Electrolyte, high-voltage-resistant lithium ion battery and preparation method
By using specific electrolyte formulas in lithium-ion batteries, combining fluorine-free nitrile-containing main solvent and low-fluorine lithium oxalate borate, the problems of high-voltage electrolyte high cost and short cycle life are solved, and low cost, high stability and High voltage performance battery system suitable for electric vehicles and energy storage systems.
Patent Information
- Application Number
- CN202411199349.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
When the existing lithium-ion battery high-voltage electrolyte meets high voltage requirements, it is expensive and has a low cycle life, making it difficult to achieve the problems of low cost and high cycle safety.
An electrolyte is used, including the first electrolyte M1 and the second electrolyte M2. The first electrolyte M1 is used for primary injection and decomposition, and the second electrolyte M2 is used for secondary injection and circulation, and a fluorine-free The main solvent containing nitrile and lithium difluorooxalate borate with low fluorine content are used as the main salt, combined with specific film forming agents and co-solvents, and the molar concentration and volume ratio of the electrolyte are adjusted to achieve high conductivity and stability of the electrolyte.
It realizes the low cost, high stability and high voltage performance of electrolyte, broadens the electrochemical window, extends the healthy life cycle of lithium-ion batteries, and is suitable for large-scale industrial production.
Smart Images

Figure CN119069812A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and more specifically, relates to an electrolyte, a high-voltage lithium ion battery and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are widely used in electric vehicles, electronic devices, and energy storage systems. With the rapid development and increasing demand in these fields, the demand for lithium is also rising. However, current lithium resources cannot meet the growing consumption. The reason is that lithium resources are very limited and unevenly distributed. The lithium resources distributed in the salt lake areas in the western region cannot be developed in winter, and the supply-demand relationship is further deteriorated. In order to cope with the shortage of lithium resources, current energy storage technology and battery materials need to be further improved to cope with the current lithium resource limitations and achieve the rational and efficient use of lithium resources.
[0003] For the current commercial lithium-ion battery system, there are mainly three systems: lithium cobalt oxide-graphite, lithium nickel cobalt manganese oxide-graphite, and lithium iron phosphate-graphite. The energy density of its single cell is about 200-250Wh / kg, which is difficult to meet the increasingly high energy density requirements of automotive batteries in the future. Therefore, it is imperative to increase the energy density of the current battery system. Without changing the use of positive electrode materials, the most suitable method to increase the energy density of the system is still to increase the battery cut-off voltage. However, due to its narrow electrochemical window, the existing commercial electrolyte is difficult to meet the needs of high-voltage battery systems (higher than 4.6V), and can only achieve stable circulation of battery positive electrode materials at around 4.3V. In order to meet the market demand for high specific energy of power batteries, the research and development of high-voltage electrolytes for lithium-ion batteries has very promising application potential.
[0004] The current system uses lithium-ion battery high-voltage electrolytes, which are mainly based on traditional electrolyte systems combined with additives. Patent CN116365038A discloses a high-voltage electrolyte additive formula, which adds 5% to 90% solid electrolyte powder to traditional organic electrolytes to achieve short-term operation of high-voltage systems. However, this type of solution has certain limitations. It has been reported that the cycle life of high-voltage electrolyte systems is low and it is difficult to reach the national standard level. And because it is an additive film, its high-temperature charging performance and high-temperature storage performance are difficult to meet national standards. At the same time, due to the complex formula of the traditional system, such as the use of solvents and special proportions in the low-temperature system, the blind use of additives will inevitably cause the low-temperature performance to disappear. In severe cases, it will cause a significant attenuation of graphite performance, causing serious battery degradation.
[0005] Therefore, current high-voltage electrolytes face many difficulties in large-scale commercial applications, either due to high costs or other risks that make them difficult to commercialize. Further research is needed on reliable high-voltage lithium-ion electrolytes to meet future power battery needs. Summary of the invention
[0006] In view of the defects of the related art, the purpose of the present invention is to provide an electrolyte, a high-voltage lithium-ion battery and a preparation method, aiming to solve the problem that it is difficult to achieve low cost and high cycle safety when the electrolyte meets the requirements of high-voltage battery systems.
