5052 secondary aluminum alloy preservation application preparation device and process

By designing the 5052 regenerated aluminum alloy relegation application preparation device, including crushers, cleaning machines, sorters, smelting furnaces and thermal simulation testing machines, the problems of rheology instability and cracking of regenerated aluminum alloys during thermal processing are solved, and the effect of improving the mechanical properties and relegation recovery rate of aluminum alloys is achieved.

CN119571103APending Publication Date: 2025-03-07CHINA NON-FERROUS METALS PROCESSING TECH CO LTD +2
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411926757.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-25
Publication Date
2025-03-07

AI Technical Summary

Technical Problem

Existing recycled aluminum alloy materials are prone to rheology instability and cracking during thermal processing, resulting in waste of resources and low relegation recovery.

Method used

A 5052 recycled aluminum alloy relegation application preparation device is designed, including crushers, cleaning machines, sorters, smelting furnaces and thermal simulation testing machines. Through multi-pass hot rolling experiments, the hot processing parameters are optimized using hot processing diagrams to improve the mechanical properties and corrosion resistance of aluminum alloys.

Benefits of technology

It effectively reduces the impurities in the recycling of 5052 aluminum alloy waste, improves the quality and relegation recovery rate of the ingot, and avoids waste of resources during the hot processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119571103A_ABST
    Figure CN119571103A_ABST
Patent Text Reader

Abstract

The invention discloses a 5052 secondary aluminum alloy preservation application preparation device and process. The 5052 secondary aluminum alloy preservation application preparation device comprises a crusher, a cleaning machine is arranged on one side of the crusher, a sorting machine is arranged on the other side of the crusher, a smelting furnace is arranged near a discharging port of the sorting machine, and a horizontal continuous casting machine is arranged near a discharging port of the smelting furnace. Thermal deformation experiments under different conditions, including heating temperature, deformation rate and deformation amount, are performed on the regenerated aluminum alloy, so that the grain structure of the regenerated aluminum alloy is improved, uniform distribution of a second phase is promoted, and the mechanical property and corrosion resistance are improved. By means of the technology, the mechanical property and the using performance of the 5-series regenerated aluminum alloy reach the level equivalent to those of a primary alloy, and preserve recycling application is achieved. The method solves the problem of performance degradation caused by high impurity content of the existing regenerated aluminum alloy, and has the advantages of simple process, low cost and wide applicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of recycled aluminum alloy materials, and in particular to a device and process for preparing 5052 recycled aluminum alloy for grade preservation application. Background Art

[0002] Recycled aluminum is an aluminum alloy derived from scrap aluminum alloy materials and scrap aluminum or aluminum-containing waste, which is then re-melted and refined. Compared to primary aluminum refined from aluminum ore, recycled aluminum consumes only 1.6% of the electricity and emits only about 5% of the carbon emissions of primary aluminum, achieving the recycling of aluminum resources and significantly reducing energy consumption and emissions. The development of recycled aluminum is of great strategic significance to my country's efforts to build an ecological civilization and promote green development.

[0003] 5052 series aluminum alloys are medium-to-high-strength aluminum alloys with excellent fatigue and weldability and good resistance to marine atmospheric corrosion. They are among the most widely used aluminum alloys, commonly used in the manufacture of sheet metal parts for vehicles and ships, aircraft fuel tanks and fuel pipes, instrument panels, and riveted streetlight brackets. For a long time, due to the complex composition of scrap aluminum raw materials, most existing recycled aluminum alloy ingots have poor ductility and can only be used to produce cast aluminum alloy products. Much high-quality wrought aluminum alloy scrap has been downgraded. This significantly reduces the recycling value of aluminum products and results in a significant waste of scrap aluminum resources. In my country, only approximately 20% of recycled aluminum annually can be reprocessed into the corresponding grade of wrought aluminum alloy for grade-preserving recycling. Furthermore, the actual hot processing of existing recycled aluminum alloys for grade-preserving recycling often suffers from rheological instability and cracking, resulting in large amounts of scrap and wasted resources, making some aluminum alloys unrecyclable. To address this issue, we propose a device and process for preparing 5052 recycled aluminum alloy for grade-preserving recycling. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to overcome the existing defects and provide a 5052 recycled aluminum alloy grade preservation application preparation device and process, which can greatly reduce the impurities in the recycled 5052 aluminum alloy scrap, improve the quality of subsequent 5052 aluminum alloy ingots, thereby improving the grade preservation recovery rate, and can effectively solve the problems in the background technology.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solutions: a 5052 recycled aluminum alloy grade preservation application preparation device, comprising a crusher, a cleaning machine is provided on one side of the crusher, a sorting machine is provided on the other side of the crusher, a smelting furnace is provided near the discharge port of the sorting machine, a horizontal continuous casting machine is provided near the discharge port of the smelting furnace, and a thermal simulation testing machine is also provided on the outside of the smelting furnace for performing hot compression tests on cylindrical specimens cut from the aluminum alloy billets smelted in the smelting furnace.

