Multi-layer composite pipe coated with bell and spigot

By using corrosion-resistant inner tube and middle layer materials in the composite pipe, combined with welding and sealing ring technology, the problems of rust and electrochemical corrosion of the composite pipe are solved, achieving a longer service life and higher protection effect.

CN221839103UActive Publication Date: 2024-10-15HUNAN ZHENHUI PIPE IND
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202323651260.9
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-30
Publication Date
2024-10-15
Estimated Expiration
2033-12-30

AI Technical Summary

Technical Problem

Existing composite pipes are prone to rust, electrochemical corrosion and lining delamination during long-term use, resulting in shortened service life and liquid contamination, and existing anti-corrosion measures are ineffective.

Method used

The inner tube of corrosion-resistant material is used to cover the inner wall and socket of the outer tube. Combined with an intermediate layer of material such as hot melt glue or rubber, the adhesion and anti-corrosion effect of the lining are ensured through welding and sealing rings to form an overall anti-corrosion structure.

Benefits of technology

Effectively prevents corrosion of outer pipes, extends service life, reduces operating energy consumption, prevents electrochemical corrosion, and enhances the stability and protective performance of pipelines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221839103U_ABST
    Figure CN221839103U_ABST
Patent Text Reader

Abstract

The multi-layer composite pipe comprises an inner pipe, a middle layer and an outer pipe, the inner pipe, the middle layer and the outer pipe are bonded to form the composite pipe or pressed to form the composite pipe, the middle layer is made of nonmetal, the outer pipe comprises a socket part, a straight pipe part and a spigot part which are sequentially connected, the inner pipe is made of corrosion-resistant metal materials, and the outer pipe is made of stainless steel. One section of the inner pipe covers part of the inner wall of the socket part and the inner wall of the straight pipe part, and the other section of the inner pipe completely covers the spigot part. The inner pipe made of corrosion-resistant materials covers the inner wall of the outer pipe, the end face of the spigot portion of the composite pipe and the outer wall of the spigot portion of the composite pipe, the cleanliness degree of the conveying environment is high, and the composite pipe is good in corrosion resistance, easy to install, stable in operation and long in service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of composite pipes, in particular to a multi-layer composite pipe with a socket and spigot coated thereon. Background Art

[0002] Composite pipes are widely used in liquid transport pipe network systems. When in use, the parts of the pipe that come into contact with the liquid are required to have good corrosion resistance to prevent the pipe from rusting due to long-term contact with the liquid, which affects the quality of the transported liquid. Existing composite pipes generally have a metal pipe as the outer layer and a plastic pipe as the inner layer, or a metal pipe as the outer layer and a stainless steel pipe as the inner layer. When composite pipes with a plastic pipe as the inner layer are composited, the inner plastic pipe melts due to heat. When the temperature is too high, it is easy to produce an uneven inner surface or partial melting. The uneven inner surface will increase the resistance when transporting liquids. The partial melting of the inner plastic pipe will cause the product to be scrapped, and the production cost will increase. The inner plastic pipe has a large thermal expansion coefficient and shrinks greatly at low temperatures. The internal stress generated by the mutual peeling with the outer metal pipe is large. There is a risk of lining delamination after long-term use. The composite pipe with a stainless steel pipe as the inner layer is prone to electrochemical corrosion due to the potential difference between the inner stainless steel pipe and the outer metal pipe, which affects the service life of the pipe; the inner lining stainless steel pipe and the outer metal pipe are not bonded, and the inner stainless steel pipe is prone to deformation and falling off under negative pressure, affecting the normal use of the pipe. In order to solve the above problems, the current solution of setting glue between the inner stainless steel pipe and the outer metal pipe is mainly adopted. However, when glue is used as the intermediate layer, the glue is prone to aging. During bonding, due to the high fluidity of the glue, it is easy for the inner stainless steel pipe to be in direct contact with the outer metal pipe locally, and the effect of preventing electrochemical corrosion and resisting negative pressure cannot be achieved. The structure of the existing composite pipe is a socket structure, with one end of the metal pipe being a spigot end and the other end being a bell end. When installing the pipe network, multiple composite pipes are connected in sequence, and the spigot end of a composite pipe is inserted into the bell end of the adjacent composite pipe. The inner wall of the socket end of the metal outer pipe is uneven and stepped. When the inner wall of the metal pipe is coated for corrosion protection, the middle part and the socket end of the metal pipe are coated with an inner plastic pipe, and the inner wall of the socket end and the outer wall of the socket end are generally directly painted with anti-corrosion paint, or sprayed / coated. However, this method does not make the anti-corrosion coating of the pipe form a whole. During use, the long-term flushing of the liquid in the pipeline will cause the liquid to penetrate into the inner wall of the metal pipe through the gap between different materials, resulting in the failure of anti-corrosion and corrosion of the pipe wall, which will affect the service life of the pipeline and pollute the liquid transported in the pipeline. Utility Model Content