[0007] To achieve the above-mentioned object, in a first aspect, the present invention provides an electrolyte, comprising a first electrolyte M1 and a second electrolyte M2; the first electrolyte M1 is used for primary injection and formation of a lithium-ion battery, and the second electrolyte M2 is used for secondary injection and circulation of a lithium-ion battery;
[0008] The first electrolyte M1 includes a main salt A1, an additive A2 and a nitrile-containing main solvent B1; the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5-1.5 mol / L, and the volume of the nitrile-containing main solvent B1 accounts for 0.2-0.4 of the total volume of the electrolyte;
[0009] The second electrolyte M2 includes a main salt A1 and a nitrile-containing main solvent B1, and the content is consistent with that in the first electrolyte M1;
[0010] Wherein, the main salt A1 is lithium difluorooxalate borate.
[0011] Optionally, the nitrile-containing main solvent B1 is at least one of acetonitrile, succinonitrile, adiponitrile, glutaronitrile, 1,3,6-hexanetricarboxylic acid nitrile, 1,3,5-pentanetricarboxylic acid nitrile and 2-fluoroadiponitrile.
[0012] Optionally, the additive A2 is at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorophosphate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium perchlorate, and lithium hexafluoroarsenate.
[0013] Optionally, the first electrolyte M1 and the second electrolyte M2 both further include: a film-forming agent B2 and a co-solvent B3;
[0014] The volume ratio of the film-forming agent B2 and the co-solvent B3 to the total volume of the electrolyte is 0.2-0.4;
[0015] The total volume fraction of the nitrile-containing main solvent B1, the film-forming agent B2 and the auxiliary solvent B3 is 1.
[0016] Optionally, the film-forming agent B2 is at least one of ethylene carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate and fluorovinylene carbonate.
[0017] Optionally, the cosolvent B3 is at least one of trifluoroethyl methyl carbonate, trifluoroethyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, bisfluoroethylene carbonate, and ethyl difluoroacetate.
[0018] In a second aspect, the present invention further provides a high-voltage lithium-ion battery, the high-voltage lithium-ion battery comprising a battery cell and an electrolyte, the electrolyte being the electrolyte as described in any one of the first aspects, and the battery cell comprising a positive electrode sheet, a negative electrode sheet and a separator.
[0019] Optionally, the positive electrode sheet is at least one of lithium iron phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium manganese oxide, and lithium nickel oxide;
[0020] The negative electrode is at least one of graphite, silicon carbon, and metallic lithium.
[0021] In a third aspect, the present invention further provides a method for preparing a high voltage resistant lithium ion battery, which is used to prepare the high voltage resistant lithium ion battery as described in any one of the second aspects, comprising:
[0022] S1: Drying the main salt A1 and the additive A2 in a glove box, wherein the additive A2 is a lithium-containing compound;
[0023] S2: The solvent is treated with molecular sieves to remove water in a glove box;
[0024] The solvent includes a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3;
[0025] S3: In a glove box, a first electrolyte M1 and a second electrolyte M2 are prepared using the treated solvent, a main salt A1 and an additive A2; wherein the first electrolyte M1 comprises a main salt A1, an additive A2, a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3, and the second electrolyte M2 comprises a main salt A1, a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3, and the contents of the main salt A1 and the nitrile-containing main solvent B1 of the two electrolytes are consistent; the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5 to 1.5 mol / L, the volume of the nitrile-containing main solvent B1, the film-forming agent B2 and the co-solvent B3 accounts for 0.2 to 0.4 of the total volume of the electrolyte, and the total volume fraction is 1;
[0026] S4: In the clean room, assemble high-voltage lithium-ion battery cells, with the positive electrode sheet being C1 and the negative electrode sheet being C2, and select the first electrolyte M1 for the first injection packaging in the glove box, and use button cell / square shell cell / soft pack cell / cylindrical cell structure sealing;
[0027] S5: pre-storing the high-voltage lithium-ion battery cell in the first electrolyte M1 for 24 hours and performing closed-cell formation at a preset temperature;
[0028] S6: subtract the air bag from the formation battery and perform secondary injection with the second electrolyte M2;
[0029] S7: placing the high-voltage lithium-ion battery cell in the second electrolyte M2 for 24 hours to obtain a high-voltage lithium-ion battery.
