Sensing element and preparation method thereof, gas sensing device and isobutanol detection method
By forming a sensing element with an appropriate thickness of MgO-SiO2 coating on the ceramic substrate and using a heating base in the gas sensing device, the large isobutanol detection equipment in the prior art is solved by the fact that the high cost, high cost and poor signal reproducibility of isobutanol in the prior art is solved. The problem of this method enables fast, sensitive and highly selective isobutanol detection and online monitoring.
Patent Information
- Application Number
- CN202411158465.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-12-13
AI Technical Summary
Although the existing isobutanol gas detection technologies such as gas chromatography and gas chromatography mass spectrometry are highly sensitive, the equipment is large in size and cost, making it difficult to achieve rapid on-site detection, and there is a problem of poor signal reproducibility.
Using a sensing element based on an MgO-SiO2 coating of suitable thickness, it is coated on the surface of the ceramic matrix by mixing nano MgO and SiO2 particles, binder and thickener, and after multiple scraping and drying Sintering to form a flat sensing element and a heating base is used in the gas sensing device to accommodate the sensing element to improve signal stability.
It realizes fast, highly sensitive and selective detection of isobutanol, has strong anti-interference ability, small equipment size, fast detection speed and low cost, and can accurately monitor isobutanol concentration online for a long time, solving the problem of poor signal reproducibility. .
Smart Images

Figure CN119125421A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of detection technology, and in particular to a sensor element and a preparation method thereof, a gas sensor device and an isobutanol detection method. Background Art
[0002] Isobutanol gas is irritating to the eyes, skin, mucous membranes and upper respiratory tract, so it should be stored in a well-ventilated place. In addition, high concentrations of isobutanol vapor can cause temporary anesthesia and form cavitation on the surface of the cornea. In the production line of the factory that produces isobutanol, there is a high concentration of isobutanol gas, and employees are easily exposed to the environment of high concentration of isobutanol gas, which endangers the health of employees. Therefore, the development of a sensor for online monitoring of isobutanol is of great significance for protecting the health of employees and online monitoring of the real-time concentration of isobutanol.
[0003] At present, the detection technology for isobutanol gas is mainly gas chromatography and gas chromatography-mass spectrometry. Gas chromatography and gas chromatography-mass spectrometry are highly sensitive and accurate, but the equipment is large, difficult to achieve rapid detection on site, and expensive.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The first object of the present invention is to provide a sensing element capable of detecting isobutanol rapidly, highly sensitively and highly selectively based on a MgO-SiO2 coating of suitable thickness.
[0006] The second object of the present invention is to provide a method for preparing the above-mentioned sensor element, which has simple steps.
[0007] The third object of the present invention is to provide a gas sensing device, which is equipped with a heating base that can accommodate a flat sensing element, effectively solving the problem of poor signal reproducibility between sensing elements due to easy detachment of materials.
[0008] The fourth object of the present invention is to provide a method for detecting isobutanol, which has small equipment size, fast detection speed, high sensitivity and selectivity, and low cost.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] The invention provides a sensing element, comprising a substrate and a coating arranged on the surface of the substrate; the coating comprises MgO and SiO2.
[0011] Furthermore, the thickness of the coating is greater than 3 μm.
[0012] Furthermore, the mass ratio of the MgO to the SiO2 is 1:(0.9-1.1).
[0013] Furthermore, the substrate includes a ceramic sheet.
[0014] The present invention also provides a method for preparing the sensor element as described above, comprising the following steps:
[0015] S1, mixing nano-MgO particles, nano-SiO2 particles, a binder, a thickener and a solvent, and heating them to obtain a slurry;
[0016] S2, coating the slurry on the surface of a substrate, drying it, and then sintering it to obtain the sensor element.
[0017] Further, step S1 includes at least one of the following features (1) to (3);
[0018] (1) The binder comprises ethyl cellulose;
[0019] (2) The thickener includes terpineol;
[0020] (3) The mass ratio of the nano-MgO particles, the nano-SiO2 particles, the binder and the thickener is 1: (0.9-1.1): (4.9-5.1): (92-94).
[0021] Furthermore, in step S2, the slurry is coated on the surface of the substrate, dried, and the coating and drying steps are repeated several times, and then sintered to obtain the sensor element.
[0022] Furthermore, the sintering includes: heating to 495-505° C. and maintaining the temperature for 3.9-4.1 hours.
