Low-temperature-resistant silicone rubber cable for oil drilling platform and preparation process thereof

By adding ethylene-methyl acrylate copolymer and multi-effect flame retardant to the silicone rubber cable and using radiation vulcanization method, the problem of insufficient low temperature and oil resistance in the petroleum drilling platform environment is solved, and the cable is realized The high-efficiency flame retardant and oxidative resistance is suitable for harsh environments of oil drilling platforms.

CN119069165APending Publication Date: 2024-12-03迈特诺技术股份有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411084980.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing silicone rubber cables lack low temperature and oil resistance in the strict environment of oil drilling platforms, and are flammable, limiting their application areas.

Method used

Using methyl vinyl silicone rubber as the protective cover material, adding ethylene-methyl acrylate copolymer, multi-effect flame retardant, antioxidant and radiation vulcanization method to prepare excellent high and low temperature resistance, oil resistance and oxidation resistance. cable.

Benefits of technology

It realizes the stable and efficient flame retardant and smoke suppression performance of the cable and a certain degree of mechanical strength, significantly improves the low temperature and oil resistance, and is suitable for harsh environments of oil drilling platforms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984920060000031
    Figure BDA0004984920060000031
  • Figure BDA0004984920060000042
    Figure BDA0004984920060000042
  • Figure BDA0004984920060000091
    Figure BDA0004984920060000091
Patent Text Reader

Abstract

The invention discloses a low-temperature-resistant silicone rubber cable for an oil drilling platform and a preparation process of the low-temperature-resistant silicone rubber cable, and belongs to the technical field of cables. The cable is composed of a conductor, an insulating layer and a protective sleeve which are sequentially arranged from inside to outside. Wherein the protective sleeve material takes methyl vinyl silicone rubber as a matrix, and ethylene-methyl acrylate copolymer is added, so that the cable is endowed with excellent high and low temperature resistance and oil resistance; molecules of the added multi-effect flame retardant contain various functional groups, so that the flame-retardant and smoke-suppression performance and the mechanical strength of the cable can be remarkably enhanced, the low-temperature resistance of the cable can be improved, and the performance is long and stable; therefore, the prepared cable has excellent high and low temperature resistance, oil resistance and oxidation resistance, has stable and efficient flame-retardant smoke suppression performance and certain mechanical strength, and has important application value in the technical field of cables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cables, and in particular relates to a low-temperature resistant silicone rubber cable for an oil drilling platform and a preparation process thereof. Background Art

[0002] With the development of economy and the continuous expansion of infrastructure construction, the wire and cable industry has developed rapidly, and cables are widely used in various fields, such as petrochemical, coal mining, metal mining, etc. In recent years, oil extraction, especially offshore oil extraction, has developed rapidly, and the number of oil drilling platforms has continued to increase. Due to the special operating environment on the oil drilling platform, the working environment of the cable is very strict, which has greater requirements on the performance of the cable.

[0003] The cable is composed of a conductive core, an insulating layer and a protective sheath. The conductive core is used to transmit current, and the main function of the insulating layer is to provide electrical isolation for the conductor in the cable, preventing current from leaking into the surrounding environment and ensuring safe and efficient transmission of electrical energy. The protective sheath is in direct contact with the external environment and plays a decisive role in the performance of the cable.

[0004] Common cable sheath materials include polyethylene, cross-linked polyethylene, polypropylene, fluoroplastics and silicone rubber, among which silicone rubber refers to a rubber whose main chain is composed of alternating silicon and oxygen atoms, and the silicon atom is usually connected to two organic groups. Since silicone rubber has excellent high temperature resistance, chemical corrosion resistance and good electrical insulation properties, it can be used for a long time in a wide temperature range (-60℃ to 200℃). It has been widely used in the fields of electronics, machinery, automobiles, chemicals, aviation, aerospace, ships, etc., and is also a commonly used material in the field of cable materials. However, the use of silicone rubber in oil drilling platforms requires silicone rubber to further improve its low temperature resistance and oil resistance in a relatively strict environment. Not only that, silicone rubber molecules contain a large amount of C and H elements, which can burn when exposed to open flames, limiting the use of silicone rubber cable materials. Therefore, based on the above problems, it is urgent to invent a silicone rubber cable with excellent low temperature resistance, flame retardancy and oil resistance to meet the higher requirements in the field of cable technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a low temperature resistant silicone rubber cable for oil drilling platform and a preparation process thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A low-temperature resistant silicone rubber cable for an oil drilling platform is composed of a conductor, an insulating layer and a protective sheath which are arranged in sequence from the inside to the outside.

