Composite solid electrolyte film and preparation method and application thereof

The composite support film of the three-dimensional conductive network was prepared by electrospinning method and loaded with halide electrolytes, which solved the problems of taking into account both electrochemical and mechanical properties of solid electrolyte membranes, and achieved efficient improvement of solid-state battery performance and feasibility of large-scale production.

CN119069775APending Publication Date: 2024-12-03CHINA FAW CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411222219.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing solid electrolyte membranes cannot take into account both the electrochemical properties, resistance variation properties and mechanical strength, and the preparation process is complicated, making it difficult to achieve high batch production and reduce internal resistance.

Method used

The composite support film with a nanofiber structure with a three-dimensional conductive network was prepared by electrospinning method, and the halide electrolyte was loaded thereon to form an ultra-thin and self-supported composite solid electrolyte membrane, which enhances the combination of the film by solution immersion and heat treatment. and coupling effect to improve electrochemical and mechanical properties.

Benefits of technology

It achieves high ionic conductivity, good mechanical strength and flexible surface, inhibits the growth of lithium dendrites, improves the cycle stability and safety of the battery, is suitable for large-scale production, and reduces internal resistance and energy consumption.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a composite solid electrolyte film and a preparation method and application thereof, and relates to the technical field of solid-state batteries, in particular to a composite solid electrolyte film which comprises a three-dimensional composite support film and halide electrolyte loaded on the support film, wherein the three-dimensional composite support membrane comprises a lithiated polymer, an oxide solid electrolyte and an inorganic filler. A lithiated polymer is filled with an inorganic filler doped oxide solid electrolyte, a three-dimensional composite support membrane skeleton is prepared by electrostatic spinning, and a halide solid electrolyte is compounded by a solution soaking method to form an integrated organic-inorganic composite solid electrolyte structure. The electrolyte is thin, low in thickness, high in ionic conductivity, good in mechanical strength and flexible surface, capable of inhibiting growth of lithium dendrites and fundamentally preventing short circuit between a positive electrode and a negative electrode, and good in safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid-state batteries, and in particular to a composite solid-state electrolyte film and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have great potential to convert intermittent renewable energy such as solar energy and wind energy into electrical energy, but the energy density of liquid lithium batteries is close to the theoretical upper limit. The safety and energy density improvement potential of all-solid-state batteries can help new energy vehicles improve in terms of long-range, high safety, and all-weather, making all-solid-state batteries have received unprecedented attention in fields such as electronic equipment and electric vehicles. To develop all-solid-state batteries, first of all, the solid electrolyte must have good comprehensive performance and can optimize the performance of the positive and negative electrodes at the same time; at the same time, the internal resistance of the electrolyte layer is positively correlated with its thickness, and reducing the thickness of the electrolyte layer will help improve battery performance.

[0003] Solid electrolytes can be divided into inorganic solid electrolytes (such as oxide or sulfide solid electrolytes) and organic polymer solid electrolytes according to their chemical composition. Among them, inorganic solid electrolytes have high ion conductivity, but due to their high rigidity, they have high interface impedance between them and the electrode; polymer solid electrolytes have good flexibility, but low ion conductivity and mechanical strength. Their mechanical strength is not enough to effectively inhibit the growth of lithium dendrites, which can easily cause short circuits and reduce the safety of solid-state batteries.

[0004] CN202210128482.3 discloses a composite electrolyte membrane based on an alumina fiber skeleton and a preparation method thereof, wherein an electrolyte powder with high ionic conductivity is synthesized by a high-energy ball milling method, and then polyethylene glycol dimethyl ether and a small amount of polyethylene oxide are selected as a polymer matrix, and a solid electrolyte powder, LiTFSI and a lithium salt component of LiNO3 are mixed evenly to form a melt with low melting point characteristics, and cast on an alumina fiber membrane after pre-lithiation treatment with a LiPF6-based electrolyte, and a composite electrolyte membrane is prepared using the fiber membrane as a skeleton. The electrolyte membrane not only has high ionic conductivity, but also has interfacial low melting point contact characteristics, and can achieve good contact with the electrode at high temperature, which is expected to reduce the interface impedance and improve the electrochemical performance of the full battery; however, the preparation process is prone to uneven distribution of solid particles in the polymer, resulting in low local mechanical strength of the electrolyte membrane, poor resistance to lithium dendrite precipitation, and poor high pressure resistance of the electrolyte membrane.