[0023] The present invention further provides a gas sensing device, comprising: a reaction chamber; a heating base and the sensing element as described above are arranged in the reaction chamber; and the sensing element is placed flatly on the heating base.
[0024] The present invention also provides a method for detecting isobutanol, comprising using the gas sensor device as described above to detect the gas to be detected.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The sensor element provided by the present invention can detect isobutanol quickly, highly sensitively and selectively based on the MgO-SiO2 coating, and has strong anti-interference ability and high precision; the gas sensing device using the sensor element can accurately monitor isobutanol online for a long time.
[0027] 2. The present invention adopts a MgO-SiO2 coating of appropriate thickness, which significantly improves the gas-sensitive performance of the sensor element and has a higher catalytic luminescence intensity for isobutanol.
[0028] 3. The gas sensing device provided by the present invention is provided with a heating base capable of accommodating a flat sensing element, which can effectively solve the problem of poor signal reproducibility between sensing elements due to easy detachment of materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 Schematic diagram of a gas sensing device of the present invention.
[0031] Figure 2 Schematic diagram of the isobutanol detection system of the present invention.
[0032] Figure 3 XRD spectra of the MS3 composite film after sintering in Example 3 of the present invention, the MgO film after sintering in Comparative Example 1, and the SiO2 film after sintering in Comparative Example 2.
[0033] Figure 4 This is a SEM image of the surface of the MS3 composite membrane after sintering in Example 3 of the present invention.
[0034] Figure 5 This is the mapping result of the surface of the MS3 composite membrane after sintering in Example 3 of the present invention.
[0035] Figure 6 This is a SEM image of the cross section of the MS3 composite membrane after sintering in Example 3 of the present invention.
[0036] Figure 7 This is the effect of different scraping coat numbers on the catalytic luminescence intensity of the present invention.
[0037] Figure 8 Catalytic luminescence signals measured by 12 sensor elements prepared by the sensor element preparation method of Example 3 of the present invention.
[0038] Fig. 9 The present invention uses the gas sensor devices of Example 3, Comparative Example 1 and Comparative Example 2 to detect the catalytic luminescence responses of different gases.
[0039] Fig.10 Comparison of catalytic luminescence signals of the gas sensor devices of Example 3 of the present invention and Comparative Example 1.
[0040] Fig.11The present invention adopts the isobutanol detection method of Example 3 to detect the catalytic luminescence signal response curve of butanol gas with different concentrations.
[0041] Fig.12 This is a catalytic luminescence signal diagram of butanol gas of different concentrations detected 20 times in parallel using the isobutanol detection method of Example 3 of the present invention.
[0042] Fig.13 This is the linear curve of the gas sensor device of Example 3 of the present invention for isobutanol.
[0043] Reference numerals:
[0044] 11-substrate; 12-coating; 2-cavity; 21-heating base; 22-air inlet; 23-air outlet; 3-upper cover; 4-temperature controller; 5-photomultiplier tube; 51-filter; 52-cooler; 6-ultra-weak luminescence detection analyzer; 61-preamplifier; 62-pulse counter; 63-identifier; 64-data processing platform; 7-display; 81-syringe pump; 82-VOCs generator; 83-six-way valve; 84-air generator; 85-gas flow meter; 86-quantitative ring. DETAILED DESCRIPTION
[0045] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0046] A sensor element and a preparation method thereof, a gas sensor device and a method for detecting isobutanol according to an embodiment of the present invention are described in detail below.
[0047] See also Figure 1 In some embodiments of the present invention, a sensor element is provided, comprising a substrate 11 and a coating 12 disposed on the surface of the substrate; the coating 12 comprises MgO and SiO2.
[0048] The sensor element of the present invention can detect isobutanol rapidly, highly sensitively and highly selectively based on the MgO-SiO2 coating, and has strong anti-interference ability and high precision.
[0049] MgO has a strong catalytic luminescence response to a variety of VOCs (for example, isobutanol, n-butanol, n-propanol, cyclohexanone and 2-methylacrolein, etc.), SiO2 has only a very weak catalytic luminescence response to some gases, and does not produce catalytic luminescence signals for most gases; and after doping SiO2 into MgO in the present invention, the microstructure of MgO can be regulated, showing new catalytic properties, showing a strong catalytic luminescence response to isobutanol, and no obvious response to other gases, showing high selectivity for isobutanol.
