A method for improving the heat stability and resistance to protein adsorption of type A crystalline starch

By subjecting the A-type starch crystal precursor to pressure heating treatment, molecular-level defect sites are eliminated, improving the starch's resistance to protein adsorption and thermal stability, thus solving the bottleneck in the application of natural starch in biomedicine and functional foods.

CN123106931APending Publication Date: 2026-11-17CHINA AGRI UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611618190.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing natural starch materials are insufficient in the field of anti-protein adsorption and have poor thermal stability, which cannot meet the application requirements of biopharmaceutical products.

Method used

By subjecting type A starch crystal precursors to pressurization treatment at specific moisture content and temperature, molecular-level defect sites on their surface are eliminated, molecular chain rearrangement is induced, and the anti-protein adsorption performance and thermal stability are improved.

Benefits of technology

It achieves a significant reduction in the non-specific adsorption capacity of proteins on the surface of starch crystals and improves their thermal stability without introducing chemical groups, making it suitable for the fields of biomedicine and functional foods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106931A_ABST
    Figure CN123106931A_ABST
Patent Text Reader

Abstract

This invention discloses a method for improving the heat resistance and resistance to protein adsorption of type A crystalline starch, belonging to the field of crystalline starch modification technology. This invention involves pressurizing and heat-treating the type A starch crystalline precursor under specific moisture content and temperature conditions, precisely eliminating molecular-level defect sites on its surface (including metastable microcrystals, lattice distortion, and exposed regions of disordered chain segments), inducing molecular chain contraction and rearrangement. This eliminates non-specific protein adsorption sites at the source, significantly reducing the non-specific adsorption capacity of the crystal surface for proteins without introducing any chemical groups, while simultaneously endowing the crystal with excellent thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for improving the heat resistance and resistance to protein adsorption of type A crystalline starch, belonging to the field of crystalline starch modification technology. Background Technology

[0002] Non-specific protein adsorption (i.e., biocontamination) is a core bottleneck restricting the long-term efficacy of biomaterials in vivo. In drug delivery systems, once plasma proteins adsorb onto the carrier surface, opsonin activity is triggered, leading to recognition and rapid clearance by the mononuclear phagocyte system, significantly shortening the in vivo circulation half-life. Therefore, constructing surfaces that can effectively resist non-specific protein adsorption is a common key technological requirement in the fields of drug sustained-release carriers, implants, and biosensors.

[0003] Currently, the mainstream anti-protein adsorption strategy is chemical modification. Among them, polyethylene glycol (PEG) grafting and zwitterionic polymer coating are the two "gold standards." PEG, with its strong hydrophilicity and highly compliant chain segment movement, forms steric hindrance and hydration layer barriers, while zwitterionic polymers form a super-strong hydration layer through the ionic solvation of equal amounts of positive and negatively charged groups. Both exhibit excellent anti-protein adsorption performance. However, both strategies have inherent limitations: the chemical grafting process is complex, and batch consistency is difficult to control precisely; the introduced non-natural chemical groups pose concerns about immunogenicity and long-term biosafety; and the coating may detach or oxidatively degrade in the in vivo environment, leading to loss of function.

[0004] These limitations have prompted researchers to turn their attention to naturally derived materials. Natural polymers such as starch, chitosan, cellulose, and silk fibroin, due to their inherent biocompatibility and biodegradability, are considered potential anti-protein adsorption substrates. However, the anti-protein adsorption function of these natural materials almost entirely depends on subsequent chemical modifications—chitosan requires quaternization or grafting with zwitterionic groups, while cellulose requires carboxymethylation or the introduction of functional coatings. The anti-protein adsorption performance of pure natural polysaccharide materials, especially neutral polysaccharides (such as starch), often falls short of application requirements, and the structural root causes of these performance defects remain unclear.

[0005] Starch, as a neutral natural polysaccharide, boasts significant advantages such as wide availability, low cost, and excellent biocompatibility, making it uniquely promising in the field of anti-protein adsorption—its surface carries no net charge, theoretically preventing protein adsorption driven by electrostatic attraction. However, research and application of natural starch in anti-protein adsorption are almost nonexistent. The core obstacle lies in the numerous molecular-level defects present on the surface of starch granules or recrystallized crystals, such as lattice distortion, microscopic inhomogeneity of interplanar spacing, metastable microcrystalline regions, and exposed disordered chain segments. These defect sites constitute non-specific adsorption targets for proteins—protein molecules tend to anchor and deposit at these high-energy, unstable structural sites. Current technologies cannot effectively eliminate these intrinsic defects, resulting in starch materials, even with neutral hydrophilic surfaces, failing to exhibit considerable anti-protein adsorption performance.

