Sweat corrosion resistant PUR hot melt adhesive and preparation method thereof

By crosslinking raw materials such as fluoropolyether polyol and end-hydroxypolybutadiene in PUR hot melt adhesive, the problem of sweat and sebum corrosion in electronic wearable devices is solved, and the service life and bonding strength of the device are significantly improved. .

CN119144273AActive Publication Date: 2024-12-17FOSHAN JIWEI NEW MATERIAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411382041.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-17
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

The existing PUR hot melt adhesives in electronic wearable devices have reduced bond strength after long-term contact with the human body, sweat and sebum penetrate, resulting in degumming and equipment damage, and shortened life.

Method used

The fluorine-containing polyether polyol, end-hydroxy polybutadiene and diisocyanate are used for cross-linking to form a polyurethane hot melt adhesive with excellent resistance to sweat and sebum corrosion. The adhesive strength is improved by introducing organic fluorine and functional modification. Chemical corrosion resistance.

Benefits of technology

It significantly improves the sweat and sebum corrosion resistance of polyurethane hot melt adhesive, extends the service life of electronic wearable devices, and maintains good bonding strength and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070135390000091
    Figure BDA0005070135390000091
Patent Text Reader

Abstract

The invention relates to a sweat corrosion resistant PUR hot melt adhesive and a preparation method thereof, and relates to the field of hot melt adhesives. The sweat corrosion resistant PUR hot melt adhesive is prepared from the following raw materials in parts by weight: 35 to 42 parts of fluorine-containing polyether polyol; 20 to 30 parts of polyester polyol; 12 to 17 parts of hydroxyl-terminated polybutadiene; 16 to 20 parts of diisocyanate; 0.05 to 0.2 part of a catalyst; 10 to 18 parts of acrylic resin; and 0.1 to 0.5 part of an antioxidant. The sweat and sebum corrosion resistance of the PUR hot melt adhesive can be improved, and the service life of electronic wearable equipment is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of hot melt adhesives, in particular to a PUR hot melt adhesive resistant to sweat corrosion and a preparation method thereof. Background Art

[0002] PUR hot melt adhesive, full name is moisture curing reactive polyurethane hot melt adhesive, the main component is terminal isocyanate polyurethane prepolymer. PUR hot melt adhesive contains polar and chemically active urethane group (-NHCOO-) or isocyanate group (-NCO) in the molecular structure, and has excellent temperature resistance, bonding strength, chemical corrosion resistance and aging resistance with materials containing active hydrogen. It is widely used in packaging, wood processing, textiles, book binding, electrical and electronic fields.

[0003] As wearable products become more and more intelligent, electronic wearable devices are growing rapidly. The internal parts of electronic wearable devices are connected with glue to form protection. PUR hot melt adhesive has the advantages of environmental protection, energy saving, fast positioning, and provides high initial adhesion strength. It is used in the bonding of electronic wearable devices.

[0004] However, when the existing PUR hot melt adhesive is used in electronic wearable devices, due to long-term contact with the human body, the sweat and oil secreted by the body slowly penetrate into the interior of the electronic wearable devices. The existing PUR hot melt adhesive has poor resistance to sweat and sebum corrosion. After sweat penetrates, it will destroy the bonding strength, causing debonding or even damage, thereby shortening the life of the electronic wearable devices. Summary of the invention

[0005] In order to improve the performance of PUR hot melt adhesive in resisting sweat and sebum corrosion and prolong the service life of electronic wearable devices, the present application provides a PUR hot melt adhesive resistant to sweat corrosion and a preparation method thereof.

[0006] The present application provides a sweat-resistant PUR hot melt adhesive and a preparation method thereof, which adopts the following technical scheme: In a first aspect, a sweat-resistant PUR hot melt adhesive comprises the following raw materials in parts by weight: 35-42 parts of fluorinated polyether polyol; 20-30 parts of polyester polyol; 12-17 parts of hydroxy-terminated polybutadiene; 16-20 parts of diisocyanate; Catalyst 0.05-0.2 parts; Acrylic resin 10-18 parts; Antioxidant 0.1-0.5 parts.