[0050] In some embodiments of the present invention, the coating 12 is disposed on one side of the substrate 11, and the thickness of the coating 12 is greater than 3 μm; preferably, the thickness of the coating 12 is 8.6-13.4 μm.
[0051] The coating thickness is a key parameter affecting the gas-sensitive performance of membrane-type sensor elements. As the coating thickness increases, the catalytic luminescence intensity gradually increases; but when the coating reaches a certain thickness, the catalytic luminescence intensity tends to saturation and no longer increases significantly.
[0052] The catalyst surface has a fixed number of active sites, which increase with the increase of the amount of catalyst, that is, the catalytic luminescence signal increases with the thickness of the coating; when the amount of catalyst is large, the reaction system may be diffusion-limited, which means that the rate at which the reactant molecules reach the catalyst surface becomes the factor that limits the rate of the entire chemical reaction, that is, the reaction speed is limited by the diffusion rate of the substance, not the number of active sites of the catalyst. Therefore, the catalytic luminescence intensity no longer increases with the increase of the number of film layers.
[0053] In some embodiments of the present invention, the mass ratio of MgO to SiO2 is 1:(0.9-1.1); preferably, the mass ratio of MgO to SiO2 is 1:1.
[0054] In some embodiments of the present invention, the substrate 11 comprises a ceramic sheet.
[0055] In some specific embodiments of the present invention, the sensing element includes a ceramic sheet and a coating 12 disposed on the surface of the ceramic sheet, and the coating 12 includes MgO and SiO2.
[0056] In some embodiments of the present invention, a method for preparing the above-mentioned sensor element is also provided, comprising the following steps:
[0057] S1, mixing nano-MgO particles, nano-SiO2 particles, a binder, a thickener and a solvent, and heating them to obtain a slurry;
[0058] S2. Apply the slurry to the surface of the substrate 11, dry it, and then sinter it to obtain a sensor element.
[0059] The method for preparing the sensor element of the present invention has simple steps and is suitable for batch manufacturing of catalytic luminescence sensor elements with good precision.
[0060] In some embodiments of the present invention, in step S1, the binder includes but is not limited to ethyl cellulose.
[0061] In some embodiments of the present invention, in step S1, the thickener includes but is not limited to terpineol.
[0062] In some embodiments of the present invention, in step S1, the solvent includes but is not limited to ethanol.
[0063] In some embodiments of the present invention, in step S1, the mass ratio of nano-MgO particles, nano-SiO2 particles, binder and thickener is 1: (0.9-1.1): (4.9-5.1): (92-94).
[0064] In some embodiments of the present invention, in step S1, the temperature of the heating treatment is 75-85° C., and the time of the heating treatment is 2.5-3.5 hours.
[0065] In some embodiments of the present invention, in step S2, the slurry is coated on the surface of the substrate 11, dried, and then the coating and drying steps are repeated several times, and then sintered to obtain a sensor element; preferably, the coating and drying steps are repeated at least twice.
[0066] In some embodiments of the present invention, in step S2, the thickness of each coating is 3.0-5.0 μm; preferably, the thickness of each coating is 4.0-5.0 μm.
[0067] In some embodiments of the present invention, in step S2, the coating method includes scraping; preferably, the scraping speed is 10 to 20 mm / s; more preferably, the scraping speed is 13 to 18 mm / s.
[0068] The present invention adopts the coating method of scraping the slurry multiple times, which is conducive to forming a uniform coating.
[0069] In some embodiments of the present invention, in step S2, the drying temperature is 75-85° C., and the drying time is 10-30 min.
[0070] In the preparation method of the sensor element of the present invention, MgO-SiO2 composite films with different numbers of layers are obtained through several coating and drying steps; MgO-SiO2 is referred to as MS for short; coating and drying are performed once to obtain one layer of composite film, recorded as MS1; coating and drying are performed twice to obtain two layers of composite film, recorded as MS2; and so on, MS3 (three-layer composite film), MS4 (four-layer composite film), and so on.
[0071] In some embodiments of the present invention, in step S2, sintering includes: heating to 495-505°C and maintaining heat for 3.9-4.1 hours; typically but not restrictively, for example, in step S2, the sintering temperature can be 495°C, 500°C, 505°C or a range of any two thereof; the sintering time can be 3.9 hours, 4.0 hours, 4.1 hours or a range of any two thereof.