[0006] Furthermore, another key drawback of natural starch is its poor thermal stability. When subjected to humid heat treatment exceeding 100°C in an aqueous system, its ordered crystalline structure is destroyed, leading to a loss of overall performance. This further limits its application in biopharmaceutical products requiring terminal sterilization.

[0007] Therefore, if a purely physical method can be developed that does not rely on any chemical modification to precisely eliminate molecular-level defects on the surface of starch crystals from the source, and simultaneously improve its anti-protein adsorption performance and thermal stability, it will open up a new path for the application of natural neutral polysaccharides in the field of high-end biomedical materials. Summary of the Invention

[0008] [Technical Issues] Existing naturally derived anti-protein adsorbent materials generally rely on chemical modification; Intrinsic molecular-level defects on the surface of starch crystals lead to severe protein adsorption. Starch materials have poor thermal stability in aqueous systems and cannot withstand terminal sterilization.

[0009] [Technical Solution] To address the aforementioned problems, this invention provides a method for improving the heat stability and resistance to protein adsorption of type A crystalline starch. Specifically, this invention involves pressurizing and heat-treating the type A starch crystal precursor under specific moisture content and temperature conditions, precisely eliminating molecular-level defect sites on its surface (including metastable microcrystals, lattice distortion, and exposed regions of disordered chain segments), inducing molecular chain contraction and rearrangement. This eliminates non-specific protein adsorption sites at the source, significantly reducing the non-specific adsorption capacity of the crystal surface for proteins without introducing any chemical groups, while simultaneously endowing the crystal with excellent thermal stability.

[0010] The first objective of this invention is to provide a method for improving the heat stability and resistance to protein adsorption of type A crystalline starch, comprising the following steps: (1) Preparation of type A starch crystal precursor: Starch was gelatinized, enzymatically debranched, and induced to crystallize by organic solvent vapor to obtain type A starch crystal precursor; (2) Pressure-induced defect elimination and conformation densification: The moisture content of the type A starch crystal precursor was adjusted to 20-35% (w / w), and it was subjected to pressure heat treatment at 115-130℃ for 5-60 min, followed by drying to obtain type A crystalline starch with both low protein adsorption performance and high thermal stability.

[0011] In one embodiment of the present invention, the gelatinization in step (1) is specifically as follows: Disperse starch in water and stir at 90-100℃ and 100-500rpm for 5-40 minutes to gelatinize the starch granules completely and the molecular chains fully swell to form a homogeneous solution; then cool to 50-60℃ to obtain the gelatinized starch solution. The starch used is waxy corn starch; the ratio of starch to water is 5-15 g: 100 mL.

[0012] In one embodiment of the present invention, the enzymatic debranching in step (1) is specifically as follows: Pullulanase was added to the gelatinized starch solution, and the enzymatic hydrolysis reaction was carried out at 50-60℃ for 6-10 hours to obtain starch hydrolysate. The ratio of starch to pullulanase is 10g:1-2mL; Pullulanase has an enzyme activity ≥1000 NPUN / g.

[0013] In one embodiment of the present invention, the organic solvent vapor-induced crystallization in step (1) is specifically as follows: The solvent vapor was pumped into the starch hydrolysate at a rate of 80-120 mL / h, and crystallization was induced at 40-80℃. After crystallization, the precipitate was obtained by centrifugation and dried to obtain type A starch crystal precursor. The solvent is one or more of ethanol, n-butanol, and acetone; The ratio of starch to solvent is 10g: 200-350mL; Centrifugation is performed at 2000-5000 rpm for 10-40 minutes; Drying is carried out at 40-50℃ for 4-20 hours.

[0014] In one embodiment of the present invention, the water content of the type A starch crystal precursor in step (2) is 25-35% (w / w), more preferably 30% (w / w).

[0015] In one embodiment of the present invention, the method of adjusting the moisture content in step (2) is one of the following: adding the corresponding moisture and balancing for more than 4 hours, balancing with a saturated salt solution, or spray humidification.

