Positive electrode active material and preparation method thereof, battery and electric device

By controlling the Mn3+ content and introducing spinel phase and lithosaline phase, combining hydrothermal reaction and sintering technology, stable nickel lithium manganate positive electrode active material is prepared, which solves the high specific capacity and circulation of spinel nickel lithium manganate material The problem of taking into account both performance has achieved high energy density and good cycle performance.

CN119069688APending Publication Date: 2024-12-03BEIJING EASPRING MATERIAL TECH CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411204356.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing spinel lithium manganate materials are difficult to take into account between high specific capacity and good cycle performance, especially under high voltage conditions, which leads to insufficient energy density and cycle performance of the battery.

Method used

By controlling the content of Mn3+ in the range of 2.5% to 8.5%, and introducing spinel phase and lithosaline phase into the nickel-manganate lithium material, combined with hydrothermal reaction and sintering process, a positive electrode active material with a composite phase structure was prepared. Ensure the stability of the body phase and surface structure of the material.

Benefits of technology

It achieves high energy density and good cycling performance, improving the overall performance of the battery, especially the stability and capacity performance under high voltage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069688A_ABST
    Figure CN119069688A_ABST
Patent Text Reader

Abstract

The invention relates to the field of batteries, in particular to a lithium nickel manganese oxide type positive electrode active material and a preparation method thereof, a battery and a power utilization device, in the lithium nickel manganese oxide type positive electrode active material, the molar percentage content of Mn < 3 + > in all transition metal elements is n, the mass percentage content of Mn < 3 + > is m, and n and m meet the condition that n is larger than 2.5% and smaller than 8.5%; and / or 1.0% < m < 5.1%. The lithium nickel manganese oxide type positive electrode active material can improve the structural stability while having relatively high capacity, and the lithium ion battery applying the lithium nickel manganese oxide type positive electrode active material has the characteristics of high energy density, good cycle performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to positive electrode active materials and preparation methods thereof, batteries and electrical devices. Background Art

[0002] In recent years, the huge demand for energy has stimulated the development of high-energy-density lithium-ion battery materials, especially in the field of electric vehicles. Currently, commercial lithium-ion batteries still cannot meet the requirements of electric vehicles for low cost and high energy density. As the most expensive part of lithium-ion batteries, the performance of positive electrode materials plays a decisive role in lithium-ion batteries.

[0003] Under the development trend of high voltage, spinel nickel manganese oxide lithium materials have become one of the mainstream directions of positive electrode development. The specific capacity of spinel nickel manganese oxide lithium materials can reach more than 120mAh / g, and the energy density can reach more than 600Wh / kg, taking into account the core advantages of high voltage, low cost, and high safety. However, there are still some challenges: due to the high platform voltage and the high required working voltage (above 4.7V), higher requirements are placed on the material's bulk structure stability and surface structure stability, and it is impossible to achieve high specific capacity while having good cycle performance.

[0004] Therefore, the current technology related to spinel nickel lithium manganese oxide materials still needs to be improved. Summary of the invention

[0005] The present application aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the present application proposes a nickel manganese oxide lithium positive electrode active material with high capacity and good cycle performance, a preparation method thereof, a battery and an electrical device.

[0006] In a first aspect of the present application, a lithium nickel manganese oxide positive electrode active material is provided. According to an embodiment of the present application, in the positive electrode active material, Mn 3+ The molar percentage of all transition metal elements is n, Mn 3+ The mass percentage content is m, and n and m satisfy: 2.5%<n<8.5%; and / or 1.0%<m<5.1%.

[0007] According to an embodiment of the present application, 3%≤n≤7.5%; and / or 1.5%≤m≤4.6%.

[0008] In the positive electrode active material of the present embodiment, an appropriate amount of Mn 3+ The presence of Mn helps improve rate performance, but 3+ Transition metal dissolution will occur in the electrolyte, controlling Mn 3+When the content is within the above range, the lithium nickel manganese oxide positive electrode active material has good rate performance, and will not cause structural instability due to the Jan-Taylor effect, and the cycle performance can also be significantly improved.

[0009] According to an embodiment of the present application, the nickel manganese oxide lithium positive electrode active material includes a spinel phase and a rock salt phase, and the mass ratio I of the rock salt phase to the spinel phase satisfies 0.005≤I≤0.15. The nickel manganese oxide lithium positive electrode active material has a composite phase structure, including a spinel structure and a rock salt phase structure, the spinel phase can contribute to the capacity, the rock salt phase can withstand high voltage, and the mass ratio of the rock salt phase to the spinel phase is controlled within the above range, while having a higher capacity, the structural stability can be improved, and the lithium ion battery using the nickel manganese oxide lithium positive electrode active material has the advantages of high energy density and good cycle performance.

[0010] According to an embodiment of the present application, 0.02≤I≤0.09. Thus, the capacity and structural stability of the lithium manganate positive electrode active material can be further improved.

[0011] According to an embodiment of the present application, the rock salt phase includes the following compounds:

[0012] Li p Ni q Mn r O

[0013] Among them, 0≤p<1, 0≤q<1, 0≤r<1, and p, q, and r are not 0 at the same time.

[0014] According to an embodiment of the present application, the spinel phase includes the following compounds:

[0015] Li 1+a Ni x Mn y M b X c O 4-c

[0016] Among them, -0.5≤a≤0.4, 0.4<x<0.6, 1.4<y<1.6, 0≤b≤0.5, x+y+b=2, 0<c≤0.5;

[0017] M includes at least one of Mg, Ca, Sr, Ba, Al, Ga, Si, Ge, Y, Ti, Zr, V, Nb, Ta, Cr, W, Fe, Ce, La and Mo;

[0018] X includes F - , Cl - Br - ,I - 、SO4 2- , BO33- PO4 3- At least one of .

[0019] According to some specific embodiments of the present application, 0<b≤0.5.

[0020] The above compound has better bulk structure stability and surface structure stability, which is beneficial to improving the capacity and cycle performance of lithium-ion batteries using the positive electrode active material.