[0072] In some embodiments of the present invention, during the sintering process, the heating rate is 10-20° C. / min.
[0073] In some embodiments of the present invention, sintering includes vacuum sintering.
[0074] See also Figure 1 In some embodiments of the present invention, a gas sensing device is further provided, comprising: a reaction chamber; a heating base 21 and the above-mentioned sensing element are arranged in the reaction chamber; and the sensing element is placed flatly on the heating base 21 .
[0075] The gas sensing device provided by the present invention is provided with a heating base capable of accommodating a flat sensing element, and can effectively solve the problem of poor signal reproducibility between sensing elements due to easy shedding of materials.
[0076] In some embodiments of the present invention, the reaction chamber includes a cavity 2, an upper cover 3, a cavity shell and a temperature controller 4; the upper cover 3 and the cavity shell form a cavity 2; the cavity 2 is provided with an air inlet 22 and an air outlet 23; a heating base 21 and a sensor element are provided inside the cavity 2, and the sensor element is placed flatly on the heating base 21; the heating base 21 is connected to the temperature controller 4.
[0077] In some embodiments of the present invention, the gas sensing device further comprises: a catalytic luminescence detector, a data processing device and a display;
[0078] The catalytic luminescence detector includes a photomultiplier tube 5, which is in contact with the upper cover 3 of the reaction chamber, and a filter 51 is provided at the end of the photomultiplier tube 5 in contact with the upper cover 3 of the reaction chamber; the photomultiplier tube 5 is provided with a cooler 52;
[0079] The data processing device includes an ultra-weak luminescence detection analyzer 6 (BPCL-2), which includes a preamplifier 61, a pulse counter 62, an identifier 63 and a data processing platform 64 connected in sequence; the preamplifier 61 is connected to the photomultiplier tube 5, and the data processing platform 64 is connected to the display 7.
[0080] See also Figure 2 , in some embodiments of the present invention, there is also provided an isobutanol detection system, comprising a sampling unit and the above-mentioned gas sensing device;
[0081] The sampling unit includes an injection pump 81, a VOCs generator 82, an air generator 84, a gas flow meter 85, a six-way valve 83 and a quantitative ring 86; the injection pump 81, the VOCs generator 82, the six-way valve 83 and the air inlet 22 of the reaction chamber of the gas sensor device are connected in sequence; the VOCs generator 82, the air generator 84, the gas flow meter 85 and the six-way valve 83 are connected in sequence; the six-way valve 83 and the quantitative ring 86 are connected.
[0082] In some embodiments of the present invention, the syringe pump 81 comprises a precision push-pull syringe pump.
[0083] In some embodiments of the present invention, a method for detecting isobutanol is also provided, comprising using the above-mentioned gas sensor device to detect the gas to be detected.
[0084] In some embodiments of the present invention, the method for detecting isobutanol comprises the following steps:
[0085] After the gas to be tested is sent into the gas sensor device through the sampling unit, it reacts under the catalysis of the sensor element, and the luminous signal of the gas after the reaction is detected.
[0086] The isobutanol detection method of the present invention has high sensitivity to isobutanol, good selectivity, rapid response, rapid recovery, and can realize repeated detection in a short time; and has good stability, which provides a guarantee for online long-term accurate monitoring of isobutanol concentration.
[0087] In some embodiments of the present invention, in the detection method of isobutanol, in an atmosphere of carrier gas (air), the temperature of the heating base 21 is raised to 330±5°C by the temperature controller 4 and kept warm for 10±1 min to remove organic impurities and water, and then adjusted to a reaction temperature of 310±5°C to react. The photomultiplier tube 5 detects the luminescence signal and converts it into an electrical signal for transmission to the ultra-weak luminescence detection analyzer 6 for amplification and processing, and then read out and displayed by the display 7.
[0088] In some embodiments of the present invention, the negative high voltage of the photomultiplier tube 5 is 950±5V.
[0089] In some embodiments of the present invention, the sampling time of the six-way valve 83 is 40±5 s, and the injection time is 35±5 s.
[0090] In some embodiments of the present invention, the detection wavelength of the luminescent signal is 425 nm.