[0003] In view of the above-mentioned problems existing in the prior art, the purpose of the utility model is to provide a multi-layer composite pipe covered with a socket, with an inner pipe made of corrosion-resistant material as an inner lining, covering the inner wall of the outer pipe, the end face of the socket part of the composite pipe and the outer wall of the socket part. The transportation environment is highly clean, the composite pipe has excellent corrosion resistance, simple installation, stable operation and long service life.

[0004] In order to achieve the above purpose, the technical solution adopted by the utility model is:

[0005] A multi-layer composite pipe with a socket-covered surface comprises an inner pipe, an intermediate layer and an outer pipe. The inner pipe, the intermediate layer and the outer pipe are bonded or compressed to form a composite pipe. The outer pipe comprises a socket portion, a straight pipe portion and a spigot portion which are connected in sequence. The inner pipe is made of a corrosion-resistant metal material. The inner wall of the socket portion is provided with steps and / or grooves. One section of the inner pipe covers part of the inner wall of the socket portion and the inner wall of the straight pipe portion, and the other section of the inner pipe completely covers the spigot portion.

[0006] As a further improvement of the above technical solution:

[0007] Preferably, the inner tube comprises an inner sleeve and a socket sleeve, and the inner sleeve, the middle layer and the outer tube are sequentially sleeved from the inside to the outside.

[0008] Preferably, the inner sleeve and the socket sleeve are integral.

[0009] More preferably, the socket sleeve is formed by spinning and turning one end of the inner tube outward.

[0010] More preferably, the socket sleeve and the inner sleeve are welded together.

[0011] More preferably, the welding point between the socket sleeve and the inner sleeve is located on the end face of the socket part, and the inner tube area covering the end face of the socket part is formed by flanging the socket sleeve and / or flanging the inner sleeve followed by welding.

[0012] Preferably, the material of the middle layer is non-metal.

[0013] More preferably, the material of the middle layer is hot melt adhesive.

[0014] More preferably, the material of the middle layer is plastic.

[0015] More preferably, the material of the middle layer is rubber.

[0016] Preferably, the outer tube is made of metal.

[0017] More preferably, the outer tube is made of ductile iron or carbon steel.

[0018] Preferably, the thickness of the middle layer is not less than 0.2 mm, and the thickness of the inner sleeve is not less than 0.1 mm.

[0019] Preferably, when the material of the middle layer is hot melt adhesive, the inner tube and the outer tube are processed into a composite tube through a composite process.

[0020] Preferably, when the material of the middle layer is plastic or rubber, the inner tube, the middle layer and the outer tube are pressed tightly to form a composite tube.

[0021] Preferably, when two adjacent composite pipes are connected, the socket portion of one composite pipe is inserted into the socket portion of the adjacent composite pipe and sealed by a sealing ring, the outer ring of the sealing ring contacts the inner wall of the inner pipe of the socket portion of one composite pipe, and the inner ring of the sealing ring contacts the outer wall of the socket sleeve on the outer wall of the socket portion of the adjacent composite pipe.

[0022] Preferably, at least one sealing ring is provided, and the sealing ring is installed in the inner wall groove of the socket part or the sealing ring is limited by a limiting member.

[0023] A method for manufacturing a multi-layer composite pipe with a socket coating, for manufacturing the composite pipe, comprises the following steps:

[0024] Step S1: processing the inner wall and outer wall of the outer tube and making the inner tube;

[0025] Step S2: arranging the inner sleeve, the middle layer and the outer tube from inside to outside in sequence;

[0026] Step S3: Press the inner sleeve onto the outer tube and the socket sleeve onto the outer wall of the socket sleeve;

[0027] Step S4: compounding;

[0028] When the middle layer is made of plastic or rubber, there is no step S4.

[0029] Preferably, in step S3, the socket sleeve is obtained by spin-forming one end of the inner tube.

[0030] Preferably, in step S1, when making the inner tube, an inner sleeve and a socket sleeve are made separately, and the socket sleeve is put on the outer wall of the socket part. Between step S3 and step S4, the inner sleeve and the socket sleeve are welded, and the welding point is located on the end face of one end of the socket part of the composite tube.