[0008] A method for preparing a low-temperature resistant silicone rubber cable for an oil drilling platform comprises the following steps:

[0009] An insulating layer is extruded on the conductor to form a cable. After three cables are stacked, they are filled with fillers, and then a protective sheath material is extruded and coated on the surface of the cable. After irradiation cross-linking, a low-temperature resistant silicone rubber cable for oil drilling platforms is obtained.

[0010] Furthermore, the material of the conductor is pure copper.

[0011] Furthermore, the material of the insulating layer is mica tape.

[0012] Furthermore, the filler is asbestos filling rope.

[0013] Furthermore, the material of the protective cover includes the following raw materials in parts by weight: 60-80 parts of methyl vinyl silicone rubber, 15-25 parts of ethylene-methyl acrylate copolymer, 5-15 parts of multi-effect flame retardant, 4-6 parts of lubricant, 6-12 parts of antioxidant, 0.1-0.3 parts of cross-linking sensitizer, and 2-4 parts of sulfur.

[0014] Furthermore, the antioxidant is prepared by compounding a phosphite antioxidant and a phenolic antioxidant in a mass ratio of 1:2.

[0015] Furthermore, the lubricant is one of epoxidized soybean oil and paraffin.

[0016] Furthermore, the cross-linking sensitizer is one of triallyl cyanurate and triallyl isocyanurate.

[0017] The prepared protective cover material is based on methyl vinyl silicone rubber, which not only gives the protective cover material good high and low temperature resistance and resistance to permanent compression deformation, but also has the characteristic of easy cross-linking; the added ethylene-methyl acrylate copolymer has good polymer compatibility and can enhance the thermal stability and oil resistance of the protective cover material; the antioxidant is a compound of a phosphite antioxidant and a phenolic antioxidant, the two can play a synergistic role and greatly enhance the antioxidant performance of the protective cover material.

[0018] Furthermore, the multi-effect flame retardant is prepared by the following steps:

[0019] S1. At room temperature and under nitrogen protection, phosphorus oxychloride, pentaerythritol and anhydrous acetonitrile were mixed uniformly in a three-necked flask equipped with a stirring reflux device, the reaction temperature was controlled to 68°C, the reaction was stirred for 6 hours, and then the temperature was raised to 110°C, and the reflux reaction was carried out until no hydrogen chloride gas was generated. After the reaction was completed, the mixture was cooled to room temperature, the solvent was distilled off under reduced pressure, washed with dichloromethane 3-4 times, and dried in vacuo to obtain intermediate 1; the ratio of phosphorus oxychloride, pentaerythritol and anhydrous acetonitrile was 32.1g:13.6g:100mL;

[0020] Phosphorus oxychloride and pentaerythritol react, and the molar ratio of the two is controlled to be close to 2:1, and the phosphorus oxychloride is excessive to obtain intermediate 1; the specific reaction process is as follows:

[0021]

[0022] S2. In a three-necked flask equipped with a stirring device, the intermediate 1, potassium carbonate and N,N-dimethylformamide (DMF) were vigorously stirred and mixed, and then 9-decenol was added dropwise. After the addition was completed, the reaction temperature was controlled to 70°C, and the reaction was kept warm for 6 hours. After the reaction was completed, it was filtered, and part of the solvent was distilled off under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 5:2), and the eluent was removed by rotary evaporation to obtain intermediate 2; the ratio of the amount of intermediate 1, potassium carbonate, N,N-dimethylformamide, and 9-decenol was 30.4g:6.3g:150mL:15.6g;

[0023] Intermediate 1 undergoes a nucleophilic substitution reaction with 9-decenol, and the molar ratio of the two is controlled to be close to 1:1, and intermediate 1 is slightly excessive, and potassium carbonate removes the hydrogen chloride generated by the reaction to obtain intermediate 2; the specific reaction process is as follows:

[0024]

[0025] S3. At room temperature, in a three-necked flask equipped with a stirring device, 4,4'-diaminodiphenyl sulfone, intermediate 2, toluene and triethylamine were mixed and stirred evenly under nitrogen protection, the reaction temperature was controlled to 75°C, and the reaction was stirred for 8 hours. After the reaction was completed, triethylamine hydrochloride was filtered out, and part of the solvent was removed by reduced pressure distillation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 5:1), the eluent was removed by rotary evaporation, and vacuum drying was performed to obtain a multi-effect flame retardant; the ratio of the amount of 4,4'-diaminodiphenyl sulfone, intermediate 2, toluene, and triethylamine was 25.2g:83.2g:200mL:15mL;

[0026] 4,4'-Diaminodiphenyl sulfone and intermediate 2 undergo a nucleophilic substitution reaction, and the molar ratio of the two is controlled to be close to 1:2 and 4,4'-diaminodiphenyl sulfone is slightly excessive, and triethylamine removes the hydrogen chloride generated by the reaction to obtain a multi-effect flame retardant; the specific reaction process is as follows:

[0027]

[0028] The prepared multi-effect flame retardant is centered on diphenyl sulfone, which has good high temperature resistance and thermal oxidation resistance, and desulfurizes when heated to produce SO2, sulfurous acid and water, which can promote the Fries rearrangement reaction of the silicone rubber matrix, accelerate the carbonization of the matrix, and effectively enhance the flame retardant and smoke suppression properties of the matrix; in addition, diphenyl sulfone contains a benzene ring structure, and introducing the benzene ring into the silicone rubber matrix can significantly enhance the low temperature resistance of the matrix; not only that, the multi-effect flame retardant also contains spirocyclic phosphate, long carbon chain and carbon-carbon double bond structure, among which spirocyclic phosphate has good flame retardant effect and has a stable six-membered heterocyclic structure. The tetraol skeleton will form a char protective layer to inhibit further combustion of the matrix, and is connected with the N element to form a PN flame retardant component, which has the synergistic flame retardant effect of phosphorus and nitrogen flame retardants, further enhancing the flame retardant properties of the matrix; in addition, the introduced long carbon chain is a methylene chain segment, which is a flexible chain segment, which can not only improve the mechanical strength of the matrix, but also be interspersed in the polymer chain of the matrix, more tightly connected to the matrix, and improve the stability of the multi-effect flame retardant; finally, the introduced carbon-carbon double bond can cross-link with the matrix, which can significantly enhance the migration and exudation resistance of the multi-effect flame retardant, so that the multi-effect flame retardant can perform its performance stably for a long time.

[0029] Beneficial effects of the present invention:

[0030] 1. The protective sheath material prepared by the present invention is based on methyl vinyl silicone rubber and added with ethylene-methyl acrylate copolymer, which gives the cable excellent high and low temperature resistance and oil resistance;

[0031] 2. The antioxidant is a compound of a phosphite antioxidant and a phenolic antioxidant, which can play a synergistic role and greatly enhance the antioxidant performance of the protective cover material;

[0032] 3. The radiation vulcanization method is faster, more energy-efficient and less environmentally polluting than traditional chemical vulcanization. In addition, the cross-linking bond during radiation vulcanization is a CC bond, which has better antioxidant properties than the CS bond produced by chemical vulcanization.

[0033] 4. The prepared multi-effect flame retardant molecules contain various functional groups, which can significantly enhance the flame retardant and smoke suppression properties of the cable and a certain degree of mechanical strength, and can also improve the low temperature resistance of the cable, and the performance is long-term and stable;

[0034] Therefore, the cable prepared by the present invention has excellent high and low temperature resistance, oil resistance and oxidation resistance, and has stable and efficient flame retardant and smoke suppression properties and a certain degree of mechanical strength, and has important application value in the field of cable technology. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] Preparation of multi-effect flame retardant:

[0038] S1. At room temperature and under nitrogen protection, 32.1 g of phosphorus oxychloride, 13.6 g of pentaerythritol and 100 mL of anhydrous acetonitrile were mixed evenly in a three-necked flask equipped with a stirring reflux device, the reaction temperature was controlled to 68°C, the reaction was stirred for 6 hours, and then the temperature was raised to 110°C, and the reaction was refluxed until no hydrogen chloride gas was generated. After the reaction was completed, the mixture was cooled to room temperature, the solvent was distilled off under reduced pressure, and the mixture was washed with dichloromethane 3-4 times and dried in vacuo to obtain intermediate 1;

[0039] S2, in a three-necked flask equipped with a stirring device, 30.4g of intermediate 1, 6.3g of potassium carbonate and 150mL of N,N-dimethylformamide were vigorously stirred and mixed, and 15.6g of 9-decenol was added dropwise. After the addition was completed, the reaction temperature was controlled to 70°C, and the reaction was kept warm for 6h. After the reaction was completed, it was filtered, and part of the solvent was distilled off under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 5:2), and the eluent was removed by rotary evaporation to obtain intermediate 2;

[0040] S3. At room temperature and under nitrogen protection, 25.2 g of 4,4'-diaminodiphenyl sulfone, 83.2 g of intermediate 2, 200 mL of toluene and 15 mL of triethylamine were mixed and stirred evenly in a three-necked flask equipped with a stirring device. The reaction temperature was controlled to 75°C and the reaction was stirred for 8 hours. After the reaction was completed, triethylamine hydrochloride was filtered out, and part of the solvent was removed by vacuum distillation. Then, it was purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 5:1), the eluent was removed by rotary evaporation, and vacuum drying was performed to obtain a multi-effect flame retardant.

[0041] Example 2

[0042] Preparation of multi-effect flame retardant:

[0043] S1. At room temperature and under nitrogen protection, 64.2 g of phosphorus oxychloride, 27.2 g of pentaerythritol and 200 mL of anhydrous acetonitrile were mixed evenly in a three-necked flask equipped with a stirring reflux device, the reaction temperature was controlled to 68°C, the reaction was stirred for 6 hours, and then the temperature was raised to 110°C, and the reaction was refluxed until no hydrogen chloride gas was generated. After the reaction was completed, the mixture was cooled to room temperature, the solvent was distilled off under reduced pressure, the mixture was washed with dichloromethane 3 times, and vacuum dried to obtain intermediate 1;

[0044] S2, in a three-necked flask equipped with a stirring device, 60.8g of intermediate 1, 12.6g of potassium carbonate and 300mL of N, N-dimethylformamide were vigorously stirred and mixed, and 31.2g of 9-decenol was added dropwise. After the addition was completed, the reaction temperature was controlled to 70°C, and the reaction was kept warm for 6h. After the reaction was completed, it was filtered, and part of the solvent was distilled off under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 5:2), and the eluent was removed by rotary evaporation to obtain intermediate 2;

[0045] S3. At room temperature and under nitrogen protection, 50.4 g of 4,4'-diaminodiphenyl sulfone, 166.4 g of intermediate 2, 400 mL of toluene and 30 mL of triethylamine were mixed and stirred evenly in a three-necked flask equipped with a stirring device. The reaction temperature was controlled to 75°C and the reaction was stirred for 8 hours. After the reaction was completed, triethylamine hydrochloride was filtered out, and part of the solvent was removed by vacuum distillation. Then, it was purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 5:1), the eluent was removed by rotary evaporation, and vacuum drying was performed to obtain a multi-effect flame retardant.

[0046] Example 3

[0047] Preparation of protective cover materials:

[0048] 60g of methyl vinyl silicone rubber and 15g of ethylene-methyl acrylate copolymer were added to an internal mixer at a mixing temperature of 110°C. After mixing for 2min, 5g of the multi-effect flame retardant prepared in Example 1 and 4g of epoxy soybean oil were added. After mixing for 2min, 6g of antioxidant (compounded with 2g of antioxidant 168 and 4g of antioxidant 1010) was added. The mixture was heat treated at 150°C for 5min, and the rubber was discharged to obtain a rubber compound. After the rubber compound was thinly passed through a wrapping roller on an open mixer, 0.1g of triallyl cyanurate and 2g of sulfur (vulcanizing agent) were added and the mixture was mixed. After the mixing was completed, a rubber compound was obtained. The rubber compound was irradiated and vulcanized to obtain a protective cover material.

