A graphene oxide dispersion, its preparation method, and a graphene thermally conductive film.

By modifying graphene oxide with a composite aqueous solution of ammonium lignosulfonate and praseodymium metal salt, and combining it with high-pressure homogenization technology, a high-solids-content graphene oxide dispersion was prepared. This solved the problem of limited thickness and thermal conductivity of graphene thermal conductive film, and achieved efficient improvement in thermal conductivity and industrial production.

CN120208218BActive Publication Date: 2026-11-10XINGTU (CHANGZHOU) CARBON MATERIALS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510462671.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-14
Publication Date
2026-11-10
Estimated Expiration
2045-04-14

AI Technical Summary

Technical Problem

The thermal conductivity of existing graphene thermal conductive films is limited by the high viscosity and poor flowability of high-concentration graphene dispersions, making it difficult to prepare ultra-thick films. Furthermore, defects in the graphene crystal structure severely affect the thermal conductivity.

Method used

Graphene oxide was modified by using a composite aqueous solution of ammonium lignosulfonate and praseodymium metal salt. A high-solids-content graphene oxide dispersion was prepared by grafting and compositing organic polymer-metal catalysts and combining them with high-pressure homogenization technology. A graphene thermal conductive film was then prepared by casting. Praseodymium was used to catalyze the rearrangement of carbon atoms to form a complete graphene crystal structure.

Benefits of technology

This improved the thickness and thermal conductivity of the graphene thermal conductive film, reduced production costs, and maintained the fluidity of the dispersion, thus achieving highly efficient thermal conductivity enhancement and industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005357623280000121
    Figure BDA0005357623280000121
  • Figure BDA0005357623280000131
    Figure BDA0005357623280000131
  • Figure HDA0005357623300000011
    Figure HDA0005357623300000011
Patent Text Reader

Abstract

This invention discloses a graphene oxide dispersion, the raw materials of which include: an aqueous organic polymer compound, a metal catalyst, graphene oxide, a pH adjuster, and deionized water; the amount of the aqueous organic polymer compound used is 0.03-0.8% of the mass of graphene oxide, and the amount of the metal catalyst used is 0.01-0.08% of the mass of graphene oxide. This invention uses an organic polymer-metal composite dispersion to modify graphene oxide, resulting in a graphene thermally conductive film with higher thickness, fewer defects, a more complete crystal structure, and excellent overall thermal conductivity. Using specific amounts of ammonium lignosulfonate and praseodymium metal salt can improve the thermal dispersibility and thermal conductivity of the thermally conductive film without significantly increasing the viscosity of the graphene oxide dispersion, allowing for casting processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-metallic element compounds, specifically to a graphene oxide dispersion and its preparation method, and a graphene thermal conductive film. Background Technology

[0002] Graphene materials possess extremely high electron mobility and excellent thermal conductivity, making them a replacement for traditional heat dissipation materials in mobile phones, computers, and electronic devices. However, the thermal conductivity of existing graphene thermal conductive films is below 1500 W / (m·K), limiting further development of their thermal conductivity. This is mainly because high-concentration graphene dispersions have high viscosity and poor flowability, which is unfavorable for the casting process to prepare ultra-thick GO films. Furthermore, defects in the graphene crystal structure during the production of industrial graphene dispersions lead to severe phonon scattering during transmission, resulting in a decrease in the thermal conductivity of the graphene thermal conductive film.

[0003] Chinese invention patent CN117263175A discloses a high-solids-content graphene oxide slurry, a graphene oxide thermal conductive film, and a preparation method thereof. By combining two dispersants, the viscosity of the graphene slurry can be reduced, and the solid content can be increased, reaching 6-10%. This yields a stable, low-viscosity, high-solids-content graphene oxide slurry. However, the solid content of the graphene slurry does not yet achieve optimal results. Chinese invention patent CN112794314B discloses a method for preparing a high-density graphene thermal conductive film with group-controlled properties and the resulting product. A group-binding agent is used to treat the graphene oxide groups, achieving effective dispersion of the slurry. A modifier is used for group repair, controlling the slurry's dispersion uniformity and viscosity applicability while simultaneously achieving the preparation of a high-solids-content slurry. However, this method uses a calendering process, which is relatively complex. Summary of the Invention

[0004] To develop a high-solids-content graphene dispersion, increase the film thickness of cast graphene thermally conductive films, improve the structural integrity of graphene thermally conductive films, reduce intrinsic defects, and enhance their thermal conductivity, the first aspect of this invention provides a graphene oxide dispersion. The raw materials for preparation include: an aqueous organic polymer compound, a metal catalyst, graphene oxide, a pH adjuster, and deionized water; the amount of the aqueous organic polymer compound used is 0.03-0.8% of the mass of the graphene oxide, and the amount of the metal catalyst used is 0.01-0.08% of the mass of the graphene oxide.

[0005] In one embodiment, the aqueous organic polymer compound is a lignin derivative; the lignin derivative is selected from at least one of ammonium lignin sulfonate, sodium lignin sulfonate, magnesium lignin sulfonate, or calcium lignin sulfonate.