[0030] Compared with the prior art, the above technical solution conceived by the present invention can achieve the following beneficial effects:
[0031] 1. The present invention provides an electrolyte, which uses a fluorine-free nitrile main solvent and a low-fluorine content lithium difluoro oxalate borate as the main salt. Compared with the traditional high-voltage electrolyte formula, the fluorination degree of the electrolyte of the present application is reduced; in the existing electrolyte scheme using nitrile as solvent, the salt concentration is usually 3-5 mol / L, but in this scheme, the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5-1.5 mol / L, the salt dosage is greatly reduced, the electrolyte cost is low, it is environmentally friendly, and it is suitable for large-scale industrial production. In addition, using nitrile as the main solvent, high nitrile addition is conducive to achieving high conductivity, low viscosity and high stability of the electrolyte, greatly broadening the electrochemical window of the electrolyte, and the strong adsorption characteristics of nitrile realize the high voltage performance of lithium batteries, and further improve the specific energy of lithium-ion battery systems. At the same time, it achieves the effects of low cost and high cycle safety, and expands its large-scale application in electric vehicles, electronic devices and energy storage systems.
[0032] 2. The present invention provides an electrolyte. Compared with the traditional high-voltage electrolyte formula, the film-forming agent and the co-solvent in the present invention have an appropriate degree of fluorination, which greatly improves the thermal stability of the electrolyte and increases the safety performance, thereby extending the healthy life cycle of the battery prepared based on the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the structure of a battery cell of a high-voltage-resistant lithium-ion battery provided in an embodiment of the present invention;
[0034] Figure 2 It is a charge and discharge curve diagram of a cell structure of a high-voltage lithium-ion battery provided by an embodiment of the present invention;
[0035] Figure 3 is a cycle curve diagram of a high voltage resistant lithium ion battery provided by an embodiment of the present invention;
[0036] Figure 4 The present invention provides a flow chart for preparing and testing a high-voltage lithium-ion battery.
[0037] The reference numerals in the drawings are: 1. battery cell main body, 2. positive electrode tab, 3. negative electrode tab, 4. polyethylene separator. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0039] The contents involved in the above embodiment are described below in conjunction with a preferred embodiment.
[0040] Embodiment 1
[0041] The present invention provides an electrolyte, including a first electrolyte M1 and a second electrolyte M2; the first electrolyte M1 is used for primary injection and formation of a lithium ion battery, and the second electrolyte M2 is used for secondary injection and circulation of the lithium ion battery;
[0042] The first electrolyte M1 includes a main salt A1, an additive A2 and a nitrile-containing main solvent B1; the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5-1.5 mol / L, and the volume of the nitrile-containing main solvent B1 accounts for 0.2-0.4 of the total volume of the electrolyte;
[0043] The second electrolyte M2 includes a main salt A1 and a nitrile-containing main solvent B1, and the content is consistent with that in the first electrolyte M1;
[0044] Wherein, the main salt A1 is lithium difluorooxalate borate.
[0045] Existing lithium-ion battery electrolytes are only applicable to low-voltage battery systems (4.3V), which are difficult to meet the defects of high-voltage battery systems and have low cycle safety. An embodiment of the present invention provides a method for preparing a high-voltage lithium-ion electrolyte based on a nitrile solvent, which uses a traditional layered spinel positive electrode material and a soft-pack lithium-ion battery with graphite / silicon carbon as the negative electrode to stably cycle at 4.55V, thereby further improving the specific energy of the lithium-ion battery system.