[0021] The second aspect of the present application provides a method for preparing the positive electrode active material described above. According to an embodiment of the present application, the method includes: mixing a mixed salt solution containing nickel and manganese, an alkaline solution and a complexing agent solution for hydrothermal reaction to obtain a nickel manganese hydroxide precursor; mixing the precursor, a lithium salt and an optional compound containing a doping element, and sintering the obtained mixture in an oxygen-containing atmosphere to obtain the positive electrode active material; wherein the sintering includes programmed heating and heat preservation and programmed cooling and heat preservation. This method can quickly and efficiently prepare positive electrode active materials with good bulk structural stability and surface stability, and the crystal structure can be controlled by programmed sintering during the preparation process. The process route is simple and has the feasibility of large-scale industrial production.

[0022] According to an embodiment of the present application, the above method satisfies at least one of the following conditions: the total concentration of salt in the mixed salt solution is 1 mol / L to 3 mol / L; the concentration of alkali in the alkaline solution is 4 mol / L to 10 mol / L; the concentration of the complexing agent in the complexing agent solution is 2 mol / L to 10 mol / L; the molar ratio of nickel to manganese in the mixed salt solution is 0.4 to 0.6:1.4 to 1.6; the molar ratio of the lithium element in the lithium salt to the sum of the metal elements in the nickel manganese hydroxide precursor is 0.48 to 0.60:1.

[0023] According to an embodiment of the present application, the pH of the hydrothermal reaction is 10-13, and the temperature is 50°C-70°C.

[0024] According to an embodiment of the present application, the programmed heating and heat preservation comprises: heating from room temperature to T2 at a heating rate of 1.0 to 6.0°C / min and maintaining t2; or the programmed heating and heat preservation comprises: heating from room temperature to T1 at a heating rate of 1.0 to 6.0°C / min and maintaining t1; then heating from T1 to T2 at a heating rate of 1.0 to 6.0°C / min and maintaining t2; wherein, 450°C≤T1≤650°C, 900°C≤T2≤1100°C, 1h≤t1≤5h, 4h≤t2≤24h. According to an embodiment of the present application, the programmed cooling and heat preservation comprises cooling from T2 to T3 at a cooling rate of 1.0 to 6.0°C / min and maintaining t3; naturally cooling to room temperature; wherein, 900°C≤T2≤1100°C, 400°C≤T3≤800°C, 1h≤t3≤14h.

[0025] The third aspect of the present application provides a battery. According to an embodiment of the present application, the battery includes the positive electrode active material described above. The battery has both high energy density and good cycle performance.

[0026] According to the embodiment of the present application, the discharge specific capacity of the above-mentioned battery during the discharge process of 4.90V to 3.5V is R, and the discharge specific capacity during the discharge process of 4.4V to 3.5V is R Mn ; Mn capacity contribution rate S = R Mn / R, satisfies: 5%<S<21%.

[0027] According to an embodiment of the present application, 6%≤S≤15%.

[0028] In a fourth aspect of the present application, an electric device is provided. According to an embodiment of the present application, the electric device includes the battery described above. The electric device has all the features and advantages of the battery described above, which will not be described one by one here. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a SEM photograph of the positive electrode active material prepared in Example 1 of the present application.

[0030] Figure 2 This is the XRD spectrum of the positive electrode active material prepared in Example 1 of the present application.

[0031] Figure 3 It is the charge and discharge curve of the battery assembled with the positive electrode active materials prepared in Example 1 and Comparative Examples 1 and 2 of the present application.

[0032] Figure 4 It is the cycle performance curve of the battery assembled with the positive electrode active materials prepared in Example 1 and Comparative Examples 1 and 2 of the present application. DETAILED DESCRIPTION

[0033] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0034] In a first aspect of the present application, a lithium nickel manganese oxide positive electrode active material is provided. According to an embodiment of the present application, in the positive electrode active material, Mn 3+ The molar percentage of all transition metal elements is n, Mn 3+ The mass percentage of is m, and n and m satisfy: 2.5%<n<8.5%; and / or 1.0%<m<5.1%. In some specific embodiments, 3%≤n≤7.5%; and / or 1.5%≤m≤4.6%. Specifically, n can be 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, etc. Specifically, m can be 1.0%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 4.6%, 5%, 5.1%, etc.

[0035] In the positive electrode active material of the present embodiment, an appropriate amount of Mn 3+ The presence of Mn helps improve rate performance, but 3+ It will react with the electrolyte to dissolve transition metals, and control the Mn 3+ When the content is within the above range, the lithium nickel manganese oxide positive electrode active material has good rate performance, and will not cause structural instability due to the Jan-Taylor effect, and the cycle performance can also be significantly improved.

[0036] For lithium nickel manganese oxide positive electrode active materials, the valence states of nickel and manganese are +2 and +4 respectively in theory, and the contribution of Ni 2+ However, since the structure of lithium nickel manganese oxide can be considered to be inherited from lithium manganese oxide, Mn is inevitably present in its crystal structure under high temperature synthesis conditions. 3+ , due to Mn 3+ The ionic radius is larger than that of Mn 4+ , a certain content of Mn 3+ It can improve the rate performance, but too high a content will lead to structural instability due to the Jan-Taylor effect. 3+ The content within a specific range is beneficial to improving the capacity and structural stability of the positive electrode active material.

[0037] Understandably, Mn 3+ The content will be reflected in the capacity share of a specific voltage range in the charge and discharge curve of the battery using the positive electrode active material. Therefore, the Mn 3+ The capacity contribution rate of Mn3+ In this article, Mn 3+ The capacity contribution rate can be obtained as follows: After the nickel manganese oxide lithium positive electrode active material is made into a button half-cell, the specific capacity R in the voltage range of 4.95V to 3.5V is recorded. This capacity is contributed by the electrochemical reaction between Ni and Mn; the specific capacity corresponding to the voltage range of 4.3V to 3.5V is calculated. The capacity in this voltage range is contributed by Mn 3+ / Mn 4+ The transformation between them is obtained, denoted as R Mn , then the Mn capacity contribution rate is S = R Mn / R; In fact, the discharge capacity corresponding to the 4V voltage platform (the platform within the voltage range of 4.3V to 3.5V) is due to the Mn 3+ / Mn 4+ The electrochemical behavior between them is obtained, and the remaining Mn is stable Mn 4+ , based on the detected S, based on the above analysis, Mn 3+ The molar percentage of all transition metal elements is n = S / 2, and the corresponding mass percentage is m = n × 2 × M (Mn 3+ ) / M(Li 1+a Ni x Mn y M b X c O 4-c ), where M(Mn 3 + ) represents the relative atomic mass of Mn, M(Li 1+a Ni x Mn y M b X c O 4-c ) represents the relative molecular mass of the corresponding lithium nickel manganese oxide.