[0005] CN202111412325.7 discloses a nanofiber polyvinylidene fluoride based composite solid electrolyte, by dispersing oxide ceramic nanoparticles in an organic solvent and obtaining oxide ceramic nanofibers by electrostatic spinning and high temperature calcination, mixing the obtained nanofibers with ion conductive polymers, lithium salts and ionic liquids to prepare mixed sols; preparing nanofiber polyvinylidene fluoride polymers by electrostatic spinning, and then uniformly dispersing the mixed sols on nanofiber polyvinylidene fluoride by casting, and drying the solvent to obtain a solid electrolyte. The electrolyte can be applied to flexible solid-state lithium batteries, with good electrochemical properties and mechanical flexibility; however, the casting method used will result in poor integrity of the prepared composite solid electrolyte membrane, and the obtained film thickness is relatively large, 100μm to 400μm, which cannot solve the technical problems of thinning and reducing internal resistance.

[0006] CN202311441923.6 discloses a cellulose-based all-solid-state polymer electrolyte membrane, which uses a cellulose membrane as a skeleton, and fills a polymer solid electrolyte in a three-dimensional skeleton of a high molecular polymer coated with an inorganic oxide nanolayer through atomic layer deposition and dip coating processes; the polymer electrolyte is kept in an amorphous structure at high temperature by instantaneous quenching, further improving the room temperature conductivity of the solid polymer electrolyte. After the surface of the electrolyte membrane is further coated with an aluminum oxide nanolayer, the electrochemical window width of the solid polymer electrolyte membrane can be significantly improved, and the decomposition of the solid polymer electrolyte membrane can be avoided under high pressure. However, the atomic layer deposition method proposed by it has a cumbersome preparation process, which is not conducive to product quality control and capacity improvement.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The first purpose of the present invention is to provide a composite solid electrolyte film, which is mainly used to solve the technical problem that the solid electrolyte membrane cannot take into account the electrochemical properties, resistance to deformation and mechanical strength. The present invention fills oxide solid electrolytes and inorganic fillers into lithium polymers to form a three-dimensional supporting skeleton, and further loads halide electrolytes to obtain an integrated composite solid electrolyte membrane with high ionic conductivity, ultra-thin and self-supporting.

[0009] The second purpose of the present invention is to provide a method for preparing the composite solid electrolyte film. By adopting the electrospinning method to prepare a composite support membrane with a nanofiber structure having a continuous three-dimensional conductive network, the mechanical properties, thermal stability and safety performance of the film can be effectively improved; the preparation method is simple and easy to implement and can achieve high-volume production.

[0010] The third object of the present invention is to provide a solid-state battery having good cycle stability and dendrite resistance, which can effectively improve the electrochemical and mechanical properties.

[0011] The fourth object of the present invention is to provide an electrical device having the relevant performance advantages introduced by the composite solid electrolyte film and the solid-state battery.

[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0013] A composite solid electrolyte film, comprising a three-dimensional composite support membrane, and a halide electrolyte supported on the three-dimensional composite support membrane;

[0014] Wherein, the three-dimensional composite support membrane comprises a lithium polymer, an oxide solid electrolyte and an inorganic filler.

[0015] A method for preparing the composite solid electrolyte film comprises the following steps:

[0016] (1) preparing a solution comprising a polymer and lithium hydroxide to obtain a first spinning solution; preparing a solution comprising an oxide solid electrolyte and an inorganic filler to obtain a second spinning solution; electrospinning the first spinning solution and the second spinning solution through a coaxial needle to obtain a composite fiber; and calcining the composite fiber to obtain a three-dimensional composite support membrane;

[0017] (2) preparing a solution containing a halide solid electrolyte to obtain a pre-dip solution; then immersing the three-dimensional composite support membrane in the pre-dip solution to obtain a precursor film; and heat-treating the precursor film to obtain a composite solid electrolyte film.

[0018] A solid-state battery comprises the composite solid-state electrolyte film.

[0019] An electrical device comprises the solid-state battery.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The ultra-thin composite electrolyte membrane for solid-state batteries provided by the present invention has the significant advantages of high ion conductivity and ultra-thin volume, and also has good mechanical strength and flexible surface. It can inhibit the growth of lithium dendrites and fundamentally prevent the short circuit between the positive electrode and the negative electrode. It has higher safety and is an electrolyte material for all-solid-state batteries with excellent comprehensive performance.

[0022] The ultra-thin composite electrolyte membrane for solid-state batteries provided by the present invention has a fully permeated skeleton structure, which can ensure efficient and continuous ion transport during long cycles, reduce the crystallinity of the polymer substrate, improve the ion conductivity and ion migration number while retaining a certain degree of flexibility, can match high-voltage oxide positive electrodes, has the advantages of strong oxidation resistance and high conductivity, and can effectively improve the battery cycle performance.

[0023] (2) In the method for preparing an ultra-thin composite electrolyte membrane for a solid-state battery provided by the present invention, first, a three-dimensional conductive support membrane network having a nanofiber structure and filled with an oxide solid electrolyte-inorganic filler in a polymer is prepared by electrospinning. The three-dimensional conductive support membrane network can provide a large number of active sites, reduce internal impedance, and provide a transmission channel for lithium ions, which is conducive to uniformly inducing lithium deposition and electrochemical reactions, and is not easy to form dead lithium.