[0006] As a preferred technical solution of the present invention, a drill hole for installing a thermocouple wire is opened at the center of the end surface of the cylindrical specimen.

[0007] As a preferred technical solution of the present invention, a graphite tantalum sheet is placed at the upper and lower ends of the cylindrical sample respectively.

[0008] Compared with the prior art, the beneficial effects of the present invention are as follows: the recycled 5052 aluminum alloy scrap is first crushed by a crusher and then put into a cleaning machine for cleaning to wash away most of the impurities therein; the cleaned 5052 aluminum alloy scrap is again put into the crusher for secondary crushing to break it into smaller blocks and then passed through a sorting machine to remove non-metallic inclusions, ferromagnetic inclusions and other non-ferrous metal inclusions, etc., which can greatly reduce the impurities in the recycled 5052 aluminum alloy scrap, improve the quality of subsequent aluminum alloy ingots, and thus improve the grade-keeping recovery rate.

[0009] The present invention also provides the following technical solution: a process for preparing recycled aluminum alloy for grade-preserving application, using the above-mentioned recycled aluminum alloy for grade-preserving application preparation device, comprising the following steps:

[0010] S1) The recovered aluminum alloy is crushed once in a crusher and then put into a cleaning machine for cleaning. After cleaning, it is sent back to the crusher for secondary crushing, and the material is broken into smaller pieces and then passed through a sorting machine to remove non-metallic inclusions, ferromagnetic inclusions and other non-ferrous metal inclusions;

[0011] S2) the aluminum alloy scrap after removing impurities and sundries is melted into billets in a melting furnace;

[0012] S3) cutting cylindrical specimens from the recycled aluminum alloy billet, performing a hot compression test on the cylindrical specimens using a thermal simulation testing machine, setting deformation amount, deformation temperature, and deformation rate, and compressing the specimens at different deformation temperatures and deformation rates;

[0013] S4) obtaining the energy dissipation rate factor η and the plastic flow instability parameter ξ at different deformation temperatures and deformation rates based on the data, and constructing a thermal processing map with a set true strain value;

[0014] S5) designing a suitable multi-pass hot rolling experiment for the blank according to the obtained optimal hot working parameters to obtain a hot rolled plate with improved mechanical properties.

[0015] As a preferred technical solution of the present invention, in step S3), the aluminum alloy sample is cut into a cylindrical specimen of φ8 mm×12 mm by wire cutting.

[0016] As a preferred technical solution of the present invention, in step S3), the deformation temperatures are set to 200°C, 300°C, 350°C, 400°C, and 500°C respectively.

[0017] As a preferred technical solution of the present invention, in step S3), the strain rates are set to: 0.001s -1 , 0.01s -1 , 0.1s -1 , 1s -1 , 10s -1 .

[0018] As a preferred technical solution of the present invention, in step S3), the deformation amount is set to 80%.

[0019] As a preferred technical solution of the present invention, in step S4), the shaded area in the hot processing diagram is the rheological instability area, and all areas except the shaded area can be selected as the alloy hot processing area. The part with a large dissipation factor in the diagram is the optimal processing area for the alloy.