[0038] In this article, lithium nickel manganese oxide positive electrode active materials should be understood in a broad sense, including both unmodified intrinsic lithium nickel manganese oxide and modified lithium nickel manganese oxide obtained by doping and / or coating intrinsic lithium nickel manganese oxide.

[0039] According to an embodiment of the present application, the lithium nickel manganese oxide positive electrode active material includes a spinel phase and a rock salt phase, and the mass ratio I of the rock salt phase and the spinel phase satisfies 0.005≤I≤0.15. In some specific embodiments, 0.02≤I≤0.09. Specifically, I can be 0.005, 0.008, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, etc.

[0040] The nickel manganese oxide lithium positive electrode active material has a composite phase structure, including a spinel phase structure and a rock salt phase structure. The spinel phase can contribute to capacity, and the rock salt phase can withstand high voltage. Controlling the mass ratio of the rock salt phase and the spinel phase within the above range can improve the structural stability while having a higher capacity. If the rock salt phase ratio is too high, it will affect the overall capacity. If the rock salt phase ratio is too low, the high-voltage resistance of the positive electrode active material will be reduced. Lithium-ion batteries using nickel manganese oxide lithium positive electrode active materials with a mass ratio of the rock salt phase and the spinel phase within the above range have the characteristics of high energy density and good cycle performance.

[0041] It can be understood that the ratio of spinel phase and rock salt phase in lithium nickel manganese oxide positive electrode active materials is related to the type of doping elements, the ratio of doping elements, preparation process parameters (such as sintering process and parameters), etc., and the above parameters can be adjusted to obtain lithium nickel manganese oxide positive electrode active materials with a mass ratio of rock salt phase and spinel phase within the above range.

[0042] In this paper, the ratio of the spinel phase to the rock salt phase can be obtained by powder XRD testing, and the testing method can be: take the lithium nickel manganese oxide positive electrode active material for powder XRD characterization, use CuKα as the ray source, and make the measurement range of the diffraction angle 2θ be greater than 10° and less than 80°. The diffraction data obtained by powder X-ray diffraction measurement is used for Rietveld refinement using analysis software; the data is imported for peak position processing and the phase is determined in the database (ICDD-PDF5+), and the crystal structure parameters and the mass ratio of the phase can be obtained by refinement.

[0043] According to an embodiment of the present application, the rock salt phase includes the following compounds:

[0044] Li p Ni q Mn r O

[0045] Among them, 0≤p<1, 0≤q<1, 0≤r<1, and p, q, and r are not 0 at the same time.

[0046] In some specific embodiments, p can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99, etc.; q can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99, etc.; r can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99, etc.

[0047] The rock salt phase having the above chemical formula is beneficial to improving the bulk structural stability and surface structural stability of the positive electrode active material, thereby improving the cycle performance.

[0048] According to an embodiment of the present application, the spinel phase includes the following compounds:

[0049] Li 1+a Ni x Mn y M b X c O 4-c

[0050] Among them, -0.5≤a≤0.4, 0.4<x<0.6, 1.4<y<1.6, 0≤b≤0.5, x+y+b=2, 0<c≤0.5;

[0051] M includes at least one of Mg, Ca, Sr, Ba, Al, Ga, Si, Ge, Y, Ti, Zr, V, Nb, Ta, Cr, W, Fe, Ce, La and Mo;

[0052] X includes F - , Cl - Br - ,I - 、SO4 2- , BO3 3- PO4 3- At least one of .

[0053] In some specific embodiments, a can be -0.5, -0.4, -0.3, -0.2, -0.1, 0, 0.1, 0.2, 0.3, 0.4, etc.; b can be greater than 0 and less than or equal to 0.5, and can be 0.1, 0.2, 0.3, 0.4, 0.5, etc.; c can be 0.1, 0.2, 0.3, 0.4, 0.5, etc.; x can be 0.41, 0.45, 0.5, 0.55, 0.59, etc.; y can be 1.41, 1.45, 1.5, 1.55, 1.59, etc.

[0054] The positive electrode active material having the above chemical formula uses metal elements as cations and adds non-metallic anions at the same time. The metal element cations can enter the spinel lattice of lithium nickel manganese oxide to stabilize the structural skeleton. At the same time, some manganese atoms on the surface of the material are replaced by metal elements, and the strong metal-oxygen bond can also stabilize the surface. In addition, the added anions can inhibit defects such as oxygen vacancies on the surface of the material, and the strong anion-metal bond interaction can further stabilize the lattice. The introduction of anions can also reduce the structural fragmentation caused by the electrochemical reaction of oxygen on the surface of the material under high voltage to a certain extent. Therefore, the stability of lithium nickel manganese oxide positive electrode active materials can be effectively improved, which is beneficial to improving the capacity and cycle performance of lithium ion batteries using the positive electrode active materials.

[0055] The second aspect of the present application provides a method for preparing the positive electrode active material described above. According to an embodiment of the present application, the method includes: mixing a mixed salt solution containing nickel and manganese, an alkaline solution and a complexing agent solution to perform a hydrothermal reaction to obtain a nickel manganese hydroxide precursor; mixing the precursor, a lithium salt and an optional compound containing a doping element, and sintering the resulting mixture in an oxygen-containing atmosphere to obtain the positive electrode active material; wherein the sintering includes programmed heating and heat preservation and programmed cooling and heat preservation. This method can quickly and efficiently prepare positive electrode active materials with good bulk structure stability and surface structure stability, and the crystal structure can be controlled by programmed sintering during the preparation process. The process route is simple and has the feasibility of large-scale industrial production.

[0056] According to an embodiment of the present application, a mixed salt solution containing nickel and manganese can be obtained by mixing a nickel salt, a manganese salt and a solvent. The nickel salts that can be used include but are not limited to nickel sulfate, nickel nitrate, nickel chloride, etc., the manganese salts that can be used include but are not limited to manganese sulfate, manganese nitrate, manganese chloride, etc., and the solvents that can be used include but are not limited to water.

[0057] According to an embodiment of the present application, the total concentration of salt in the mixed salt solution may be 1 mol / L to 3 mol / L, such as 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, etc. This concentration range is conducive to sufficient reaction and has high reaction efficiency.