[0024] Secondly, the buffer layer of oxide composite polymer with nanofiber morphology can improve the thermal stability and mechanical properties of the film, effectively resist the damage of lithium dendrites, and provide effective protection for the cycle stability and safety of lithium-ion batteries.

[0025] Thirdly, nanofibers with a high aspect ratio can produce continuous ion transport paths over longer distances and minimize the connections between particles, enhancing the ion transport strength, effectively inhibiting the growth of lithium dendrites without reducing ionic conductivity.

[0026] In addition, the present invention further prepares an ultra-thin composite solid electrolyte membrane by a solution immersion method based on the three-dimensional composite support membrane, immerses the three-dimensional conductive composite support skeleton into a pre-impregnation solution, and then spontaneously precipitates the halide electrolyte onto the three-dimensional composite support skeleton through heat treatment. This process can effectively achieve thinning; compared with traditional solid electrolyte membrane preparation methods such as slurry technology, vapor deposition, magnetron sputtering electron beam thermal evaporation or atomic layer deposition, the solution immersion method used in the present invention has relatively loose requirements on the experimental environment, a short experimental cycle, good film uniformity, is suitable for large-scale production, and has significant cost advantages.

[0027] (3) The present invention introduces inorganic fillers as sintering aids at the same time. By introducing such nano-scale dispersed powders, a small amount of liquid phase can be produced, so that the sintering mechanism of the composite fiber and the precursor film is transformed from solid-phase sintering to liquid-phase sintering, thereby enhancing the sintering driving force, lowering the sintering temperature and reducing energy consumption; at the same time, the inorganic fillers also help to reduce the porosity of the film, promote the densification of the film layer and obtain a dense continuous three-dimensional conductive composite support film.

[0028] In addition, the particles of the lithiated inorganic filler have a certain volume expansion coefficient, which can produce gaps in the solid electrolyte membrane during the operation of the solid-state battery, relieve the stress caused by dendrite growth, and make the lithium dendrites contact with the volume expansion material in the solid electrolyte, unable to contact the positive electrode and cause a short circuit. At the same time, the growth of lithium dendrites is inhibited, fundamentally improving the safety of the solid-state battery.

[0029] Furthermore, the strong Lewis acid-base interaction between the surface chemical groups of the inorganic filler and the ionic components in the polymer matrix is ​​conducive to the dissociation of the lithium salt. When the anions in the lithium salt are adsorbed on the surface of the inorganic filler, the free Li + The concentration will increase, improving the cation migration number of the electrolyte and reducing concentration polarization, making the solid-state battery have good cycle and rate performance.

[0030] Furthermore, after the inorganic filler particles are chemically bonded to the polymer, a fibrous volume expansion buffer layer is formed through electrospinning. At this time, the polymer chains are tightly locked on the surface of the inorganic filler through physical and chemical actions, forming an amorphous-rich region around the inorganic particles, which can realize the rapid transport of lithium ions.

[0031] (4) The halide electrolyte material loaded on the surface of the three-dimensional composite support skeleton of the present invention has the advantages of wide electrochemical window and stable interface of high-voltage oxide positive electrode, and is not easy to decompose during the cycle process, which is beneficial to reduce the internal resistance, inhibit the volume expansion of the negative electrode and the formation of lithium dendrites, and thus improve the overall performance of the battery. In addition, the present invention can enhance the degree of bonding and coupling between the halide electrolyte and the three-dimensional conductive support skeleton during the composite process, regulate ion coordination at the molecular level, and improve the interface ion conduction dynamics by combining solution immersion method and heat treatment. DETAILED DESCRIPTION

[0032] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. The terms "one", "two", and "1" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0033] The first aspect of the present invention is to provide a composite solid electrolyte film, including a three-dimensional composite support membrane and a halide electrolyte loaded on the three-dimensional composite support membrane; wherein the three-dimensional composite support membrane includes a lithiated polymer, an oxide solid electrolyte and an inorganic filler.

[0034] As a preferred embodiment, the thickness of the composite solid electrolyte film is 15 μm to 35 μm, including but not limited to any one of 15, 18, 20, 24, 25, 28, 30, 32, 35 (μm) or a numerical range consisting of any two of them.

[0035] As a preferred embodiment, the polymer component of the lithiated polymer includes at least one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polypropylene carbonate, polyethylene carbonate or polymethyl methacrylate; in some more preferred embodiments, the lithiated polymer is polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP).

[0036] As a preferred embodiment, the lithiating agent of the lithiated polymer includes lithium hydroxide (LiOH).