[0020] As a preferred technical solution of the present invention, the parameters used for hot rolling in step S5) are actual hot working parameters obtained according to the hot working diagram.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: 5052 aluminum alloy scrap after removing impurities and debris is melted into billets in a melting furnace, and several cylindrical specimens are cut into pieces before being put into a horizontal continuous casting machine for casting, and are sent to a thermal simulation test machine for hot compression testing, and the samples are compressed at different deformation temperatures and deformation rates to obtain rheological stress and strain data at different deformation temperatures and deformation rates, and the energy dissipation rate factor η and the plastic flow instability parameter ξ at different deformation temperatures and deformation rates are obtained based on the data, and a thermal processing diagram with a set strain value is constructed, and then the recycled 5052 aluminum alloy billets are subjected to multiple hot rolling experiments based on the obtained hot processing parameters to finally obtain hot rolled plates. The recycled 5052 aluminum alloy may have problems such as rheological instability and cracking during actual hot processing, and smaller samples are used to simulate the thermal deformation of the alloy, thereby avoiding the waste of resources caused by a large amount of scrap in the actual production hot processing experiment, and further improving the grade-keeping recovery rate of the 5052 aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a structural schematic diagram of the present invention;

[0023] Figure 2 It is a structural schematic diagram of the cylindrical specimen of the present invention;

[0024] Figure 3 It is a structural schematic diagram of the cleaning machine of the present invention;

[0025] Figure 4 It is a side structural schematic diagram of the cleaning machine of the present invention;

[0026] Figure 5 It is a front view structural schematic diagram of the cleaning machine of the present invention.

[0027] In the figure: 1 crusher, 2 cleaning machine, 201 cleaning box, 202 lifting cage, 203 hanging ring, 204 movable plate, 205 driving motor, 206 stirring shaft, 207 stirring blade, 208 telescopic rod, 209 supporting block, 3 sorting machine, 4 melting furnace, 5 thermal simulation test machine, 6 horizontal continuous casting machine, 7 cylindrical specimen, 8 drilling, 9 graphite tantalum sheet. DETAILED DESCRIPTION

[0028] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0029] See also Figure 1-5 The present invention provides a technical solution: a 5052 recycled aluminum alloy grade preservation application preparation device, comprising a crusher 1, the crusher 1 can be a common roller crusher, etc., a cleaning machine 2 is provided on one side of the crusher 1, and a sorting machine 3 is provided on the other side of the crusher 1. The sorting machine 3 can be selected from one or more of the commonly used magnetic separators, air separators, flotation machines, and eddy current separators, and can be flexibly selected according to the specific type of 5052 aluminum alloy being recycled. Before preparing the 5052 recycled aluminum alloy, first The recycled 5052 aluminum alloy scrap is crushed once by the crusher 1 and then put into the cleaning machine 2 for cleaning to remove most of the impurities therein. The cleaned 5052 aluminum alloy scrap is put into the crusher 1 again for secondary crushing to break it into smaller blocks and then pass through the sorting machine 3 to remove non-metallic inclusions, ferromagnetic inclusions and other non-ferrous metal inclusions. This can greatly reduce the impurities in the recycled 5052 aluminum alloy scrap, improve the quality of subsequent 5052 aluminum alloy ingots, and thus improve the grade-keeping recovery rate.

[0030] A smelting furnace 4 is provided near the discharge port of the sorting machine 3. The 5052 aluminum alloy scrap after removing impurities and sundries is melted into billets in the smelting furnace 4. A horizontal continuous casting machine 6 is provided near the discharge port of the smelting furnace 4. A thermal simulation tester 5 for performing a hot compression test on a cylindrical sample 7 cut from the aluminum alloy billet melted in the smelting furnace 4 is also provided on the outside of the smelting furnace 4. The thermal simulation tester 5 is preferably a Gleeble-1500D thermal simulation tester. Before the billet is put into the horizontal continuous casting machine 6 for casting, several cylindrical samples 7 are cut and sent to the thermal simulation tester 5 for hot compression testing. The samples are compressed at different deformation temperatures and deformation rates to obtain The flow stress and strain data at different deformation temperatures and deformation rates were obtained. The energy dissipation rate factor η and plastic flow instability parameter ξ at different deformation temperatures and deformation rates were obtained based on the data. A hot working diagram with a set strain value was constructed. Then, according to the obtained hot working parameters, multiple hot rolling experiments were carried out on the recycled 5052 aluminum alloy billet, and finally a hot-rolled plate was obtained. In order to prevent the rheological instability and cracking problems that may occur in the actual hot working process of the recycled 5052 aluminum alloy during the actual hot working process, a smaller sample was used to simulate the hot deformation of the alloy, thereby avoiding the waste of resources caused by a large amount of waste in the actual production hot working experiment, and further improving the grade preservation recovery rate of the 5052 aluminum alloy.

