Forging and heat treatment process for single-row tapered roller bearing ring

Through improved forging and heat treatment processes, the problem of single-row tapered roller bearing rings being prone to cracking under special circumstances has been solved, the yield rate and assembly rate have been improved, and production costs have been reduced.

CN120734240APending Publication Date: 2025-10-03哈尔滨轴承制造有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202511152571.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-18
Publication Date
2025-10-03

AI Technical Summary

Technical Problem

When existing single-row tapered roller bearing rings are made of high-carbon chromium stainless bearing steel G102Cr18Mo under special conditions, they are prone to cracking and large elliptical deformation during the forging process, resulting in a high scrap rate and increased production costs.

Method used

The cutting, forging, annealing, turning and heat treatment processes are adopted, including preheating of material sections, final heating, forging, rolling and forming, ash cooling process and multiple preheating quenching and cooling. Nitrogen protection and high-pressure nitrogen cooling are used to control the heating temperature and time to avoid cracks and deformation.

Benefits of technology

It improves the material yield, reduces forging and rolling cracks, ensures the quality of forgings, reduces production costs, and improves the fit rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120734240A_ABST
    Figure CN120734240A_ABST
Patent Text Reader

Abstract

The invention discloses a forging and heat treatment process for a single-row tapered roller bearing ring. Raw materials are sequentially subjected to cutting, forging, annealing, turning and heat treatment, and then the single-row tapered roller bearing ring is obtained. The hot-rolled polished bar is used as the raw material, so that the surface smoothness of the bar is ensured, no crack occurs during forging, and the yield of the material is improved; a secondary heating process is adopted after forging, it is guaranteed that the forge piece is in a reasonable temperature interval during rolling expansion, the phenomenon of rolling expansion cracks does not occur, and the product quality of the forge piece is guaranteed; the ash cooling process is adopted to replace slow cooling along with a furnace in an electric furnace, the process method is simple, practical and low in cost, and electric energy is saved on the premise that the quality of the forge piece is guaranteed; three-time preheating is adopted. The vacuum heating and heat conduction mode is radiation heating, and a repeated preheating mode is adopted, so that the ferrule in the furnace can be uniformly heated, the heating temperature is slowly increased, thermal stress in the ferrule can be reduced, and the quality of the quenched ferrule is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of forging and heat treatment of a single-row tapered roller bearing ring, and more particularly to a forging and heat treatment process of a single-row tapered roller bearing ring. Background Art

[0002] Single-row tapered roller bearings are widely used in industries such as automobiles, rolling mills, food processing machinery, metallurgical machinery, plastics machinery, and medical equipment. They consist of inner and outer rings, rolling elements, and a retainer. Conventional single-row tapered roller bearing rings are made of GCr15 / GCr15SiMn high-carbon chromium bearing steel. However, for machinery operating in special environments, such as humid and marine environments, single-row tapered roller bearings must exhibit a certain degree of corrosion resistance. Therefore, high-carbon chromium stainless steel G102Cr18Mo is used for the rings during bearing manufacturing.

[0003] The main chemical components of high carbon chromium stainless bearing steel G102Cr18Mo are: C0.95-1.10%, Si≤0.80%, Mn≤0.80%, Cr16.0-18.0%, Mo0.40-0.70%, Ni≤0.25%, Cu≤0.25%.

[0004] High-carbon chromium stainless steel G102Cr18Mo is used in bearing rings with outer diameters ranging from 50 to 200 mm. Bearing rings made of this material are prone to cracking during forging and exhibit significant elliptical deformation during vacuum heat treatment. Consequently, rings produced using this material have a high scrap rate, affecting the bearing's fit rate and increasing production costs. Summary of the Invention

[0005] In view of this, the present invention provides a forging and heat treatment process for a single-row tapered roller bearing ring to solve the technical problems encountered in the background technology.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A forging and heat treatment process for a single-row tapered roller bearing ring, wherein the raw material is sequentially cut, forged, annealed, turned, and heat treated to obtain the single-row tapered roller bearing ring;

[0008] Wherein, the forging includes:

[0009] Material section preheating: preheating temperature: 800-850℃, holding time after color transparency 40±5min, protective atmosphere: nitrogen;

[0010] Final heating of material section: After the material section reaches the set preheating time, it is automatically taken out from the preheating furnace and transferred to a high-temperature rotary bottom heating furnace. The heating temperature is 1100±10℃. The holding time after color transparency is 6-15 minutes. The protective atmosphere is nitrogen.

[0011] Segment forging: Use a press or free forging for forging. Before forging, the forging die is preheated at 150-300°C. The forging process is divided into: upsetting, forming, punching, and obtaining a ring forging. The final forging temperature should be ≥950°C.