[0049] Example 4

[0050] Preparation of protective cover materials:

[0051] 70g of methyl vinyl silicone rubber and 20g of ethylene-methyl acrylate copolymer are added to an internal mixer at a mixing temperature of 115°C. After mixing for 3 minutes, 10g of the multi-effect flame retardant prepared in Example 2 and 5g of paraffin are added. After mixing for 2 minutes, 9g of antioxidant (3g of antioxidant 168 and 6g of antioxidant 1010 are compounded) is added. The mixture is heat treated at 155°C for 5 minutes, and the rubber is discharged to obtain a rubber compound. After the rubber compound is thinly passed through a wrap roller on an open mixer, 0.2g of triallyl isocyanurate and 3g of sulfur (vulcanizing agent) are added and the mixture is mixed. After the mixing is completed, a rubber compound is obtained. The rubber compound is irradiated and vulcanized to obtain a protective cover material.

[0052] Example 5

[0053] Preparation of protective cover materials:

[0054] 80g of methyl vinyl silicone rubber and 25g of ethylene-methyl acrylate copolymer are added to an internal mixer at a mixing temperature of 120°C. After mixing for 3 minutes, 15g of the multi-effect flame retardant prepared in Example 2 and 6g of paraffin are added. After mixing for 2 minutes, 12g of antioxidant (4g of antioxidant 168 and 8g of antioxidant 1010 are compounded) is added. The mixture is heat treated at 160°C for 5 minutes, and the rubber is discharged to obtain a rubber compound. After the rubber compound is thinly passed through a wrap roller on an open mixer, 0.3g of triallyl isocyanurate and 4g of sulfur (vulcanizing agent) are added and the mixture is mixed. After the mixing is completed, a rubber compound is obtained. The rubber compound is irradiated and vulcanized to obtain a protective cover material.

[0055] Example 6

[0056] A mica tape insulation layer was extruded on a pure copper conductor to form a cable. Three cables were stacked and filled with asbestos filling ropes. 80 g of methyl vinyl silicone rubber and 25 g of ethylene-methyl acrylate copolymer were added to an internal mixer at a mixing temperature of 120° C. After mixing for 3 min, 15 g of the multi-effect flame retardant prepared in Example 2 and 6 g of paraffin were added. After mixing for 2 min, 12 g of an antioxidant (4 g of antioxidant 168 and 8 g of antioxidant 1010 were compounded) was added. The cable was heat treated at 160° C. for 5 min, and the rubber was discharged to obtain a rubber compound. After the rubber compound was thinly passed through a wrapping roller on an open mixer, 0.3 g of triallyl isocyanurate and 4 g of sulfur (vulcanizing agent) were added and the mixing was completed. The mixed rubber was coated on the surface of the cable through an extruder, and irradiated and vulcanized to obtain a low-temperature resistant silicone rubber cable for an oil drilling platform.

[0057] Comparative Example 1

[0058] The multi-effect flame retardant in Example 5 was replaced by a commercially available phosphorus-based flame retardant of equal quality, and the remaining steps were the same as those in Example 5 to prepare a protective cover material.

[0059] Comparative Example 2

[0060] Use commercially available low-temperature resistant silicone rubber.

[0061] The protective cover materials of Examples 3-5 and Comparative Examples 1-2 were made into corresponding shapes to be tested according to different test standards, and the following performance tests were performed:

[0062] The limiting oxygen index is determined using the national standard GB / T 10707-2008 "Determination of combustion properties of rubber";

[0063] The smoke density is measured using the national standard GB / T 8627-2007;

[0064] The tensile strength is determined using the national standard GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber";

[0065] The national standard GB / T 3512-2001 "Hot air accelerated aging and heat resistance test for vulcanized rubber or thermoplastic rubber" is used to measure the tensile strength after hot air aging;

[0066] Place the sample in a -70°C environment and measure the tensile strength after 72 hours;

[0067] Immerse the sample in IRM902 # Oil (mineral oil), and placed in a thermostat set at 100°C for 72 hours to measure the tensile strength after immersion;

[0068] The national standard GB / T 3511-2001 "Direct natural climate aging test method for vulcanized rubber or thermoplastic rubber" is used to measure the limiting oxygen index of the sample after 6 months of outdoor aging;

[0069] The measured results are shown in the following table:

[0070]

[0071]

[0072] It can be seen from the above table that the cable sheath material prepared in the embodiment of the present invention has excellent high and low temperature resistance, oil resistance and antioxidant properties, and has stable and efficient flame retardant and smoke suppression properties and a certain degree of mechanical strength, and has important application value in the field of cable technology.