[0016] In one embodiment of the present invention, the pressure heating temperature in step (2) is preferably 120-130°C and the time is preferably 5-30 min; more preferably 120°C and 10 min.

[0017] In one embodiment of the present invention, the drying in step (2) is performed at 35-60°C for 6-20 hours.

[0018] In one embodiment of the present invention, step (2) is not equivalent to conventional "annealing" treatment; conventional annealing is carried out in a large amount of excess water at a temperature slightly below the gelatinization temperature, which can only improve minor crystal defects. Step (2) of the present invention is carried out in a semi-dry state with a water content of 20-35% and a temperature significantly higher than 100°C. This condition provides sufficient molecular chain mobility to allow conformational shrinkage rearrangement and metastable phase elimination, while avoiding the erosion of crystals by excess free water at high temperatures. This is the key to achieving "defect elimination" rather than "structural destruction".

[0019] The second objective of this invention is to prepare type A crystalline starch with both low protein adsorption properties and high thermal stability using the method described herein.

[0020] In one embodiment of the present invention, the DSC gelatinization peak temperature (Tp) of type A crystalline starch, which has both low protein adsorption performance and high thermal stability, is ≥121℃, preferably 121-135℃.

[0021] In one embodiment of the present invention, the BSA adsorption rate of type A crystalline starch, which has both low protein adsorption performance and high thermal stability, is less than 12%.

[0022] The third objective of this invention is the application of the type A crystalline starch, which possesses both low protein adsorption properties and high thermal stability, in the fields of biomedicine or functional foods.

[0023] In one embodiment of the present invention, the biomedical field includes drug sustained-release carriers, implants, biosensors, etc.

[0024] In one embodiment of the present invention, functional foods include low-GI foods, baked goods, and flour products.

[0025] The fourth objective of this invention is to provide an absorbable scaffold in which type A crystalline starch, as described in this invention, possesses both low protein adsorption properties and high thermal stability.

[0026] [Beneficial Effects] (1) This invention is the first to obtain type A crystalline starch with both low protein adsorption performance and high thermal stability through purely physical means. Unlike existing strategies that rely on chemical grafting / coating to achieve antifouling properties in natural materials, this invention discovers that molecular-level defects on the starch crystal surface are the structural root cause of non-specific protein adsorption, and precisely eliminates these defects through pressurization under specific conditions. Adsorption experiments using bovine serum albumin (BSA) as a model protein confirm that the BSA adsorption amount of the treated crystals is significantly reduced compared to the precursor, and this effect is completely independent of enzyme-substrate specific recognition. This purely physical process is green, produces pure products, and has no exogenous chemical residues, fundamentally avoiding the biosafety risks and coating peeling risks associated with chemical modification strategies.

[0027] (2) The heat resistance of the type A crystalline starch prepared by the present invention, which has both low protein adsorption performance and high thermal stability, has achieved a qualitative leap; the gelatinization peak temperature (Tp) is ≥121℃, which can withstand conventional moist heat sterilization conditions (121℃), thus solving the application bottleneck of natural starch materials that cannot be terminally sterilized in water-containing systems.

[0028] (3) The process of the present invention is simple and suitable for industrial production. In the present invention, conformational densification only involves moisture adjustment and one-step pressurization. The XRD shoulder peak fusion feature directly proves that the molecular chain arrangement has achieved uniform densification after defect elimination, which provides structural guarantee for batch consistency.

[0029] (4) This invention opens up a new dimension of application for starch materials in the biomedical field. Based on its dual characteristics of low protein adsorption and heat resistance, it is expected to become a brand-new natural "green" carrier material that can withstand terminal sterilization and can "invisibly" blend into the immune system in the field of drug delivery.