[0012] Secondary heating: The ring forging is subjected to secondary heating, the heating temperature is 1100±10℃, the holding time after reaching the temperature is 3-6min, and the protective atmosphere is nitrogen;

[0013] Rolling forming: Before rolling, apply yellow glycerin on the rolling shaft and then roll the ring forging. The rolling time is 10-15 seconds. The temperature after rolling is ≥900℃. After rolling, spray water to cool the rolling shaft and use tooling to grind off the oxide scale on the rolling shaft.

[0014] Slow cooling after forging: The forgings after rolling are immediately buried in an ash box filled with dry lime, and the forgings are taken out when they are cooled to below 200℃ in the dry lime.

[0015] Preferably, the heat treatment comprises:

[0016] Before cleaning the outer and inner rings of bearings:

[0017] The bearing parts are placed on the tooling according to the process requirements and enter the pre-cleaning station, where they are cleaned with detergent and then with water. The cleaning temperature is 50-80°C and the cleaning time for each step is 6-10 minutes. After cleaning, they are dried at 110-130°C and the drying time is 6-10 minutes.

[0018] Quenching heating:

[0019] The cleaned bearing parts enter the vacuum heating furnace, are evacuated to 5-10Pa, and heated. The first preheating stage: preheating temperature: 500±10℃, from room temperature to 500℃, the heating rate of the equipment is 8-12℃ / min, and after reaching temperature, it is kept warm for 15-30min; the second preheating stage: preheating temperature: 800±10℃, from 500 to 800℃, the heating rate of the equipment is 8-12℃ / min, and after reaching temperature, it is kept warm for 30-50min; the third preheating stage: preheating temperature: 1000±10℃, from 800 to 1000℃, the heating rate of the equipment is 6-10℃ / min, and after reaching temperature, it is kept warm for 10-20min; final heating: final heating temperature: 1050±10℃, from 1000 to 1050℃, the heating rate of the equipment is 1-3℃ / min, and after reaching temperature, it is kept warm for 60-80min;

[0020] Quenching cooling:

[0021] The heated bearing parts are cooled in the furnace using high-pressure nitrogen. The gas quenching pressure is 4-6 bar. When the bearing rings are cooled to below 60°C in the furnace, they are taken out of the furnace and air-cooled to room temperature.

[0022] Cold treatment

[0023] The quenched bearing rings are placed in a cold treatment device at a temperature of -70 to -80°C.

[0024] Cold treatment time: 120±10min. After the cold treatment is completed, turn off the liquid nitrogen, and the bearing parts will be slowly heated to room temperature in the deep cold box, and then immediately undergo tempering treatment;

[0025] One tempering

[0026] The first tempering treatment, tempering temperature: 160 ~ 180 ℃, tempering time: 2.5 ~ 3.5h;

[0027] Secondary tempering

[0028] After the first tempering is completed, the bearing parts are cooled to room temperature and then subjected to a second tempering treatment. The tempering temperature is 160-180°C and the tempering time is 2.5-3.5 hours.

[0029] Preferably, the cutting comprises:

[0030] The raw materials are hot-rolled polished bars. The weight dispersion of the material sections after cutting is controlled within ±5g. After cutting, the burrs are removed to ensure that the cut surface is smooth and flat.

[0031] Preferably, the annealing is as follows: preheating temperature: 750±10℃, holding time after reaching temperature: 4h±10min; heating temperature: 850±10℃, holding time after reaching temperature: 4h±10min; cooling with the furnace to 730℃, isothermal temperature 730±10℃, isothermal time 4h±10min, cooling with the furnace to 600℃ at a cooling rate of 10-15℃ / min, and then taking out of the furnace and air cooling to room temperature after reaching 600℃.

[0032] Preferably, the turning process is: using a horizontal lathe to process the annealed workpiece into a turned workpiece of qualified size according to the process drawing.

[0033] It can be seen from the above technical solutions that compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The raw materials used in the existing process are hot-rolled bars. During forging, the proportion of forging cracks is 60%. However, the raw materials of the present invention use hot-rolled polished bars to ensure the surface smoothness of the bars. During forging, no cracks appear, thereby improving the yield rate of the material.

[0035] 2. The existing process is to directly roll-form after forging. Since small forgings cool down quickly, especially in winter, and the toughness of high-carbon chromium stainless bearing steel is poor, the temperature is low during rolling, which will cause rolling cracks. According to statistics, the proportion of cracks occurring during rolling is 5%. The present invention adopts a secondary heating process after forging to ensure that the forgings are in a reasonable temperature range during rolling. The method of the present invention does not cause rolling cracks, thereby ensuring the product quality of the forgings.

[0036] 3. Compared with the existing process, the process method of the present invention adopts the ash cooling process to replace the slow cooling in the electric furnace. The process method is simple, practical, low-cost, and saves electricity while ensuring the quality of forgings.

