strength of the material. The ratio of Y and Sr is controlled between 8-10:1, which can maximize the synergistic effect of the two. Under this ratio, Y element is used as a core additive element, and the Al2Y dispersed phase formed can effectively refine the grains and improve the tensile strength; while Sr element is used as an auxiliary element to further refine the grains and optimize the formation of Mg2Si strengthening phase. The combination of the two not only improves the strengthening effect of the Mg2Si phase in the alloy, but also increases the recrystallization temperature, avoiding the decrease in the mechanical properties of the alloy. In summary, the role of the mass fraction ratio of Y to Sr in this application is mainly to improve the mechanical properties and plasticity of the aluminum alloy through grain refinement, the formation of strengthening phases, the inhibition of recrystallization and synergistic effects, while maintaining a good lightweight effect.

[0013] Preferably, the nano-titanium dioxide-graphene-copper-aluminum alloy comprises the following raw materials, by mass: 9-10 parts of graphene oxide, 900 parts of ethanol, 3-4 parts of nano-titanium dioxide, 8-9 parts of ethanol copper, 40-43 parts of aluminum powder, 2-3 parts of hydroxyphenylethanolamine and 130-150 parts of tris(hydroxymethyl)aminomethane hydrochloride solution with a pH of 7.5, wherein the average particle size of the nano-titanium dioxide is 10 nanometers.

[0014] Preferably, the method for preparing the nano titanium dioxide-graphene-copper aluminum alloy comprises the following steps: S51, mixing graphene oxide, hydroxyphenylethanolamine and ethanol according to parts by mass to prepare a graphene oxide dispersion; S52, adding nano-titanium dioxide, ethanol copper, aluminum powder and tris(hydroxymethyl)aminomethane hydrochloride) solution to the graphene oxide dispersion according to their mass fractions, stirring evenly, heating to 50° C. for reaction for 3 hours, concentrating to dryness, and collecting the solid phase; S53, calcining the solid phase at 1210-1230° C. for 3.5 hours in a reducing atmosphere, and cooling to room temperature to obtain nano titanium dioxide-graphene-copper aluminum alloy, wherein the reducing atmosphere is a mixed gas of argon and hydrogen, and the volume fraction of hydrogen is 10%.

[0015] By adopting the above technical scheme, graphene oxide, hydroxyphenylethanolamine and ethanol are mixed according to the mass fraction to obtain a graphene oxide dispersion. The purpose of this step is to use hydroxyphenylethanolamine to nitrogen-modify graphene oxide so that its surface has abundant oxygen-containing functional groups and nitrogen-containing groups. According to the mass fraction, nano titanium dioxide, ethanol copper, aluminum powder and trishydroxymethylaminomethane hydrochloride solution are added to the graphene oxide dispersion and stirred evenly, then heated to 50°C for reaction for 3 hours, concentrated to dryness, and solid phase is collected. The purpose of this step is to fully disperse nano titanium dioxide, copper element and aluminum powder on the surface of graphene oxide to form an intermediate alloy with a smaller particle size. The solid phase is calcined at 1210-1230°C for 3.5 hours in a reducing atmosphere, cooled to room temperature, and nano titanium dioxide-graphene-copper-aluminum alloy is obtained. Wherein, the reducing atmosphere is a mixed gas of argon and hydrogen, and the volume fraction of hydrogen is 10%. The purpose of this step is to make the nano-titanium dioxide, copper element, aluminum powder and graphene oxide in the intermediate alloy fully react at high temperature to form a nano-titanium dioxide-graphene-copper-aluminum alloy with specific structure and performance. The present application utilizes the rich oxygen-containing functional groups on the surface of graphene oxide, and hydroxyphenylethanolamine is used to nitrogen-modify graphene oxide, and the nano-titanium dioxide, copper element, and aluminum powder are fully dispersed through nitrogen-containing groups and oxygen-containing functional groups to obtain an intermediate alloy with a smaller particle size; thereby further improving the dispersibility of the above components in the final aluminum alloy material, and significantly improving the mechanical properties of the aluminum alloy material. Nano-titanium dioxide is in a crystalline state, and its crystalline state can first form nucleation particles when the aluminum alloy solidifies, which can effectively refine the aluminum alloy microstructure, thereby improving the mechanical properties of the aluminum alloy material. Cu can increase the dispersion of the precipitated phase in the aluminum alloy, and can also play a role in solid solution strengthening, so that the aluminum alloy has good comprehensive properties.