[0091] In some embodiments of the present invention, in the method for detecting isobutanol, the configuration of the gas sample to be tested comprises the following steps:
[0092] Load the liquid injection needle loaded with reagent into the syringe pump, adjust the injection rate of the syringe pump, the temperature of the vaporization unit of the VOCs generator (slightly higher than the boiling point of the liquid reagent) and the dilution gas flow rate to obtain the target concentration of VOCs gas. The gas concentration calculation formula is as follows: Where c is the gas concentration (mg / m 3 ), ρ is the density of the liquid reagent (kg / m 3 ), ν is the injection pump perfusion rate (μL / min), w is the purity of the liquid reagent (%), and V is the diluent gas flow rate (mL / min).
[0093] Examples 1 to 8
[0094] The method for preparing the sensor element provided in this embodiment comprises the following steps:
[0095] S1. Weigh 1.25g of ethyl cellulose, 0.25g of nano magnesium oxide particles and 0.25g of nano silicon dioxide particles respectively and disperse them in 20mL of anhydrous ethanol, and oscillate them ultrasonically for 10min; then add 25mL of pinene alcohol and stir them magnetically for 4h; finally, heat them at 80℃ on a heating table for 3h to obtain a viscous slurry;
[0096] S2. Soak a ceramic sheet of size 19 cm × 14 cm in anhydrous ethanol and ultrapure water for ultrasonic cleaning for 5 minutes to remove surface contamination. Let the cleaned ceramic sheet stand and dry. Place the dried ceramic sheet on the workbench of a scraper, set the scraping speed to 15 mm / s, and the scraping thickness to 4-5 μm. Drop the slurry on the ceramic sheet, press the start button on the scraper interface, and start the heating table to heat to 80°C and dry for 20 minutes after scraping. Repeat the above scraping and drying steps 0, 1, 2, 3, 4, 5, 6, 7, and 8 times respectively; obtain MS1 composite membrane, MS2 composite membrane, MS3 composite membrane, MS4 composite membrane, MS5 composite membrane, MS6 composite membrane, MS7 composite membrane, MS8 composite membrane; then placed in a vacuum muffle furnace for sintering, heated to 500°C at a rate of 15°C / min and kept warm for 4 hours, taken out after the temperature in the muffle furnace naturally cooled to room temperature, to obtain a coating; after cutting with a laser cutter, a circular sensor element with a diameter of 3 cm was obtained; the coating thickness of the sensor elements of Examples 1 to 5 were 3.9μm, 8.6μm, 13.4μm, 18.1μm, and 22.9μm, respectively.
[0097] The gas sensing device provided in this embodiment includes a reaction chamber, a catalytic luminescence detector, an ultra-weak luminescence detection analyzer 6 (BPCL-2) and a display 7;
[0098] The reaction chamber includes a rectangular cavity 2, an upper cover 3, a cavity shell and a temperature controller 4; the upper cover 3 and the cavity shell form the cavity 2; the cavity 2 is provided with an air inlet 22 and an air outlet 23, a heating base 21 and a sensor element are provided inside the cavity 2, and the sensor element is placed flat on the heating base 21; the heating base 21 is connected to the temperature controller 4;
[0099] The catalytic luminescence detector includes a photomultiplier tube 5, which is in contact with the upper cover 3 of the reaction chamber, and a filter 51 is provided at the end of the photomultiplier tube 5 in contact with the upper cover of the reaction chamber; the photomultiplier tube 5 is provided with a cooler 52;
[0100] The ultra-weak luminescence detection analyzer 6 includes a preamplifier 61 , a pulse counter 62 , an identifier 63 and a data processing platform 64 which are connected in sequence; the preamplifier 61 is connected to the photomultiplier tube 5 ; and the data processing platform 64 is connected to the display 7 .
[0101] The isobutanol detection system provided in this embodiment includes a sampling unit and a gas sensor device;
[0102] The sampling unit includes an injection pump 81, a VOCs generator 82, an air generator 84, a gas flow meter 85, a six-way valve 83 and a quantitative ring 86; the injection pump 81, the VOCs generator 82, the six-way valve 83 and the air inlet 22 of the reaction chamber of the gas sensor device are connected in sequence; the VOCs generator 82, the air generator 84, the gas flow meter 85 and the six-way valve 83 are connected in sequence; the six-way valve 83 and the quantitative ring 86 are connected.