[0037] 4. The existing process uses one preheating step during the vacuum heating stage of heat treatment, while the method of the present invention uses three preheating steps. Because vacuum heating uses radiation heating as the heat conduction method, the use of multiple preheating steps can ensure uniform heating of the ferrule in the furnace and a slow rise in the heating temperature, which can reduce the thermal stress in the ferrule and ensure the quality of the ferrule after quenching. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0039] Figure 1 This is a photo of the material segment cracking during forging using the existing process;

[0040] Figure 2 This is a photo of the cracking of the material section after forging and rolling using the existing process;

[0041] Figure 3 This is a photo of the material section after forging and rolling according to the process of the present invention. DETAILED DESCRIPTION

[0042] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0043] Example 1

[0044] The heat treatment process of the outer ring of a single-row tapered roller bearing 33010 made of G102Cr18Mo high carbon chromium stainless bearing steel comprises the following steps:

[0045] 1. Cutting

[0046] The raw material used is hot-rolled, polished bar stock with a diameter of 40mm. The bar surface is not allowed to have exposed oxide scale, scratches, scars, or other defects. The bar stock is cut using a band saw into sections of 57.6mm in length. After cutting, if the outer diameter of the section has burrs greater than 1mm in height, they should be manually removed using an angle grinder to ensure a smooth cut surface.

[0047] 2. Forging

[0048] 2.1 Preheating of Material Sections: Material sections are placed into the rotary furnace one by one according to the equipment cycle settings. The preheating temperature is 850°C, and the holding time after color transparency is 40±5 minutes. The protective atmosphere is nitrogen. The material sections are arranged in a fixed gap within the rotary furnace and heated independently. The first-in-first-out system ensures that the heating and holding times of the same batch of material sections are consistent.

[0049] 2.2 Final Heating of Segments: After the preheating time has elapsed, the segments are automatically removed from the preheating furnace and transferred to a high-temperature rotary furnace. The heating temperature is 1100 ± 10°C, and the holding time after color transparency is 8 minutes. The protective atmosphere is nitrogen. Segments are spaced apart within the rotary furnace and heated independently, using a first-in, first-out (FIFO) system to ensure consistent heating and holding times for all segments within the same batch.

[0050] 2.3 Segment Forging: Forging is performed using a 160T press. The press must be preheated to 200°C before forging. The forging process includes upsetting, forming, and punching to produce ring-shaped forgings. The final forging temperature should be ≥ 950°C and is measured using an infrared thermometer.

[0051] 2.4 Secondary heating: The temperature after final forging is relatively low. In order to ensure the quality after rolling and reduce the occurrence of rolling cracks, the ring forgings need to be placed in a high-temperature rotary bottom heating furnace for secondary heating. The heating temperature is: 1100±10℃, the holding time after reaching temperature is: 5min, and the protective atmosphere is: nitrogen.

[0052] 2.5 Rolling forming: Before each rolling, apply yellow glycerin on the rolling shaft and then roll the ring forging. The rolling time is 12S to obtain the ring forging that meets the process size. The temperature after rolling is ≥900℃. After rolling, spray water to cool the rolling shaft and use tooling to grind off the oxide scale on the rolling shaft.

[0053] 2.6 Slow Cooling After Forging: Immediately bury the rolled forgings in an ash box filled with dry lime. The ash box should be 60 cm long, 40 cm wide, and 40 cm high. Place the ash box next to the rolling machine and support it with heat-resistant furnace bricks. Once buried, the forgings must not come into contact with the ash box walls. Remove the forgings from the dry lime after slowly cooling to less than 200°C.

[0054] 3. Annealing

[0055] Place the forgings in a special heat-resistant steel basket of a box-type annealing furnace. The annealing process is as follows: preheating temperature: 750±10℃, holding time after reaching temperature: 4h±10min; heating temperature: 850±10℃, holding time after reaching temperature: 4h±10min; cooling with the furnace to 730℃, isothermal temperature 730±10℃, isothermal time 4h±10min, cooling with the furnace to 600℃ at a cooling rate of 10-15℃ / min, and air cooling to room temperature after reaching 600℃.

[0056] 4. Turning

[0057] Use a horizontal lathe to process forgings into turned workpieces of qualified size according to the process drawings.

[0058] 5. Heat treatment

[0059] 5.1 Clean the outer and inner rings of the bearings before use

[0060] Pre-cleaning removes impurities such as cutting fluid, dust, and oil from the bearing surface, ensuring a consistent appearance and color after quenching and tempering. Bearing parts are placed on a fixture according to process requirements and proceed to the pre-cleaning station, where they are cleaned with both a detergent and water. The cleaning temperature is 80°C, and each cleaning cycle lasts 10 minutes. After cleaning, drying is performed at 120°C for 10 minutes.