[0006] In one embodiment, the aqueous organic polymer compound is ammonium lignosulfonate.

[0007] In one embodiment, the metal catalyst is a rare earth metal catalyst, and the rare earth metal catalyst is a praseodymium metal salt.

[0008] In one embodiment, the praseodymium metal salt is selected from at least one of praseodymium chloride, praseodymium carbonate, praseodymium sulfate, or praseodymium nitrate.

[0009] In one embodiment, the praseodymium metal salt is praseodymium chloride.

[0010] In one embodiment, the pH adjuster is ammonia.

[0011] During the experiment, the inventors discovered that modifying graphene oxide with a composite aqueous solution of ammonium lignosulfonate and praseodymium chloride can yield a graphene thermally conductive template with high thickness and excellent overall thermal conductivity. The reason is that ammonium lignosulfonate contains a large number of phenolic hydroxyl groups, alcoholic hydroxyl groups, carboxyl groups, and carbonyl groups. The lone pairs of electrons on the oxygen atoms in graphene oxide can form coordinate bonds with the metal ion praseodymium. At the same time, the carboxyl and carbonyl groups react with the oxygen-containing functional groups on the surface of graphene oxide, so that the structure with catalytic graphitization is precisely linked to the defects of graphene oxide. During the graphitization stage, the praseodymium atoms exert their catalytic effect, forming double bonds with carbon atoms and then forming benzene rings. They then quickly detach from the benzene ring structure and continue to combine with the remaining non-benzene ring carbon atoms to produce benzene rings, thereby gradually reducing the number of defects in graphene and gradually making the crystal structure more complete.

[0012] A second aspect of the present invention provides a method for preparing a graphene oxide dispersion, comprising the following steps:

[0013] S1: Preparation of aqueous organic polymer solutions;

[0014] S2: Adjusts the pH of aqueous organic polymer solutions;

[0015] S3: Add the metal catalyst to the aqueous organic polymer solution after pH adjustment in step S2, seal and sonicate to obtain an organic polymer-metal composite dispersion;

[0016] S4: Add graphene oxide to deionized water and stir to obtain graphene oxide slurry;

[0017] S5: Add the organic polymer-metal composite dispersion to the graphene oxide slurry and stir to mix. Add a pH adjuster to adjust the pH and obtain a mixture.

[0018] S6: Homogenize the mixture from step S5 under high pressure to obtain a graphene oxide dispersion.

[0019] In one embodiment, the aqueous organic polymer solution is a solution of an aqueous organic polymer and deionized water, and the mass concentration of the aqueous organic polymer solution is 0.178-0.952 mg / mL.

[0020] In one embodiment, the pH of the aqueous organic polymer solution is adjusted to 9-9.5 in step S2.

[0021] In one embodiment, the pH of the aqueous organic polymer solution is adjusted to 9.32-9.34 in step S2.

[0022] In one embodiment, the pH of the aqueous organic polymer solution is adjusted to 9.33 in step S2.

[0023] In one implementation, the ultrasonic frequency in step S3 is 0.3-1KW, and the ultrasonic time in step S3 is 1-3h.

[0024] In one embodiment, in step S4, graphene oxide is added to deionized water in 3-5 portions, with each addition of graphene oxide being 2-4% of the mass of deionized water. The solid content of the graphene oxide slurry obtained in step S4 is 10-15 wt%.

[0025] In one embodiment, in step S4, graphene oxide is added to deionized water in four separate steps, and the solid content of the graphene oxide slurry obtained in step S4 is 12 wt%.

[0026] In one embodiment, the stirring rate in step S4 is 1500-3000 rpm.

[0027] In one embodiment, the stirring rate in step S5 is 1500-3000 rpm, and the homogenization pressure in step S6 is 15-55 MPa.

[0028] In one implementation, the pH is adjusted to 5.5-6.5 in step S5.

[0029] The excellent thermal conductivity of graphene thermal conductive films is mainly attributed to the long-range ordered carbon atoms (SP) in the graphene thermal conductive films. 2 Hybrid aromatic ring structure, with a large number of SP 2Hybridized carbon atoms form a six-membered carbon ring aromatic structure through covalent bonds, exhibiting thermal conductivity an order of magnitude higher than that of traditional metals. Although graphene has a theoretically high thermal conductivity, defects in its crystal structure during industrial mass production lead to severe phonon scattering during transmission, resulting in reduced thermal conductivity of the graphene thermal conductive film. Increasing the solid content of the GO dispersion helps to increase the thickness of the GO film, thereby increasing the thickness of the graphene thermal conductive film and achieving the goal of increasing heat flux. This further enhances the heat dissipation capacity of the graphene thermal conductive film and also reduces production costs. However, the large specific surface area, hydrogen bonds, and intermolecular forces of graphene oxide result in extremely high viscosity of the high-concentration GO dispersion, essentially eliminating its fluidity, which is unfavorable for the preparation of ultra-thick GO films by the casting method.