[0031] Specifically, a hot compression cylindrical specimen 7 is cut out from the recycled aluminum alloy billet by a wire cutting method, and a drill hole 8 for installing a thermocouple wire is opened at the center of the end face of the cylindrical specimen 7; a hot compression test is performed on the cylindrical specimen 7 using a thermal simulation test machine 5, and a graphite tantalum sheet 9 is placed at the upper and lower ends of the cylindrical specimen 7, respectively, in order to reduce friction and improve the accuracy of the test; the deformation amount, deformation temperature and deformation rate are set, and the sample is compressed at different deformation temperatures and deformation rates to obtain the flow stress and strain data at different deformation temperatures and deformation rates, and the energy dissipation rate factor η and the plastic flow instability parameter ξ at different deformation temperatures and deformation rates are obtained based on the data; a hot processing diagram with a set strain value is constructed; and a multi-pass hot rolling experiment is performed on the recycled 5052 aluminum alloy billet according to the obtained hot processing parameters to finally obtain a hot-rolled plate.

[0032] Thermal deformation experiments conducted under different conditions on recycled aluminum alloys have shown that they can improve their grain structure, promote the uniform distribution of secondary phases, and enhance their mechanical properties and corrosion resistance. This process has enabled the mechanical properties and performance of 5-series recycled aluminum alloys to reach levels comparable to those of virgin alloys, enabling grade-preserving recycling applications.

[0033] Thermal processing diagram is a commonly used tool for evaluating the processing performance of materials. By drawing and analyzing the thermal processing diagram, the optimal thermal processing range and unstable area in the diagram can be intuitively reflected, providing a theoretical reference for the actual thermal processing production of recycled 5 series aluminum alloys, and ensuring the value of recycled aluminum in maintaining grade utilization.

[0034] Alternatively, to prevent oxidation and burnout and remove inclusions and gases, 5052 recycled aluminum can easily react with moisture in the air during smelting, causing oxidation and burnout, reducing the yield of the recycled aluminum alloy. Inclusions can also reduce the mechanical properties of the recycled aluminum alloy. Therefore, a dual-chamber furnace process is preferred, with enclosed conveyor belts used for material transport to isolate the material from air, and effective gas collection devices installed at relevant dust-generating points.

[0035] Optional technical solution, the cleaning machine 2 includes a cleaning box 201 and a lifting cage 202 for placing the aluminum alloy fragments that have been crushed once by the crusher 1. The upper side of the cleaning box 201 is provided with a liquid inlet pipe connected to the external cleaning liquid tank, and the lower side is provided with a sewage pipe for discharging sewage and impurities after cleaning. Hanging rings 203 are provided at the four corners of the upper surface of the lifting cage 202. The upper surface of the cleaning box 201 is open. The hoisting mechanism places the 5052 aluminum alloy fragments that have been crushed once through the hanging ring 203. The lifting cage 202 of the fragments is moved to the top of the cleaning box 201 and lowered into the cleaning box 201, and the corresponding cleaning liquid is added into the cleaning box 201 through the liquid inlet pipe to clean the 5052 aluminum alloy fragments after the primary crushing to remove oil stains and impurities on the surface. After cleaning, the lifting cage 202 and the 5052 aluminum alloy fragments inside are lifted to the corresponding position by the hoisting mechanism, drained and dried, and then put into the crusher 1 for secondary crushing to break them into smaller blocks for subsequent smelting.