[0061] 5.2 Quenching heating:

[0062] The quenching heating uses Beijing Zhongfu Yueda JVTF966 vacuum heating furnace;

[0063] The cleaned bearing parts enter the vacuum heating furnace, and after closing the furnace door, vacuuming begins. When the vacuum reaches 6 Pa, the equipment begins to heat up. The first preheating stage: preheating temperature: 500±10℃, from room temperature to 500℃, the equipment's heating rate is 8℃ / min, and after reaching temperature, it is kept warm for 20 minutes. The second preheating stage: preheating temperature: 800±10℃, from 500 to 800℃, the equipment's heating rate is 8℃ / min, and after reaching temperature, it is kept warm for 40 minutes. The third preheating stage: preheating temperature: 1000±10℃, from 800 to 1000℃, the equipment's heating rate is 6℃ / min, and after reaching temperature, it is kept warm for 15 minutes. The final heating stage: final heating temperature: 1050±10℃, from 1000 to 1050℃, the equipment's heating rate is 2℃ / min, and after reaching temperature, it is kept warm for 60 minutes.

[0064] 5.3 Quenching and cooling:

[0065] Vacuum gas quenching: After heating, the bearing parts are cooled in a furnace using high-pressure nitrogen. The gas quenching pressure is 4 bar. When the bearing rings are cooled to below 60°C in the furnace, they are taken out of the furnace and air-cooled to room temperature.

[0066] 5.4 Cold treatment

[0067] The quenched bearing rings are placed in a cold treatment device at a temperature of -80°C.

[0068] Cold treatment time: 120±10min. After the cold treatment is completed, turn off the liquid nitrogen, and the bearing parts will be slowly heated to room temperature in the deep cold box, and then immediately undergo tempering treatment.

[0069] 5.5 Primary tempering

[0070] The first tempering treatment, tempering temperature: 170℃, tempering time: 3h.

[0071] 5.6 Secondary tempering

[0072] After the first tempering is completed, the bearing parts are cooled to room temperature and then subjected to a second tempering treatment at a tempering temperature of 170°C and a tempering time of 3 hours.

[0073] Example 2

[0074] The heat treatment process of the outer ring of a single-row tapered roller bearing 32008 made of G102Cr18Mo high carbon chromium stainless bearing steel comprises the following steps:

[0075] 1. Cutting

[0076] The raw material used is hot-rolled, polished bar stock with a diameter of 35mm. The bar surface is not allowed to have exposed oxide scale, scratches, scars, or other defects. The bar stock is cut using a band saw into sections of 52.5mm in length. After cutting, if the outer diameter of the section has burrs greater than 1mm in height, they should be manually removed using an angle grinder to ensure a smooth cut surface.

[0077] 2. Forging

[0078] 2.1 Preheating of Material Sections: Material sections are placed into the rotary furnace one by one according to the equipment cycle settings. The preheating temperature is 850°C, and the holding time after color transparency is 40±5 minutes. The protective atmosphere is nitrogen. The material sections are arranged in a fixed gap within the rotary furnace and heated independently. The first-in-first-out system ensures that the heating and holding times of the same batch of material sections are consistent.

[0079] 2.2 Final Heating of Segments: After the preheating time has elapsed, the segments are automatically removed from the preheating furnace and transferred to a high-temperature rotary furnace. The heating temperature is 1100 ± 10°C, and the holding time after color transparency is 8 minutes. The protective atmosphere is nitrogen. Segments are spaced apart within the rotary furnace and heated independently, using a first-in, first-out (FIFO) system to ensure consistent heating and holding times for all segments within the same batch.

[0080] 2.3 Segment Forging: Forging is performed using a 160T press. The press must be preheated to 200°C before forging. The forging process includes upsetting, forming, and punching to produce ring-shaped forgings. The final forging temperature should be ≥ 950°C and is measured using an infrared thermometer.

[0081] 2.4 Secondary heating: The temperature after final forging is relatively low. In order to ensure the quality after rolling and reduce the occurrence of rolling cracks, the ring forgings need to be placed in a high-temperature rotary bottom heating furnace for secondary heating. The heating temperature is: 1100±10℃, the holding time after reaching temperature is: 5min, and the protective atmosphere is: nitrogen.

[0082] 2.5 Rolling forming: Before each rolling, apply yellow glycerin on the rolling shaft and then roll the ring forging. The rolling time is 10S to obtain the ring forging that meets the process size. The temperature after rolling is ≥900℃. After rolling, spray water to cool the rolling shaft and use tooling to grind off the oxide scale on the rolling shaft.

[0083] 2.6 Slow Cooling After Forging: Immediately bury the rolled forgings in an ash box filled with dry lime. The ash box should be 60 cm long, 40 cm wide, and 40 cm high. Place the ash box next to the rolling machine and support it with heat-resistant furnace bricks. Once buried, the forgings must not come into contact with the ash box walls. Remove the forgings from the dry lime after slowly cooling to less than 200°C.

[0084] 3. Annealing

[0085] Place the forgings in a special heat-resistant steel basket of a box-type annealing furnace. The annealing process is as follows: preheating temperature: 750±10℃, holding time after reaching temperature: 4h±10min; heating temperature: 850±10℃, holding time after reaching temperature: 4h±10min; cooling with the furnace to 730℃, isothermal temperature 730±10℃, isothermal time 4h±10min, cooling with the furnace to 600℃ at a cooling rate of 10-15℃ / min, and air cooling to room temperature after reaching 600℃.