[0030] This invention develops an industrially producible ultra-thick high-performance graphene thermal conductive film by grafting and compositing organic polymers with metal compounds. This increases the single-film thickness of the graphene thermal conductive film, thereby increasing its heat flux. Furthermore, the presence of praseodymium transforms non-sp2 hybrid carbon into sp2 hybrid carbon, improving the crystallinity of graphene crystals, eliminating the performance degradation caused by intrinsic defects, and improving the overall thermal conductivity of the graphene thermal conductive film.

[0031] The inventors further discovered that, along with the carbonization of ammonium lignin sulfonate, lignin is cracked into carbon, providing an additional carbon source for the subsequent repair of carbon atom rearrangement defects. At the same time, it provides free carbon for oxygen-containing functional groups to carry carbon out, avoiding the consumption of carbon atoms on the complete six-membered ring and causing more defects to appear.

[0032] A third aspect of the present invention provides a graphene thermally conductive film prepared using the above-described graphene oxide dispersion.

[0033] A fourth aspect of the present invention provides a method for preparing the above-mentioned graphene thermally conductive film, comprising the following steps:

[0034] H1: The graphene oxide dispersion was coated and dried to obtain a graphene precursor film.

[0035] H2: The graphene precursor film is subjected to low-temperature heat treatment to obtain a graphene pretreated film.

[0036] H3: Carbonize the pretreated graphene film to obtain a carbonized graphene film;

[0037] H4: Graphene carbonization film is graphitized and then rolled to obtain graphene thermal conductive film.

[0038] In one embodiment, the coating thickness in step H1 is 2.5-5 mm, the drying temperature is 50-85℃, and the drying time is 3-5 h.

[0039] In one embodiment, the coating thickness in step H1 is 3 mm, the drying temperature is 85°C, and the drying time is 3.5 h.

[0040] In one embodiment, the low-temperature heat treatment temperature in step H2 is 75-150℃, and the low-temperature heat treatment time is 170-180h.

[0041] In one embodiment, the low-temperature heat treatment temperature in step H2 is 150°C, the heating rate is 0.5°C / min, and the low-temperature heat treatment time is 172h.

[0042] In one embodiment, the carbonization reaction temperature in step H3 is 1300-1500℃, the atmosphere is argon, the heating rate is 2-5℃ / min, and the carbonization reaction time is 2-5h.

[0043] In one embodiment, the carbonization reaction in step H3 is carried out at a temperature of 1400°C, under an argon atmosphere, with a heating rate of 2.5°C / min and a carbonization reaction time of 3 hours.

[0044] In step H3, the oxygen-containing functional groups in the graphene carbonized film are basically removed. At the same time, ammonium lignosulfonate is carbonized, and praseodymium reacts with free carbon to form a double-bonded benzene ring structure. The defects are repaired for the first time, and the carbonized film is obtained by natural cooling.

[0045] In one implementation, the graphitization treatment temperature in step H4 is 2600-3000℃, the heating rate is 0.5-7℃ / min, and the holding time is 3-4h.

[0046] In one implementation, the graphitization process in step H4 is a stepped heating program, which is as follows: heating to 1000-1100℃ at a heating rate of 4-5℃ / min; then heating to 2600-2800℃ at a heating rate of 1-2℃ / min and holding for 2 hours; finally heating to 2600-3000℃ at a heating rate of 0.5-1℃ / min and holding for 1 hour, and then cooling to room temperature after the holding period.

[0047] In one implementation, the graphitization process in step H4 is a stepped heating program, which is as follows: heating to 1000℃ at a heating rate of 5℃ / min; then heating to 2600℃ at a heating rate of 2℃ / min and holding for 2 hours; finally heating to 2800℃ at a heating rate of 0.5℃ / min and holding for 1 hour, and then cooling to room temperature after the holding period.

[0048] In one implementation, the rolling pressure in step H4 is 300-800t.

[0049] In one implementation, the rolling pressure in step H4 is 500t.

[0050] As one implementation method, step H4 specifically involves: stacking graphene carbonized films and intercalating graphite films between single or multiple graphene carbonized films, transferring the film to a graphitization furnace, using a 5 kg graphite plate for natural load-bearing, and raising the temperature to 1000 °C at a heating rate of 5 °C / min; then raising the temperature to a mid-range temperature of 2600 °C at a heating rate of 2 °C / min, and holding it at that temperature for 2 hours; finally, raising the temperature to a graphitization temperature of 2800 °C at a heating rate of 0.5 °C, and holding it at that temperature for 1 hour, cooling it to room temperature after the holding period, and then calendering it at 500 tons to obtain a graphene thermally conductive film.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] (1) The graphene oxide dispersion of the present invention uses an organic polymer-metal composite dispersion to modify graphene oxide, which can obtain a graphene thermal conductive film with higher thickness, fewer defects, more complete crystal structure and excellent comprehensive thermal conductivity.

[0053] (2) The graphene oxide dispersion of the present invention uses a specific amount of ammonium lignosulfonate and praseodymium metal salt, which can improve the thermal dispersibility and thermal conductivity of the thermally conductive film without significantly increasing the viscosity of the graphene oxide dispersion, and can be processed by casting process.