[0058] According to an embodiment of the present application, the molar ratio of nickel to manganese in the mixed salt solution is 0.4-0.6:1.4-1.6. Specifically, the molar ratio of nickel to manganese can be 0.4:1.4, 0.4:1.5, 0.4:1.6, 0.5:1.4, 0.5:1.5, 0.5:1.6, 0.6:1.4, 0.6:1.5, 0.6:1.6, etc. Within this ratio range, it is beneficial to obtain a positive electrode active material with better performance.

[0059] According to an embodiment of the present application, the alkaline solution may be a sodium hydroxide aqueous solution, and the concentration of the alkali in the alkaline solution may be 4 mol / L to 10 mol / L, specifically 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, etc. Thus, the reaction is sufficient and has a high reaction efficiency.

[0060] According to the embodiments of the present application, the complexing agent may be aqueous ammonia, specifically aqueous ammonia with a concentration of 2 mol / L to 10 mol / L (such as 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, etc.), thereby facilitating a sufficient reaction and having a higher reaction efficiency.

[0061] According to the embodiments of the present application, there is no particular restriction on mixing the mixed salt solution, alkaline solution and complexing agent solution containing nickel and manganese. The mixed salt solution, alkaline solution and complexing agent solution can be mixed in advance and then added to the reaction vessel, or the mixed salt solution, alkaline solution and complexing agent solution can be directly added to the reaction vessel together, and the order of adding the mixed salt solution, alkaline solution and complexing agent solution is also not particularly limited, and can be flexibly selected according to actual conditions. In some specific embodiments, the mixed salt solution, alkaline solution and complexing agent solution can be added to the reaction vessel in parallel.

[0062] According to an embodiment of the present application, the pH of the hydrothermal reaction can be 10-13 (specifically 10, 10.5, 11, 11.5, 12, 12.5, 13, etc.), and the temperature is 50°C-70°C (specifically 50°C, 55°C, 60°C, 65°C, 70°C, etc.). The reaction conditions are mild, which is conducive to the formation of nickel manganese hydroxide precursors, has fewer side reactions, and has a higher reaction efficiency.

[0063] It can be understood that the product of the hydrothermal reaction is generally in the form of a slurry containing a nickel manganese hydroxide precursor. Therefore, the prepared nickel manganese hydroxide precursor slurry can be subjected to solid-liquid separation, washing, drying, and screening to obtain a spherical nickel manganese hydroxide precursor.

[0064] According to the embodiment of the present application, the chemical formula of the nickel manganese hydroxide precursor obtained by the hydrothermal reaction is Ni x Mn y (OH)2; wherein x and y are as defined above and are not described in detail here.

[0065] According to the embodiments of the present application, there is no particular limitation on the specific manner of mixing the precursor, the lithium salt and the optional compound containing the doping element, and the mixing method and the order of adding materials can be flexibly adjusted and selected according to actual needs. It is understandable that the compound containing the doping element can be added or not added as needed. Specifically, when the product is an undoped lithium nickel manganese oxide material, the precursor and the lithium salt are directly mixed in this step; when the product is a lithium nickel manganese oxide material with a doping element, the precursor, the lithium salt and the compound containing the doping element are mixed in this step.

[0066] In some embodiments, the above-mentioned compounds containing doping elements are not particularly limited, including but not limited to oxides, hydroxides, etc. Specifically, they can be compounds containing M elements and compounds containing X. M and X are consistent with the above definitions and are not repeated here. Specifically, compounds containing M elements include but are not limited to magnesium oxide, aluminum oxide, titanium oxide, molybdenum oxide, tungsten oxide, yttrium oxide, zirconium oxide, magnesium carbonate, aluminum hydroxide, aluminum hydroxide, etc.; compounds containing X include but are not limited to lithium fluoride, lithium phosphate, lithium chloride, ammonium fluoride, ammonium chloride, diammonium phosphate, etc.

[0067] According to the embodiments of the present application, the specific type of lithium salt is not particularly limited, including but not limited to one or two of lithium carbonate and lithium hydroxide. Thus, it is beneficial to obtain a positive electrode active material with better performance.

[0068] According to an embodiment of the present application, the ratio of the precursor, the lithium salt and the compound containing the doping element can be selected according to the chemical formula of the finally obtained lithium nickel manganese oxide positive electrode active material. In some embodiments, the molar ratio of the lithium element in the lithium salt to the sum of the metal elements in the nickel manganese hydroxide precursor is 0.48 to 0.60:1, specifically 0.48:1, 0.5:1, 0.52:1, 0.55:1, 0.58:1, 0.6:1, etc. This is conducive to obtaining a lithium nickel manganese oxide positive electrode active material with better performance.

[0069] In order to better control Mn 3+ The content of Mn and the ratio of rock salt phase to spinel phase are determined by the program sintering process including program heating and heat preservation and program cooling and heat preservation, which can realize oxygen defect regulation under program cooling and heat preservation conditions, so that Mn 3+ The content of is in a suitable range, and at the same time, different crystal forms in the nickel manganese oxide positive electrode active material can be regulated, and the ratio of the main phase (i.e., spinel phase) to the secondary phase (i.e., rock salt phase) is within the above range, so that the obtained nickel manganese oxide positive electrode active material has both high capacity and good cycle performance.

[0070] According to an embodiment of the present application, the programmed temperature rise and insulation may be one stage of programmed temperature rise and insulation, or two stages of programmed temperature rise and insulation. In some embodiments, the programmed temperature rise and insulation may include heating from room temperature to T2 at a heating rate of 1.0 to 6.0°C / min and maintaining t2. In other embodiments, the programmed temperature rise and insulation may include heating from room temperature to T1 at a heating rate of 1.0°C / min to 6.0°C / min and maintaining t1; then heating from T1 to T2 at a heating rate of 1.0°C / min to 6.0°C / min, and maintaining t2. Wherein, 450°C≤T1≤650°C, 900°C≤T2≤1100°C, 1h≤t1≤5h, 4h≤t2≤24h.

[0071] In some embodiments, the heating rates of programmed temperature rise and insulation can be 1.0°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6.0°C / min, etc.

[0072] In some embodiments, T1 may be 450° C., 500° C., 550° C., 600° C., 650° C., etc.

[0073] In some embodiments, t1 may specifically be 1h, 2h, 3h, 4h, 5h, etc.