[0046] The method for preparing a high-voltage lithium-ion electrolyte specifically includes preparing a first electrolyte M1 and a second electrolyte M2, specifically in the following steps:
[0047] (1) Dry the main salt A1 and additive A2 in a glove box.
[0048] The main salt A1 is lithium difluorooxalatoborate, and the additive A2 is any one or more combinations of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorophosphate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium perchlorate, and lithium hexafluoroarsenate.
[0049] (2) In a glove box, the solvent is treated with molecular sieves to remove water, and CaH2 is used to remove water from the solvent. Then, sodium tablets are added to determine whether the solvent dehydration is complete, until all the water is removed.
[0050] Among them, the solvent includes a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3; the nitrile-containing main solvent B1 is at least one of acetonitrile, succinonitrile, adiponitrile, glutaronitrile, 1,3,6-hexanetricarboxylic acid nitrile, 1,3,5-pentanetricarboxylic acid nitrile, and 2-fluoroadiponitrile; the film-forming agent B2 is at least one of ethylene carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate and fluorovinylene carbonate; the co-solvent B3 is at least one of trifluoroethyl methyl carbonate, trifluoroethyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, difluoroethylene carbonate, and ethyl difluoroacetate.
[0051] (3) In a glove box, a first electrolyte M1 and a second electrolyte M2 are prepared using the treated solvent, a main salt A1 and an additive A2; wherein the first electrolyte M1 comprises a main salt A1, an additive A2, a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3, and the second electrolyte M2 comprises a main salt A1, a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3, and the contents of the main salt A1 and the nitrile-containing main solvent B1 of the two electrolytes are consistent; the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5 to 1.5 mol / L, the volume ratio of the nitrile-containing main solvent B1, the film-forming agent B2 and the co-solvent B3 to the total volume of the electrolyte is 0.2 to 0.4, and the total volume fraction is 1.
[0052] In a specific embodiment, illustratively, the first electrolyte M1 is prepared: the molar concentrations of the main salt A1 and the additive A2 are adjustable, the main salt A1 is lithium difluorooxalatoborate, and the molar concentration is 1.0 mol / L, the additive A2 is lithium difluorophosphate, and the molar concentration is 0.2 mol / L; the nitrile-containing main solvent B1 is acetonitrile, and the volume fraction is 40%; the film-forming agent B2 is fluorovinylidene carbonate, and the volume fraction is 30%; the co-solvent B3 is trifluoroethyl methyl carbonate, and the volume fraction is 30%.
[0053] The prepared second electrolyte M2: the main salt A1 is lithium difluorooxalatoborate with a molar concentration of 1.0 mol / L; the nitrile-containing main solvent B1 is acetonitrile with a volume fraction of 40%; the film-forming agent B2 is fluorovinylene carbonate with a volume fraction of 30%; the co-solvent B3 is trifluoroethyl methyl carbonate with a volume fraction of 30%.
[0054] Mix and stir at room temperature and fully dissolve to obtain the electrolyte of the present invention. The degree of fluorination of the above-mentioned electrolyte is reduced, the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5-1.5 mol / L, the amount of salt used is greatly reduced, the electrolyte cost is low, it is environmentally friendly, and it is suitable for large-scale industrial production. Using nitrile as the main solvent greatly broadens the electrochemical window of the electrolyte, and the strong adsorption characteristics of nitrile realize the high voltage performance of the lithium battery. Furthermore, compared with the traditional high-voltage electrolyte formula, the difluoro solvent of this embodiment is a film-forming agent and a co-solvent, and the degree of fluorination is appropriate, so that the thermal stability of the electrolyte is greatly improved, the safety performance is increased, and the battery prepared therefrom has a long healthy life cycle. It solves the problem that it is difficult to achieve low cost and high cycle safety when the electrolyte meets the needs of the high-voltage battery system. The effects of low cost and high safety are achieved, and the lithium battery prepared therefrom has high voltage performance and a long healthy life cycle.