[0037] As a preferred embodiment, in the lithiated polymer, the molar ratio of polymer to lithium atoms is 10-20; in some more preferred embodiments, the molar ratio is 12-16.

[0038] As a preferred embodiment, the oxide solid electrolyte includes a lithium lanthanum zirconium oxygen solid electrolyte (LLZO); in some more preferred embodiments, the atomic molar ratio of lithium, lanthanum and zirconium is 0.5-0.9:0.2-0.4:0.1-0.3, or it can be understood that the oxide solid electrolyte includes Li x La y Zr z O n Or xLi2O·yLa2O3·zZrO2, x:y:z=0.5~0.9:0.2~0.4:0.1~0.3.

[0039] As a preferred embodiment, the inorganic filler includes at least one of zinc oxide, aluminum oxide, silicon oxide, tin oxide, zirconium oxide or copper oxide; in some more preferred embodiments, the inorganic filler contains at least zinc oxide (ZnO).

[0040] As a preferred implementation, the inorganic filler is nano-scale; the particle size of the inorganic filler is 0.1 nm to 100 nm.

[0041] As a preferred embodiment, the ratio of the sum of the moles of metal atoms in the oxide solid electrolyte to the mole number of the inorganic filler is 0.8-1.6:0.01-0.1.

[0042] As a preferred embodiment, the halide electrolyte includes Li a M b X c , wherein M (metal element) includes at least one of Zr, Hf, In, La, Sm, Eu, Sc, Y, Gd, Tb, Ce, Pr, and Nb, and X (halogen element) includes at least one of F, Cl, Br, and I; it can be understood that the halide electrolyte includes lithium halide and a halide of M; in some more preferred embodiments, the halide electrolyte includes Li3MX6, M is Cl, and X is In.

[0043] The second aspect of the present invention is to provide a method for preparing the composite solid electrolyte film, which mainly includes the following two steps.

[0044] (1) preparing a solution comprising a polymer and lithium hydroxide to obtain a first spinning solution; preparing a solution comprising an oxide solid electrolyte and an inorganic filler to obtain a second spinning solution; electrospinning the first spinning solution and the second spinning solution through a coaxial needle to obtain a composite fiber; and calcining the composite fiber to obtain a three-dimensional composite support membrane.

[0045] As a preferred embodiment, the solvent of the first spinning solution is water; the solvent of the second spinning solution includes at least one of anhydrous ethanol, n-butanol or acetone. In some more preferred embodiments, the solvent of the second spinning solution is anhydrous ethanol.

[0046] As a preferred embodiment, a lithium source, a lanthanum source, a zirconium source and an inorganic filler are dispersed in a solvent to prepare the second spinning solution.

[0047] As a more preferred embodiment, the lithium source includes at least one of lithium carbonate, lithium hydroxide or lithium cobaltate, the lanthanum source includes at least one of lanthanum oxide, lanthanum boride or lanthanum nitrate, and the zirconium source includes at least one of zirconium oxychloride octahydrate, zirconium acetate, zirconium nitrate or zirconium oxide. In a further preferred embodiment, the lithium source is lithium carbonate, the lanthanum source is lanthanum oxide, and the zirconium source is zirconium oxide.

[0048] As a preferred embodiment, the preparation process of the first spinning solution and the second spinning solution includes means such as stirring, oscillation, centrifugation, ultrasound, bubbling, etc. to achieve rapid dissolution and uniform dispersion of the solute.

[0049] As a more preferred embodiment, the ball mill speed of the ball milling treatment is 500 rpm to 800 rpm, and the ball milling treatment time is 3 h to 10 h. In a further preferred embodiment, the ball mill speed of the ball milling treatment is 500 rpm, and the ball milling treatment time is 5 h.

[0050] As a preferred embodiment, the usage ratio of the first spinning solution to the second spinning solution is 0.01 to 0.5:1 by mass; in some more preferred embodiments, the usage ratio is 0.06 to 0.5:1.

[0051] As a preferred embodiment, the conditions for electrospinning include: a spinning solution flow rate of 1 mL / h to 5 mL / h, a voltage of 0.5 kV / cm to 2.0 kV / cm, and a distance between the emission needle and the collector of 5 cm to 30 cm; in some more preferred embodiments, the spinning solution flow rate is 1 mL / h to 2 mL / h, the voltage is 1.0 kV / cm to 2.0 kV / cm, and the distance between the emission needle and the collector is 15 cm.

[0052] It can be understood that the flow rates of the first spinning solution and the second spinning solution in the electrospinning process can be consistent or inconsistent, and the technical personnel in this field can independently select within the above-mentioned flow rate range; furthermore, the technical personnel in this field can control the mass ratio of each component in the composite fiber according to the flow rate control of the spinning solution.