[0074] In some embodiments, T2 may specifically be 900° C., 950° C., 1000° C., 1050° C., 1100° C., etc.

[0075] In some embodiments, t2 can specifically be 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, etc.

[0076] According to an embodiment of the present application, the programmed cooling and heat preservation may include cooling from T2 to T3 at a cooling rate of 1.0℃ / min to 6.0℃ / min, and maintaining t3; naturally cooling to room temperature; wherein, 900℃≤T2≤1100℃, 400℃≤T3≤800℃, 1h≤t3≤14h.

[0077] In some embodiments, the cooling rate of programmed cooling and insulation can be 1.0℃ / min, 1.5℃ / min, 2℃ / min, 2.5℃ / min, 3℃ / min, 3.5℃ / min, 4℃ / min, 4.5℃ / min, 5℃ / min, 5.5℃ / min, 6.0℃ / min, etc.

[0078] In some embodiments, T2 may specifically be 900° C., 950° C., 1000° C., 1050° C., 1100° C., etc. It can be understood that the programmed heating and heat preservation and the programmed cooling and heat preservation steps are performed sequentially, that is, in actual operation, the T2 described in the programmed heating and heat preservation step is the same as the T2 described in the programmed cooling and heat preservation step.

[0079] In some embodiments, T3 may be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, etc.

[0080] In some embodiments, t3 may specifically be 1h, 2h, 3h, 4h, etc.

[0081] According to an embodiment of the present application, the above-mentioned sintering is carried out in an oxygen-containing atmosphere, and the oxygen-containing atmosphere can specifically be air, oxygen, or a mixed gas of air and oxygen.

[0082] Under the above sintering process, by finely controlling the cooling rate and holding time of the cooling process, oxygen defect control can be achieved under appropriate cooling conditions, so that Mn 3+ The content is in an optimal range, and at the same time, the different crystal forms in the nickel manganese oxide positive electrode active material can be regulated, and the ratio of the main phase to the secondary phase is in an optimal range, so that the obtained nickel manganese oxide positive electrode active material has both high capacity and good cycle performance.

[0083] According to a specific embodiment of the present application, a method for preparing a lithium nickel manganese oxide positive electrode active material may include:

[0084] (1) Dissolve the nickel and manganese salt solutions to obtain a 1 mol / L to 3 mol / L mixed salt solution; dissolve sodium hydroxide into an alkaline solution with a concentration of 4 mol / L to 10 mol / L; dissolve ammonia water into a complexing agent solution with a concentration of 2 mol / L to 10 mol / L. Add the mixed salt solution, alkaline solution, and complexing agent solution into a reactor in parallel for reaction, keep stirring during the process, control the reaction pH value to 10 to 13, and the reaction temperature to 50°C to 70°C. After solid-liquid separation, washing, drying, and screening of the obtained nickel manganese hydroxide precursor slurry, spherical nickel manganese hydroxide Ni x Mn y (OH)2;

[0085] (2) Ni obtained in step (1) x Mn y (OH)2 is mixed evenly with a lithium salt (one or both of lithium carbonate and lithium hydroxide), a compound containing M, and a compound containing X;

[0086] (3) In an atmosphere of oxygen-containing gas, the mixture obtained in step (2) is heated from room temperature to 450°C to 650°C at a heating rate of 1.0°C / min to 6.0°C / min and maintained for 1h to 5h; the mixture is further heated to 900°C to 1100°C at a heating rate of 1.0°C / min to 6.0°C / min and maintained for 4h to 24h; the mixture is cooled to 400°C to 800°C at a heating rate of 1.0°C / min to 6.0°C / min and maintained for 1h to 4h; and then naturally cooled to room temperature. After cooling, the mixture is crushed and sieved to obtain a lithium manganate positive electrode active material Li 1+ a Ni x Mn y M b X cO 4-c .

[0087] The third aspect of the present application provides a battery. According to an embodiment of the present application, the battery includes the positive electrode active material described above. The battery has both high energy density and good cycle performance.

[0088] It can be understood that there is no particular limitation on the specific type of the battery, including but not limited to lithium-ion batteries, lithium metal batteries, and the like. The specific structure of the battery can refer to conventional technology, and this application has no particular limitation. Taking lithium-ion batteries as an example, they usually include an outer package and an electrode assembly and an electrolyte (including a solid electrolyte, a gel electrolyte, an electrolyte, etc.) contained in the outer package. The electrode assembly usually includes a positive electrode sheet, a negative electrode sheet, and a separator between the positive electrode sheet and the negative electrode sheet, which is prepared by a lamination process or a winding process; wherein the positive electrode sheet may include a positive electrode collector and a positive electrode film layer located on at least one surface of the positive electrode collector, and the positive electrode film layer contains the aforementioned lithium nickel manganese oxide positive electrode active material, a positive electrode binder, and a positive electrode conductive agent; the negative electrode sheet may include a negative electrode collector and a negative electrode film layer located on at least one surface of the negative electrode collector, and the negative electrode film layer contains a negative electrode active material (carbon-based active material, silicon-based active material, etc.), a negative electrode binder, and a negative electrode conductive agent.

[0089] According to the embodiment of the present application, the discharge specific capacity of the above-mentioned battery during the discharge process of 4.95V to 3.5V is R, and the discharge specific capacity during the discharge process of 4.4V to 3.5V is R Mn ; Mn capacity contribution rate S = R Mn / R, 5%<S<21%. In some embodiments, 6%≤S≤15%. Specifically, S can be 5.1%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 0.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 20.9%, etc.

[0090] Specifically, the Mn capacity contribution rate S can reflect the Mn content in the positive electrode active material. 3+ The battery having the above Mn capacity contribution rate S has a suitable Mn 3+ content, so that the battery has good rate performance and cycle performance.

[0091] In a fourth aspect of the present application, an electric device is provided. According to an embodiment of the present application, the electric device includes the battery described above. The electric device has all the features and advantages of the battery described above, which will not be described one by one here.

[0092] According to an embodiment of the present application, the battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0093] The embodiments of the present application are described in detail below.