[0036] A further optional technical solution is that a movable plate 204 is hingedly provided on the upper part of the side surface of the cleaning box 201, and the width of the movable plate 204 is greater than half the width of the opening above the cleaning box 201. Two drive motors 205 are symmetrically provided on the outer surface of the movable plate 204. The output shaft of the drive motor 205 passes through the inner surface of the movable plate 204 and is connected to the stirring shaft 206 through a coupling. A number of stirring blades 207 are evenly provided on the outer peripheral side surface of the stirring shaft 206. After the lifting cage 202 is put into the cleaning box 201, the movable plate 204 can be rotated to the top of the cleaning box 201, so that the stirring shaft 206 and the stirring blades 207 enter the lifting cage 202, and then the drive motor 205 is turned on. The two drive motors 205 drive the stirring blades 207 to rotate in opposite directions through their respective stirring shafts 206, which can improve the cleaning efficiency and cleaning effect, thereby improving the quality of the recycled aluminum alloy.

[0037] Furthermore, two telescopic rods 208 are symmetrically hinged on the two side surfaces of the cleaning box 201, and the ends of the two telescopic rods 208 are hinged to the two side surfaces of the movable plate 204 respectively. The telescopic rods 208 can be made of commonly used electric push rods or cylinders, hydraulic cylinders, etc. The telescopic rods 208 are hinged to drive the movable plate 204 to rotate automatically through the extension and contraction of the hinged telescopic rods 208, which greatly improves the degree of automation and enhances work efficiency.

[0038] The crusher 1, drive motor 205, telescopic rod 208, sorting machine 3, melting furnace 4, thermal simulation test machine 5 and horizontal continuous casting machine 6 used in this application are all electronic components or equipment commonly used in the prior art. Their specific structure, working principle and circuit connection are all well-known technologies, and the control devices and control methods of each part are also prior art, which will not be described in detail.

[0039] Optionally, a support block 209 corresponding to the movable plate 204 is fixedly provided on the outer surface of the cleaning box 201 on the same side as the movable plate 204, and is used to support the fully opened movable plate 204. When the movable plate 204 is fully opened, the stirring shaft 206 and the stirring blade 207 are located away from the top of the cleaning box 201 and do not affect the in and out operation of the lifting cage 202. In addition, the support block 209 can also serve as a limit protection for the movable plate 204 and the telescopic rod 208.

[0040] Example 1: (1) The recycled 5052 aluminum alloy is crushed once in a crusher 1 and then put into a cleaning machine 2 for cleaning. After cleaning, it is sent back to the crusher 1 for secondary crushing, and is broken into smaller blocks. The blocks are then passed through a sorter 3 to remove non-metallic inclusions, ferromagnetic inclusions and other non-ferrous metal inclusions. After the impurities and debris are removed, the 5052 aluminum alloy scrap is melted into billets in a melting furnace 4. A cylindrical sample of φ8×12mm is cut from the recycled 5052 aluminum alloy billet by wire cutting, and a small hole of φ1mm×2mm is drilled in the center of the sample for the purpose of installing a thermocouple wire.

[0041] (2) The Gleeble-1500D thermal simulation tester was used to perform thermal compression deformation on the specimens. Graphite tantalum sheets were placed at both ends of the specimens to reduce friction and improve the accuracy of the test. The deformation temperatures were set to 200°C, 300°C, 350°C, 400°C, and 500°C, respectively; the strain rates were set to 0.001s. -1 , 0.01s -1 , 0.1s -1 , 1s -1 , 10s -1 The deformation was set to 80%. The sample was heated to the predetermined temperature at a rate of 5°C / s and kept at that temperature for 5 minutes to ensure uniform temperature distribution. The sample was then compressed at different deformation temperatures and strain rates to obtain flow stress and strain data at different deformation temperatures and strain rates.

[0042] (3) According to the data, the energy dissipation factor η and the plastic flow instability parameter ξ at different deformation temperatures and deformation rates under a true strain of 0.3 are obtained; the deformation temperature is set as the X-axis, the strain rate is set as the Y-axis, the energy dissipation factor η and the plastic flow instability parameter ξ are set as the Z-axis, and the origin software is used to draw a plane diagram in the form of contour lines. The instability diagram and the dissipation diagram are superimposed and drawn into a thermal processing diagram, and finally the thermal processing parameters are obtained.