[0053] As a preferred embodiment, the calcination temperature is 500°C to 1100°C, and the calcination holding time is 2h to 10h; in some more preferred embodiments, the calcination temperature is 600°C, and the calcination holding time is 4h.

[0054] In the oxide solid electrolyte used in the present invention, the ionic conductivity of the cubic phase LLZO is nearly two orders of magnitude higher than that of the tetragonal phase. Only when the sintering temperature exceeds 1000°C, the tetragonal phase LLZO will undergo a phase change, the c-axis in the unit cell is elongated, and the a and b axes are contracted to the same length as the c-axis, becoming a cubic phase LLZO; however, high temperature and long sintering time will cause excessive lithium volatilization. The inorganic filler used in the present invention is also a good sintering aid, which can enable the LLZO electrolyte to obtain a higher density at a lower sintering temperature; specifically, part of the inorganic filler second phase forms a low-melting-point amorphous glass phase at the grain boundary position, so that the sintering becomes mainly liquid phase sintering, the diffusion rate is increased, the densification sintering temperature is reduced, and the flow and bonding of the glass phase allow the pores to be fully discharged and disappear, thereby improving the density of the sintered body. When the inorganic filler is zinc oxide, since the radius of zinc ions is not much different from that of zirconium ions and their electronegativity is equivalent, a solid solution is easily formed, which causes the chemical potential of the system to decrease, increases the sintering driving force, and promotes sintering; in addition, zinc oxide stabilizes the cubic phase LLZO by doping, making the crystal structure more compact and dense.

[0055] (2) preparing a solution containing a halide solid electrolyte to obtain a pre-dip solution; then immersing the three-dimensional composite support membrane in the pre-dip solution to obtain a precursor film; and heat-treating the precursor film to obtain a composite solid electrolyte film.

[0056] As a preferred embodiment, the solvent of the pre-dip liquid includes at least one of anhydrous ethanol, n-butanol or acetone; in some more preferred embodiments, the solvent of the pre-dip liquid is anhydrous ethanol.

[0057] As a preferred embodiment, the concentration of the pre-soak is 0.1 g / L to 0.8 g / L; in some more preferred embodiments, the concentration of the pre-soak is 0.2 g / L to 0.6 g / L.

[0058] As a preferred embodiment, the time for immersing the three-dimensional composite support membrane in the pre-dip solution should be based on the complete wetting of the membrane.

[0059] As a preferred embodiment, the heat treatment is carried out in a vacuum environment, the temperature of the heat treatment is 100°C to 500°C, and the insulation time of the heat treatment is 10h to 15h; in some more preferred embodiments, the temperature of the heat treatment is 200°C to 400°C, and the insulation time of the heat treatment is 12h to 14h.

[0060] The third aspect of the present invention is to provide a solid-state battery, including the composite solid-state electrolyte film. It is understandable that, in addition to the composite solid-state electrolyte film, the solid-state battery should include at least a positive electrode and a negative electrode, or add other necessary or unnecessary functional elements, packaging and safety components according to actual functions and packaging requirements, and those skilled in the art can make any selection and combination thereof; when the composite solid-state electrolyte film of the present invention is included in the solid-state battery, whether or not other electrolyte or diaphragm functional parts are used in the solid-state battery, it can be regarded as an embodiment of the present invention.

[0061] The fourth aspect of the present invention is to provide an electrical device, including the solid-state battery. The electrical device can be any device or apparatus that relies on electrical energy to work or operate, including but not limited to new energy vehicles, building electrical equipment, industrial electrical appliances, household and agricultural electrical appliances, etc.; when including the solid-state battery, any electrical device equipped with the solid-state battery can belong to an embodiment of the present invention.

[0062] Example 1

[0063] S1. Preparation of three-dimensional electrospinning support skeleton: PVDF-HFP was added to an aqueous solution of LiOH (the molar ratio of PVDF-HFP:LiOH was 12), and ultrasonic treatment was performed to obtain a uniform slurry, which was used as electrospinning solution A.

[0064] 40 g of Li2CO3, 85 g of La2O3, 21 g of ZrO2 and 2 g of ZnO were weighed in sequence and mixed. The obtained mixed raw materials, anhydrous ethanol and zirconium oxide were added into the ball mill in a mass ratio of 1:5:3. The ball mill speed was set to 500 r / min and the ball milling time was set to 5 h. After the ball milling, the electrospinning solution B was obtained.

[0065] The electrospinning solutions A and B were placed on the positive voltage side of electrospinning at a weight ratio of 0.1:1, and a coaxial needle was used for spinning. The flow rate of the fluid was 0.5 mL / h, the voltage was set to 12 kV, and the collection distance between the emission needle and the collector was 15 cm. After the electrospinning treatment, the collected composite fibers were placed in a muffle furnace and calcined at 600 ° C for 4 hours to obtain a three-dimensional composite support membrane.