[0094] Example 1

[0095] (1) Nickel sulfate and manganese sulfate are used as raw materials. Nickel sulfate and manganese sulfate are dissolved in water at a molar ratio of Ni:Mn=25:75 to prepare a 2.0 mol / L uniform mixed salt solution, an alkaline solution with a sodium hydroxide concentration of 6.0 mol / L, and a complexing agent solution with an ammonia concentration of 6 mol / L. Under a nitrogen atmosphere, the mixed salt solution, the alkaline solution, and the complexing agent solution are added to a reactor in parallel for reaction. The stirring speed is set to 150 rpm, the pH is controlled to 12.0, and the reaction temperature is 60°C. After the reaction is completed, the obtained nickel manganese hydroxide slurry is filtered and washed, and the obtained filter cake is dried at 120°C for 6 hours to obtain a spherical nickel cobalt manganese hydroxide precursor Ni 0.25 Mn 0.75 (OH)2.

[0096] (2) The precursor Ni obtained in step (1) 0.25 Mn 0.75 (OH)2, lithium carbonate, aluminum oxide, and lithium fluoride are mixed in a high-speed mixer according to a molar ratio of Li:(Ni+Mn):Al:F=1.04:1.95:0.05:0.05;

[0097] (3) The mixture obtained in step (2) is sintered in an air atmosphere. The sintering process adopted is: heating from room temperature to 500°C at 3°C / min, keeping warm for 5 hours, then continuing to heat to 1000°C at 3°C / min, keeping warm for 12 hours, and then cooling to 700°C at 5°C / min, keeping warm for 5 hours, and finally naturally cooling to room temperature.

[0098] The sintered sample was crushed and sieved to obtain a 5V spinel nickel manganese oxide lithium positive electrode material. The scanning electron microscope (SEM) photo is shown in Figure 1 , XRD spectrum see Figure 2 .

[0099] Example 2

[0100] Steps (1) and (3) are consistent with the preparation steps in Example 1.

[0101] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni 0.25 Mn 0.75 (OH)2, lithium carbonate, aluminum oxide and lithium fluoride are mixed in a high-speed mixer according to the molar ratio of Li:(Ni+Mn):Al:F=1.04:1.98:0.02:0.02.

[0102] Example 3

[0103] Steps (1) and (3) are consistent with the preparation steps in Example 1.

[0104] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni 0.25 Mn 0.75 (OH)2, lithium carbonate, aluminum oxide and lithium fluoride are mixed in a high-speed mixer according to the molar ratio of Li:(Ni+Mn):Al:F=1.04:1.9:0.1:0.05.

[0105] Example 4

[0106] Steps (1) and (3) are consistent with the preparation steps in Example 1.

[0107] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni 0.25 Mn 0.75 (OH)2, lithium carbonate, aluminum oxide and lithium fluoride are mixed in a high-speed mixer according to the molar ratio of Li:(Ni+Mn):Al:F=1.04:1.95:0.05:0.1.

[0108] Example 5

[0109] Step (1) is consistent with the preparation steps in Example 1.

[0110] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni 0.25 Mn 0.75 (OH)2, lithium carbonate, aluminum oxide, molybdenum oxide, and lithium fluoride are mixed in a high-speed mixer according to a molar ratio of Li:(Ni+Mn):Al:Mo:F=1.04:1.9:0.05:0.05:0.05;

[0111] The difference is that the sintering conditions adopted in step (3) are: heating from room temperature to 500°C at 5°C / min, keeping warm for 5 hours, then continuing to heat to 1000°C at 2°C / min, keeping warm for 20 hours, and then cooling to 700°C at 2°C / min, keeping warm for 3 hours, and finally naturally cooling to room temperature.

[0112] Example 6

[0113] Step (1) is consistent with the preparation steps in Example 1.

[0114] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni 0.25 Mn 0.75 (OH)2, lithium carbonate, aluminum oxide, and lithium phosphate are mixed in a high-speed mixer according to a molar ratio of Li:(Ni+Mn):Al:P=1.04:1.95:0.05:0.1;

[0115] The difference also lies in that the sintering conditions adopted in step (3) are: heating from room temperature to 500°C at 5°C / min, keeping warm for 5 hours, then continuing to heat to 950°C at 2°C / min, keeping warm for 12 hours, and then cooling to 700°C at 3°C / min, keeping warm for 6 hours, and finally naturally cooling to room temperature.

[0116] Example 7

[0117] Step (1) is consistent with the preparation steps in Example 1.

[0118] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni 0.25 Mn 0.75 (OH)2, lithium carbonate, titanium oxide and lithium chloride are mixed in a high-speed mixer according to a molar ratio of Li:(Ni+Mn):Ti:Cl=1.04:1.95:0.05:0.1;

[0119] The difference lies in that the sintering conditions adopted in step (3) are: heating from room temperature to 500°C at 5°C / min, keeping warm for 4 hours, then continuing to heat to 1020°C at 5°C / min, keeping warm for 12 hours, and then cooling to 700°C at 2°C / min, keeping warm for 5 hours, and finally naturally cooling to room temperature.

[0120] Example 8

[0121] Step (1) is consistent with the preparation steps in Example 1.

[0122] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni 0.25 Mn 0.75(OH)2, lithium carbonate, titanium oxide and lithium phosphate are mixed in a high-speed mixer according to a molar ratio of Li:(Ni+Mn):Ti:P=1.04:1.95:0.05:0.1;

[0123] The difference is that the sintering conditions adopted in step (3) are: heating from room temperature to 500°C at 4°C / min, keeping warm for 4 hours, then continuing to heat to 1000°C at 3°C / min, keeping warm for 18 hours, and then cooling to 700°C at 5°C / min, keeping warm for 4 hours, and finally naturally cooling to room temperature.

[0124] Example 9

[0125] Step (1) is consistent with the preparation steps in Example 1.

[0126] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni obtained in step (1) is 0.25 Mn 0.75 (OH)2, lithium carbonate and lithium fluoride are mixed in a high-speed mixer according to a molar ratio of Li:(Ni+Mn):F=1.04:2:0.05;

[0127] The difference is that the sintering conditions adopted in step (3) are: heating from room temperature to 500°C at 3°C / min, then continuing to heat to 1000°C at 3°C / min, keeping warm for 12 hours, then cooling to 700°C at 7°C / min, keeping warm for 5 hours, and finally naturally cooling to room temperature.

[0128] Example 10

[0129] Steps (1) and (2) are consistent with the preparation steps of Example 9.