[0073] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0074] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. Low temperature resistant silicone rubber cable for oil drilling platform, consisting of conductor, insulation layer and protective sheath arranged in sequence from inside to outside, characterized in that: The material of the protective cover includes the following raw materials in parts by weight: 60-80 parts of methyl vinyl silicone rubber, 15-25 parts of ethylene-methyl acrylate copolymer, 5-15 parts of multi-effect flame retardant, 4-6 parts of lubricant, 6-12 parts of antioxidant, 0.1-0.3 parts of cross-linking sensitizer, and 2-4 parts of sulfur; Wherein, the multi-effect flame retardant is prepared by the following steps: S1. At room temperature and under nitrogen protection, phosphorus oxychloride, pentaerythritol and anhydrous acetonitrile were mixed evenly, stirred and reacted at 68°C for 6 hours, heated to 110°C, refluxed and reacted until no hydrogen chloride gas was generated. After the reaction was completed, the mixture was cooled, distilled under reduced pressure, washed and dried to obtain intermediate 1. S2, after mixing the intermediate 1, potassium carbonate and N,N-dimethylformamide, 9-decenol was added dropwise, after the addition was completed, the mixture was reacted at 70° C. for 6 h, after the reaction was completed, the mixture was filtered, distilled under reduced pressure, purified by column chromatography, and rotary evaporated to obtain the intermediate 2; S3. At room temperature, 4,4'-diaminodiphenyl sulfone, intermediate 2, toluene and triethylamine were mixed and stirred evenly under nitrogen protection, and reacted at 75°C for 8 hours. After the reaction was completed, the mixture was filtered, distilled under reduced pressure, purified by column chromatography, rotary evaporated, and vacuum dried to obtain a multi-effect flame retardant.

2. The low temperature resistant silicone rubber cable for oil drilling platform according to claim 1, characterized in that: In step S1, the ratio of phosphorus oxychloride, pentaerythritol and anhydrous acetonitrile is 32.1 g:13.6 g:100 mL.

3. The low temperature resistant silicone rubber cable for oil drilling platform according to claim 1, characterized in that: In step S2, the ratio of the amount of intermediate 1, potassium carbonate, N,N-dimethylformyl and 9-decenol used is 30.4 g:6.3 g:150 mL:15.6 g.

4. The low temperature resistant silicone rubber cable for oil drilling platform according to claim 1, characterized in that: In step S3, the ratio of 4,4'-diaminodiphenyl sulfone, intermediate 2, toluene and triethylamine is 25.2 g:83.2 g:200 mL:15 mL.

5. The low temperature resistant silicone rubber cable for oil drilling platform according to claim 1, characterized in that: The antioxidant is prepared by compounding a phosphite antioxidant and a phenolic antioxidant in a mass ratio of 1:

2.

6. The low temperature resistant silicone rubber cable for oil drilling platform according to claim 1, characterized in that: The lubricant is one of epoxidized soybean oil and paraffin.

7. The low temperature resistant silicone rubber cable for oil drilling platform according to claim 1, characterized in that: The cross-linking sensitizer is one of triallyl cyanurate and triallyl isocyanurate.

8. The method for preparing a low temperature resistant silicone rubber cable for an oil drilling platform according to claim 1, characterized in that: The following steps are involved: An insulating layer is extruded on the conductor to form a cable. After three cables are stacked, they are filled with fillers, and then a protective sheath material is extruded and coated on the surface of the cable. After irradiation cross-linking, a low-temperature resistant silicone rubber cable for oil drilling platforms is obtained.

Citation Information

Cited By

  • Halogen-free flame-retardant engineering plastic and preparation method thereof

    CN120988441A