[0066] S2. Preparation of solid electrolyte precursor film: weigh 32 g of LiCl and 55 g of InCl3, add anhydrous ethanol, and magnetically stir for 1 hour to obtain a mixed solution with a total concentration of 0.2 g / L; immerse the three-dimensional composite support membrane in the mixed solution, and obtain a solid electrolyte precursor film after sufficient infiltration.

[0067] S3: Preparation of composite solid electrolyte film: Put the solid electrolyte precursor film into a vacuum oven, set the drying temperature to 200° C., and keep it warm for 3 hours to obtain the composite solid electrolyte film of this embodiment.

[0068] Example 2

[0069] It is basically the same as Example 1, except that the mass of ZnO in step S1 is 4 g.

[0070] Example 3

[0071] It is basically the same as Example 1, except that the mass of ZnO in step S1 is 8 g.

[0072] Example 4

[0073] The method is basically the same as Example 1, except that in step S1, the electrospinning solutions A and B are mixed in a mass ratio of 0.2:1.

[0074] Example 5

[0075] The method is basically the same as Example 1, except that in step S1, the electrospinning solutions A and B are mixed in a mass ratio of 0.5:1.

[0076] Example 6

[0077] It is basically the same as Example 1, except that the calcination temperature in step S1 is 500°C.

[0078] Example 7

[0079] It is basically the same as Example 1, except that the calcination temperature in step S1 is 800°C.

[0080] Example 8

[0081] It is basically the same as Example 1, except that the calcination temperature in step S1 is 1100°C.

[0082] Example 9

[0083] The method is basically the same as Example 1, except that the calcination holding time in step S1 is 6 hours.

[0084] Example 10

[0085] It is basically the same as Example 2, except that the calcination temperature in step S1 is 800°C.

[0086] Embodiment 11

[0087] The method is basically the same as Example 1, except that the amount of anhydrous ethanol added is adjusted in step S2 to obtain a mixed solution with a total concentration of 0.4 g / L.

[0088] Example 12

[0089] The method is basically the same as Example 1, except that the amount of anhydrous ethanol added is adjusted in step S2 to obtain a mixed solution with a total concentration of 0.8 g / L.

[0090] Embodiment 13

[0091] It is basically the same as Example 1, except that 2 g of ZnO in step S1 is replaced by 3 g of Al2O3.

[0092] Comparative Example 1

[0093] The method is basically the same as Example 1, except that there is no ZnO in step S1.

[0094] Comparative Example 2

[0095] It is basically the same as Example 1, except that:

[0096] The electrospinning solution B in step S1 is replaced by: weighing 100 g of LLZO solid electrolyte powder doped with inorganic filler ZnO that has been sintered in advance, and mixing it with anhydrous ethanol at a mass ratio of 1:5, and then mixing them evenly by magnetic stirring to obtain electrospinning solution B;

[0097] After the electrospinning in step S1 is completed: the collected composite fibers are placed in a muffle furnace and calcined at 200° C. for 3 hours to obtain a three-dimensional composite support membrane.

[0098] Comparative Example 3

[0099] It is basically the same as Example 1, except that in the preparation process of the electrospinning solution B in step S1, the ball mill is replaced by magnetic stirring.

[0100] Comparative Example 4

[0101] It is basically the same as Example 1, except that:

[0102] The electrospinning solution A in step S1 is replaced by: dissolving PVDF-HFP and LiTFSI (the molar ratio of the two is 12) in DMF, and ultrasonically treating to obtain a uniform slurry to obtain an electrospinning solution A.

[0103] Comparative Example 5

[0104] It is basically the same as Example 1, except that step S1 is replaced as a whole by:

[0105] Weigh 40g of Li2CO3, 85g of La2O3, 21g of ZrO2 and 4g of ZnO and mix them. Add the obtained mixed raw materials, anhydrous ethanol and zirconium oxide to the ball mill in a mass ratio of 1:5:3. Set the ball mill speed to 500r / min and the ball milling time to 5h. After the ball milling, place the obtained suspension in a vacuum drying oven for 12h, and set the temperature in the drying oven to 70℃; place the dried raw materials in a zirconium oxide crucible and put them in a muffle furnace for sintering at 900℃ and heat preservation for 6h. After sintering, grind and sieve to obtain a sintered material. Add PVDF-HFP to an aqueous solution of LiOH (the molar ratio of PVDF-HFP:LiOH is 12) and ultrasonically treat until a uniform slurry is obtained. The sintered material is added to the slurry (the mass ratio of the sintered material to the slurry is 1:0.1), and then added to a ball mill for ball milling; after ball milling, the obtained mixed solution is coated on a substrate using a scraper and placed in a vacuum drying oven for 12 hours. The temperature in the drying oven is set to 70°C, thereby obtaining the LLZO solid composite electrolyte membrane coated with a lithium polymer of this comparative example.