[0055] Embodiment 2
[0056] The first electrolyte M1 and the second electrolyte M2 were prepared by the same method as in Example 1. The first electrolyte M1 generated was as follows: the main salt A1 was lithium difluorooxalatoborate with a molar concentration of 1.1 mol / L, the additive A2 was lithium bis(fluorosulfonyl)imide salt with a molar concentration of 0.2 mol / L; the nitrile-containing main solvent B1 was succinonitrile with a volume fraction of 33%; the film-forming agent B2 was ethylene carbonate with a volume fraction of 33%; and the co-solvent B3 was bis(fluoroethylene carbonate) with a volume fraction of 33%.
[0057] The second electrolyte M2: the main salt A1 is lithium difluorooxalatoborate with a molar concentration of 1.1 mol / L; the nitrile-containing main solvent B1 is succinonitrile with a volume fraction of 33%; the film-forming agent B2 is ethylene carbonate with a volume fraction of 33%; the co-solvent B3 is difluoroethylene carbonate with a volume fraction of 33%.
[0058] Mix and stir at room temperature to fully dissolve to obtain the electrolyte of the present invention, which has the same effect as the above embodiment and will not be described in detail here.
[0059] Embodiment 3
[0060] The first electrolyte M1 and the second electrolyte M2 were prepared by the same method as in Example 1. The first electrolyte M1 generated was as follows: the main salt A1 was lithium difluorooxalatoborate with a molar concentration of 1.2 mol / L, the additive A2 was lithium bistrifluoromethanesulfonyl imide with a molar concentration of 0.2 mol / L; the nitrile-containing main solvent B1 was adiponitrile with a volume fraction of 20%; the film-forming agent B2 was vinylene carbonate with a volume fraction of 40%; and the co-solvent B3 was ethyl difluoroacetate with a volume fraction of 40%.
[0061] The second electrolyte M2: the main salt A1 is lithium difluorooxalatoborate with a molar concentration of 1.2 mol / L; the nitrile-containing main solvent B1 is adiponitrile with a volume fraction of 20%; the film-forming agent B2 is vinylene carbonate with a volume fraction of 40%; the co-solvent B3 is ethyl difluoroacetate with a volume fraction of 40%.
[0062] Mix and stir at room temperature to fully dissolve to obtain the electrolyte of the present invention, which has the same effect as the above embodiment and will not be described in detail here.
[0063] Embodiment 4
[0064] The first electrolyte M1 and the second electrolyte M2 were prepared by the same method as in Example 1. The first electrolyte M1 was prepared as follows: the main salt A1 was lithium difluorooxalatoborate with a molar concentration of 1.0 mol / L, the additive A2 was lithium perchlorate with a molar concentration of 0.1 mol / L; the nitrile-containing main solvent B1 was glutaronitrile, the film-forming agent B2 was ethylene carbonate, the co-solvent B3 was trifluoroethyl carbonate, and the nitrile-containing main solvent B1, the film-forming agent B2 and the co-solvent B3 were mixed in equal volumes.
[0065] The second electrolyte M2: the main salt A1 is lithium difluorooxalatoborate with a molar concentration of 1.0 mol / L; the nitrile-containing main solvent B1 is glutaronitrile, the film-forming agent B2 is ethylene carbonate, the auxiliary solvent B3 is trifluoroethyl carbonate, and the nitrile-containing main solvent B1, the film-forming agent B2 and the auxiliary solvent B3 are mixed in equal volumes.
[0066] Mix and stir at room temperature to fully dissolve to obtain the electrolyte of the present invention, which has the same effect as the above embodiment and will not be described in detail here.