[0086] 4. Turning

[0087] Use a horizontal lathe to process forgings into turned workpieces of qualified size according to the process drawings.

[0088] 5. Heat treatment

[0089] 5.1 Clean the outer and inner rings of the bearings before use

[0090] Pre-cleaning removes impurities such as cutting fluid, dust, and oil from the bearing surface, ensuring a consistent appearance and color after quenching and tempering. Bearing parts are placed on a fixture according to process requirements and proceed to the pre-cleaning station, where they are cleaned with both a detergent and water. The cleaning temperature is 80°C, and each cleaning cycle lasts 10 minutes. After cleaning, drying is performed at 120°C for 10 minutes.

[0091] 5.2 Quenching heating:

[0092] The quenching heating uses Beijing Zhongfu Yueda JVTF966 vacuum heating furnace;

[0093] The cleaned bearing parts enter the vacuum heating furnace, and after closing the furnace door, vacuuming begins. When the vacuum reaches 6 Pa, the equipment begins to heat up. The first preheating stage: preheating temperature: 500±10℃, from room temperature to 500℃, the equipment's heating rate is: 10℃ / min, after reaching temperature, keep warm for 15 minutes; the second preheating stage: preheating temperature: 800±10℃, from 500 to 800℃, the equipment's heating rate is: 10℃ / min, after reaching temperature, keep warm for 30 minutes; the third preheating stage: preheating temperature: 1000±10℃, from 800 to 1000℃, the equipment's heating rate is: 8℃ / min, after reaching temperature, keep warm for 10 minutes; the final heating stage: final heating temperature: 1050±10℃, from 1000 to 1050℃, the equipment's heating rate is: 2℃ / min, after reaching temperature, keep warm for 60 minutes.

[0094] 5.3 Quenching and cooling:

[0095] Vacuum gas quenching: After heating, the bearing parts are cooled in a furnace using high-pressure nitrogen. The gas quenching pressure is 4 bar. When the bearing rings are cooled to below 60°C in the furnace, they are taken out of the furnace and air-cooled to room temperature.

[0096] 5.4 Cold treatment

[0097] The quenched bearing rings are placed in a cold treatment device at a temperature of -80°C.

[0098] Cold treatment time: 120±10min. After the cold treatment is completed, turn off the liquid nitrogen, and the bearing parts will be slowly heated to room temperature in the deep cold box, and then immediately undergo tempering treatment.

[0099] 5.5 Primary tempering

[0100] The first tempering treatment, tempering temperature: 170℃, tempering time: 3h.

[0101] 5.6 Secondary tempering

[0102] After the first tempering is completed, the bearing parts are cooled to room temperature and then subjected to a second tempering treatment at a tempering temperature of 170°C and a tempering time of 3 hours.

[0103] Example 3

[0104] The heat treatment process of the inner ring of a single-row tapered roller bearing 32016 made of G102Cr18Mo high carbon chromium stainless bearing steel comprises the following steps:

[0105] 1. Cutting

[0106] The raw material used is hot-rolled, polished bar stock with a diameter of 45mm. The bar surface is not allowed to have exposed oxide scale, scratches, scars, or other defects. The bar stock is cut using a band saw into sections of 65mm in length. After cutting, if there are burrs on the outer diameter of the section with a height greater than 1mm, they should be manually removed using an angle grinder to ensure a smooth cut surface.

[0107] 2. Forging

[0108] 2.1 Preheating of Material Sections: Material sections are placed into the rotary furnace one by one according to the equipment cycle settings. The preheating temperature is 850°C, and the holding time after color transparency is 40±5 minutes. The protective atmosphere is nitrogen. The material sections are arranged in a fixed gap within the rotary furnace and heated independently. The first-in-first-out system ensures that the heating and holding times of the same batch of material sections are consistent.

[0109] 2.2 Final Heating of Segments: After the preheating time has elapsed, the segments are automatically removed from the preheating furnace and transferred to a high-temperature rotary furnace. The heating temperature is 1100 ± 10°C, and the holding time after color transparency is 8 minutes. The protective atmosphere is nitrogen. Segments are spaced apart within the rotary furnace and heated independently, using a first-in, first-out (FIFO) system to ensure consistent heating and holding times for all segments within the same batch.

[0110] 2.3 Segment Forging: Forging is performed using a 160T press. The press must be preheated to 200°C before forging. The forging process includes upsetting, forming, and punching to produce ring-shaped forgings. The final forging temperature should be ≥ 950°C and is measured using an infrared thermometer.

[0111] 2.4 Secondary heating: The temperature after final forging is relatively low. In order to ensure the quality after rolling and reduce the occurrence of rolling cracks, the ring forgings need to be placed in a high-temperature rotary bottom heating furnace for secondary heating. The heating temperature is: 1100±10℃, the holding time after reaching temperature is: 5min, and the protective atmosphere is: nitrogen.