[0030] (5) The type A crystalline starch prepared by this invention, which has both low protein adsorption performance and high thermal stability, has broad application prospects in the field of biomedical materials; Specifically as follows: In drug delivery systems, it possesses two core advantages: First, it can completely withstand terminal moist heat sterilization (121℃) without structural changes, overcoming the industry bottleneck that natural starch materials cannot be terminally sterilized; second, its pure, defect-free surface effectively resists non-specific adsorption of plasma proteins, reducing the risk of the carrier being recognized and cleared by the mononuclear phagocytic cell system, and is expected to significantly extend in vivo circulation time. This "green and stealthy" characteristic, compared with existing long-circulation strategies involving PEGylation or zwitterionic chemical modification, has significant advantages in terms of simple processing, no chemical residues, and high biosafety. In tissue engineering and regenerative medicine, as a reinforcing filler for absorbable scaffolds, it can maintain a rigid reinforcing effect in the polymer matrix for a long time, and is suitable for products such as absorbable bone screws and bone plates that require long-term mechanical support. In bio-based polymer materials, the gelatinization temperature of 125℃ makes it possible to participate in high-temperature processing technologies that traditional starch cannot participate in, such as melt blending and hot pressing, providing a feasible path for designing novel absorbable starch-based polymer composite materials. Attached Figure Description

[0031] Figure 1 XRD patterns of type A starch crystal precursor (Comparative Example 2) and type A crystalline starch (Example 1), which has both low protein adsorption properties and high thermal stability, are superimposed for comparison.

[0032] Figure 2 The XRD patterns of Examples 1-3 and Comparative Examples 1-4 are compared. Detailed Implementation

[0033] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explanation of the present invention and are not intended to limit the present invention.

[0034] Test method: 1. XRD Testing An X-ray diffractometer was used, with a 2θ scanning range of 4–40°, a step size of 0.05°, and a scanning speed of 2° / min. Relative crystallinity was calculated as the ratio of the crystal diffraction peak area to the total diffraction area.

[0035] 2. DSC thermal performance analysis The gelatinization peak temperature (Tp) was measured and recorded within the range of 40-160℃ at a heating rate of 10℃ / min.

[0036] 3. Assessment of non-specific protein adsorption Bovine serum albumin (BSA) was used as the model protein. BSA was dissolved in PBS buffer (pH 7.4) to prepare a 1 mg / mL protein solution. The sample to be tested was added to the BSA solution (sample to BSA solution mass ratio 1:15), incubated at 37℃ for 24 h, and then centrifuged to collect the supernatant. The supernatant protein concentration was determined using the BCA method, and the adsorption rate of BSA on the sample was calculated.

[0037] Raw materials used in the examples: Waxy corn starch: purchased from Shandong Fuyang Biotechnology; Pullulanase: enzyme activity ≥1000 NPUN / g, purchased from Sigma-Aldrich; Ethanol: 100%, purchased from Tianjin Zhiyuan; n-Butanol: 99.5%, purchased from Sinopharm Shanghai Laboratory. Acetone: 99.5%, purchased from Sinopharm Shanghai Laboratory. Bovine serum albumin (BSA): purity ≥98%.

[0038] Example 1 A method for improving the heat stability and resistance to protein adsorption of type A crystalline starch includes the following steps: (1) Preparation of type A starch crystal precursor: 10g of waxy corn starch was dispersed in 100mL of water and gelatinized by stirring in a boiling water bath (100℃) at 300rpm for 30min. The mixture was then cooled to 58℃ to obtain a gelatinized starch solution. 1mL of pullulanase was added to the gelatinized starch solution, and the mixture was enzymatically hydrolyzed at 58℃ for 8h to obtain a starch hydrolysate. 300mL of ethanol was evaporated to obtain ethanol vapor. The ethanol vapor was pumped into the starch hydrolysate at a rate of 100mL / h, and crystallization was induced at 58℃ for 3h. After crystallization, the precipitate was obtained by centrifugation at 4000rpm for 10min and dried at 45℃ for 12h to obtain type A starch crystal precursor. (2) The water content of the A-type starch crystal precursor was adjusted to 30% (w / w) by adding the appropriate amount of water and balancing for 4 hours. The mixture was then sealed and subjected to pressure heat treatment at 120°C for 10 min, followed by drying at 45°C for 12 h to obtain A-type crystalline starch with both low protein adsorption performance and high thermal stability.

[0039] Example 2 The temperature of the pressure treatment in step (2) of Example 1 was adjusted to 115°C and the pressure heating time was 60 min. Other aspects remained the same as in Example 1, resulting in type A crystalline starch with both low protein adsorption performance and high thermal stability.

[0040] Example 3 The water content of the type A starch crystal precursor in step (2) of Example 1 was adjusted to 25% (w / w), while the rest remained the same as in Example 1, to obtain type A crystalline starch with both low protein adsorption performance and high thermal stability.