[0106] The electrolyte membrane is used to replace the three-dimensional composite support membrane in step S2 of Example 1, and the composite solid electrolyte film of this comparative example is obtained based on S3.

[0107] Comparative Example 6

[0108] It is basically the same as Example 1, except that steps S2 and S3 are replaced as follows:

[0109] Appropriate amounts of commercially available halide solid electrolyte Li3InCl6 and binder PTFE are weighed in a weight percentage of 95%:5%, mixed evenly by ball milling, and then rolled to obtain a halide solid electrolyte layer. The three-dimensional composite support membrane and the halide solid electrolyte layer are aligned and stacked, and hot rolled at a temperature of 100°C to obtain the composite solid electrolyte membrane of this comparative example.

[0110] Test example

[0111] (1) PVDF was dispersed in NMP until it was completely dissolved; then LiFePO4 and Super-P were mixed and ground in an agate mortar for 30 min, the mixed powder was poured into the mixed solution and stirred for 6 h, the obtained slurry was evenly coated on aluminum foil, and then vacuum dried at 100 ° C for 24 h to obtain a positive electrode sheet.

[0112] (2) Using lithium-indium alloy as the negative electrode; cutting the composite solid electrolyte membranes prepared in each embodiment and comparative example into membrane sheets, stacking the positive electrode, solid electrolyte membrane, and negative electrode in sequence, pressurizing and assembling to obtain solid-state batteries for testing.

[0113] (3) The cycling performance of each all-solid-state battery was tested using the Blue Electric Battery Test System; the voltage range of the test was 2.5 V to 4.0 V. Before the test, the all-solid-state battery was left to stand for 12 h to reach a stable state. First, 5 cycles of charge and discharge were performed at a small rate of 0.1C to activate the battery. Then, 100 cycles of charge and discharge were performed at a rate of 0.5C. After the 100th cycle, the battery capacity retention rate was recorded. The results are shown in Table 1.

[0114] (4) The composite solid electrolyte films prepared in the embodiment and the comparative example were subjected to electrochemical impedance spectroscopy (EIS) tests respectively, and the ionic conductivity of the solid electrolyte was calculated based on the results. The results are shown in Table 1. In the EIS test, a stainless steel sheet was used as a blocking electrode to form a symmetrical battery with the composite solid electrolyte film, and an Autolab electrochemical workstation was used to measure the electrochemical impedance spectrum. The impedance frequency used was 1 Hz to 100 KHz, and the test temperature was 25°C. Furthermore, the calculation formula for ionic conductivity is σ=L / (R·S), where σ is the ionic conductivity of the sample (S / cm), L is the thickness of the solid electrolyte (cm), and S is the effective cross-sectional area of ​​the solid electrolyte (cm 2 ), R is the resistance value of the solid electrolyte (Ω).

[0115] Table 1

[0116] Ionic conductivity (mS / cm) 100 cycles capacity retention rate (%) Example 1 1.16 80% Example 2 1.28 88% Example 3 0.86 87% Example 4 0.72 89% Example 5 0.68 75% Example 6 0.74 82% Example 7 1.22 85% Example 8 1.43 78% Example 9 1.65 83% Example 10 1.83 92% Embodiment 11 1.36 83% Example 12 1.62 74% Embodiment 13 0.98 76% Comparative Example 1 0.84 Short Circuit Comparative Example 2 1.34 68% Comparative Example 3 0.88 59% Comparative Example 4 1.10 Short Circuit Comparative Example 5 1.25 Short Circuit Comparative Example 6 0.48 52%

[0117] Taking Example 1 of the present invention as an example, the inorganic filler ZnO doped LLZO oxide solid electrolyte nanofiber film is used as a three-dimensional composite support membrane framework, and the polyvinylidene fluoride-hexafluoropropylene polymer prepared by electrospinning is used as a matrix. The three-dimensional composite support membrane and the halide solid electrolyte are compounded by a solution method to form an integrated composite solid electrolyte structure. The three-dimensional composite support membrane prepared by a simple electrospinning method has abundant cation defects, which can be coordinated with anions to adjust the original molecular coupling in the composite electrolyte, weaken the solid phase solvation of lithium ions and improve their diffusion dynamics, so that the migration speed on the polymer matrix interface is faster, and the ionic conductivity of the composite electrolyte is further improved. Due to the continuous extension of the ceramic nanofiber-polymer interface, the composite electrolyte based on the ceramic nanofiber 3D framework has higher ionic conductivity, overcomes the problem that the isolated inorganic particles inside the composite electrolyte do not form a connected lithium ion transfer network, and makes the organic-inorganic interface enhance the advantages better; and the inorganic filler nanofiber provides sufficient contact sites for the polymer electrolyte matrix, so that the prepared electrolyte structure is stable and more ion fast channels are generated. From the data performance of the test examples, it can be seen that the embodiments of the present invention have significantly higher ion conductivity and capacity retention rate than the comparative examples.