[0054] (3) In the graphene oxide dispersion prepared by the present invention, the lignin is decomposed into carbon during the carbonization stage of the graphene pretreatment film, which provides an additional carbon source for the subsequent carbon atom rearrangement defect repair and also provides free carbon for the oxygen-containing functional groups to carry carbon out, thus avoiding the consumption of carbon atoms on the complete six-membered ring and causing more defects to appear.

[0055] (4) The thermally conductive film prepared by the graphene oxide dispersion of the present invention adopts a graphitization treatment temperature of 2600-3000℃. Praseodymium is tightly bonded to carbon. After the carbon atom double bond is connected to form a benzene ring, the praseodymium quickly escapes and continues to bond to free carbon atoms, cyclically catalyzing graphitization, thereby making the graphene crystal structure tend to be complete.

[0056] (5) The thermally conductive film prepared by the graphene oxide dispersion of the present invention has a high thickness and is prepared by casting method, which has a more efficient preparation efficiency and lower energy consumption. Attached Figure Description

[0057] Figure 1 This is a front view of the graphene thermal conductive film of Embodiment 1 of the present invention;

[0058] Figure 2 This is a cross-section of the graphene thermal conductive film of Embodiment 1 of the present invention;

[0059] Figure 3 This is a SEM microstructure image of the graphene carbonized film after H3 carbonization treatment in Example 1 of the present invention.

[0060] Figure 4 This is a SEM microstructure image of the graphene thermal conductive film prepared in Example 1 of the present invention.

[0061] Figure 5 Raman diagrams of the graphene thermal conductive films of Embodiment 1 and Comparative Example 1 of the present invention;

[0062] Figure 5 In Chinese: 1. Example 1; 2. Comparative Example 1.

[0063] Figure 6 The image shows the XRD pattern of the graphene thermal conductive film of Embodiment 1 of the present invention.

[0064] Figure 7 This is a hot-stage test diagram of the graphene thermal conductive film in Embodiment 1 of the present invention;

[0065] Figure 8 This is a hot-stage test diagram of the graphene thermal conductive film in Embodiment 2 of the present invention;

[0066] Figure 9 This is a hot-stage test diagram of the graphene thermal conductive film in Embodiment 3 of the present invention;

[0067] Figure 10 This is a hot-stage test diagram of the graphene thermal conductive film of Comparative Example 1 of the present invention.

[0068] Figure 11 This is a hot-stage test diagram of the graphene thermal conductive film of Comparative Example 2 of the present invention.

[0069] Figure 12 This is a hot-stage test diagram of the graphene thermal conductive film of Comparative Example 3 of the present invention.

[0070] Figure 13 This is a hot-stage test diagram of the graphene thermal conductive film of Comparative Example 4 of the present invention.

[0071] Figure 14 This is a wide-angle X-ray scattering test image of the graphene thermal conductive film prepared in Example 1 of the present invention;

[0072] Figure 15 This is an azimuth angle-intensity curve of the graphene thermal conductive film prepared in Example 1 of the present invention;

[0073] Figure 16 XPS peak image of the graphene thermal conductive film prepared in Example 1 of this invention;

[0074] Figure 17Images showing the flowability test of the graphene oxide dispersion prepared in Example 1 of this invention;

[0075] Figure 18 The image shows a flowability test result of the graphene oxide dispersion prepared in Comparative Example 3 of this invention. Detailed Implementation

[0076] Example 1

[0077] A graphene oxide dispersion is prepared from the following raw materials: an aqueous organic polymer compound, a metal catalyst, graphene oxide, a pH adjuster, and deionized water; the amount of the aqueous organic polymer compound used is 0.03% of the mass of the graphene oxide, and the amount of the metal catalyst used is 0.01% of the mass of the graphene oxide.

[0078] The aqueous organic polymer compound is ammonium lignosulfonate.

[0079] The metal catalyst is praseodymium chloride. The pH adjuster is ammonia.

[0080] A method for preparing a graphene oxide dispersion includes the following steps:

[0081] S1: Preparation of aqueous organic polymer solutions;

[0082] S2: Adjusts the pH of aqueous organic polymer solutions;

[0083] S3: Add the metal catalyst to the aqueous organic polymer solution after pH adjustment in step S2, seal and sonicate to obtain an organic polymer-metal composite dispersion;

[0084] S4: Add graphene oxide to deionized water and stir to obtain graphene oxide slurry;

[0085] S5: Add the organic polymer-metal composite dispersion to the graphene oxide slurry and stir to mix. Add a pH adjuster to adjust the pH and obtain a mixture.

[0086] S6: Homogenize the mixture from step S5 under high pressure to obtain a graphene oxide dispersion.

[0087] The aqueous organic polymer solution is a solution of 0.0178g of aqueous organic polymer and 300mL of deionized water.

[0088] In step S2, the pH of the aqueous organic polymer solution is adjusted to 9.33.

[0089] The ultrasonic frequency in step S3 is 0.6KW, and the ultrasonic time in step S3 is 1.5h.