[0112] 2.5 Rolling forming: Before each rolling, apply yellow glycerin on the rolling shaft and then roll the ring forging. The rolling time is 10S to obtain the ring forging that meets the process size. The temperature after rolling is ≥900℃. After rolling, spray water to cool the rolling shaft and use tooling to grind off the oxide scale on the rolling shaft.

[0113] 2.6 Slow Cooling After Forging: Immediately bury the rolled forgings in an ash box filled with dry lime. The ash box should be 80 cm long, 50 cm wide, and 50 cm high. Place the ash box next to the rolling machine and support it with heat-resistant furnace bricks. Once buried, the forgings must not come into contact with the ash box walls. Remove the forgings from the dry lime after slowly cooling to less than 200°C.

[0114] 3. Annealing

[0115] Place the forgings in a special heat-resistant steel basket of a box-type annealing furnace. The annealing process is as follows: preheating temperature: 750±10℃, holding time after reaching temperature: 4h±10min; heating temperature: 850±10℃, holding time after reaching temperature: 4h±10min; cooling with the furnace to 730℃, isothermal temperature 730±10℃, isothermal time 4h±10min, cooling with the furnace to 600℃ at a cooling rate of 10-15℃ / min, and air cooling to room temperature after reaching 600℃.

[0116] 4. Turning

[0117] Use a horizontal lathe to process forgings into turned workpieces of qualified size according to the process drawings.

[0118] 5. Heat treatment

[0119] 5.1 Clean the outer and inner rings of the bearings before use

[0120] Pre-cleaning removes impurities such as cutting fluid, dust, and oil from the bearing surface, ensuring a consistent appearance and color after quenching and tempering. Bearing parts are placed on a fixture according to process requirements and proceed to the pre-cleaning station, where they are cleaned with both a detergent and water. The cleaning temperature is 80°C, and each cleaning cycle lasts 10 minutes. After cleaning, drying is performed at 120°C for 10 minutes.

[0121] 5.2 Quenching heating:

[0122] The quenching heating uses Beijing Zhongfu Yueda JVTF966 vacuum heating furnace;

[0123] The cleaned bearing parts enter the vacuum heating furnace, and after closing the furnace door, vacuuming begins. When the vacuum reaches 6 Pa, the equipment begins to heat up. The first preheating stage: preheating temperature: 500±10℃, from room temperature to 500℃, the equipment's heating rate is 8℃ / min, and after reaching temperature, it is kept warm for 20 minutes. The second preheating stage: preheating temperature: 800±10℃, from 500 to 800℃, the equipment's heating rate is 8℃ / min, and after reaching temperature, it is kept warm for 40 minutes. The third preheating stage: preheating temperature: 1000±10℃, from 800 to 1000℃, the equipment's heating rate is 8℃ / min, and after reaching temperature, it is kept warm for 15 minutes. The final heating stage: final heating temperature: 1050±10℃, from 1000 to 1050℃, the equipment's heating rate is 2℃ / min, and after reaching temperature, it is kept warm for 70 minutes.

[0124] 5.3 Quenching and cooling:

[0125] Vacuum gas quenching: After heating, the bearing parts are cooled in a furnace using high-pressure nitrogen. The gas quenching pressure is 6 bar. When the bearing rings are cooled to below 60°C in the furnace, they are taken out of the furnace and air-cooled to room temperature.

[0126] 5.4 Cold treatment

[0127] The quenched bearing rings are placed in a cold treatment device at a temperature of -80°C.

[0128] Cold treatment time: 120±10min. After the cold treatment is completed, turn off the liquid nitrogen, and the bearing parts will be slowly heated to room temperature in the deep cold box, and then immediately undergo tempering treatment.

[0129] 5.5 Primary tempering

[0130] The first tempering treatment, tempering temperature: 170℃, tempering time: 3h.

[0131] 5.6 Secondary tempering

[0132] After the first tempering is completed, the bearing parts are cooled to room temperature and then subjected to a second tempering treatment at a tempering temperature of 170°C and a tempering time of 3 hours.

[0133] Comparative Example 1 (Existing Process)

[0134] 1. Cutting

[0135] The raw materials are hot-rolled bars, which are cut using a circular saw or band saw to ensure that the weight dispersion of the material segments is controlled within ±5g. After cutting, if there are burrs on the outer diameter surface of the material segment with a height of >1mm, the burrs should be removed manually using a grinding wheel or angle grinder to ensure a smooth and flat cut surface.

[0136] 2. Forging

[0137] 2.1 Preheating of Material Sections: Material sections are placed into the rotary furnace one by one according to the equipment cycle settings. The preheating temperature is 850°C, and the holding time after color transparency is 40±5 minutes. The protective atmosphere is nitrogen. The material sections are arranged in a fixed gap within the rotary furnace and heated independently. The first-in-first-out system ensures that the heating and holding times of the same batch of material sections are consistent.