[0067] Embodiment 5
[0068] The first electrolyte M1 and the second electrolyte M2 were prepared by the same method as in Example 1. The first electrolyte M1 generated was as follows: the main salt A1 was lithium difluorooxalatoborate with a molar concentration of 1.0 mol / L, the additive A2 was lithium trifluoromethanesulfonate with a molar concentration of 0.1 mol / L; the nitrile-containing main solvent B1 was 1,3,6-hexanetricarbonitrile with a volume fraction of 20%; the film-forming agent B2 was 4,5-dimethylvinylidene carbonate with a volume fraction of 40%; and the cosolvent B3 was trifluoroethyl carbonate with a volume fraction of 40%.
[0069] The second electrolyte M2: the main salt A1 is lithium difluorooxalatoborate with a molar concentration of 1.0 mol / L; the nitrile-containing main solvent B1 is 1,3,6-hexanetricarbonitrile with a volume fraction of 20%; the film-forming agent B2 is 4,5-dimethylvinylidene carbonate with a volume fraction of 40%; the co-solvent B3 is trifluoroethyl carbonate with a volume fraction of 40%.
[0070] Mix and stir at room temperature to fully dissolve to obtain the electrolyte of the present invention, which has the same effect as the above embodiment and will not be described in detail here.
[0071] The components and proportions in the above embodiments can be freely selected and configured within a limited range and have the same effect.
[0072] Embodiment 6
[0073] The present invention also provides a high-voltage resistant lithium-ion battery, which comprises a battery cell and an electrolyte, wherein the electrolyte is the electrolyte described in any one of the above embodiments, and the battery cell comprises a positive electrode sheet, a negative electrode sheet and a separator.
[0074] Optionally, the positive electrode sheet is at least one of lithium iron phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium manganese oxide, and lithium nickel oxide;
[0075] The negative electrode is at least one of graphite, silicon carbon, and metallic lithium.
[0076] Based on the electrolyte prepared in the above embodiment, a high-voltage resistant lithium-ion battery is prepared. For example, a lithium cobalt oxide positive electrode sheet and a graphite negative electrode sheet are selected, and a three-layer polyethylene diaphragm is used for winding and assembly to obtain the main body of the battery cell, wherein the lithium cobalt oxide positive electrode sheet ears and the graphite negative electrode sheet ears are respectively located at the edges of the winding.
[0077] The high-voltage lithium-ion battery prepared achieves the high-voltage performance of lithium batteries and further improves the specific energy of lithium-ion battery systems. At the same time, it achieves the effect of low production cost and high cycle safety of lithium batteries, expanding its large-scale application in electric vehicles, electronic devices and energy storage systems.
[0078] Embodiment 7
[0079] The present invention also provides a method for preparing a high-voltage lithium-ion battery, which is used to prepare the high-voltage lithium-ion battery as described in Example 6, comprising:
[0080] S1: Drying the main salt A1 and the additive A2 in a glove box, wherein the main salt A1 is lithium difluorooxalate borate, and the additive A2 is a lithium-containing compound;
[0081] S2: The solvent is treated with molecular sieves to remove water in a glove box;
[0082] The solvent includes a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3; the water removal treatment specifically includes: firstly using a molecular sieve to remove water, then using CaH2 to remove water from the solvent, and then adding a sodium sheet to determine whether the solvent dehydration is completed, until the water is completely removed.
[0083] S3: In a glove box, a first electrolyte M1 and a second electrolyte M2 are prepared using the treated solvent, a main salt A1 and an additive A2; wherein the first electrolyte M1 comprises a main salt A1, an additive A2, a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3, and the second electrolyte M2 comprises a main salt A1, a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3, and the contents of the main salt A1 and the nitrile-containing main solvent B1 of the two electrolytes are consistent; the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5 to 1.5 mol / L, the volume of the nitrile-containing main solvent B1, the film-forming agent B2 and the co-solvent B3 accounts for 0.2 to 0.4 of the total volume of the electrolyte, and the total volume fraction is 1;
[0084] S4: In the clean room, assemble high-voltage lithium-ion battery cells, with the positive electrode sheet being C1 and the negative electrode sheet being C2, and select the first electrolyte M1 for the first injection packaging in the glove box, and use button cell / square shell cell / soft pack cell / cylindrical cell structure sealing;
[0085] S5: pre-storing the high-voltage lithium-ion battery cell in the first electrolyte M1 for 24 hours and performing closed-cell formation at a preset temperature;
[0086] S6: subtract the air bag from the formation battery and perform secondary injection with the second electrolyte M2;
[0087] S7: placing the high-voltage lithium-ion battery cell in the second electrolyte M2 for 24 hours to obtain a high-voltage lithium-ion battery.