[0041] Comparative Example 1 Adjust step (1) of Example 1 as follows: Disperse 10g of waxy corn starch in 100mL of water and stir in a boiling water bath (100℃) at 300rpm for 30min to gelatinize. Cool to 58℃ to obtain a gelatinized starch solution. Add 1 mL pullulanase to the gelatinized starch solution and enzymatically hydrolyze at 58℃ for 8 h to obtain starch hydrolysate; place the starch hydrolysate in a boiling water bath for 10 min to inactivate the enzyme, then centrifuge at 4500 rpm for 10 min and collect the supernatant. The supernatant was recrystallized at 4℃ for 24 h; after crystallization, the precipitate was obtained by centrifugation at 4000 rpm for 10 min and dried at 45℃ for 12 h to obtain type B crystalline starch. Everything else remained the same as in Example 1, resulting in the processed crystalline starch.

[0042] Comparative Example 2 Step (2) of Example 1 is omitted, and everything else remains the same as in Example 1 to obtain type A starch crystal precursor.

[0043] Comparative Example 3 Adjust step (2) of Example 1 as follows: After adding the appropriate amount of water and equilibrating for 4 hours to adjust the water content of the type A starch crystal precursor to 70% (w / w), the mixture was sealed and annealed at 55°C for 24 hours. Then, it was centrifuged at 4000 rpm for 10 minutes, and the precipitate was dried at 45°C for 12 hours to obtain the annealed crystalline starch.

[0044] Comparative Example 4 Sodium alginate powder (viscosity 200±20 mpa.s, purity 90%, purchased from Maclean) was used directly as a natural anti-protein adsorption material.

[0045] Comparative Example 5 The temperature of the pressure treatment in step (2) of Example 1 was adjusted to 135°C, while other steps remained the same as in Example 1, to obtain crystalline starch.

[0046] Comparative Example 6 The temperature of the pressure treatment in step (2) of Example 1 was adjusted to 110°C, while other aspects remained the same as in Example 1, to obtain crystalline starch.

[0047] The obtained crystalline starch was subjected to performance tests, and the test results are as follows: Table 1 shows the results of the crystal form and relative crystallinity tests. As can be seen from Table 1, the A-type crystalline starch prepared in Examples 1-3, possessing both low protein adsorption performance and high thermal stability, is of type A crystal form with a crystallinity above 60%. Compared to Comparative Example 2, the crystal form did not change after pressure heating treatment. Comparative Example 3 showed no change in crystal form after annealing treatment. Although the crystal type of the sample in Comparative Example 5 is type A, its relative crystallinity is below 60%, indicating that the pressure heating treatment intensity was too high, which damaged some of the type A crystals in the sample. Although the crystal type of the sample in Comparative Example 6 is type A, its relative crystallinity is below 60%, indicating that the pressure heating treatment intensity was insufficient to promote the formation of more dense type A crystal structures.

[0048] Table 1. Results of Crystal Form and Relative Crystallinity Tests

[0049] Table 2 shows the test results of DSC gelatinization peak temperature and gelatinization enthalpy. As can be seen from Table 2, the gelatinization peak temperature (Tp) of Example 1 reached 125.09℃, an increase of 13.29℃ compared to Comparative Example 2 (without pressure heating, 111.80℃), exceeding the conventional sterilization temperature of 121℃. Comparative Example 1 (Type B crystals) had a Tp of only 105.82℃, indicating that the Type B precursor could not achieve effective heat resistance through pressure heating. The limited increase in Tp in Comparative Examples 2-3 proves that pressure heating is the key to achieving effective densification.

[0050] Table 2 Test results of DSC gelatinization peak temperature and gelatinization enthalpy

[0051] Table 3 shows the test results of BSA adsorption. As can be seen from Table 3, the BSA adsorption in Example 1 is significantly lower than that of the precursor (Comparative Example 2), proving that step (2) effectively reduces non-specific protein adsorption sites by eliminating molecular-level defects on the crystal surface. The adsorption decrease in Comparative Example 3 is not significant, further confirming that pressure-heated water content is a key condition for defect elimination. The BSA adsorption rate of Comparative Example 4 (sodium alginate, a known natural anti-protein adsorption material) is 46.57%, significantly higher than the 9.34% in Example 1, further demonstrating that the defect elimination strategy of this invention has a significant advantage in anti-protein adsorption performance.