[0007] By adopting the above technical scheme, terminal hydroxyl polybutadiene is selected to modify the polyurethane hot melt adhesive. Terminal hydroxyl polybutadiene has the advantages of good oil resistance, excellent water resistance and aging resistance. The hydroxyl group at the end of the molecular chain is cross-linked and cured with diisocyanate, and the obtained polyurethane hot melt adhesive has excellent acid and alkali resistance, sweat corrosion resistance and good bonding strength. By adopting fluorine-containing polyether polyol, organic fluorine is introduced into the soft segment to make the polyurethane hot melt adhesive contain organic fluorine. The introduction of fluorine element is conducive to improving the oil and water repellency and chemical corrosion resistance of the polyurethane hot melt adhesive. The polyurethane hot melt adhesive is formed by cross-linking fluorine-containing polyether polyol, polyester polyol, terminal hydroxyl polybutadiene and diisocyanate, which has good sweat and sebum corrosion resistance, is suitable for the bonding of electronic wearable devices, and prolongs the service life of electronic wearable devices.

[0008] Optionally, the number average molecular weight of the fluorine-containing polyether polyol is 1500-3000, and the fluorine content is 10-30%.

[0009] By adopting the above technical solution, too high fluorine content will affect the toughness and elongation at break of the polyurethane hot melt adhesive. Controlling the number average molecular weight and fluorine content of the fluorinated polyether polyol will make the polyurethane hot melt adhesive have good fluidity and toughness and be able to withstand certain deformation.

[0010] Optionally, the fluorinated polyether polyol is prepared from the following raw materials in parts by weight: 20-30 parts of isophorone diisocyanate; 25-40 parts of octafluoropentanol; 85-98 parts of glycidol; 42-47 parts of tetrahydrofuran; Boron trifluoride etherate 0.3-0.8 parts; 1-3 parts of ethylene glycol; 65-72 parts of solvent.

[0011] By adopting the above technical scheme, isophorone diisocyanate, octafluoropentanol and glycidol are selected to react to form a fluorinated epoxy compound, which is then reacted with tetrahydrofuran to form a fluorinated polyether polyol. The fluorinated polyether polyol contains isocyanate groups, which can react with polyester polyols and terminal hydroxyl polybutadiene during cross-linking, thereby increasing the cross-linking density of the polyurethane system, which is beneficial to improving the bonding strength and sweat and sebum corrosion resistance of the polyurethane hot melt adhesive.

[0012] Optionally, the hydroxy-terminated polybutadiene is modified hydroxy-terminated polybutadiene, and the modified hydroxy-terminated polybutadiene is prepared from the following raw materials in parts by weight: 10-14 parts of hydroxyl-terminated polybutadiene; 1.5-2.2 parts of 1-chloro-2,4-dinitrobenzene; 20-25 parts of dichloromethane; 1.7-2 parts of sodium hydroxide.

[0013] By adopting the above technical scheme, 1-chloro-2,4-dinitrobenzene is selected to functionally modify the terminal carbon atom of the terminal hydroxyl polybutadiene, and phenyl and nitro groups are introduced. The benzene ring has a rigid structure, and the isocyanate group and the nitro group produce hydrogen bonds, which is beneficial to increase the crosslinking density of the polyurethane system and improve the mechanical properties and bonding strength of the polyurethane hot melt adhesive.

[0014] Optionally, the polyester polyol is polymerized from adipic acid and at least one diol selected from the group consisting of 1,4-butanediol, neopentyl glycol, ethylene glycol, diethylene glycol and 1,6-hexanediol.

[0015] Optionally, the diisocyanate is selected from one or more of diphenylmethane diisocyanate, toluene diisocyanate, xylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, and carbodiimide-modified diisocyanate.

[0016] Optionally, the catalyst is one or more of dibutyltin dilaurate, stannous octoate, dibutyl acetate, triethylenediamine, and bismorpholinyl diethyl ether.