[0118] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A composite solid electrolyte film, characterized in that: The composite solid electrolyte film includes a three-dimensional composite support membrane and a halide electrolyte supported on the three-dimensional composite support membrane; Wherein, the three-dimensional composite support membrane comprises a lithium polymer, an oxide solid electrolyte and an inorganic filler.

2. The composite solid electrolyte film according to claim 1, characterized in that: The thickness of the composite solid electrolyte film is 15 μm to 35 μm.

3. The composite solid electrolyte film according to claim 1, characterized in that: The polymer component of the lithiated polymer includes at least one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polypropylene carbonate, polyethylene carbonate or polymethyl methacrylate; In the lithiated polymer, the molar ratio of polymer to lithium atoms is 10-20.

4. The composite solid electrolyte film according to claim 1, characterized in that: The oxide solid electrolyte includes a lithium lanthanum zirconium oxygen solid electrolyte; In the lithium lanthanum zirconium oxygen solid electrolyte, the atomic molar stoichiometric ratio of lithium, lanthanum and zirconium is 0.5-0.9:0.2-0.4:0.1-0.

3.

5. The composite solid electrolyte film according to claim 1, characterized in that: The inorganic filler includes at least one of zinc oxide, aluminum oxide, silicon oxide, tin oxide, zirconium oxide or copper oxide.

6. The composite solid electrolyte film according to claim 1, characterized in that: The halide electrolyte includes Li a M b X c , wherein M includes at least one of Zr, Hf, In, La, Sm, Eu, Sc, Y, Gd, Tb, Ce, Pr, and Nb, and X includes at least one of F, Cl, Br, and I.

7. The composite solid electrolyte film according to claim 1, characterized in that: The ratio of the sum of the moles of metal atoms in the oxide solid electrolyte to the mole number of the inorganic filler is 0.8-1.6:0.01-0.

1.

8. The method for preparing a composite solid electrolyte film according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) preparing a solution comprising a polymer and lithium hydroxide to obtain a first spinning solution; preparing a solution comprising an oxide solid electrolyte and an inorganic filler to obtain a second spinning solution; electrospinning the first spinning solution and the second spinning solution through a coaxial needle to obtain a composite fiber; and calcining the composite fiber to obtain a three-dimensional composite support membrane; (2) preparing a solution containing a halide solid electrolyte to obtain a pre-dip solution; Then, the three-dimensional composite support membrane is immersed in the prepreg liquid to obtain a precursor membrane; The precursor film is heat treated to obtain a composite solid electrolyte film.

9. The method for preparing a composite solid electrolyte film according to claim 8, characterized in that: The preparation method of the second spinning solution comprises: dispersing a lithium source, a lanthanum source, a zirconium source and an inorganic filler into a solvent to prepare the second spinning solution; The lithium source includes at least one of lithium carbonate, lithium hydroxide or lithium cobaltate, the lanthanum source includes at least one of lanthanum oxide, lanthanum boride or lanthanum nitrate, and the zirconium source includes at least one of zirconium oxychloride octahydrate, zirconium acetate, zirconium nitrate or zirconium oxide.

10. The method for preparing a composite solid electrolyte film according to claim 8, characterized in that: The conditions for the electrospinning include: a spinning solution flow rate of 1 mL / h to 5 mL / h, a voltage of 0.5 kV / cm to 2.0 kV / cm, and a distance between an emission needle and a collector of 5 cm to 30 cm.

11. The method for preparing a composite solid electrolyte film according to claim 8, characterized in that: The calcination temperature is 500°C to 1100°C, and the calcination holding time is 2h to 10h; And / or, the heat treatment is performed in a vacuum environment, the temperature of the heat treatment is 100° C. to 500° C., and the insulation time of the heat treatment is 10 h to 15 h.

12. A solid-state battery, characterized in that: The solid-state battery comprises the composite solid electrolyte film according to any one of claims 1 to 7.

13. An electrical equipment, characterized in that: The electrical device comprises the solid-state battery as claimed in claim 12.

Citation Information

Cited By

  • Composite solid-state electrolyte membrane with Lewis acid and Lewis base sites and solid-state battery

    CN120933443A

  • A composite solid electrolyte membrane having lewis acid and lewis base sites and a solid-state battery

    CN120933443B

  • LLZO composite solid electrolyte and preparation method and application thereof

    CN120987359A

  • Chloride enhanced polymer electrolyte, preparation method and application thereof

    CN121035317A