[0103] The detection method of isobutanol provided in this embodiment comprises the following steps:
[0104] The sampling time of the six-way valve 83 is set to 40s, and the injection time is set to 35s. The gas to be tested is automatically sampled and injected through the sampling unit, and the gas to be tested is sent to the gas sensor device. In the atmosphere of carrier gas (air), the temperature of the heating base 21 is raised to 330°C and kept warm for 10 minutes through the temperature controller 4 to remove organic impurities and water, and then adjusted to a reaction temperature of 310°C to react. The photomultiplier tube 5 detects the luminescence signal, converts it into an electrical signal, transmits it to the ultra-weak luminescence detection analyzer 6 for amplification and processing, and is read out and displayed by the display 7.
[0105] Comparative Example 1
[0106] The preparation method of the sensor element provided in this comparative example refers to Example 3, except that in step S1, 0.25 g of nano-magnesium oxide particles and 0.25 g of nano-silicon dioxide particles are replaced with 0.5 g of nano-magnesium oxide particles; in step S2, a MgO film is obtained after scraping and drying.
[0107] The gas sensor device, isobutanol detection system and isobutanol detection method provided in this comparative example refer to Example 3.
[0108] Comparative Example 2
[0109] The preparation method of the sensor element provided in this comparative example refers to Example 3, except that in step S1, 0.25 g of nano-magnesium oxide particles and 0.25 g of nano-silicon dioxide particles are replaced with 0.5 g of nano-silicon dioxide particles; in step S2, a SiO2 film is obtained after scraping and drying.
[0110] The gas sensor device, isobutanol detection system and isobutanol detection method provided in this comparative example refer to Example 3.
[0111] Test Example 1
[0112] A small amount of the MS3 composite film sintered in Example 3, the MgO film sintered in Comparative Example 1, and the SiO2 film sintered in Comparative Example 2 was scraped off for XRD testing (Cu Kα ray, ), the result is as follows Figure 3 shown.
[0113] from Figure 3 It can be seen that the diffraction peaks of nano-MgO mainly appear at 2θ of 37.08°, 43.04°, 62.40°, 74.78° and 78.74°; these diffraction peaks correspond to the (111), (200), (220), (311) and (222) crystal planes of MgO respectively; the positions and relative intensities of these peaks are consistent with the MgO standard card PDF#04-006-7451, indicating that nano-MgO has a cubic crystal phase structure. The diffraction peaks of nano-SiO2 mainly show bulge-shaped hillocks in the range of 2θ of 15° to 40°, indicating that SiO2 is an amorphous structure. The main diffraction peaks of MgO and bulge-shaped hillocks of SiO2 appeared in the sintered MS3 composite film material, and the main diffraction peak position slightly shifted to the right, indicating that nano-MgO and nano-SiO2 are effectively doped together.
[0114] The sintered MS3 composite membrane containing ceramic sheets in Example 3 was broken into small pieces by liquid nitrogen and the surface and cross-section were tested by SEM. The results are as follows: Figure 4 , Figure 5 and Figure 6 shown.
[0115] Figure 4 This is the surface morphology of the MS3 composite membrane after sintering. The surface of the MS3 composite membrane after sintering is loose and porous, which is conducive to the diffusion of gas molecules in the material.
[0116] Figure 5This is the surface mapping result of the sintered MS3 composite film. The MS3 composite film contains Mg and Si elements, indicating that MgO and SiO2 are successfully doped.
[0117] Figure 6 This is the cross-section of the MS3 composite membrane after sintering. The overall thickness of the membrane layer is about 13.4 μm. The material is stacked on the substrate to form a dense membrane layer. The surface of the membrane layer is relatively flat, and no layered structure formed by multiple coatings is observed.
[0118] Test Example 2
[0119] The isobutanol detection methods of Examples 1 to 8 were used to detect the sample gas; the concentration was 263 mg / m 3 The isobutyl alcohol gas was used as the sample gas, and the catalytic luminescence signal was collected under the working conditions of working temperature of 310℃ and carrier gas flow rate of 550mL / min. The results are as follows Figure 7 shown.