[0043] Table 1 Hot working parameters of recycled 5052 alloy

[0044]

[0045] (4) A test billet measuring 200 mm × 50 mm × 25 mm was processed from an ingot casting machine. The billet was hot rolled in multiple passes with small deformation and a slow hot rolling rate at a temperature range of 450 ± 10 °C, and the sample was rolled from 25 mm to 10 mm. The hot rolled sheet was free of defects such as cracks and voids. The ultimate tensile strength and yield strength of the rolled alloy were measured to be 210 MPa and 120 MPa, respectively, which were 10.5% and 39.53% higher than those of the billet alloy. The elongation was 28.4%.

[0046] Example 2: (1) The recycled 5052 aluminum alloy is crushed once in a crusher 1 and then put into a cleaning machine 2 for cleaning. After cleaning, it is sent back to the crusher 1 for secondary crushing, and is broken into smaller blocks. The blocks are then passed through a sorter 3 to remove non-metallic inclusions, ferromagnetic inclusions and other non-ferrous metal inclusions. After the impurities and debris are removed, the 5052 aluminum alloy scrap is melted into billets in a melting furnace 4. A cylindrical sample of φ8×12mm is cut from the recycled 5052 aluminum alloy billet by wire cutting, and a small hole of φ1mm×2mm is drilled in the center of the sample for the purpose of installing a thermocouple wire.

[0047] (2) The Gleeble-1500D thermal simulation tester was used to perform thermal compression deformation on the specimens. Graphite tantalum sheets were placed at both ends of the specimens to reduce friction and improve the accuracy of the test. The deformation temperatures were set to 200°C, 300°C, 350°C, 400°C, and 500°C, respectively; the strain rates were set to 0.001s. -1 , 0.01s -1 , 0.1s -1 , 1s -1 , 10s -1 The deformation was set to 80%. The sample was heated to the predetermined temperature at a rate of 5°C / s and kept at that temperature for 5 minutes to ensure uniform temperature distribution. The sample was then compressed at different deformation temperatures and strain rates to obtain flow stress and strain data at different deformation temperatures and strain rates.

[0048] (3) According to the data, the energy dissipation factor η and the plastic flow instability parameter ξ at different deformation temperatures and deformation rates under a true strain of 0.3 are obtained; the deformation temperature is set as the X-axis, the strain rate is set as the Y-axis, the energy dissipation factor η and the plastic flow instability parameter ξ are set as the Z-axis, and the origin software is used to draw a plane diagram in the form of contour lines. The instability diagram and the dissipation diagram are superimposed and drawn into a thermal processing diagram, and finally the thermal processing parameters are obtained.

[0049] Table 2 Hot working parameters of recycled 5052 alloy

[0050]

[0051] (4) A test billet measuring 200 mm × 50 mm × 25 mm was processed from an ingot casting machine. The billet was hot rolled in multiple passes with small deformation and a fast hot rolling rate at a temperature range of 450 ± 10 °C, and the sample was rolled from 25 mm to 10 mm. The hot rolled sheet was free of defects such as cracks and voids. The ultimate tensile strength and yield strength of the rolled alloy were measured to be 221 MPa and 132 MPa, respectively, which were increases of 16.3% and 53.4%, respectively, compared to the billet alloy. The elongation was 24.3%.

[0052] Example 3: (1) The recycled 5052 aluminum alloy is crushed once by a crusher 1 and then put into a cleaning machine 2 for cleaning. After cleaning, it is sent back to the crusher 1 for secondary crushing, and is broken into smaller blocks. Then, non-metallic inclusions, ferromagnetic inclusions and other non-ferrous metal inclusions are removed by a sorting machine 3. After the impurities and debris are removed, the 5052 aluminum alloy waste is melted into billets in a melting furnace 4. A cylindrical sample of φ8×12mm is cut from the recycled 5052 aluminum alloy billet by wire cutting, and a small hole of φ1mm×2mm is drilled in the center of the sample for the purpose of installing a thermocouple wire.

[0053] (2) The Gleeble-1500D thermal simulation tester was used to perform thermal compression deformation on the specimens. Graphite tantalum sheets were placed at both ends of the specimens to reduce friction and improve the accuracy of the test. The deformation temperatures were set to 200°C, 300°C, 350°C, 400°C, and 500°C, respectively; the strain rates were set to 0.001s. -1 , 0.01s -1 , 0.1s -1 , 1s -1 , 10s -1 The deformation was set to 80%. The sample was heated to the predetermined temperature at a rate of 5°C / s and kept at that temperature for 5 minutes to ensure uniform temperature distribution. The sample was then compressed at different deformation temperatures and strain rates to obtain flow stress and strain data at different deformation temperatures and strain rates.