[0016] In a second aspect, the present application provides a method for preparing a high-strength aluminum alloy, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned high-strength aluminum alloy, comprising the following steps: S61, selecting an aluminum ingot with a purity of 99.9%, a magnesium ingot with a purity of 99.95%, and an AlFe10 master alloy, an AlMn1O master alloy, an A1Y5 master alloy, an AlCr10 master alloy, an AlSi20 master alloy, an AlSr5 master alloy, and a nano-titanium dioxide-graphene-copper aluminum alloy as raw materials; S62, smelting the aluminum ingot until it is completely melted, and then sequentially adding AlSi20 master alloy, AlMn10 master alloy, AlCr10 master alloy, A1Y5 master alloy, AlFe10 master alloy, AlSr5 master alloy and magnesium ingot until they are completely melted, stirring evenly, and then keeping warm to obtain melt A; S63, adding nano-titanium dioxide-graphene-copper aluminum alloy to melt A and smelting again to obtain aluminum alloy melt; S64, adding hexachloroethane to the aluminum alloy melt for degassing, then removing slag, controlling the temperature to be 697° C.-705° C. for casting, and obtaining an aluminum alloy ingot A after cooling, wherein the mass ratio of the hexachloroethane to the aluminum alloy melt is 1:250; S65, homogenizing the aluminum alloy ingot A, and then quenching it after keeping it warm for 2-2.5 hours; the process conditions of the quenching treatment are: the cooling medium is room temperature water, the quenching water temperature is 550-560°C, and the cooling rate is 80°C / s, to obtain an aluminum alloy ingot B; S66, grinding the surface of the aluminum alloy ingot B, extruding it at 430-440° C., and then cooling it to room temperature to obtain an extruded aluminum alloy; S67. The extruded aluminum alloy is subjected to solution treatment, quenching and aging treatment in sequence to obtain a high-strength aluminum alloy.

[0017] By adopting the above technical scheme, high-purity raw materials are selected (S61): the purity and quality of the aluminum alloy are ensured, providing a basis for the subsequent preparation process. Melting and adding intermediate alloys (S62): After the aluminum ingot is completely melted, various intermediate alloys and magnesium ingots are added in turn, stirred evenly, and melt A is obtained. The purpose of this step is to fully mix the various alloy elements to lay the foundation for the preparation of high-strength aluminum alloys. Adding nano-titanium dioxide-graphene-copper aluminum alloy (S63): This special alloy material is added to the melt A and melted again to obtain an aluminum alloy melt. The purpose of this step is to introduce nano-titanium dioxide, nitrogen-containing graphene and copper elements to improve the structure and properties of the aluminum alloy. Degassing, deslagging and casting (S64): Hexachloroethane is added to the aluminum alloy melt for degassing, then deslagging, the temperature is controlled for casting, and aluminum alloy ingot A is obtained after cooling. The purpose of this step is to remove gas and impurities in the melt to ensure the quality of the aluminum alloy. Homogenization and quenching (S65): The aluminum alloy ingot A is homogenized, and then quenched after being kept warm for a period of time. The purpose of this step is to optimize the organizational structure of the aluminum alloy and improve its mechanical properties. Extrusion molding (S66): After the aluminum alloy ingot B is surface-polished, it is extruded at a certain temperature and then cooled to room temperature to obtain an extruded aluminum alloy. The purpose of this step is to give the aluminum alloy good plasticity for subsequent processing. Solution, quenching and aging treatment (S67): The extruded aluminum alloy is sequentially solutionized, quenched and aged to obtain a high-strength aluminum alloy. The purpose of this step is to further improve the mechanical properties of the aluminum alloy so that it has high strength, high toughness and good plasticity. Through the synergistic effect of the above steps, the high-strength aluminum alloy prepared in this application has good mechanical properties, tensile strength ≥390MPa, yield strength ≥350MPa, elongation ≥12.0%, and the bending angle can be maintained above 60°. In addition, the aluminum alloy also has lightweight characteristics, and the weight reduction effect can reach more than 20%, which is suitable for new energy vehicles and other fields.

[0018] Preferably, in step S62, the smelting temperature is 750-760°C; the stirring time is 130-150 seconds, and the insulation time is 3-4 minutes.

[0019] Preferably, in step S63, the temperature of the re-smelting is 710°C-720°C.

[0020] Preferably, in step S65, the homogenization treatment includes: primary homogenization treatment and secondary homogenization treatment in sequence, wherein the primary homogenization treatment temperature is 380-420°C, and the insulation time is 3-4 hours; the secondary homogenization treatment temperature is 550-560°C, and the insulation time is 4-5 hours.

[0021] By adopting the above technical solution, through two-stage homogenization treatment, the internal stress and component segregation in the aluminum alloy ingot can be more effectively eliminated, making the alloy structure more uniform. This helps to improve the mechanical properties and plasticity of the aluminum alloy. The first-stage homogenization treatment mainly dissolves the low-melting point phase, such as Al2 Y, etc. This helps to refine the alloy grains, improve the tensile strength, and improve the deformation toughness of the material. The second-stage homogenization treatment mainly dissolves the high-melting point phase, such as Mg2Si, etc. This helps to improve the alloy strength and recrystallization temperature, and prevent the Si phase from segregating at the grain boundary.

[0022] Preferably, in step S67, the process parameters of the solution treatment are: temperature of 550-560°C, time of 2-3 hours; the process parameters of the aging treatment are: temperature of 150°C, time of 4 hours, temperature of 175°C, time of 8 hours; the cooling medium of the quenching is room temperature water.