[0088] For example, the design capacity of the small test in this example is 0.6Ah, and the amount of electrolyte added is 1.5Ah g -1 (Based on the mass of the positive and negative electrodes). The lithium cobalt oxide current collector is aluminum foil, which is coated on both sides, with a single-side surface loading of 9 mg cm -2 The graphite negative electrode collector is copper foil, which is coated on both sides and has a single-side surface loading of 6.5 mg cm -2 , N / P ratio is 1.08, and appropriate excess graphite is used to prevent lithium precipitation risk. In this example, the nitrile-containing high-voltage lithium-ion battery cell is made using a winding process. The cell structure is as follows Figure 1 As shown, the main body 1 of the battery cell is formed by winding and assembling a lithium cobalt oxide positive electrode sheet, a graphite negative electrode sheet, and a three-layer polyethylene separator 4. The lithium cobalt oxide positive electrode sheet tab 2 and the graphite negative electrode sheet tab 3 are located at the edge of the winding.
[0089] After the battery is left for 24 hours to fully activate, the device is built. It should be noted that the actual nitrile-containing high-voltage lithium-ion battery cell is placed in a constant temperature phase, and the constant temperature box temperature is set to 45°C. The actual test of the nitrile-containing high-voltage lithium-ion battery cell needs to be fixed with a clamp. The battery is connected to the constant current charge and discharge instrument by a bipolar ear for subsequent data collection.
[0090] This example uses a high-temperature closed-cup formation process with a formation temperature of 45°C to ensure that the electrolyte can be completely decomposed to form a dense solid electrolyte membrane, thereby ensuring the actual operating life of the battery. The formation adopts a constant current and constant voltage charge and discharge mode, and the formation current is 0.1C. Specifically for this example, the upper limit of the operating voltage is 4.55V, the lower limit is 3V, and the constant voltage cutoff condition in the constant current and constant voltage charging is that the current is less than 0.1A, and the standby time in the formation charge and discharge is still 10min. In the constant current and constant voltage test, the battery voltage, current, stress, and heat generation data are collected synchronously, and the collection time accuracy is not less than 1s, to facilitate subsequent formation analysis.
[0091] Then the data of the high-voltage lithium-ion battery cells were analyzed. Figure 2 and Figure 3 The cell curve of the high-voltage lithium-ion battery containing nitrile in this example is shown. The battery operates well overall and its healthy life cycle reaches 900 weeks. Figure 4 The flowchart of battery preparation and battery testing in this embodiment is shown.
[0092] The high-voltage lithium-ion battery prepared according to the above preparation method has the beneficial effects of low cost, suitability for large-scale industrial production, improved high-voltage performance of the battery, high safety performance, and long healthy life cycle.
[0093] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An electrolyte, characterized in that: It includes a first electrolyte M1 and a second electrolyte M2; the first electrolyte M1 is used for primary injection and formation of the lithium-ion battery, and the second electrolyte M2 is used for secondary injection and circulation of the lithium-ion battery; The first electrolyte M1 includes a main salt A1, an additive A2 and a nitrile-containing main solvent B1; the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5-1.5 mol / L, and the volume of the nitrile-containing main solvent B1 accounts for 0.2-0.4 of the total volume of the electrolyte; The second electrolyte M2 includes a main salt A1 and a nitrile-containing main solvent B1, and the content is consistent with that in the first electrolyte M1; Wherein, the main salt A1 is lithium difluorooxalate borate.