[0031] Preferably, when the material of the middle layer is hot melt adhesive or plastic, in step S2, the middle layer is made into a round tube and then the inner sleeve, the middle layer and the outer tube are sequentially connected, or the powdered raw material of the middle layer is sprayed or coated on the outer wall of the inner sleeve and the outer wall of the socket part, or the powdered raw material of the middle layer is sprayed or coated on the inner wall of the outer tube and the outer wall of the socket part, and then the inner sleeve is inserted into the outer tube.

[0032] Preferably, in step S3, the inner sleeve is pressed tightly against the inner wall of the straight pipe portion, the inner wall of the socket portion and the inner wall of the plug portion by spin forming or hydraulic forming.

[0033] The beneficial effects of the utility model are:

[0034] (1) The inner tube made of corrosion-resistant material covers the inner wall of the outer tube, the end face of the socket and the outer wall of the socket, completely isolating the outer tube from the liquid flowing in the composite tube, effectively preventing the outer tube from rusting, playing a good anti-corrosion role, and increasing the service life of the pipe, avoiding the rust of the outer tube from polluting the water quality, and improving the liquid transportation performance.

[0035] (2) The inner pipe made of corrosion-resistant material as the lining improves the smoothness of the inner surface of the composite pipe compared with the plastic pipe lining. The lining thickness is smaller, which improves the water delivery efficiency of the pipeline and reduces the operating energy consumption.

[0036] (3) The inner lining is made of corrosion-resistant material. Compared with the plastic pipe lining, it greatly reduces the internal stress caused by the mutual peeling between the inner pipe and the outer pipe due to the inconsistent material expansion coefficient, and the inner lining is not easy to delaminate or deform.

[0037] (4) The inner tube made of corrosion-resistant material is used as the inner lining. Compared with the plastic pipe lining, the pipe can be used to transport high-temperature liquid media. When the pipe is affected by high temperature such as external fire, the inner lining will not be damaged.

[0038] (5) The middle layer also acts as an insulator to prevent electrochemical corrosion between the outer tube and the inner tube.

[0039] (6) During installation, the spigot of the composite pipe is inserted into the socket of the adjacent composite pipe and sealed by a sealing ring. The outer ring of the sealing ring presses tightly against the inner wall of the inner pipe of the socket, and the inner ring presses tightly against the spigot sleeve of the outer wall of the spigot, thereby preventing the inner pipe serving as the lining from falling off and preventing the water flow from directly impacting the lining port and causing delamination of the composite pipe.

[0040] (7) After two adjacent composite pipes are connected, there is a gap between the end face of the spigot portion of one composite pipe and the end face of the straight pipe portion of the adjacent composite pipe. Liquid will penetrate through this gap and contact the outer wall of the spigot portion. At this time, the spigot sleeve made of corrosion-resistant material will play an anti-corrosion role. At the same time, the inner ring of the sealing ring presses the outer wall of the spigot portion, completely isolating the straight pipe portion and the socket portion from the liquid, thereby preventing the straight pipe portion and the socket portion from contacting the liquid and causing corrosion.

[0041] (8) When the middle layer is made of hot melt adhesive, the middle layer also plays a connecting role and has a high bonding strength, thereby preventing the inner tube from being delaminated and deformed under negative pressure. Using hot melt adhesive as the bonding material eliminates the inner lining delamination caused by the aging of ordinary glue, the uneven glue layer caused by the flow of ordinary liquid glue, the inner lining delamination and electrochemical corrosion caused by the direct contact between the inner lining and the outer tube without being bonded, and overcomes the technical problems of low bonding strength, poor hygienic performance, poor insulation effect, and uneven inner wall of the outer tube resulting in the inner lining being suspended (i.e., there are areas in the corrosion-resistant lining that are not bonded to the outer tube).

[0042] (9) The socket sleeve and the inner sleeve are connected by welding, and the welding point is set on the end face of the socket part, which is convenient for manufacturing and processing, and the weld has no effect on the installation of the pipe. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a schematic structural diagram of the case where the outer wall of the straight pipe portion and the outer wall of the socket sleeve of the first embodiment of the utility model are flush.

[0044] Figure 2 It is a structural schematic diagram of the first embodiment of the present invention when the thickness of the straight pipe portion is equal to the thickness of the socket portion.

[0045] Figure 3 It is a schematic diagram of connecting two adjacent composite pipes whose outer walls of the straight pipe portion and the outer wall of the socket sleeve are flush with each other in Example 1 of the utility model.