[0017] In a second aspect, the present application discloses a method for preparing a sweat-resistant PUR hot melt adhesive, comprising the following steps: adding polyester polyol, fluorinated polyether polyol, hydroxyl-terminated polybutadiene and acrylic resin into a reaction kettle, stirring and mixing evenly, heating to 120-130° C., vacuum degree of -0.095-0.05 MPa, and dehydrating for 2-2.5 hours; Cool down to 75-80℃, add diisocyanate and catalyst, and react at 85-90℃ for 2-3h; add antioxidant, and stir rapidly at 110-120℃ for 20-30min; The material is quickly discharged and packaged under nitrogen protection to obtain PUR hot melt adhesive resistant to sweat corrosion.

[0018] By adopting the above technical scheme, the preparation process is relatively simple. Under the synergistic effect of multiple raw materials, the prepared PUR hot melt adhesive improves the acid, alkali, sweat and sebum resistance while ensuring the bonding strength and mechanical properties.

[0019] Optionally, the fluorinated polyether polyol is prepared by the following steps: Put isophorone diisocyanate and octafluoropentanol into a reactor, react at 40-45°C for 2-2.5h, raise the temperature to 65-68°C, add glycidol and continue to react for 2-2.5h to obtain a fluorine-containing epoxy compound; Add solvent, ethylene glycol and boron trifluoride etherate to the reaction kettle, stir at 0-2°C for 15-20 minutes, add fluorinated epoxy compound and tetrahydrofuran dropwise, the temperature should not exceed 5°C, and react for 5-6 hours; Add a small amount of deionized water and stir for 20-30 minutes to stop the reaction. Wash with deionized water until the organic phase is neutral. Use a separatory funnel to separate the layers statically. Take the lower organic phase and distill under reduced pressure to obtain fluorinated polyether polyol.

[0020] By adopting the above technical scheme, isophorone diisocyanate, octafluoropentanol and glycidol are selected to react to form a fluorinated epoxy compound, which is then reacted with tetrahydrofuran to form a fluorinated polyether polyol. Ethylene glycol and boron trifluoride etherate are used as a co-initiator and a cationic initiator, respectively, so that the polymerization process is controllable and the molecular weight of the fluorinated polyether polyol can be conveniently controlled.

[0021] Optionally, when the hydroxy-terminated polybutadiene is modified hydroxy-terminated polybutadiene, the preparation steps are as follows: Weigh terminal hydroxyl polybutadiene and dichloromethane in a stirring kettle, stir to dissolve, add sodium hydroxide under nitrogen protection and stir for 20-30 minutes, add 1-chloro-2,4-dinitrobenzene to the stirring kettle, stir for 2-3 hours, and then react at room temperature for 10-12 hours, wash with anhydrous methanol and n-hexane, separate by static stratification, and obtain modified terminal hydroxyl polybutadiene after distillation.

[0022] By adopting the technical scheme, the preparation process is simple and the yield of the modified hydroxy-terminated polybutadiene is high.

[0023] In summary, this application has the following beneficial effects: 1. Use terminal hydroxyl polybutadiene to modify the polyurethane hot melt adhesive. Terminal hydroxyl polybutadiene has the advantages of good oil resistance, excellent water resistance and aging resistance. The hydroxyl group at the end of the molecular chain is cross-linked and cured with diisocyanate. The obtained polyurethane hot melt adhesive has excellent acid and alkali resistance, sweat corrosion resistance and good bonding strength. Use fluorine-containing polyether polyols, introduce organic fluorine into the soft segment to make the polyurethane hot melt adhesive contain organic fluorine. The introduction of fluorine element is conducive to improving the oil and water repellency and chemical corrosion resistance of the polyurethane hot melt adhesive. The polyurethane hot melt adhesive is formed by cross-linking fluorine-containing polyether polyols, polyester polyols, terminal hydroxyl polybutadiene and diisocyanate. It has good sweat and sebum corrosion resistance, is suitable for the bonding of electronic wearable devices, and extends the service life of electronic wearable devices.