[0054] (3) According to the data, the energy dissipation factor η and the plastic flow instability parameter ξ at different deformation temperatures and deformation rates under a true strain of 0.5 are obtained; the deformation temperature is set as the X-axis, the strain rate is set as the Y-axis, the energy dissipation factor η and the plastic flow instability parameter ξ are set as the Z-axis, and the origin software is used to draw a plane diagram in the form of contour lines. The instability diagram and the dissipation diagram are superimposed and drawn into a thermal processing diagram, and finally the thermal processing parameters are obtained.

[0055] Table 3 Hot working parameters of recycled 5052 alloy

[0056]

[0057] (4) A test billet measuring 200 mm × 50 mm × 30 mm was processed from an ingot casting machine. The billet was hot rolled in multiple passes with large deformation and a slow hot rolling rate at a temperature range of 400 ± 10 °C, and the sample was rolled from 30 mm to 10 mm. The hot rolled sheet was free of defects such as cracks and voids. The ultimate tensile strength and yield strength of the rolled alloy were measured to be 229 MPa and 138 MPa, respectively, which were 20.2% and 60.4% higher than those of the billet alloy, respectively. The elongation was 23.5%.

[0058] Example 4: (1) The recycled 5052 aluminum alloy is crushed once by a crusher 1 and then put into a cleaning machine 2 for cleaning. After cleaning, it is sent back to the crusher 1 for secondary crushing, and is broken into smaller blocks. The blocks are then passed through a sorter 3 to remove non-metallic inclusions, ferromagnetic inclusions and other non-ferrous metal inclusions. After the impurities and debris are removed, the 5052 aluminum alloy scrap is melted into billets in a melting furnace 4. A cylindrical sample of φ8×12mm is cut from the recycled 5052 aluminum alloy billet by wire cutting, and a small hole of φ1mm×2mm is drilled in the center of the sample for the purpose of installing a thermocouple wire.

[0059] (2) The Gleeble-1500D thermal simulation tester was used to perform thermal compression deformation on the specimens. Graphite tantalum sheets were placed at both ends of the specimens to reduce friction and improve the accuracy of the test. The deformation temperatures were set to 200°C, 300°C, 350°C, 400°C, and 500°C, respectively; the strain rates were set to 0.001s. -1 , 0.01s -1 , 0.1s -1 , 1s -1 , 10s -1 The deformation was set to 80%. The sample was heated to the predetermined temperature at a rate of 5°C / s and kept at that temperature for 5 minutes to ensure uniform temperature distribution. The sample was then compressed at different deformation temperatures and strain rates to obtain flow stress and strain data at different deformation temperatures and strain rates.

[0060] (3) According to the data, the energy dissipation factor η and the plastic flow instability parameter ξ at different deformation temperatures and deformation rates under a true strain of 0.5 are obtained; the deformation temperature is set as the X-axis, the strain rate is set as the Y-axis, the energy dissipation factor η and the plastic flow instability parameter ξ are set as the Z-axis, and the origin software is used to draw a plane diagram in the form of contour lines. The instability diagram and the dissipation diagram are superimposed and drawn into a thermal processing diagram, and finally the thermal processing parameters are obtained.

[0061] Table 4 Hot working parameters of recycled 5052 alloy

[0062]

[0063]

[0064] (4) The test billets with a size of 200 mm × 50 mm × 30 mm were processed from the ingot casting machine. The billets were hot rolled in multiple passes with large deformation and a fast hot rolling rate. The hot rolling temperature range was 400 ± 10 ° C. The samples were rolled from 30 mm to 10 mm. Finally, the hot rolled plates had no defects such as cracks and voids. The ultimate tensile strength and yield strength of the rolled alloy were measured to be 237 MPa and 144 MPa, respectively, which were increased by 24.7% and 67.4% respectively compared with the billet alloy. The elongation was 20.2%.