[0023] By adopting the above technical scheme, solution treatment: by subjecting the aluminum alloy ingot B to solution treatment, the strengthening phase in the alloy can be fully dissolved into the matrix, thereby improving the strength and hardness of the alloy. At the same time, solution treatment can also eliminate the residual stress in the alloy and make the structure of the alloy more uniform. In the present application, the temperature of the solution treatment is 550-560°C and the time is 2-3 hours. Such process parameters can ensure that the strengthening phase in the alloy is fully dissolved, while avoiding excessive temperature causing the alloy grain to grow. Aging treatment: Aging treatment is one of the important means of strengthening aluminum alloys. By keeping the temperature at a certain temperature for a period of time, fine strengthening phases are precipitated in the alloy after solution treatment, thereby improving the strength and hardness of the alloy. In the present application, the aging treatment is divided into two stages, the temperature of the first stage is 150°C, the time is 4 hours, and the temperature of the second stage is 175°C, and the time is 8 hours. Such process parameters can make the strengthening phase in the alloy more fine and uniform, further improving the mechanical properties of the alloy. Quenching treatment: Quenching treatment is to quickly cool the alloy after solution treatment to room temperature, so that the strengthening phase in the alloy remains dissolved and forms a supersaturated solid solution, creating conditions for subsequent aging treatment. In this application, the cooling medium for quenching is room temperature water. This cooling method can quickly cool the alloy, avoid the precipitation of strengthening phases, and reduce the deformation and cracking tendency of the alloy.

[0024] In summary, the beneficial technical effects of this application are: 1. By adjusting the Si / Mg ratio, Y / Sr ratio and adding nano-titanium dioxide-graphene-copper aluminum alloy, the particle size and second phase characteristics in the alloy structure can be effectively changed, thereby improving the mechanical properties of aluminum alloy.

[0025] 2. The aluminum alloy prepared in the present application has good mechanical properties, with a tensile strength of ≥390MPa, a yield strength of ≥350MPa, an elongation of ≥13.0%, and a bending angle that can be maintained above 60°.

[0026] 3. The aluminum alloy of this application has better lightweight properties, as well as stronger rigidity and toughness, which can ensure that the whole vehicle collision, head-on collision and offset collision reach a better level. The product can be used in SUV new energy vehicles with higher requirements as an anti-collision beam, while maintaining a good lightweight effect. The lightweight weight reduction effect can reach more than 20%.

[0027] 4. The graphene oxide surface is rich in oxygen-containing functional groups, and hydroxyphenylethanolamine is used to nitrogen-modify the graphene oxide. The nitrogen-containing groups and oxygen-containing functional groups are used to fully disperse the nano-titanium dioxide, copper elements, and aluminum powder, thereby obtaining an intermediate alloy with a smaller particle size; thereby further improving the dispersibility of the above components in the final aluminum alloy material, thereby significantly improving the mechanical properties of the aluminum alloy material.

[0028] 5. Improve alloy strength and recrystallization temperature: Si and Mg are the main alloying elements that form strengthening phases. When they exist at the same time, they will form aging strengthening phases such as Mg2Si. The Mg2Si precipitation phase is easy to dissolve, so the solution heat treatment is simple. This application improves the alloy strength and recrystallization temperature by controlling the ratio of Si and Mg, and prevents the Si phase from segregating at the grain boundary. DETAILED DESCRIPTION

[0029] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0030] In the following examples, preparation examples and comparative preparation examples, 1 part represents 100 g, the purity of the aluminum powder is 99.9%, and the particle size is 1-5 μm.

[0031] Preparation Example 1 Preparation of Nano-TiO2-Graphene-Copper-Aluminum Alloy The nano-titanium dioxide-graphene-copper-aluminum alloy comprises the following raw materials, measured by mass: 9 parts of graphene oxide, 900 parts of ethanol, 3 parts of nano-titanium dioxide, 8 parts of ethanol copper, 40 parts of aluminum powder, 2 parts of hydroxyphenylethanolamine and 130 parts of tris(hydroxymethyl)aminomethane hydrochloride solution with a pH of 7.5, wherein the average particle size of the nano-titanium dioxide is 10 nanometers.

[0032] The preparation method of nano titanium dioxide-graphene-copper aluminum alloy comprises the following steps: S51, mixing graphene oxide, hydroxyphenylethanolamine and ethanol according to parts by mass to prepare a graphene oxide dispersion; S52, adding nano-titanium dioxide, ethanol copper, aluminum powder and tris(hydroxymethyl)aminomethane hydrochloride) solution to the graphene oxide dispersion according to their mass fractions, stirring evenly, heating to 50° C. for reaction for 3 hours, concentrating to dryness, and collecting the solid phase; S53, calcining the solid phase at 1210° C. for 3.5 hours in a reducing atmosphere, and cooling to room temperature to obtain nano titanium dioxide-graphene-copper aluminum alloy, wherein the reducing atmosphere is a mixed gas of argon and hydrogen, and the volume fraction of hydrogen is 10%.

[0033] Preparation Example 2 Preparation of Nano-TiO2-Graphene-Copper-Aluminum Alloy The nano-titanium dioxide-graphene-copper-aluminum alloy comprises the following raw materials, measured by mass: 10 parts of graphene oxide, 900 parts of ethanol, 4 parts of nano-titanium dioxide, 9 parts of ethanol copper, 43 parts of aluminum powder, 3 parts of hydroxyphenylethanolamine and 150 parts of tris(hydroxymethyl)aminomethane hydrochloride solution with a pH of 7.5, wherein the average particle size of the nano-titanium dioxide is 10 nanometers.