[0090] In step S4, graphene oxide is added to deionized water in four portions, and the solid content of the graphene oxide slurry obtained in step S4 is 12 wt%.

[0091] Step S4 specifically involves adding 160g of graphene oxide filter cake (the solid content of graphene oxide in the graphene oxide filter cake is 37.2wt%) into 500g of deionized water in four portions, and stirring for 20 minutes after all the graphene oxide has been added.

[0092] The graphene oxide filter cake was purchased from Baotailong New Materials Co., Ltd.

[0093] The stirring speed in step S4 is 2000 rpm.

[0094] In step S5, the pH is adjusted to 5.5. The stirring rate in step S5 is 2000 rpm, and the homogenization pressure in step S6 is 50 MPa.

[0095] A graphene thermally conductive film is prepared using the above-mentioned graphene oxide dispersion.

[0096] A method for preparing a graphene thermally conductive film includes the following steps:

[0097] H1: The graphene oxide dispersion was coated and dried to obtain a graphene precursor film.

[0098] H2: The graphene precursor film is subjected to low-temperature heat treatment to obtain a graphene pretreated film.

[0099] H3: Carbonize the pretreated graphene film to obtain a carbonized graphene film;

[0100] H4: The graphene carbonized film is graphitized and then rolled at 500t to obtain a graphene thermal conductive film.

[0101] In step H1, the coating thickness is 3 mm, the drying temperature is 85°C, and the drying time is 3.5 h.

[0102] In step H2, the low-temperature heat treatment temperature is 150℃, the heating rate is 0.5℃ / min, and the low-temperature heat treatment time is 172h.

[0103] In step H3, the carbonization reaction temperature is 1400℃, the atmosphere is argon, the heating rate is 2.5℃ / min, and the carbonization reaction time is 3h.

[0104] In step H4, the graphitization process is a stepped heating program, which is as follows: the temperature is increased to 1000℃ at a heating rate of 5℃ / min; then increased to 2600℃ at a heating rate of 2℃ / min and held for 2 hours; finally, the temperature is increased to 2800℃ at a heating rate of 0.5℃ / min and held for 1 hour, and then cooled to room temperature after the holding period.

[0105] A front view of the prepared graphene thermally conductive film is shown. Figure 1 A side view of the prepared graphene thermally conductive film is shown in the image. Figure 2 The SEM microstructure of the graphene carbonized film after H3 carbonization treatment is shown in the figure. Figure 3 The SEM microstructure of the prepared graphene thermally conductive film is shown in the figure. Figure 4 The Raman plot of the prepared graphene thermally conductive film is shown below. Figure 5 The XRD pattern of the prepared graphene thermally conductive film is shown in the figure. Figure 6 .

[0106] Example 2

[0107] A graphene oxide dispersion is prepared from the following raw materials: an aqueous organic polymer compound, a metal catalyst, graphene oxide, a pH adjuster, and deionized water; the amount of the aqueous organic polymer compound used is 0.04% of the mass of the graphene oxide, and the amount of the metal catalyst used is 0.016% of the mass of the graphene oxide.

[0108] In step H1, the coating thickness is 3.5 mm, the drying temperature is 85°C, and the drying time is 3.5 h.

[0109] The remaining specific implementation methods are the same as in Example 1.

[0110] Example 3

[0111] A graphene oxide dispersion is prepared from the following raw materials: an aqueous organic polymer compound, a metal catalyst, graphene oxide, a pH adjuster, and deionized water; the amount of the aqueous organic polymer compound used is 0.06% of the mass of the graphene oxide, and the amount of the metal catalyst used is 0.023% of the mass of the graphene oxide.

[0112] In step H1, the coating thickness is 3.5 mm, the drying temperature is 85°C, and the drying time is 3.5 h.

[0113] The remaining specific implementation methods are the same as in Example 1.

[0114] Comparative Example 1

[0115] A graphene oxide dispersion, the raw materials for which are prepared include: graphene oxide, pH adjuster, and deionized water.

[0116] A method for preparing a graphene oxide dispersion includes the following steps:

[0117] S1: Add graphene oxide to deionized water and stir to obtain graphene oxide slurry;

[0118] S2: A pH adjuster is added to the graphene oxide slurry to obtain a mixture;

[0119] S3: Homogenize the mixture from step S2 under high pressure to obtain a graphene oxide dispersion.

[0120] In step S1, graphene oxide is added to deionized water in four portions, and the solid content of the graphene oxide slurry obtained in step S4 is 12 wt%.

[0121] Step S1 specifically involves adding 160g of graphene oxide filter cake (the solid content of graphene oxide in the graphene oxide filter cake is 37.2wt%) into 500g of deionized water in four portions, and stirring for 20 minutes after all the graphene oxide has been added.

[0122] The stirring speed in step S1 is 2000 rpm.

[0123] In step S2, the pH is adjusted to 5.5. The stirring rate in step S2 is 2000 rpm, and the homogenization pressure in step S3 is 50 MPa.

[0124] A graphene thermal conductive film and its preparation method are described, with the specific implementation method being the same as in Example 1.

[0125] The Raman plot of the prepared graphene thermally conductive film is shown below. Figure 4 .