[0120] from Figure 7 It can be seen that with the increase in the number of composite film layers, the catalytic luminescence intensity gradually increases; but when the composite film is accumulated to the fourth layer, the catalytic luminescence intensity tends to saturation and no longer increases significantly. This phenomenon is caused by the following reasons: the catalyst surface has a fixed number of active sites, and the active sites increase with the increase in the amount of catalyst. At this time, the catalytic luminescence signal increases with the increase in the number of film layers. When the amount of catalyst is large, the reaction system may be diffusion-limited, which means that the rate at which the reactant molecules reach the catalyst surface becomes a factor that limits the rate of the entire chemical reaction, that is, the reaction rate is limited by the diffusion rate of the substance, not the number of catalyst active sites. Therefore, the catalytic luminescence intensity no longer increases with the increase in the number of film layers, so at the third film layer, the catalytic luminescence signal reaches a saturation value.
[0121] In order to evaluate the precision of batch sensor elements, 12 sensor elements (serial numbers 1 to 12) were prepared by the preparation method of the sensor element in Example 3. The above 12 sensor elements were respectively used to measure the concentration of 263 mg / m 3 The isobutanol sample gas was used, with the operating temperature being 310°C and the carrier gas flow rate being 550 mL / min. Figure 8 shown.
[0122] The mass production of high-precision sensor elements is crucial for practical applications. The relative standard deviation (RSD) of the catalytic luminescence signals measured by the 12 sensor elements of the present invention is only 1.8%, indicating that the sensor elements of the present invention have good precision and that the scraping method is suitable for mass production of catalytic luminescence sensor elements with good precision.
[0123] It is very important that the gas sensor device has excellent sensitivity and selectivity. The gas sensor devices of Example 3, Comparative Example 1 and Comparative Example 2 were used to test the catalytic luminescence response of 34 VOCs. The results are as follows: Fig. 9 The catalytic luminescence signals of the gas sensor device of Example 3 and Comparative Example 1 for 10 kinds of VOCs are shown in FIG. Fig.10 shown.
[0124] Fig. 9 Among them, 1: isobutyl alcohol; 2: n-butyl alcohol; 3: sec-butyl alcohol; 4: tert-butyl alcohol; 5: isobutylaldehyde; 6: methanol; 7: acetone; 8: cyclopropylcarbinol; 9: n-pentanol; 10: n-propyl alcohol; 11: ethanol; 12: isopropyl alcohol; 13: 2-methylacrolein; 14: formaldehyde; 15: cyclohexanone; 16: 4-heptanone; 17: vinyl acetate; 18: ethyl acetate; 19: methyl acetate; 20: acetic acid; 21: phenylacetaldehyde; 22: acetophenone; 23: butyl phenone; 24: ethylbenzene; 25: m-xylene; 26: p-xylene; 27: benzaldehyde; 28: benzene; 29: 1-hexene; 30: acetonitrile; 31: n-pentane; 32: n-hexane; 33: carbon dioxide; 34: carbon monoxide.
[0125] from Fig. 9 It can be seen that the MgO film has a strong catalytic luminescence response to a variety of VOCs (isobutanol, n-butanol, n-propanol, cyclohexanone and 2-methylacrolein, etc.), the SiO2 film has only a very weak catalytic luminescence response to some gases, and no catalytic luminescence signal is generated for most gases, while the MS3 composite film shows a strong catalytic luminescence response to isobutanol, and no obvious response to other gases. This shows that after MgO doped SiO2, the selectivity of the composite film material for isobutanol has been greatly improved.
[0126] from Fig. 9 and Fig.10 It can be seen that except for the signal decrease of isobutanol and isobutyraldehyde at 23% to 31%, the signal decrease of other gases exceeded 85%, indicating that the MS3 composite membrane has excellent catalytic luminescence selectivity for isobutanol gas. MgO may have abundant surface active sites, so it exhibits high catalytic activity in catalytic oxidation reactions. SiO2 is relatively inert. After MgO doped with SiO2, the microstructure of MgO can be regulated, and the MgO-SiO2 composite membrane formed exhibits new catalytic properties.
[0127] The isobutanol detection method in Example 3 was used to determine the concentration of 98.6 mg / m 3 , 195.6mg / m 3 , 290.2mg / m 3 , 342.9mg / m 3498.6mg / m 3 The catalytic luminescence signal response curve is as follows: Fig.11 shown.
[0128] from Fig.11 It can be seen that the catalytic luminescence signal increases with the increase of isobutanol concentration, and the curve shape becomes more sharp from flat as the concentration of isobutanol increases. The catalytic luminescence signal reaches a maximum value 10s after sample injection, and the half-life is about 3.5s, which shows that the detection method of isobutanol of the present invention responds quickly to isobutanol, has the advantages of fast determination speed and rapid recovery, and can achieve repeated detection in a short time.