[0034] The preparation method of nano titanium dioxide-graphene-copper aluminum alloy comprises the following steps: S51, mixing graphene oxide, hydroxyphenylethanolamine and ethanol according to parts by mass to prepare a graphene oxide dispersion; S52, adding nano-titanium dioxide, ethanol copper, aluminum powder and tris(hydroxymethyl)aminomethane hydrochloride) solution to the graphene oxide dispersion according to their mass fractions, stirring evenly, heating to 50° C. for reaction for 3 hours, concentrating to dryness, and collecting the solid phase; S53, calcining the solid phase at 1230° C. for 3.5 hours in a reducing atmosphere, and cooling to room temperature to obtain nano titanium dioxide-graphene-copper aluminum alloy, wherein the reducing atmosphere is a mixed gas of argon and hydrogen, and the volume fraction of hydrogen is 10%.

[0035] Preparation Example 3 Preparation of Nano-TiO2-Graphene-Copper-Aluminum Alloy The nano-titanium dioxide-graphene-copper-aluminum alloy comprises the following raw materials, measured by mass: 9.5 parts of graphene oxide, 900 parts of ethanol, 3.5 parts of nano-titanium dioxide, 8.5 parts of ethanol copper, 42 parts of aluminum powder, 2.6 parts of hydroxyphenylethanolamine and 140 parts of tris(hydroxymethyl)aminomethane hydrochloride solution with a pH of 7.5, wherein the average particle size of the nano-titanium dioxide is 10 nanometers.

[0036] The preparation method of nano titanium dioxide-graphene-copper aluminum alloy comprises the following steps: S51, mixing graphene oxide, hydroxyphenylethanolamine and ethanol according to parts by mass to prepare a graphene oxide dispersion; S52, adding nano-titanium dioxide, ethanol copper, aluminum powder and tris(hydroxymethyl)aminomethane hydrochloride) solution to the graphene oxide dispersion according to their mass fractions, stirring evenly, heating to 50° C. for reaction for 3 hours, concentrating to dryness, and collecting the solid phase; S53, calcining the solid phase at 1220° C. for 3.5 hours in a reducing atmosphere, and cooling to room temperature to obtain nano titanium dioxide-graphene-copper aluminum alloy, wherein the reducing atmosphere is a mixed gas of argon and hydrogen, and the volume fraction of hydrogen is 10%.

[0037] Preparation Comparative Example 1 9.5 parts of graphene oxide, 3.5 parts of nano titanium dioxide, 3.54 parts of copper powder with a purity of 99.9% and a particle size of 1.5 microns, and 42 parts of aluminum powder were mixed evenly to obtain a mixture; wherein the average particle size of the nano titanium dioxide was 10 nanometers. Example 1 A high-strength aluminum alloy comprises the following raw materials, measured by mass percentage: Fe: 0.16%, Mn: 0.65%, Si: 0.8%, Mg: 1%, Cr: 0.15%, Y: 0.13%, Sr: 0.01%, nano titanium dioxide-graphene-copper aluminum alloy 8.8%, and the balance Al.

[0038] The raw materials for preparing the high-strength aluminum alloy in this embodiment are as follows: Aluminum ingots with a purity of 99.9%, magnesium ingots with a purity of 99.95%, and AlFe10 master alloy (10.00% Fe, 0.001% impurity elements, the rest is aluminum), AlMn1O master alloy (10.00% Mn, 0.001% impurity elements, the rest is aluminum), A1Y5 master alloy (5.00% Y, 0.001% impurity elements, the rest is aluminum), AlCr10 master alloy (10.00% Cr, 0.001% impurity elements, the rest is aluminum), AlSi20 master alloy (20.00% Si, 0.001% impurity elements, the rest is aluminum), AlSr5 master alloy (5.00% Sr, 0.001% impurity elements, the rest is aluminum) and nano titanium dioxide - graphene - copper aluminum alloy prepared in Preparation Example 1.

[0039] The above-mentioned method for preparing a high-strength aluminum alloy comprises the following steps: S62, smelting the aluminum ingot at a temperature of 750° C. until it is completely melted, and then sequentially adding AlSi20 master alloy, AlMn10 master alloy, AlCr10 master alloy, A1Y5 master alloy, AlFe10 master alloy, AlSr5 master alloy and magnesium ingot until they are completely melted, stirring for 130 seconds, and then keeping the temperature for 3 minutes to obtain melt A; S63, adding nano-titanium dioxide-graphene-copper aluminum alloy to melt A and re-melting, wherein the re-melting temperature is 710° C. to obtain aluminum alloy melt; S64, adding hexachloroethane to the aluminum alloy melt for degassing, then removing slag, controlling the temperature to be 697° C. for casting, and obtaining an aluminum alloy ingot A after cooling, wherein the mass ratio of the hexachloroethane to the aluminum alloy melt is 1:250; S65, subjecting the aluminum alloy ingot A to homogenization treatment, and then subjecting it to quenching treatment after keeping it warm for 2 hours; the homogenization treatment sequentially comprises: a primary homogenization treatment and a secondary homogenization treatment, wherein the primary homogenization treatment temperature is 380° C., and the holding time is 4 hours; the secondary homogenization treatment temperature is 550° C., and the holding time is 5 hours; the process conditions of the quenching treatment are: the cooling medium is room temperature water, the quenching water temperature is 550° C., and the cooling rate is 80° C. / s, to obtain an aluminum alloy ingot B; S66, grinding the surface of the aluminum alloy ingot B, extruding it at 430° C., and then cooling it to room temperature to obtain an extruded aluminum alloy; S67. The extruded aluminum alloy is subjected to solution treatment, quenching and aging treatment in sequence to obtain a high-strength aluminum alloy. The process parameters of the solution treatment are: temperature of 550°C and time of 3 hours; the process parameters of the aging treatment are: temperature of 150°C and time of 4 hours, temperature of 175°C and time of 8 hours; the cooling medium of the quenching is room temperature water.