[0024] 2. Isophorone diisocyanate, octafluoropentanol, and glycidol are used to react to form a fluorinated epoxy compound, which is then reacted with tetrahydrofuran to form a fluorinated polyether polyol. The fluorinated polyether polyol contains an isocyanate group, which can react with polyester polyols and terminal hydroxyl polybutadiene during cross-linking, thereby increasing the cross-linking density of the polyurethane system, which is beneficial to improving the bonding strength of the polyurethane hot melt adhesive and its resistance to sweat and sebum corrosion.

[0025] 3. 1-Chloro-2,4-dinitrobenzene is used to functionally modify the terminal carbon atoms of terminal hydroxyl polybutadiene, introducing phenyl and nitro groups. The benzene ring is a rigid structure, and the isocyanate group and the nitro group produce hydrogen bonds, which is beneficial to increase the crosslinking density of the polyurethane system and improve the mechanical properties and bonding strength of the polyurethane hot melt adhesive. DETAILED DESCRIPTION

[0026] The present application is further described in detail below in conjunction with Examples 1-8 and Comparative Examples 1-2.

[0027] Preparation Example Preparation Example 1 The preparation of fluorinated polyether polyol includes the following raw materials in parts by weight: 20 parts of isophorone diisocyanate; 25 parts of octafluoropentanol; 85 parts of glycidol; 42 parts of tetrahydrofuran; 0.3 parts of boron trifluoride etherate; 1 part of ethylene glycol; 65 parts of solvent, dichloromethane is selected as the solvent.

[0028] The fluorinated polyether polyol is prepared by the following steps: Put isophorone diisocyanate and octafluoropentanol into a reactor, react at 40°C for 2 hours, raise the temperature to 65°C, add glycidol and continue to react for 2 hours to obtain a fluorinated epoxy compound; Add solvent, ethylene glycol and boron trifluoride etherate to the reaction kettle, stir at 0°C for 15 minutes, add fluorinated epoxy compound and tetrahydrofuran dropwise, the temperature of the addition process should not exceed 5°C, and react at 0°C for 5 hours; Add a small amount of deionized water and stir for 20 minutes to stop the reaction. Wash with deionized water twice the volume of the reaction solution and stir for 5 minutes until the organic phase is neutral. Use a separatory funnel to separate the reaction solution into layers, take the lower organic phase and distill it under reduced pressure to obtain fluorinated polyether polyol.

[0029] The molecular weight of the prepared fluorine-containing polyether polyol is 1600 and the fluorine content is 12%.

[0030] Preparation Example 2 The preparation of fluorinated polyether polyol includes the following raw materials in parts by weight: 30 parts of isophorone diisocyanate; 40 parts of octafluoropentanol; 98 parts of glycidol; 47 parts of tetrahydrofuran; 0.8 parts of boron trifluoride etherate; 3 parts of ethylene glycol; 72 parts of solvent, 52 parts of dichloromethane and 20 parts of chloroform are selected as the solvent.

[0031] The fluorinated polyether polyol is prepared by the following steps: Put isophorone diisocyanate and octafluoropentanol into a reactor, react at 45°C for 2.5 hours, heat to 68°C, add glycidol and continue to react for 2.5 hours to obtain a fluorinated epoxy compound; Add solvent, ethylene glycol and boron trifluoride etherate to the reaction kettle, stir at 2°C for 20 minutes, add fluorinated epoxy compound and tetrahydrofuran dropwise, the temperature of the addition process should not exceed 5°C, and react at 2°C for 6 hours; Add a small amount of deionized water and stir for 30 minutes to stop the reaction. Wash with deionized water twice the volume of the solution after the reaction. Stir for 5 minutes until the organic phase is neutral. Use a separatory funnel to separate the solution after the reaction. Take the lower organic phase and distill it under reduced pressure to obtain fluorinated polyether polyol.

[0032] The molecular weight of the prepared fluorine-containing polyether polyol is 2200 and the fluorine content is 23%.

[0033] Preparation Example 3 The modified hydroxy-terminated polybutadiene is prepared from the following raw materials in parts by weight: 10 parts of hydroxy-terminated polybutadiene; 1.5 parts of 1-chloro-2,4-dinitrobenzene; 20 parts of dichloromethane; 1.7 parts of sodium hydroxide.