[0126] Comparative Example 2

[0127] A graphene oxide dispersion and its preparation method are described, with the specific implementation method being the same as in Example 1.

[0128] A graphene thermally conductive film is prepared using the above-mentioned graphene oxide dispersion.

[0129] A method for preparing a graphene thermally conductive film includes the following steps:

[0130] H1: The graphene oxide dispersion was coated and dried to obtain a graphene precursor film.

[0131] H2: The graphene precursor film is subjected to low-temperature heat treatment to obtain a graphene pretreated film.

[0132] H3: Carbonize the pretreated graphene film to obtain a carbonized graphene film;

[0133] H4: Graphene carbonization film is graphitized to obtain graphene thermal conductive film.

[0134] In step H1, the coating thickness is 3 mm, the drying temperature is 85°C, and the drying time is 3.5 h.

[0135] In step H2, the low-temperature heat treatment temperature is 150℃, the heating rate is 0.5℃ / min, and the low-temperature heat treatment time is 172h.

[0136] In step H3, the carbonization reaction temperature is 1400℃, the atmosphere is argon, the heating rate is 2.5℃ / min, and the carbonization reaction time is 3h.

[0137] In step H4, the graphitization process is a stepped heating program, which is as follows: the temperature is increased to 1000℃ at a heating rate of 5℃ / min; then increased to 2600℃ at a heating rate of 2℃ / min and held for 2 hours; finally, the temperature is increased to 3050℃ at a heating rate of 0.5℃ / min and held for 1 hour, and then cooled to room temperature after the holding period.

[0138] Comparative Example 3

[0139] A graphene oxide dispersion is prepared from raw materials including: a metal catalyst, graphene oxide, a pH adjuster, and deionized water; the amount of the metal catalyst used is 0.01% of the mass of the graphene oxide.

[0140] The metal catalyst is praseodymium chloride. The pH adjuster is ammonia.

[0141] A method for preparing a graphene oxide dispersion includes the following steps:

[0142] S1: Add the metal catalyst to 300 mL of deionized water, seal and sonicate to obtain a metal catalyst dispersion;

[0143] S2: Add graphene oxide to deionized water and stir to obtain graphene oxide slurry;

[0144] S3: Add the metal catalyst dispersion to the graphene oxide slurry and stir to mix. Add a pH adjuster to adjust the pH and obtain a mixture.

[0145] S4: Homogenize the mixture from step S3 under high pressure to obtain a graphene oxide dispersion.

[0146] The ultrasonic frequency in step S1 is 0.6KW, and the ultrasonic time in step S1 is 1.5h.

[0147] In step S2, graphene oxide is added to deionized water in four portions, and the solid content of the graphene oxide slurry obtained in step S2 is 12 wt%.

[0148] Step S2 specifically involves adding 160g of graphene oxide filter cake (the solid content of graphene oxide in the graphene oxide filter cake is 37.2wt%) into 500g of deionized water in four portions, and stirring for 20 minutes after all the graphene oxide has been added.

[0149] The stirring speed in step S2 is 2000 rpm.

[0150] In step S3, the pH is adjusted to 5.5. The stirring rate in step S3 is 2000 rpm, and the homogenization pressure in step S4 is 50 MPa.

[0151] A graphene thermal conductive film and its preparation method are described, with the specific implementation method being the same as in Example 1.

[0152] Comparative Example 4

[0153] A graphene oxide dispersion and its preparation method are described, with the specific implementation method being the same as in Example 1.

[0154] A graphene thermally conductive film is prepared using the above-mentioned graphene oxide dispersion.

[0155] A method for preparing a graphene thermally conductive film includes the following steps:

[0156] H1: The graphene oxide dispersion was coated and dried to obtain a graphene precursor film.

[0157] H2: The graphene precursor film is subjected to low-temperature heat treatment to obtain a graphene pretreated film.

[0158] H3: Carbonize the pretreated graphene film to obtain a carbonized graphene film;

[0159] H4: Graphene carbonization film is graphitized to obtain graphene thermal conductive film.

[0160] In step H1, the coating thickness is 3 mm, the drying temperature is 85°C, and the drying time is 3.5 h.

[0161] In step H2, the low-temperature heat treatment temperature is 150℃, the heating rate is 0.5℃ / min, and the low-temperature heat treatment time is 172h.

[0162] In step H3, the carbonization reaction temperature is 1400℃, the atmosphere is argon, the heating rate is 2.5℃ / min, and the carbonization reaction time is 3h.

[0163] In step H4, the graphitization process is a stepped heating program, which is as follows: the temperature is increased to 1000℃ at a heating rate of 10℃ / min; then increased to 2600℃ at a heating rate of 5℃ / min and held for 2 hours; finally, the temperature is increased to 2800℃ at a heating rate of 1℃ / min and held for 1 hour, and then cooled to room temperature after the holding period.