[0040] Example 2 A high-strength aluminum alloy comprises the following raw materials by mass percentage: Fe: 0.25%, Mn: 0.9%, Si: 1.20%, Mg: 0.80%, Cr: 0.22%, Y: 0.20%, Sr: 0.02%, nano titanium dioxide-graphene-copper aluminum alloy 9.7%, and the balance Al.

[0041] The raw materials for preparing the high-strength aluminum alloy in this embodiment are as follows: Aluminum ingots with a purity of 99.9%, magnesium ingots with a purity of 99.95%, and AlFe10 master alloy (10.00% Fe, 0.001% impurity elements, the rest is aluminum), AlMn1O master alloy (10.00% Mn, 0.001% impurity elements, the rest is aluminum), A1Y5 master alloy (5.00% Y, 0.001% impurity elements, the rest is aluminum), AlCr10 master alloy (10.00% Cr, 0.001% impurity elements, the rest is aluminum), AlSi20 master alloy (20.00% Si, 0.001% impurity elements, the rest is aluminum), AlSr5 master alloy (5.00% Sr, 0.001% impurity elements, the rest is aluminum) and nano titanium dioxide - graphene - copper aluminum alloy prepared in Preparation Example 2.

[0042] The above-mentioned method for preparing a high-strength aluminum alloy comprises the following steps: S62, smelting the aluminum ingot at a temperature of 760° C. until it is completely melted, and then sequentially adding AlSi20 master alloy, AlMn10 master alloy, AlCr10 master alloy, A1Y5 master alloy, AlFe10 master alloy, AlSr5 master alloy and magnesium ingot until they are completely melted, stirring for 150 seconds, and then keeping the temperature for 4 minutes to obtain melt A; S63, adding nano-titanium dioxide-graphene-copper aluminum alloy to melt A and re-melting, wherein the re-melting temperature is 720° C. to obtain aluminum alloy melt; S64, adding hexachloroethane to the aluminum alloy melt for degassing, then removing slag, controlling the temperature to 705° C. for casting, and obtaining an aluminum alloy ingot A after cooling, wherein the mass ratio of the hexachloroethane to the aluminum alloy melt is 1:250; S65, subjecting the aluminum alloy ingot A to homogenization treatment, and then subjecting it to quenching treatment after keeping it warm for 2.5 hours; the homogenization treatment sequentially comprises: a primary homogenization treatment and a secondary homogenization treatment, wherein the primary homogenization treatment temperature is 420° C., and the holding time is 3 hours; the secondary homogenization treatment temperature is 560° C., and the holding time is 4 hours; the process conditions of the quenching treatment are: the cooling medium is room temperature water, the quenching water temperature is 560° C., and the cooling rate is 80° C. / s, to obtain an aluminum alloy ingot B; S66, grinding the surface of the aluminum alloy ingot B, extruding it at 440° C., and then cooling it to room temperature to obtain an extruded aluminum alloy; S67. The extruded aluminum alloy is subjected to solution treatment, quenching and aging treatment in sequence to obtain a high-strength aluminum alloy. The process parameters of the solution treatment are: temperature of 560°C and time of 2 hours; the process parameters of the aging treatment are: temperature of 150°C and time of 4 hours, temperature of 175°C and time of 8 hours; the cooling medium of the quenching is room temperature water.

[0043] Example 3 A high-strength aluminum alloy comprises the following raw materials, measured by mass percentage: Fe: 0.2%, Mn: 0.8%, Si: 1.0%, Mg: 1.0%, Cr: 0.19%, Y: 0.16%, Sr: 0.014%, nano titanium dioxide-graphene-copper aluminum alloy 9.3%, and the balance Al.

[0044] The raw materials for preparing the high-strength aluminum alloy in this embodiment are as follows: Aluminum ingots with a purity of 99.9%, magnesium ingots with a purity of 99.95%, and AlFe10 master alloy (10.00% Fe, 0.001% impurity elements, the rest is aluminum), AlMn1O master alloy (10.00% Mn, 0.001% impurity elements, the rest is aluminum), A1Y5 master alloy (5.00% Y, 0.001% impurity elements, the rest is aluminum), AlCr10 master alloy (10.00% Cr, 0.001% impurity elements, the rest is aluminum), AlSi20 master alloy (20.00% Si, 0.001% impurity elements, the rest is aluminum), AlSr5 master alloy (5.00% Sr, 0.001% impurity elements, the rest is aluminum) and nano titanium dioxide - graphene - copper aluminum alloy prepared in Preparation Example 3.