[0034] The preparation method of modified hydroxy-terminated polybutadiene comprises the following steps: Weigh terminal hydroxyl polybutadiene and dichloromethane in a stirring kettle, stir to dissolve, add sodium hydroxide under nitrogen protection and stir for 20 minutes, add 1-chloro-2,4-dinitrobenzene to the stirring kettle, stir for 2 hours and then react at room temperature for 10 hours, wash with anhydrous methanol and n-hexane several times, pour into a separating funnel, separate by static stratification, and obtain modified terminal hydroxyl polybutadiene after distillation.

[0035] Preparation Example 4 The modified hydroxy-terminated polybutadiene is prepared from the following raw materials in parts by weight: 14 parts of hydroxy-terminated polybutadiene; 2.2 parts of 1-chloro-2,4-dinitrobenzene; 25 parts of dichloromethane; 2 parts of sodium hydroxide.

[0036] The preparation method of modified hydroxy-terminated polybutadiene comprises the following steps: Weigh terminal hydroxyl polybutadiene and dichloromethane in a stirring kettle, stir to dissolve, add sodium hydroxide under nitrogen protection and stir for 30 minutes, add 1-chloro-2,4-dinitrobenzene to the stirring kettle, stir for 3 hours and then react at room temperature for 12 hours, wash with anhydrous methanol and n-hexane several times, pour into a separating funnel, separate by static stratification, and obtain modified terminal hydroxyl polybutadiene after distillation. Example

[0037] Example 1 The sweat-resistant PUR hot melt adhesive comprises the following raw materials in parts by weight: 35 parts of fluorine-containing polyether polyol, specifically BHD-1801F, with a number average molecular weight of 3000 and a fluorine content of 25%, purchased from Beijing Beihua Engineering Technology Co., Ltd.; 20 parts of polyester polyol, specifically a polyester polyol with an average molecular weight of 2000 prepared by polymerization of adipic acid and 1,6-hexanediol; 12 parts of hydroxy-terminated polybutadiene; 16 parts of diisocyanate, specifically hexamethylene diisocyanate; 0.05 parts of catalyst, specifically dibutyltin dilaurate; 10 parts of acrylic resin, specifically BASF 682 acrylic resin; 0.1 part of antioxidant, specifically antioxidant 1010 is selected.

[0038] The preparation method of the sweat-resistant PUR hot melt adhesive comprises the following steps: Add polyester polyol, fluorinated polyether polyol, hydroxyl-terminated polybutadiene and acrylic resin into a reaction kettle, stir and mix evenly, heat to 120°C, set the vacuum degree to -0.095MPa, and dehydrate for 2h; Cool down to 75°C, add diisocyanate and catalyst, and react at 85°C for 2h; add antioxidant, and stir rapidly at 110°C for 20min; The material is quickly discharged and packaged under nitrogen protection to obtain PUR hot melt adhesive resistant to sweat corrosion.

[0039] Example 2 The sweat-resistant PUR hot melt adhesive comprises the following raw materials in parts by weight: 42 parts of fluorinated polyether polyol, specifically FX1402, with a number average molecular weight of 2400 and a fluorine content of 15%, purchased from Tianjin Feixin Trading Co., Ltd.; 30 parts of polyester polyol, specifically a polyester polyol with an average molecular weight of 2400 prepared by polymerization of adipic acid and neopentyl glycol; 17 parts of hydroxy-terminated polybutadiene; 20 parts of diisocyanate, specifically diphenylmethane diisocyanate; 0.2 parts of catalyst, specifically bismorpholinyl diethyl ether; 18 parts of acrylic resin, specifically Xinlian 902 acrylic resin; 0.5 parts of antioxidant, specifically antioxidant 168 is selected.