[0065] Any undisclosed portions of the present invention are prior art, and their specific structures, materials, and operating principles will not be described in detail. Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the present invention. The scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A 5052 recycled aluminum alloy grade preservation application preparation device, characterized by: The invention comprises a crusher (1), a cleaning machine (2) is arranged on one side of the crusher (1), a sorting machine (3) is arranged on the other side of the crusher (1), a smelting furnace (4) is arranged near the discharge port of the sorting machine (3), a horizontal continuous casting machine (6) is arranged near the discharge port of the smelting furnace (4), and a thermal simulation test machine (5) for performing a hot compression test on a cylindrical sample (7) cut from an aluminum alloy billet smelted in the smelting furnace (4) is also arranged outside the smelting furnace (4).

2. The 5052 recycled aluminum alloy grade-preserving application preparation device according to claim 1 is characterized in that: A drill hole (8) for installing a thermocouple wire is provided at the center of the end surface of the cylindrical sample (7).

3. The 5052 recycled aluminum alloy grade-preserving application preparation device according to claim 1 is characterized in that: A graphite tantalum sheet (9) is placed at the upper and lower ends of the cylindrical sample (7), respectively.

4. A 5052 recycled aluminum alloy grade-preserving application preparation process, characterized in that: The 5052 recycled aluminum alloy grade preservation application preparation device according to any one of claims 1 to 3 comprises the following steps: S1) The recycled 5052 aluminum alloy is crushed by a crusher (1) and then put into a cleaning machine (2) for cleaning. After cleaning, it is sent back to the crusher (1) for secondary crushing, and is crushed into smaller blocks. The blocks are then passed through a sorting machine (3) to remove non-metallic inclusions, ferromagnetic inclusions and other non-ferrous metal inclusions; S2) the 5052 aluminum alloy scrap after removing impurities and debris is melted into billets in a melting furnace (4); S3) cutting a cylindrical sample (7) from a 5052 recycled aluminum alloy billet, performing a hot compression test on the cylindrical sample using a thermal simulation test machine (5), setting a deformation amount, a deformation temperature and a deformation rate, and compressing the sample at different deformation temperatures and deformation rates; S4) obtaining the energy dissipation rate factor η and the plastic flow instability parameter ξ at different deformation temperatures and deformation rates according to the data, and constructing a thermal processing diagram with a set true strain value; S5) Designing appropriate multi-pass hot rolling experiments for the blank according to the obtained optimal hot working parameters to obtain hot rolled plates with improved mechanical properties.

5. A 5052 recycled aluminum alloy grade-preserving application preparation process according to claim 4, characterized in that: In the step S3), the aluminum alloy sample is cut into a cylindrical specimen (7) of φ8 mm×12 mm by wire cutting.

6. A 5052 recycled aluminum alloy grade-preserving application preparation process according to claim 4, characterized in that: In the step S3), the deformation temperatures are set to 200°C, 300°C, 350°C, 400°C, and 500°C respectively.

7. The 5052 recycled aluminum alloy grade-preserving application preparation process according to claim 4 is characterized in that: In step S3), the strain rates are set to: 0.001s -1 、0.01s -1 , 0.1s -1 , 1s -1 , 10s -1 .

8. The 5052 recycled aluminum alloy grade-preserving application preparation process according to claim 4 is characterized in that: In the step S3), the deformation amount is set to 80%.

9. The 5052 recycled aluminum alloy grade-preserving application preparation process according to claim 4 is characterized by: In the step S4), the shaded area in the hot working diagram is the rheological instability area, and all areas except the shaded area can be selected as the alloy hot working area. The part with a large dissipation factor in the diagram is the best processing area for the alloy.

10. The 5052 recycled aluminum alloy grade-preserving application preparation process according to claim 4, characterized in that: The parameters used for hot rolling in step S5) are actual hot working parameters obtained according to the hot working diagram.

Citation Information

Cited By

  • 6063 secondary aluminum alloy for 3C electronic product and preparation method thereof

    CN121518843A

  • Preparation method of 7003 secondary aluminum alloy for 3C electronic products

    CN121555815A

  • 5083 regenerated aluminum alloy for air separation equipment and preparation method thereof

    CN121629232A