[0045] The above-mentioned method for preparing a high-strength aluminum alloy comprises the following steps: S62, smelting the aluminum ingot at a temperature of 755° C. until it is completely melted, and then sequentially adding AlSi20 master alloy, AlMn10 master alloy, AlCr10 master alloy, A1Y5 master alloy, AlFe10 master alloy, AlSr5 master alloy and magnesium ingot until they are completely melted, stirring for 140 seconds, and then keeping the temperature for 3.5 minutes to obtain melt A; S63, adding nano-titanium dioxide-graphene-copper aluminum alloy to melt A and re-melting, wherein the re-melting temperature is 715° C. to obtain aluminum alloy melt; S64, adding hexachloroethane to the aluminum alloy melt for degassing, then removing slag, controlling the temperature to 700° C. for casting, and obtaining an aluminum alloy ingot A after cooling, wherein the mass ratio of the hexachloroethane to the aluminum alloy melt is 1:250; S65, subjecting the aluminum alloy ingot A to homogenization treatment, and then subjecting it to quenching treatment after keeping it warm for 2.3 hours; the homogenization treatment sequentially comprises: primary homogenization treatment and secondary homogenization treatment, wherein the primary homogenization treatment temperature is 390° C., and the holding time is 3.6 hours; the secondary homogenization treatment temperature is 555° C., and the holding time is 4.5 hours; the process conditions of the quenching treatment are: the cooling medium is room temperature water, the quenching water temperature is 555° C., and the cooling rate is 80° C. / s, to obtain an aluminum alloy ingot B; S66, grinding the surface of the aluminum alloy ingot B, extruding it at 435° C., and then cooling it to room temperature to obtain an extruded aluminum alloy; S67. The extruded aluminum alloy is subjected to solution treatment, quenching and aging treatment in sequence to obtain a high-strength aluminum alloy. The process parameters of the solution treatment are: temperature of 555°C and time of 2.5 hours; the process parameters of the aging treatment are: temperature of 150°C and time of 4 hours, temperature of 175°C and time of 8 hours; the cooling medium of the quenching is room temperature water.

[0046] Example 4 The same as Example 3 except that Y: 0.144% and Sr: 0.018%.

[0047] Example 5 The same as Example 3, except that Y: 0.15% and Sr: 0.015%.

[0048] Comparative Example 1 The same as Example 5, except that Si: 1.7% and Mg: 0.3%.

[0049] Comparative Example 2 The same as Example 5, except that Si: 0.3% and Mg: 1.7%.

[0050] Comparative Example 3 The same as Example 5, except that Y: 0.174% and Sr: 0%.

[0051] Comparative Example 4 The same as Example 5, except that Y: 0% and Sr: 0.02%.

[0052] Comparative Example 5 The same as Example 5, except that an equal amount of the mixture prepared in Comparative Example 1 is used to replace the nano-titanium dioxide-graphene-copper-aluminum alloy.

[0053] Comparative Example 6 The same as the fifth embodiment, except that in step S65, the primary homogenization process is not used, but the secondary homogenization process is directly used.

[0054] Comparative Example 7 The same as Example 5, except that in step S67, no aging treatment is performed on the extruded aluminum alloy.

[0055] Performance Testing The high-strength aluminum alloys prepared in Examples 1 to 5 and Comparative Examples 1 to 7 were sampled and subjected to the following performance tests: Tensile strength, elongation and yield strength: refer to GB / T228.1-2010 Metallic Materials Tensile Test Part 1: Room Temperature Test Methods to test the tensile strength, elongation and yield strength of aluminum alloys, and use CMT4305 microelectronic universal testing machine to measure the room temperature tensile properties of materials; The bending angle test method is carried out according to the standard VDA238-100-2017 method.

[0056] Table 1 Performance test project Tensile strength / MPa Yield strength / MPa Elongation / % Bending angle / ° Example 1 390.2 350.2 12.1 60 Example 2 393.4 355.7 12.4 62 Example 3 410.3 364.3 13.1 66 Example 4 419.5 377.2 13.8 69 Example 5 421.3 381.5 14.2 70 Comparative Example 1 321.6 316.3 7.9 45 Comparative Example 2 318.4 311.2 7.6 43 Comparative Example 3 314.6 307.4 7.4 41 Comparative Example 4 309.5 298.3 6.7 35 Comparative Example 5 336.2 322.3 9.9 48 Comparative Example 6 412.1 361.3 13.1 66 Comparative Example 7 414.3 368.2 12.8 65 Analyzing the data in Table 1, we can see that: 1) The high-strength aluminum alloys prepared in Examples 1 to 5 can effectively change the particle size and second phase characteristics in the alloy structure by adjusting the Si / Mg ratio, Y / Sr ratio and adding nano-titanium dioxide-graphene-copper aluminum alloy, and combined with the special setting of the preparation process, thereby improving the mechanical properties of the aluminum alloy, so that the aluminum alloy has good plasticity under the premise of high strength, and can be prepared by extrusion molding. The aluminum alloy prepared in this application has good mechanical properties, with a tensile strength of ≥390MPa, a yield strength of ≥350MPa, an elongation of ≥12.0%, and a bending angle of more than 60°; the aluminum alloy in this application has better lightweight characteristics, as well as stronger rigidity and toughness, which can ensure that the whole vehicle collision, head-on collision and offset collision reach a better level. The product can be used in SUV new energy vehicles with higher requirements as an anti-collision beam, while maintaining a good lightweight effect.