[0040] The preparation method of the sweat-resistant PUR hot melt adhesive comprises the following steps: Add polyester polyol, fluorinated polyether polyol, hydroxyl-terminated polybutadiene and acrylic resin into a reaction kettle, stir and mix evenly, heat to 130°C, set the vacuum degree to 0.05MPa, and dehydrate for 2.5h; Cool down to 80°C, add diisocyanate and catalyst, and react at 90°C for 3h; add antioxidant, and stir rapidly at 120°C for 30min; The material is quickly discharged and packaged under nitrogen protection to obtain PUR hot melt adhesive resistant to sweat corrosion.

[0041] Example 3 The sweat-resistant PUR hot melt adhesive comprises the following raw materials in parts by weight: 38 parts of fluorinated polyether polyol, specifically FX3302, with a number average molecular weight of 2000 and a fluorine content of 20%, purchased from Tianjin Feixin Trading Co., Ltd.; 25 parts of polyester polyol, specifically a polyester polyol with an average molecular weight of 2800 prepared by polymerization of adipic acid, 1,4-butanediol and diethylene glycol; 14 parts of hydroxy-terminated polybutadiene; 18 parts of diisocyanate, specifically toluene diisocyanate; 0.13 parts of catalyst, specifically stannous octoate; 15 parts of acrylic resin, specifically Hanhua Soluryl-70 acrylic resin; 0.3 parts of antioxidant, specifically antioxidant 1010 is selected.

[0042] The preparation method of the sweat-resistant PUR hot melt adhesive comprises the following steps: Add polyester polyol, fluorinated polyether polyol, hydroxyl-terminated polybutadiene and acrylic resin into a reaction kettle, stir and mix evenly, heat to 125°C, set the vacuum degree to 0.03MPa, and dehydrate for 2h; Cool down to 78°C, add diisocyanate and catalyst, and react at 87°C for 3h; add antioxidant, and stir rapidly at 115°C for 25min; The material is quickly discharged and packaged under nitrogen protection to obtain PUR hot melt adhesive resistant to sweat corrosion.

[0043] Example 4 The difference between this embodiment and embodiment 1 is that the fluorine-containing polyether polyol in the raw material is different.

[0044] The fluorinated polyether polyol of this embodiment is the fluorinated polyether polyol prepared in Preparation Example 1.

[0045] Example 5 The difference between this embodiment and embodiment 1 is that the fluorine-containing polyether polyol in the raw material is different.

[0046] The fluorinated polyether polyol of this embodiment is the fluorinated polyether polyol prepared in Preparation Example 2.

[0047] Example 6 The difference between this embodiment and embodiment 1 is that the hydroxy-terminated polybutadiene in the raw material is different.

[0048] The hydroxy-terminated polybutadiene in this embodiment is the modified hydroxy-terminated polybutadiene prepared in Preparation Example 3.

[0049] Example 7 The difference between this embodiment and embodiment 1 is that the hydroxy-terminated polybutadiene in the raw material is different.

[0050] The hydroxy-terminated polybutadiene in this embodiment is the modified hydroxy-terminated polybutadiene prepared in Preparation Example 4.

[0051] Example 8 The difference between this embodiment and embodiment 1 is that the fluorine-containing polyether polyol and the terminal hydroxyl polybutadiene in the raw materials are different.

[0052] The fluorinated polyether polyol of this embodiment is the fluorinated polyether polyol prepared in Preparation Example 2, and the terminal hydroxyl polybutadiene is the modified terminal hydroxyl polybutadiene prepared in Preparation Example 3.

[0053] Comparative Example Comparative Example 1 The difference between this comparative example and Example 1 is that no hydroxy-terminated polybutadiene is added to the hot melt adhesive raw material.

[0054] Comparative Example 2 The difference between this comparative example and Example 1 is that in this comparative example, polytetramethylene ether diol with a molecular weight of 2000 is selected to replace the fluorine-containing polyether polyol.

[0055] Performance Testing The PUR hot melt adhesives prepared in Examples 1-8 and Comparative Examples 1-2 were tested. When the PUR hot melt adhesive was used in the process, the heating system was first turned on, the temperature was set to 100-130°C, and the adhesive was applied with a glue gun. The adhesive application process was ensured to be completed within the open time, and then the test was performed according to the regulations.