[0138] 2.2 Final heating of material section: After the material section reaches the set preheating time, it is automatically taken out from the preheating furnace and transferred to the high temperature

[0139] The rotary furnace is heated to 1100 ± 10°C, with a 10-minute hold time after color transparency. Nitrogen is used as the protective atmosphere. The sections are spaced apart and heated independently, using a first-in, first-out (FIFO) system to ensure consistent heating and hold times for the same batch of sections.

[0140] 2.3 Segment Forging: Forging is performed using a press or open die forging machine. The press / open die forging die must be preheated to 250°C before forging. The forging process includes upsetting, forming, and punching to produce ring-shaped forgings. The final forging temperature should be ≥ 950°C and measured using an infrared thermometer.

[0141] 2.4 Rolling forming: Before each rolling, apply yellow glycerin on the rolling shaft and then roll the ring forging. The rolling time is 12S to obtain the ring forging that meets the process size. The temperature after rolling is ≥850℃. After rolling, the rolling shaft is water-cooled and the oxide scale stuck on the rolling shaft is ground with tooling.

[0142] 2.5 Slow cooling after forging: Place the rolled forgings into a mesh bag tempering furnace for slow cooling. The temperature setting is: 400±10℃, and the slow cooling time is 120±5min. After the slow cooling is completed, take them out of the furnace and cool them naturally to room temperature.

[0143] 3. Annealing

[0144] Place the forgings in a special heat-resistant steel basket of a box-type annealing furnace. The annealing process is as follows: preheating temperature: 750±10℃, holding time after reaching temperature: 4h±10min; heating temperature: 850±10℃, holding time after reaching temperature: 4h±10min; cooling with the furnace to 730℃, isothermal temperature 730±10℃, isothermal time 4h±10min, cooling with the furnace to 600℃ at a cooling rate of 15℃ / min, and after reaching 600℃, take out of the furnace and air-cool to room temperature.

[0145] 4. Turning

[0146] Use a horizontal lathe to process forgings into turned workpieces of qualified size according to the process drawings.

[0147] 5. Heat treatment

[0148] 5.1 Clean the outer and inner rings of the bearings before use

[0149] Pre-cleaning removes impurities such as cutting fluid, dust, and oil from the bearing surface, ensuring a consistent appearance and color after quenching and tempering. Bearing parts are placed on a fixture according to process requirements and proceed to the pre-cleaning station, where they are cleaned with a detergent and then with water. The cleaning temperature is 60°C, and each cleaning cycle lasts 8 minutes. After cleaning, drying is performed at 120°C for 8 minutes.

[0150] 5.2 Quenching heating:

[0151] Vacuum heating furnace is used for quenching heating

[0152] The cleaned bearing rings are placed in a vacuum heating furnace. After closing the furnace door, vacuuming begins. When the vacuum reaches 6 Pa, the equipment begins heating. Preheating temperature: 850±10°C. From room temperature to 850°C, the equipment's heating rate is 10°C / min. Once at temperature, the temperature is maintained for 40 minutes. Final heating temperature: 1050±10°C. From 850°C to 1050°C, the equipment's heating rate is 8°C / min. Once at temperature, the temperature is maintained for 70 minutes.

[0153] 5.3 Quenching and cooling:

[0154] Vacuum oil quenching: After heating, the bearing parts are immersed in vacuum quenching oil for rapid cooling. The quenching oil temperature is 80℃ and the cooling time is 20 minutes. After cooling, the parts are taken out of the furnace.

[0155] 5.4 Cleaning

[0156] Spray cleaning, two stations in total, each station cleaning time 10 minutes: 1. Cleaning and degreasing: water temperature 80℃, cleaning agent: 6% sodium bicarbonate aqueous solution; 2. Rust prevention treatment, water temperature: room temperature, rust prevention agent 0.5% sodium nitrite aqueous solution.

[0157] 5.5 Cold treatment

[0158] After cleaning, the bearing parts are placed in a cold treatment device at a temperature of -80°C for 120 ± 10 minutes. After the cold treatment is completed, the liquid nitrogen is turned off and the bearing parts are allowed to slowly warm up to room temperature in the deep freezer before being immediately tempered.

[0159] 5.6 Primary tempering

[0160] The first tempering treatment, tempering temperature: 170℃, tempering time: 3h.

[0161] 5.7 Secondary tempering

[0162] After the first tempering is completed, the bearing parts are cooled to room temperature and then subjected to a second tempering treatment at a tempering temperature of 170°C and a tempering time of 3 hours.

[0163] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. Reference can be made to the common and similar parts between the various embodiments. For the devices disclosed in the embodiments, since they correspond to the methods disclosed in the embodiments, the description is relatively simple, and the relevant parts can be referred to the method description.