[0057] 2) The performance comparison analysis of the high-strength aluminum alloy obtained in combination with Example 5 and Comparative Examples 1-2 shows that when the mass fraction ratio of Si to Mg is 1:1, the synergistic effect between Si and Mg elements in the aluminum alloy can form a Mg2Si aging strengthening phase, and this precipitation phase is easy to dissolve, so the solid solution heat treatment is simple. By controlling the ratio of Si and Mg, the alloy strength and recrystallization temperature can be improved, and the Si phase can be prevented from segregating at the grain boundary. When Si and Mg are present in the aluminum alloy at the same time, they will form a Mg2Si aging strengthening phase. This precipitation phase has higher hardness and strength, which helps to improve the overall mechanical properties of the aluminum alloy.

[0058] 3) The performance comparison analysis of the high-strength aluminum alloy obtained by combining Example 5 and Comparative Examples 3-4 shows that when the mass fraction ratio of Y to Sr is 10:1, the Y element forms an Al2Y dispersed phase in the aluminum alloy, which can effectively refine the alloy grains and improve the tensile strength and deformation toughness. The Sr element improves the overall performance of the alloy by refining the grains. The ratio of Y and Sr is controlled between 10:1, which can maximize the synergistic effect of the two. Under this ratio, the Y element is used as a core additive element, and the Al2Y dispersed phase formed can effectively refine the grains and improve the tensile strength; while the Sr element is used as an auxiliary element to further refine the grains and optimize the formation of the Mg2Si strengthening phase. The combination of the two not only improves the strengthening effect of the Mg2Si phase in the alloy, but also increases the recrystallization temperature, avoiding the decline in the mechanical properties of the alloy.

[0059] 4) The performance comparison analysis of the high-strength aluminum alloy prepared in combination with Example 5 and Comparative Example 5 shows that the nano-titanium dioxide-graphene-copper aluminum alloy prepared in the present application utilizes the rich oxygen-containing functional groups on the surface of graphene oxide, and hydroxyphenylethanolamine nitrogen-modifies graphene oxide, and fully disperses nano-titanium dioxide, copper elements, and aluminum powder through nitrogen-containing groups and oxygen-containing functional groups, thereby obtaining an intermediate alloy with a smaller particle size; thereby further improving the dispersibility of the above components in the final aluminum alloy material, thereby significantly improving the mechanical properties of the aluminum alloy material. Nano-titanium dioxide is in a crystalline state, and its crystalline state can first form nucleation particles when the aluminum alloy solidifies, which can effectively refine the aluminum alloy microstructure, thereby improving the mechanical properties of the aluminum alloy material. Cu can increase the dispersion of the precipitated phase in the aluminum alloy, and can also play a role in solid solution strengthening, so that the aluminum alloy has good comprehensive properties.

[0060] 5) The performance comparison analysis of the high-strength aluminum alloy obtained in combination with Example 5 and Comparative Example 6 shows that the present application can more effectively eliminate the internal stress and component segregation in the aluminum alloy ingot through two-stage homogenization treatment, making the alloy structure more uniform. This helps to improve the mechanical properties and plasticity of the aluminum alloy. The first-stage homogenization treatment mainly dissolves low-melting point phases, such as Al2Y, etc. This helps to refine the alloy grains, improve tensile strength, and improve the deformation toughness of the material. The second-stage homogenization treatment mainly dissolves high-melting point phases, such as Mg2Si, etc. This helps to improve the alloy strength and recrystallization temperature, and prevent the Si phase from segregating at the grain boundaries.

[0061] 7) The performance comparison analysis of the high-strength aluminum alloy obtained in combination with Example 5 and Comparative Example 7 shows that aging treatment is one of the important means of strengthening aluminum alloys. By keeping the alloy at a certain temperature for a period of time, fine strengthening phases are precipitated in the alloy after solution treatment, thereby improving the strength and hardness of the alloy. In this application, the aging treatment is divided into two stages, the first stage temperature is 150°C, the time is 4 hours, and the second stage temperature is 175°C, the time is 8 hours. Such process parameters can make the strengthening phase in the alloy more fine and uniform, and further improve the mechanical properties of the alloy.

[0062] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A high-strength aluminum alloy, It is characterized in that The preparation raw materials include the following by mass percentage: Fe: 0.16-0.25%, Mn: 0.65-0.9%, Si: 0.8-1.20%, Mg: 0.80-1.0%, Cr: 0.15-0.22%, Y: 0.13-0.20%, Sr: 0.01-0.02%, nano titanium dioxide-graphene-copper aluminum alloy 8.8-9.7%, and the balance is Al.

2. A high-strength aluminum alloy according to claim 1, It is characterized in that The mass ratio of Si to Mg is 1-1.1:

1.

3. A high-strength aluminum alloy according to claim 1, It is characterized in that The mass ratio of Y to Sr is 8-10:

1.