[0056] The bonding strength, sweat corrosion resistance and sebum corrosion resistance of the PUR hot melt adhesive were tested, and the test results are recorded in Table 1.

[0057] Bonding strength: Refer to GB / T 7124-2008 to prepare samples to test the tensile shear strength of PUR hot melt adhesive bonded to PC materials, where the samples are cured for 7 days at 25°C and 50% RH.

[0058] Sweat corrosion resistance: PUR hot melt adhesive was used to stick PC material to prepare samples, the samples were immersed in artificial simulated sweat, packaged (sealed) with PE bags, immersed in a constant temperature and humidity chamber at 25°C, 50% RH for 7 days, taken out and dried, the corresponding shear strength was tested, and the attenuation rate 1 was calculated.

[0059] Sebum corrosion resistance: PUR hot melt adhesive is pasted to PC material to prepare samples, the samples are immersed in artificial sebum that conforms to ASTMD4265-14, packaged (sealed) with PE bags, immersed in a constant temperature and humidity chamber at 25°C, 50% RH for 7 days, taken out and dried, the corresponding shear strength is tested, and the attenuation rate 2 is calculated.

[0060] Table 1 According to Table 1, the PUR hot melt adhesive prepared in the present application is a combination of fluorinated polyether polyols and polyester polyols, and the polyurethane hot melt adhesive is modified by terminal hydroxyl polybutadiene. The cross-linked polyurethane hot melt adhesive has good bonding strength and excellent resistance to sweat and sebum corrosion, and is suitable for the bonding of electronic wearable devices.

[0061] Compared with Example 1, Example 4-5 adopts homemade fluorinated polyether polyol. The fluorinated polyether polyol contains isocyanate groups, which can participate in the reaction with hydroxyl groups, increase the crosslinking density of the polyurethane system, and help improve the bonding strength and sweat and sebum corrosion resistance of the polyurethane hot melt adhesive.

[0062] Compared with Example 1, Example 6-7 uses 1-chloro-2,4-dinitrobenzene to functionally modify the terminal carbon atom of the terminal hydroxyl polybutadiene, introducing a rigid benzene ring structure. At the same time, the introduced nitro group can produce hydrogen bonds with the isocyanate group, thereby enhancing the intermolecular force and the cross-linking density of the system, which is beneficial to improving the bonding strength. At the same time, the polyurethane system with strong cross-linking can better withstand the corrosion of sweat and skin, and is less prone to degumming and damage.

[0063] Compared with Example 1, Comparative Examples 1-2 lack the introduction of organic fluorine and the modification of terminal hydroxyl polybutadiene in the raw materials of the hot melt adhesive, respectively, so that the oil resistance and water resistance of the PUR hot melt adhesive are reduced, and the resistance to sweat and sebum corrosion is reduced.

[0064] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A sweat-resistant PUR hot melt adhesive, characterized in that: The invention comprises the following raw materials in parts by weight: 35-42 parts of fluorinated polyether polyol; 20-30 parts of polyester polyol; 12-17 parts of hydroxy-terminated polybutadiene; 16-20 parts of diisocyanate; Catalyst 0.05-0.2 parts; Acrylic resin 10-18 parts; Antioxidant 0.1-0.5 parts.

2. The sweat-resistant PUR hot melt adhesive according to claim 1, characterized in that: The number average molecular weight of the fluorine-containing polyether polyol is 1500-3000, and the fluorine content is 10-30%.

3. The sweat-resistant PUR hot melt adhesive according to claim 1, characterized in that: The fluorinated polyether polyol is prepared from the following raw materials in parts by weight: 20-30 parts of isophorone diisocyanate; 25-40 parts of octafluoropentanol; 85-98 parts of glycidol; 42-47 parts of tetrahydrofuran; Boron trifluoride etherate 0.3-0.8 parts; 1-3 parts of ethylene glycol; 65-72 parts of solvent.