[0129] The isobutanol detection method in Example 3 was used to measure the concentration of 263.3 mg / m 3 , 305.4mg / m 3 and 437 mg / m 3 The results are as follows: Fig.12 shown.
[0130] from Fig.12 It can be seen that the RSDs of the detection results are 1.2%, 2.2% and 1.9%, respectively, indicating that the detection method of isobutanol of the present invention has good stability, which provides a guarantee for online long-term accurate monitoring of isobutanol concentration.
[0131] The linear range and detection limit are key indicators for measuring the performance of a gas sensor device. The gas sensor device of Example 3 was used to detect isobutanol gas with a concentration of 25.1 to 1003.8 mg / m3 according to the isobutanol detection method. The measured response intensity was linearly regressed against the concentration. The results are as follows: Fig.13 shown.
[0132] from Fig.13 It can be seen that the gas sensor device using the MS3 composite membrane has a high sensitivity when the isobutanol concentration is 25.1-1003.8 mg / m 3 The catalytic luminescence signal showed a good linear relationship with the isobutanol concentration within the range, and the linear regression equation was S = 274.5c-7509.2, where S was the response intensity and c was the isobutanol concentration; the detection limit LOD was 8.4 mg / m 3 .
[0133] In order to further verify the practical application value of the gas sensing device, an interference experiment was designed to determine the recovery rate. 3 ) was mixed with n-butanol, sec-butanol, tert-butanol, methanol, ethanol and acetone in concentration ratios of 1:10, 1:30, 1:50 and 1:100, and the isobutanol detection method of Example 3 was used for parallel testing 3 times. The results are shown in Table 1.
[0134] Table 1
[0135]
[0136]
[0137] As can be seen from Table 1, when isobutanol coexists with 100 times its content of n-butanol, sec-butanol, tert-butanol, ethanol, and acetone, its recovery rate is between 94.3% and 112.0%, indicating that these gases hardly interfere with the determination of isobutanol; when it coexists with 100 times its content of methanol, the isobutanol recovery rate is 136.9%, indicating that methanol causes significant positive interference; but when it coexists with 50 times its content of methanol, the isobutanol recovery rate is 109.6%, which fully demonstrates that the gas sensor device of the present invention has good anti-interference ability.
[0138] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A sensor element, characterized in that: It comprises a substrate and a coating arranged on the surface of the substrate; the coating comprises MgO and SiO2.
2. The sensor element according to claim 1, characterized in that The thickness of the coating is greater than 3 μm.
3. The sensor element according to claim 1, characterized in that The mass ratio of the MgO to the SiO2 is 1:(0.9-1.1).
4. The sensor element according to claim 1, characterized in that The substrate includes a ceramic sheet.
5. The method for preparing the sensor element according to any one of claims 1 to 4, characterized in that: The steps include: S1, mixing nano-MgO particles, nano-SiO2 particles, a binder, a thickener and a solvent, and heating them to obtain a slurry; S2, coating the slurry on the surface of a substrate, drying it, and then sintering it to obtain the sensor element.
6. The method for preparing the sensor element according to claim 5, characterized in that: In step S1, at least one of the following features (1) to (3) is included; (1) The binder comprises ethyl cellulose; (2) The thickener includes terpineol; (3) The mass ratio of the nano-MgO particles, the nano-SiO2 particles, the binder and the thickener is 1: (0.9-1.1): (4.9-5.1): (92-94).
7. The method for preparing the sensor element according to claim 5, characterized in that: In step S2, the slurry is coated on the surface of the substrate, dried, and the coating and drying steps are repeated several times, and then sintered to obtain the sensor element.
8. The method for preparing the sensor element according to claim 5, characterized in that: In step S2, the sintering includes: heating to 495-505°C and maintaining the temperature for 3.9-4.1 hours.
9. A gas sensing device, characterized in that: include: Reaction chamber; The reaction chamber is provided with a heating base and a sensing element according to any one of claims 1 to 5; The sensing element is placed flatly on the heating base.
10. A method for detecting isobutanol, characterized in that: The method comprises using the gas sensor device as claimed in claim 9 to detect the gas to be detected.
Citation Information
Cited By
Photoelectric dual-mode virtual electronic nose