[0130] The difference is that the sintering conditions adopted in step (3) are: heating from room temperature to 500°C at 3°C / min, keeping warm for 3h, then continuing to heat to 1000°C at 3°C / min, keeping warm for 12h, then cooling to 700°C at 5°C / min, keeping warm for 5h, and finally naturally cooling to room temperature.

[0131] Comparative Example 1

[0132] Step (1) is consistent with the preparation steps of Comparative Example 1.

[0133] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni obtained in step (1) is 0.25 Mn 0.75 (OH)2 and lithium carbonate are mixed in a high-speed mixer at a molar ratio of Li:(Ni+Mn)=1.04:2.

[0134] The difference is that the sintering conditions adopted in step (3) are: heating from room temperature to 850°C at 3°C / min, keeping warm for 12h, then cooling to 700°C at 5°C / min, and then naturally cooling to room temperature.

[0135] Comparative Example 2

[0136] Step (1) is consistent with the preparation steps of Comparative Example 1.

[0137] The difference is that the mixing conditions adopted in step (2) are: the precursor Ni obtained in step (1) is 0.25 Mn 0.75 (OH)2, lithium carbonate and aluminum oxide were mixed in a high-speed mixer according to the molar ratio of Li:(Ni+Mn):Al=1.04:1.95:0.05.

[0138] The difference is that the sintering conditions adopted in step (3) are: heating from room temperature to 1000°C at 3°C / min, keeping warm for 12h, then cooling to 700°C at 7°C / min, and then naturally cooling to room temperature.

[0139] Performance Test:

[0140] The button-type half-cell is made from the spinel nickel lithium manganese oxide embodiment or the comparative example positive electrode active material, and the specific steps are as follows:

[0141] ① The positive electrode active material, the conductive agent acetylene black, and the binder PVDF were weighed in a mass ratio of 95:2.5:2.5 and added to a mixer, and then the solvent NMP was added and stirred thoroughly to obtain a positive electrode slurry; ② The positive electrode slurry was evenly coated on the surface of the positive electrode collector aluminum foil, dried at room temperature, and then transferred to an oven at 135°C for drying; ③ The obtained positive electrode sheet was rolled using a roller press; ④ The positive electrode sheet was cut as needed to obtain a positive electrode sheet; ⑤ In an argon-filled glove box with a water content and an oxygen content of less than 5ppm, the positive electrode sheet, the diaphragm, the negative electrode sheet lithium sheet and the electrolyte were assembled into a 2025 button battery and left to stand for 6 hours.

[0142] Capacity and rate performance test: The electrochemical performance test of the obtained 2025 button battery was carried out using Shenzhen Xinweier Battery Testing System: the charge and discharge current density of 0.1C during the test was 12mA / g, the charge and discharge voltage range was controlled to be 3.5V-4.95V, and the button battery was charged and discharged at 0.1C at 25°C to evaluate the initial charge and discharge specific capacity and efficiency; then the discharge specific capacity at different rates was tested. The test results are shown in Table 3. The charge and discharge curves of the batteries composed of the positive electrode active materials in Example 1, Comparative Example 1 and Comparative Example 2 are shown in Table 3. Figure 3 .

[0143] Cyclic performance test: The charge and discharge voltage range was controlled to be 3.5V-4.95V. At a constant temperature of 45°C, the button cell was charged and discharged for 2 cycles at 0.1C, and then charged and discharged for 80 cycles at 1C to evaluate the high temperature capacity retention rate. The test results are shown in Table 3. The cycle performance curves of the batteries composed of the positive electrode active materials in Example 1, Comparative Example 1 and Comparative Example 2 are shown in Table 3. Figure 4 .

[0144] Mn capacity contribution rate: After the nickel manganese oxide lithium positive electrode active material is made into a button half-cell according to the steps described above, the specific capacity R in the voltage range of 4.95V to 3.5V is recorded; the specific capacity corresponding to the voltage range of 4.3V to 3.5V is calculated and recorded as R Mn , then the Mn capacity contribution rate is S = R Mn / R.

[0145] Mn 3+ Mole percentage n and Mn 3+ Mass percentage content m: Mn 3+ The molar percentage of all transition metal elements is n = S / 2, and the corresponding mass percentage is m = n × 2 × M (Mn 3+ ) / M(Li 1+a Ni x Mn y M b X c O 4-c ), where M(Mn 3+ ) represents the relative atomic mass of Mn, M(Li 1+a Ni x Mn y M b X c O 4-c ) represents the relative molecular mass of the corresponding lithium nickel manganese oxide. Based on the Mn capacity contribution rate obtained from the test, Mn can be calculated according to the above formula 3+ Mole percentage n and Mn 3+ Mass percentage m.

[0146] Test of the mass ratio of rock salt phase and spinel phase I: Take lithium nickel manganese oxide positive electrode active material for powder XRD characterization, use CuKα as the radiation source, and make the measurement range of the diffraction angle 2θ be above 10° and below 80°. The diffraction data obtained by powder X-ray diffraction measurement are subjected to Rietveld refinement using analysis software; the data is imported for peak position processing and the phase is determined in the database (ICDD-PDF5+), and the crystal structure parameters and the mass ratio of the phase are obtained by refinement. The XRD spectrum of the positive electrode active material obtained in Example 1 is shown in Figure 2 .

[0147] Table 1: Process parameters for the preparation of positive electrode active materials

[0148]

[0149] Table 2: Test results of positive electrode active materials

[0150]

[0151]

[0152] Table 3: Battery performance test results

[0153]

[0154] It can be seen from the above test data that in the positive electrode active material of the embodiment of the present application, the Mn 3+ Within the appropriate content range, the battery has both high capacity and good cycle performance. When the mass ratio I of the rock salt phase and the spinel phase satisfies 0.005≤I≤0.15, the capacity and cycle performance of the battery are also improved.

[0155] Specifically, it can be seen from Comparative Example 1 that without the use of doping and sintering process to adjust the phase composition, the Mn 3+ The content is very low, and the proportion of rock salt phase is also low. The material cannot produce sufficient stability under high-voltage cycling. As a result, the half-cell capacity of the corresponding material is high, but the rate performance is poor, and the high-temperature cycle performance is particularly poor, which is far lower than that of the embodiment.