4. The sweat-resistant PUR hot melt adhesive according to claim 1, characterized in that: The terminal hydroxyl polybutadiene is selected from modified terminal hydroxyl polybutadiene, and the modified terminal hydroxyl polybutadiene is prepared by the following raw materials in parts by weight: 10-14 parts of hydroxyl-terminated polybutadiene; 1.5-2.2 parts of 1-chloro-2,4-dinitrobenzene; 20-25 parts of dichloromethane; 1.7-2 parts of sodium hydroxide.

5. The sweat-resistant PUR hot melt adhesive according to claim 1, characterized in that: The polyester polyol is polymerized from adipic acid and at least one diol selected from 1,4-butanediol, neopentyl glycol, ethylene glycol, diethylene glycol and 1,6-hexanediol.

6. The sweat-resistant PUR hot melt adhesive according to claim 1, characterized in that: The diisocyanate is selected from one or more of diphenylmethane diisocyanate, toluene diisocyanate, xylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, and carbodiimide-modified diisocyanate.

7. The sweat-resistant PUR hot melt adhesive according to claim 1, characterized in that: The catalyst is one or more of dibutyltin dilaurate, stannous octoate, dibutylene acetate, triethylenediamine, and bismorpholinyl diethyl ether.

8. The method for preparing a sweat-resistant PUR hot melt adhesive according to any one of claims 1 to 7, characterized in that: The following steps are involved: Add polyester polyol, fluorinated polyether polyol, hydroxyl-terminated polybutadiene and acrylic resin into a reaction kettle, stir and mix evenly, heat to 120-130°C, set the vacuum degree to -0.095-0.05MPa, and dehydrate for 2-2.5h; Cool down to 75-80℃, add diisocyanate and catalyst, and react at 85-90℃ for 2-3h; add antioxidant, and stir rapidly at 110-120℃ for 20-30min; The material is quickly discharged and packaged under nitrogen protection to obtain PUR hot melt adhesive resistant to sweat corrosion.

9. The method for preparing a sweat-resistant PUR hot melt adhesive according to claim 8, characterized in that: The fluorinated polyether polyol is prepared by the following steps: Put isophorone diisocyanate and octafluoropentanol into a reactor, react at 40-45°C for 2-2.5h, raise the temperature to 65-68°C, add glycidol and continue to react for 2-2.5h to obtain a fluorine-containing epoxy compound; Add solvent, ethylene glycol and boron trifluoride etherate to the reaction kettle, stir at 0-2°C for 15-20 minutes, add fluorinated epoxy compound and tetrahydrofuran dropwise, the temperature should not exceed 5°C, and react for 5-6 hours; Add a small amount of deionized water and stir for 20-30 minutes to stop the reaction. Wash with deionized water until the organic phase is neutral. Use a separatory funnel to separate the layers statically. Take the lower organic phase and distill under reduced pressure to obtain fluorinated polyether polyol.

10. The method for preparing a sweat-resistant PUR hot melt adhesive according to claim 8, characterized in that: When the hydroxy-terminated polybutadiene is modified hydroxy-terminated polybutadiene, the preparation steps are as follows: Weigh terminal hydroxyl polybutadiene and dichloromethane in a stirring kettle, stir to dissolve, add sodium hydroxide under nitrogen protection and stir for 20-30 minutes, add 1-chloro-2,4-dinitrobenzene to the stirring kettle, stir for 2-3 hours, and then react at room temperature for 10-12 hours, wash with anhydrous methanol and n-hexane, separate by static stratification, and obtain modified terminal hydroxyl polybutadiene after distillation.

Citation Information

Patent Citations

  • Preparation method of polyurethane hot-melt adhesive being sweat resistant

    CN106634776A

  • Preparation method of high-strength sweat-resistant polyurethane hot melt adhesive

    CN111040712A

  • Anti-adhesive low-compression set polyurethane foam material for nasal hemostasis and preparation method of polyurethane foam material

    CN111420116A

  • Preparation method of sebum-resistant and sweat-resistant moisture-curable polyurethane hot melt adhesive

    CN113462339A

  • Moisture-curing polyurethane hot melt adhesive with high initial adhesion strength and high adhesion fastness and preparation method of moisture-curing polyurethane hot melt adhesive

    CN113861927A