2. The electrolyte according to claim 1, characterized in that The nitrile-containing main solvent B1 is at least one of acetonitrile, succinonitrile, adiponitrile, glutaronitrile, 1,3,6-hexanetricarboxylic acid nitrile, 1,3,5-pentanetricarboxylic acid nitrile and 2-fluoroadiponitrile.
3. The electrolyte according to claim 1, characterized in that The additive A2 is at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorophosphate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium perchlorate, and lithium hexafluoroarsenate.
4. The electrolyte according to claim 1, characterized in that The first electrolyte M1 and the second electrolyte M2 both further include: a film-forming agent B2 and a co-solvent B3; The volume ratio of the film-forming agent B2 and the co-solvent B3 to the total volume of the electrolyte is 0.2-0.4; The total volume fraction of the nitrile-containing main solvent B1, the film-forming agent B2 and the auxiliary solvent B3 is 1.
5. The electrolyte according to claim 4, characterized in that The film-forming agent B2 is at least one of ethylene carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate and fluorovinylene carbonate.
6. The electrolyte according to claim 4, characterized in that The cosolvent B3 is at least one of trifluoroethyl methyl carbonate, trifluoroethyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, bisfluoroethylene carbonate, and ethyl difluoroacetate.
7. A high voltage resistant lithium ion battery, characterized in that: The high-voltage lithium-ion battery comprises a battery cell and an electrolyte, wherein the electrolyte is the electrolyte as claimed in any one of claims 1 to 6, and the battery cell comprises a positive electrode sheet, a negative electrode sheet and a separator.
8. The high voltage lithium ion battery according to claim 7, characterized in that: The positive electrode sheet is at least one of lithium iron phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium manganese oxide, and lithium nickel oxide; The negative electrode is at least one of graphite, silicon carbon, and metallic lithium.
9. A method for preparing a high voltage resistant lithium ion battery, for preparing the high voltage resistant lithium ion battery as claimed in any one of claims 7 to 8, characterized in that: include: S1: Drying the main salt A1 and the additive A2 in a glove box, wherein the additive A2 is a lithium-containing compound; S2: The solvent is treated with molecular sieves to remove water in a glove box; The solvent includes a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3; S3: In a glove box, a first electrolyte M1 and a second electrolyte M2 are prepared using the treated solvent, a main salt A1 and an additive A2; wherein the first electrolyte M1 comprises a main salt A1, an additive A2, a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3, and the second electrolyte M2 comprises a main salt A1, a nitrile-containing main solvent B1, a film-forming agent B2 and a co-solvent B3, and the contents of the main salt A1 and the nitrile-containing main solvent B1 of the two electrolytes are consistent; the total molar concentration of the main salt A1 and the additive A2 in the electrolyte is 0.5 to 1.5 mol / L, the volume of the nitrile-containing main solvent B1, the film-forming agent B2 and the co-solvent B3 accounts for 0.2 to 0.4 of the total volume of the electrolyte, and the total volume fraction is 1; S4: In the clean room, assemble high-voltage lithium-ion battery cells, with the positive electrode sheet being C1 and the negative electrode sheet being C2, and select the first electrolyte M1 for the first injection packaging in the glove box, and use button cell / square shell cell / soft pack cell / cylindrical cell structure sealing; S5: pre-storing the high-voltage lithium-ion battery cell in the first electrolyte M1 for 24 hours and performing closed-cell formation at a preset temperature; S6: subtract the air bag from the formation battery and perform secondary injection with the second electrolyte M2; S7: placing the high-voltage lithium-ion battery cell in the second electrolyte M2 for 24 hours to obtain a high-voltage lithium-ion battery.
Citation Information
Patent Citations
High-voltage electrolyte, preparation method thereof and battery
CN116365038A
Cited By
Lithium ion battery electrolyte, electrolyte injection method thereof, and lithium ion battery
CN122931045A