[0164] Performance testing

[0165] The SEM microstructure of the graphene thermally conductive film prepared in Example 1 is shown in Figure 1. Figure 4 ,from Figure 3 As can be seen in Figure 4, the carbonized graphene oxide film layers are not tightly stacked and there are pores between the layers; while after graphitization and calendering, the graphene layers are tightly stacked and have a high degree of orientation.

[0166] Raman plots of the graphene thermally conductive films prepared in Example 1 and Comparative Example 1 are shown below. Figure 5 ,Depend on Figure 5 It can be seen that after graphitization treatment, the sample is at 2681 cm⁻¹ -1 2D peak, 1350cm -1 The D peak and 1500cm -1 Characteristic peaks were observed in all G values, with the 2D peak exhibiting a sharp and symmetrical pattern and a perfect single Lorentzian peak shape. This indicates that the number of graphene layers is close to that of monolayer graphene. Furthermore, it can be seen that the I value of Example 1 with the addition of the organic polymer-metal composite dispersion... D / I G The ratio decreased significantly, indicating that the defect density of graphene was significantly reduced.

[0167] The XRD pattern of the graphene thermally conductive film prepared in Example 1 is shown in Figure 1. Figure 6 ,Depend on Figure 6 It can be seen that after graphitization treatment, the crystal structure of Example 1 tends to be similar to the crystal structure of natural graphite.

[0168] The hot-stage test diagram of the graphene thermally conductive film prepared in Example 1 is shown below. Figure 7 ,Depend on Figure 7 It can be seen that the graphene thermal conductive film prepared in Example 1 has a better actual heat dissipation effect than the graphene thermal conductive film in Comparative Example 1.

[0169] The hot-stage test diagrams of the graphene thermally conductive films prepared in Examples 2 and 3, and Comparative Examples 1, 2, 3, and 4 are shown in Figures 8-13.

[0170] The wide-angle X-ray scattering test image of the graphene thermally conductive film prepared in Example 1 is shown below. Figure 14 The azimuth angle-intensity curve of the graphene thermally conductive film prepared in Example 1 is shown in the figure. Figure 15 ,Depend on Figure 14 As shown in Figure 15, the graphene thermally conductive film prepared in Example 1 has a smaller wide-angle XRD diffraction spot, and at the same time... Figure 15 The full width at half maximum (FWHM) value is relatively large at 16.1°, f = 0.91, and the peaks at 0° and 180° azimuth angles are relatively sharp, indicating that the carbon atoms in graphene have a high degree of crystal orientation, which provides a structural basis for the high thermal conductivity.

[0171] The XPS elemental peak shape of the graphene thermally conductive film prepared in Example 1 is shown in the figure. Figure 16 The analysis results are shown in Table 1 below.

[0172] Table 1

[0173] Binding energy / eV Peak height / eV Peak area (cps, eV) Percentage / % C = C 283.94 1.44 13738.36 7.27 CC 284.8 0.68 135865.4 71.92 CO 285.8 1.34 33876.71 17.94 C=O 287.45 1.41 5408.95 2.87

[0174] The results show that the carbon spectrum contains carbon-carbon single bonds, carbon-carbon double bonds, carbon-oxygen single bonds, and carbon-oxygen double bonds. Among them, the carbon-carbon bond content is 79.19%, which indicates high carbon-carbon bond content and good thermal conductivity, while the carbon-oxygen bond content is 20.81%.

[0175] Equal amounts of the graphene oxide dispersions prepared in Example 1 and Comparative Example 3 were dropped onto one end of a steel ruler, tilted at the same angle, and the flowability was tested. The test results for Example 1 are shown below. Figure 17 The test results for Comparative Example 3 are shown below. Figure 18 .

[0176] The test results show that the flowability of the graphene oxide slurry in Example 1 is better than that in Comparative Example 3, indicating that the presence of lignosulfonate greatly reduces the viscosity of the slurry and improves its flowability.

[0177] Thermal diffusivity performance test: The LFA (laser flare method) was used to test the graphene thermal conductive films of the examples and comparative examples. The films were cut into a certain size, with a diameter of 25.2 mm and a thickness of 0.15 mm, and the thermal diffusivity and thermal conductivity were tested. The test results are shown in Table 2.

[0178] Table 2

[0179]

[0180]

[0181] Analysis: The viscosity of the graphene oxide dispersion prepared in Comparative Example 1 was too high to be measured (>100,000 cps). This was because no organic polymer-metal composite dispersion was introduced. Compared with the graphene thermal conductive film prepared in Example 1, simply using high temperature to promote carbon atom rearrangement to repair defects resulted in low efficiency and more defects, thereby reducing phonon transmission efficiency. Secondly, due to the high concentration of the graphene oxide dispersion, the interaction between graphene oxide sheets was strong. Simply using shear dispersion and homogenization could not suppress or eliminate the strong interaction between sheets, resulting in an excessively high actual viscosity of the slurry, which lost its fluidity and was not conducive to coating.

[0182] Example 1 obtained a graphene thermally conductive film with a higher thermal conductivity than Comparative Example 2 at a graphitization temperature lower than that of Comparative Example 2. The reason is that simply increasing the graphitization temperature cannot fundamentally solve the problem of the high energy barrier of carbon atom rearrangement. This leads to the existence of "diminishing marginal returns," that is, as the temperature increases, the number of defect repairs tends to stabilize, the resistance to carbon atom rearrangement gradually increases, the defect repair efficiency decreases, and the rate of increase in thermal conductivity decreases.