4. The high-strength aluminum alloy according to claim 1, It is characterized in that The nano titanium dioxide-graphene-copper aluminum alloy comprises the following raw materials by weight: 9-10 parts of graphene oxide, 900 parts of ethanol, 3-4 parts of nano titanium dioxide, 8-9 parts of ethanol copper, 40-43 parts of aluminum powder, 2-3 parts of hydroxyphenylethanolamine and 130-150 parts of tris(hydroxymethyl)aminomethane hydrochloride solution with a pH of 7.5, wherein the average particle size of the nano titanium dioxide is 10 nanometers.

5. A high-strength aluminum alloy according to claim 4, It is characterized in that The preparation method of the nano titanium dioxide-graphene-copper aluminum alloy comprises the following steps: S51, mixing graphene oxide, hydroxyphenylethanolamine and ethanol according to parts by mass to prepare a graphene oxide dispersion; S52, adding nano-titanium dioxide, ethanol copper, aluminum powder and tris(hydroxymethyl)aminomethane hydrochloride) solution to the graphene oxide dispersion according to their mass fractions, stirring evenly, heating to 50° C. for reaction for 3 hours, concentrating to dryness, and collecting the solid phase; S53, calcining the solid phase at 1210-1230° C. for 3.5 hours in a reducing atmosphere, and cooling to room temperature to obtain nano titanium dioxide-graphene-copper aluminum alloy, wherein the reducing atmosphere is a mixed gas of argon and hydrogen, and the volume fraction of hydrogen is 10%.

6. A method for preparing a high-strength aluminum alloy according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S61, select aluminum ingots with a purity of 99.9%, magnesium ingots with a purity of 99.95%, AlFe10 master alloy, AlMn1O master alloy, A1Y5 master alloy, AlCr10 master alloy, AlSi20 master alloy, AlSr5 master alloy and nano-titanium dioxide-graphene-copper aluminum alloy as raw materials; S62, smelting the aluminum ingot until it is completely melted, and then sequentially adding AlSi20 master alloy, AlMn10 master alloy, AlCr10 master alloy, A1Y5 master alloy, AlFe10 master alloy, AlSr5 master alloy and magnesium ingot until they are completely melted, stirring evenly, and then keeping warm to obtain melt A; S63, adding nano-titanium dioxide-graphene-copper aluminum alloy to melt A and smelting again to obtain aluminum alloy melt; S64, adding hexachloroethane to the aluminum alloy melt for degassing, then removing slag, controlling the temperature to be 697° C.-705° C. for casting, and obtaining an aluminum alloy ingot A after cooling, wherein the mass ratio of the hexachloroethane to the aluminum alloy melt is 1:250; S65, homogenizing the aluminum alloy ingot A, and then quenching it after keeping it warm for 2-2.5 hours; the process conditions of the quenching treatment are: the cooling medium is room temperature water, the quenching water temperature is 550-560°C, and the cooling rate is 80°C / s, to obtain an aluminum alloy ingot B; S66, grinding the surface of the aluminum alloy ingot B, extruding it at 430-440° C., and then cooling it to room temperature to obtain an extruded aluminum alloy; S67. The extruded aluminum alloy is subjected to solution treatment, quenching and aging treatment in sequence to obtain a high-strength aluminum alloy.

7. A method for preparing a high-strength aluminum alloy according to claim 6, It is characterized in that In step S62, the smelting temperature is 750-760°C; the stirring time is 130-150 seconds, and the heat preservation time is 3-4 minutes.

8. A method for preparing a high-strength aluminum alloy according to claim 6, It is characterized in that In step S63, the re-melting temperature is 710°C-720°C.

9. A method for preparing a high-strength aluminum alloy according to claim 6, It is characterized in that In step S65, the homogenization treatment includes: primary homogenization treatment and secondary homogenization treatment in sequence, wherein the primary homogenization treatment temperature is 380-420°C, and the insulation time is 3-4 hours; the secondary homogenization treatment temperature is 550-560°C, and the insulation time is 4-5 hours.

10. A method for preparing a high-strength aluminum alloy according to claim 6, It is characterized in that In step S67, the process parameters of the solution treatment are: temperature of 550-560°C, time of 2-3 hours; the process parameters of the aging treatment are: temperature of 150°C, time of 4 hours, temperature of 175°C, time of 8 hours; the cooling medium of the quenching is room temperature water.

Citation Information

Patent Citations

  • Aluminum alloy extrusion material with impact-resistant energy absorption characteristic and manufacturing method thereof

    CN109468502A

  • Medium-high strength aluminum alloy and preparation method thereof

    CN116219237A

  • Sheet made of rolled aluminum alloy and method for producing such sheet

    CN116324005A

  • Aluminum alloy for light-weight new energy automobile and preparation method of aluminum alloy

    CN116875856A

  • High-toughness aluminum-magnesium alloy composite material and preparation method thereof

    CN117965973A

Cited By

  • High-conductivity wear-resistant copper alloy and preparation method and application thereof

    CN120174231A

  • Graphene aluminum alloy rod for electrician and preparation method of graphene aluminum alloy rod

    CN120330543A

  • Low-voltage aluminum conductor and preparation method thereof

    CN120432221A

  • High-temperature-resistant and high-strength aluminum alloy material and preparation method thereof

    CN120866678A

  • Extrusion aluminum alloy material for liquid cooling shell of light-weight driving motor of new energy automobile and preparation method of extrusion aluminum alloy material

    CN121674798A