[0052] Table 3. Test results of BSA adsorption capacity

[0053] Figure 1 The XRD patterns of type A starch crystal precursor (Comparative Example 2) and type A crystalline starch (Example 1), which combines low protein adsorption and high thermal stability, are superimposed for comparison. Figure 1 It can be seen that the pressurization treatment led to significant defect elimination; the shoulder peaks merged into a single symmetrical peak: the precursor had multiple shoulder peaks near the 23° main diffraction peak, reflecting the microscopic uneven distribution of interplanar spacing. After treatment, the shoulder peaks merged into a symmetrical and sharp single peak, indicating that the molecular chain arrangement tended to be highly uniform and the lattice defects were eliminated.

[0054] Figure 2 A comparison of the XRD patterns of Examples 1-3 and Comparative Examples 1-4. From... Figure 2 It can be seen that the diffraction peaks at 2θ≈7.5°, 13-14°, and 19-21° in Examples 1-3 almost completely disappeared, indicating that the metastable V-type arrangement was reorganized into a more stable A-type compact conformation; indicating that the pressurization treatment successfully induced the elimination of defects and the ordered rearrangement at the molecular scale.

[0055] In summary, detailed XRD analysis (shoulder peak fusion and disappearance of metastable peaks) confirmed that step (2) induced defect elimination at the molecular scale; DSC confirmed that the gelatinization peak temperature increased to 125℃, exceeding the conventional sterilization temperature of 121℃; and BSA protein adsorption experiments confirmed that the non-specific protein adsorption capacity on the crystal surface was significantly reduced after defect elimination. All these evidences indicate that this invention is the first to discover and realize a purely physical post-treatment of type A starch crystals through "pressure-induced defect elimination," resulting in crystalline starch with both low protein adsorption performance and high thermal stability.

[0056] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the claims.

Claims

1. A method for improving the heat stability and resistance to protein adsorption of type A crystalline starch, characterized in that, Includes the following steps: (1) Preparation of type A starch crystal precursor: Starch was gelatinized, enzymatically debranched, and induced to crystallize by organic solvent vapor to obtain type A starch crystal precursor; (2) Pressure-induced defect elimination and conformation densification: The moisture content of the type A starch crystal precursor was adjusted to 20-35% w / w, and it was subjected to pressure heat treatment at 115-130℃ for 5-60 min, followed by drying to obtain type A crystalline starch with both low protein adsorption performance and high thermal stability.

2. The method according to claim 1, characterized in that, The gelatinization process in step (1) is as follows: Disperse starch in water and stir at 90-100℃ and 100-500rpm for 5-40 minutes to gelatinize the starch granules completely and the molecular chains fully swell to form a homogeneous solution; then cool to 50-60℃ to obtain the gelatinized starch solution. The starch used is waxy corn starch; the ratio of starch to water is 5-15 g: 100 mL.

3. The method according to claim 1, characterized in that, The enzymatic debranching in step (1) is as follows: Pullulanase was added to the gelatinized starch solution, and the enzymatic hydrolysis reaction was carried out at 50-60℃ for 6-10 hours to obtain starch hydrolysate. The ratio of starch to pullulanase is 10g:1-2mL; Pullulanase has an enzyme activity ≥1000 NPUN / g.

4. The method according to claim 1, characterized in that, The organic solvent vapor-induced crystallization in step (1) is as follows: The solvent vapor was pumped into the starch hydrolysate at a rate of 80-120 mL / h, and crystallization was induced at 40-80℃. After crystallization, the precipitate was obtained by centrifugation and dried to obtain type A starch crystal precursor. The solvent is one or more of ethanol, n-butanol, and acetone; The ratio of starch to solvent is 10g: 200-350mL; Centrifugation is performed at 2000-5000 rpm for 10-40 minutes; Drying is carried out at 40-50℃ for 4-20 hours.

5. The method according to claim 1, characterized in that, In step (2), the water content of the type A starch crystal precursor is 25-35% w / w; the pressure heating temperature is 120-130℃, and the time is 5-30 min.

6. The method according to claim 5, characterized in that, In step (2), the pressure heating temperature is 120℃ and the time is 10min.

7. The method according to claim 5, characterized in that, In step (2), the water content of the type A starch crystal precursor is 30% w / w.

8. The method according to claim 1, characterized in that, In step (2), the drying process involves drying at 35-60℃ for 6-20 hours.