[0156] It can be seen from Comparative Example 2 that a certain doping element is added to induce the formation of a rock salt phase, and a certain proportion of a rock salt phase is achieved after single cation doping, so that the cycle performance is improved to a certain extent compared with Comparative Example 1. However, due to the Mn 3+ The content is not adjusted to the appropriate range, too high Mn 3+ On the one hand, the content affects the capacity, and on the other hand, it also causes the material structure to be unstable, affecting high-rate and high-current discharge, making the overall capacity and cycle performance still relatively low.

[0157] It can be seen from Example 9 that the introduction of anion doping can induce the formation of rock salt phase. At the same time, anions can also stabilize the transition metals in the material, improve the stability of the material bulk structure, and thus improve the cycle performance. Similarly, due to the relatively high proportion of rock salt phase, Mn 3+ The content is relatively high. Although the cycle and rate performance are significantly improved compared with comparative example 1, the capacity is relatively low.

[0158] It can be seen from Example 10 that the introduction of anion doping and better adjustment of the sintering process, as the rock salt phase ratio is in an appropriate range, the cycle performance is relatively better, but due to the Mn 3+The content is relatively high, but the capacity is still relatively low.

[0159] In this application, the rock salt phase is induced by combining cationic elements with anionic doping, and the Mn content in the material is regulated by a programmed sintering process. 3+ content, by combining the rock salt phase with Mn 3+ By adjusting the content to the preferred range, it is possible to improve the material capacity while taking into account the high-temperature cycle performance, thereby obtaining a lithium nickel manganese oxide spinel positive electrode material with good performance in capacity, rate, and cycle.

[0160] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0161] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0162] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A lithium nickel manganese oxide positive electrode active material, characterized in that: In the lithium nickel manganese oxide positive electrode active material, Mn 3 + The molar percentage of all transition metal elements is n, Mn 3+ The mass percentage content is m, and n and m satisfy: 2.5%<n<8.5%; and / or 1.0%<m<5.1%.

2. The positive electrode active material according to claim 1, characterized in that 3%≤n≤7.5%; and / or 1.5%≤m≤4.6%.

3. The positive electrode active material according to claim 1, characterized in that It includes a spinel phase and a rock salt phase, and a mass ratio I of the rock salt phase to the spinel phase satisfies 0.005≤I≤0.

15.

4. The positive electrode active material according to claim 3, characterized in that 0.02≤I≤0.09。 5. The positive electrode active material according to claim 3, characterized in that The rock salt phase includes the following compounds: Li p Ni q Mr r O Among them, 0≤p<1, 0≤q<1, 0≤r<1, and p, q, and r are not 0 at the same time.

6. The positive electrode active material according to claim 3, characterized in that The spinel phase includes the following compounds: Li 1+a Ni x Mr y M b X c O 4-c Among them, -0.5≤a≤0.4, 0.4<x<0.6, 1.4<y<1.6, 0≤b≤0.5, x+y+b=2, 0<c≤0.5; M includes at least one of Mg, Ca, Sr, Ba, Al, Ga, Si, Ge, Y, Ti, Zr, V, Nb, Ta, Cr, W, Fe, Ce, La and Mo; X includes F - , Cl - Br - ,I - 、SO4 2- , BO3 3- PO4 3- At least one of .

7. The positive electrode active material according to claim 6, characterized in that 0<b≤0.5。 8. A method for preparing the positive electrode active material according to any one of claims 1 to 7, characterized in that: include: A mixed salt solution containing nickel and manganese, an alkali solution and a complexing agent solution are mixed and subjected to a hydrothermal reaction to obtain a nickel manganese hydroxide precursor; Mixing the precursor, the lithium salt and an optional compound containing a doping element, and sintering the resulting mixture in an oxygen-containing atmosphere to obtain the positive electrode active material; Wherein, the sintering includes programmed heating and heat preservation and programmed cooling and heat preservation.

9. The method according to claim 8, characterized in that: Satisfy at least one of the following conditions: The total concentration of salt in the mixed salt solution is 1 to 3 mol / L; The concentration of the alkali in the alkali solution is 4 to 10 mol / L; The concentration of the complexing agent in the complexing agent solution is 2 to 10 mol / L; The molar ratio of nickel to manganese in the mixed salt solution is 0.4-0.6:1.4-1.6; The molar ratio of the lithium element in the lithium salt to the sum of the metal elements in the nickel manganese hydroxide precursor is 0.48-0.60:

1.

10. The method according to claim 8, characterized in that: The pH of the hydrothermal reaction is 10-13, and the temperature is 50°C-70°C.

11. The method according to claim 8, characterized in that: The programmed temperature increase and temperature preservation include: increasing the temperature from room temperature to T2 at a heating rate of 1.0 to 6.0° C. / min and maintaining t2; or The programmed temperature increase and heat preservation comprises: increasing the temperature from room temperature to T1 at a temperature increase rate of 1.0 to 6.0°C / min and maintaining the temperature at t1; then increasing the temperature from T1 to T2 at a temperature increase rate of 1.0 to 6.0°C / min and maintaining the temperature at t2; Among them, 450℃≤T1≤650℃, 900℃≤T2≤1100℃, 1h≤t1≤5h, 4h≤t2≤24h.

12. The method according to claim 8, characterized in that: The programmed cooling and heat preservation comprises cooling from T2 to T3 at a cooling rate of 1.0 to 6.0°C / min, and maintaining t3; cooling naturally to room temperature; Among them, 900℃≤T2≤1100℃, 400℃≤T3≤800℃, 1h≤t3≤14h.

13. A battery, characterized in that: The invention comprises the positive electrode active material according to any one of claims 1 to 7.

14. The battery according to claim 13, characterized in that The discharge capacity corresponding to the discharge process of 4.95V to 3.5V is R, and the discharge capacity corresponding to the discharge process of 4.4V to 3.5V is R Mn ; Mn capacity contribution rate S = R Mn / R, satisfying 5%<S<21%.

15. The battery according to claim 14, characterized in that 6%≤S≤15%。 16. An electrical device, characterized in that: A battery comprising the battery according to any one of claims 13 to 15.

Citation Information

Cited By

  • Lithium nickel manganese oxide positive electrode material, preparation method thereof and battery

    CN119370911A

  • Cathode active material and preparation method thereof, secondary battery and electric device

    CN119674057A

  • Positive electrode active material and preparation method therefor, positive electrode sheet, and battery

    WO2026144165A1