[0164] The above description of the disclosed embodiments is intended to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be readily apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not limited to the embodiments shown herein but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A forging and heat treatment process for a single-row tapered roller bearing ring, characterized in that: The raw materials are sequentially cut, forged, annealed, turned and heat treated to obtain single-row tapered roller bearing rings; Wherein, the forging includes: Material section preheating: preheating temperature: 800-850℃, holding time after color transparency 40±5min, protective atmosphere: nitrogen; Final heating of material section: After the material section reaches the set preheating time, it is automatically taken out from the preheating furnace and transferred to a high-temperature rotary bottom heating furnace. The heating temperature is 1100±10℃. The holding time after color transparency is 6-15 minutes. The protective atmosphere is nitrogen. Segment forging: Use a press or free forging for forging. Before forging, the forging die is preheated at 150-300°C. The forging process is divided into: upsetting, forming, punching, and obtaining a ring forging. The final forging temperature should be ≥950°C. Secondary heating: The ring forging is subjected to secondary heating, the heating temperature is 1100±10℃, the holding time after reaching the temperature is 3-6min, and the protective atmosphere is nitrogen; Rolling forming: Before rolling, apply yellow glycerin on the rolling shaft and then roll the ring forging. The rolling time is 10-15 seconds. The temperature after rolling is ≥900℃. After rolling, spray water to cool the rolling shaft and use tooling to grind off the oxide scale on the rolling shaft. Slow cooling after forging: The forgings after rolling are immediately buried in an ash box filled with dry lime, and the forgings are taken out when they are cooled to below 200℃ in the dry lime.

2. The forging and heat treatment process for a single-row tapered roller bearing ring according to claim 1, characterized in that: The heat treatment comprises: Before cleaning the outer and inner rings of bearings: The bearing parts are placed on the tooling according to the process requirements and enter the pre-cleaning station, where they are cleaned with detergent and then with water. The cleaning temperature is 50-80°C and the cleaning time for each step is 6-10 minutes. After cleaning, they are dried at 110-130°C and the drying time is 6-10 minutes. Quenching heating: The cleaned bearing parts enter the vacuum heating furnace, are evacuated to 5-10Pa, and heated. The first preheating stage: preheating temperature: 500±10℃, from room temperature to 500℃, the heating rate of the equipment is 8-12℃ / min, and after reaching temperature, it is kept warm for 15-30min; the second preheating stage: preheating temperature: 800±10℃, from 500 to 800℃, the heating rate of the equipment is 8-12℃ / min, and after reaching temperature, it is kept warm for 30-50min; the third preheating stage: preheating temperature: 1000±10℃, from 800 to 1000℃, the heating rate of the equipment is 6-10℃ / min, and after reaching temperature, it is kept warm for 10-20min; final heating: final heating temperature: 1050±10℃, from 1000 to 1050℃, the heating rate of the equipment is 1-3℃ / min, and after reaching temperature, it is kept warm for 60-80min; Quenching cooling: The heated bearing parts are cooled in the furnace using high-pressure nitrogen. The gas quenching pressure is 4-6 bar. When the bearing rings are cooled to below 60°C in the furnace, they are taken out of the furnace and air-cooled to room temperature. Cold treatment The quenched bearing rings are placed in a cold treatment device at a temperature of -70 to -80°C for 120 ± 10 minutes. After the cold treatment is completed, the liquid nitrogen is turned off and the bearing parts are allowed to slowly heat up to room temperature in the deep freezer before being immediately tempered. One tempering The first tempering treatment, tempering temperature: 160 ~ 180 ℃, tempering time: 2.5 ~ 3.5h; Secondary tempering After the first tempering is completed, the bearing parts are cooled to room temperature and then subjected to a second tempering treatment. The tempering temperature is 160-180°C and the tempering time is 2.5-3.5 hours.

3. The forging and heat treatment process for a single-row tapered roller bearing ring according to claim 1, characterized in that: The cutting material comprises: The raw materials are hot-rolled polished bars. The weight dispersion of the material sections after cutting is controlled within ±5g. After cutting, the burrs are removed to ensure that the cut surface is smooth and flat.

4. The forging and heat treatment process for a single-row tapered roller bearing ring according to claim 1, characterized in that: The annealing process is as follows: preheating temperature: 750±10°C, holding time after reaching the temperature: 4h±10min; Heating temperature: 850±10℃, holding time after reaching temperature: 4h±10min; cool with the furnace to 730℃, isothermal temperature 730±10℃, isothermal time 4h±10min, cool with the furnace to 600℃ at a cooling rate of 10~15℃ / min, and after reaching 600℃, take out of the furnace and air cool to room temperature.

5. The forging and heat treatment process for a single-row tapered roller bearing ring according to claim 1, characterized in that: The turning process is as follows: using a horizontal lathe to process the annealed workpiece into a workpiece of qualified size according to the process drawing.

Citation Information

Cited By

  • Forging process method for eliminating twin-crystal carbides in forging of high-nitrogen stainless steel bearing ring

    CN122007300A