[0183] The viscosity of the graphene oxide dispersion prepared in Comparative Example 3 was too high to be measured (>100,000 cps). This was because ammonium lignosulfonate was not introduced. The addition of praseodymium chloride alone would disrupt the charge distribution on the surface of the graphene oxide sheets, thereby causing a surge in the absolute value of the Zata potential of the system, resulting in increased viscosity and severe loss of fluidity. On the other hand, due to the severe loss of fluidity of the slurry, the self-assembly orientation of the graphene oxide sheets was reduced during coating, ultimately resulting in no significant improvement in the thermal conductivity of the graphene thermal conductive film with praseodymium chloride alone.

[0184] The graphene thermal conductive film in Comparative Example 4 was partially cracked. Due to the excessively rapid temperature rise rate, the diffusion of praseodymium atoms was too fast, preventing complete repair of the defects and reducing the defect repair efficiency. Consequently, the thermal conductivity of the graphene thermal conductive film was lower than that in Example 1. Furthermore, the excessively rapid heating rate exacerbated the stress imbalance in the film, leading to cracking and breakage.

Claims

1. A graphene oxide dispersion, characterized in that, The raw materials for preparation include: an aqueous organic polymer compound, a metal catalyst, graphene oxide, a pH adjuster, and deionized water; the amount of the aqueous organic polymer compound used is 0.03-0.8% of the mass of graphene oxide, and the amount of the metal catalyst used is 0.01-0.08% of the mass of graphene oxide. The aqueous organic polymer compound is a lignin derivative; The metal catalyst is a praseodymium metal salt.

2. The graphene oxide dispersion according to claim 1, characterized in that, The lignin derivative is selected from at least one of ammonium lignin sulfonate, sodium lignin sulfonate, magnesium lignin sulfonate, or calcium lignin sulfonate.

3. A method for preparing the graphene oxide dispersion according to any one of claims 1-2, characterized in that, Includes the following steps: S1: Preparation of aqueous organic polymer solutions; S2: Adjusts the pH of aqueous organic polymer solutions; S3: Add the metal catalyst to the aqueous organic polymer solution after pH adjustment in step S2, seal and sonicate to obtain an organic polymer-metal composite dispersion; S4: Add graphene oxide to deionized water and stir to obtain graphene oxide slurry; S5: Add the organic polymer-metal composite dispersion to the graphene oxide slurry and stir to mix. Add a pH adjuster to adjust the pH and obtain a mixture. S6: Homogenize the mixture from step S5 under high pressure to obtain a graphene oxide dispersion.

4. The method for preparing the graphene oxide dispersion according to claim 3, characterized in that, In step S2, the pH of the aqueous organic polymer solution is adjusted to 9-9.

5.

5. The method for preparing the graphene oxide dispersion according to claim 3, characterized in that, In step S4, graphene oxide is added to deionized water in 3-5 portions, with each addition of graphene oxide being 2-4% of the mass of deionized water. The solid content of the graphene oxide slurry obtained in step S4 is 10-15 wt%.

6. A graphene thermally conductive film, characterized in that, It was prepared using the graphene oxide dispersion according to any one of claims 1-2.

7. A method for preparing a graphene thermally conductive film according to claim 6, characterized in that, Includes the following steps: H1: The graphene oxide dispersion was coated and dried to obtain a graphene precursor film. H2: The graphene precursor film is subjected to low-temperature heat treatment to obtain a graphene pretreated film. H3: Carbonize the pretreated graphene film to obtain a carbonized graphene film; H4: Graphene carbonization film is graphitized and then rolled to obtain graphene thermal conductive film.

8. The method for preparing the graphene thermally conductive film according to claim 7, characterized in that, In step H4, the graphitization treatment temperature is 2600-3000℃, the heating rate is 0.5-7℃ / min, and the holding time is 3-4h.

9. The method for preparing the graphene thermally conductive film according to claim 7, characterized in that, In step H4, the graphitization process is a stepped heating procedure, which is as follows: the temperature is increased to 1000-1100℃ at a heating rate of 4-5℃ / min; then increased to 2600-2800℃ at a heating rate of 1-2℃ / min and held for 2 hours; finally, the temperature is increased to 2600-3000℃ at a heating rate of 0.5-1℃ / min and held for 1 hour, and then cooled to room temperature after the holding period.

Citation Information

Patent Citations

  • Preparation method and product of high-density graphene thermally conductive film with functional group regulation

    CN112794314B

  • High-solid-content graphene oxide slurry, graphene oxide heat-conducting film and preparation methods of graphene oxide slurry and graphene oxide heat-conducting film

    CN117263175A

  • Method for preparing graphene compounds and graphene oxide compounds with high efficiency

    CN101857221A

  • Method for preparing natural high-molecular material by utilization of rare earth metal ion coordination

    CN106243240A