[0046] Figure 4 It is a schematic diagram of connecting two adjacent composite pipes with equal thickness of the straight pipe portion and the socket portion in the first embodiment of the present invention.

[0047] Figure 5 It is a schematic structural diagram of the second embodiment of the utility model when the outer wall of the straight pipe portion and the outer wall of the socket sleeve are flush.

[0048] Figure 6 It is a structural schematic diagram of the second embodiment of the present invention when the thickness of the straight pipe portion is equal to the thickness of the socket portion.

[0049] Figure 7 It is a schematic diagram of connecting two adjacent composite pipes whose outer walls of the straight pipe portion and the outer wall of the socket sleeve are flush with each other in Example 2 of the utility model.

[0050] Figure 8 It is a schematic diagram of connecting two adjacent composite pipes with equal thickness of the straight pipe portion and the socket portion in the second embodiment of the present invention. DETAILED DESCRIPTION

[0051] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0052] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0053] Embodiment 1

[0054] A multi-layer composite pipe with a socket coating, such as Figure 1 to Figure 4 As shown, it includes an inner tube 2, an intermediate layer 3 and an outer tube 1. The inner tube 2 includes an inner sleeve 22 and a socket sleeve 21. The inner sleeve 22, the intermediate layer 3 and the outer tube 1 are sequentially sleeved from the inside to the outside.

[0055] The outer tube 1 includes a socket portion 11, a straight tube portion 12 and a spigot portion 13 which are sequentially connected along the axial direction thereof, i.e., the socket portion 11, the straight tube portion 12 and the spigot portion 13 share a common center line. The straight tube portion 12 and the spigot portion 13 are both cylindrical, and the end of the spigot portion 13 away from the straight tube portion 12 is chamfered along the circumferential direction. The inner surface of the socket portion 11 is provided with steps and / or grooves, i.e., the socket portion 11 can be regarded as being formed by sequentially connecting a plurality of cylindrical structures with different inner diameters.

[0056] The outer tube 1 is made of metal, preferably ductile iron or carbon steel, and the socket portion 11, the straight tube portion 12 and the spigot portion 13 are integrally cast, or the straight tube portion 12 and the spigot portion 13 are integrally formed as a tube body, and the socket portion 11 is made separately, and then the socket portion 11 and the tube body are welded. The inner diameter of the spigot portion 13 is equal to the inner diameter of the straight tube portion 12.

[0057] The inner tube 2 is made of a material with corrosion resistance, including but not limited to stainless steel, titanium, and composite materials, preferably stainless steel. One end of the inner tube 2 covers part of the inner wall of the socket portion 11, the middle part of the inner tube 2 covers the inner wall of the straight tube portion 12, and the other end of the inner tube 2 covers the inner wall of the socket portion 13, the end face of the socket portion 13, and the outer wall of the socket portion 13. In other words, the inner tube 2 can cover the entire socket portion 13. Specifically, the part of the inner tube 2 covering the outer wall of the socket portion 13 is the socket sleeve 21, and the part of the inner tube 2 covering the inner wall of the outer tube 1 is the inner sleeve 22. Obviously, the inner sleeve 22 is the inner lining of the composite pipe. The inner tube 2 formed by the inner sleeve 22 and the socket sleeve 21 is a whole, and there are no holes on the inner tube 2. It is a continuous medium, which can completely cover at least most of the inner wall of the socket portion 11, all of the inner wall of the straight tube portion 12, all of the inner wall of the socket portion 13, the end face of the socket portion 13, and the outer wall of the socket portion 13.

[0058] The thickness of the socket sleeve 21 may be greater than, less than or equal to the thickness of the inner sleeve 22 .

[0059] The spigot sleeve 21 can be formed by spinning and turning one end of the inner tube 2 outward; or the spigot sleeve 21 and the inner sleeve 22 are welded together, preferably, the welding point is located on the end surface of the spigot portion 13 of the composite pipe. Specifically, the stainless steel covering the end surface of the spigot portion 13 is formed by welding after flanging the spigot sleeve 21 and / or flanging the inner sleeve 22.

[0060] The material of the middle layer 3 is non-metal, preferably hot melt adhesive, plastic or rubber, and the inner tube 2, the middle layer 3 and the outer tube 1 are pressed together or bonded together. When the material of the middle layer 3 is hot melt adhesive, the hot melt adhesive has bonding properties, and the middle layer 3 firmly connects the inner tube 2 to the outer tube 1 through the composite process. When the material of the middle layer 3 is plastic or rubber, plastic and rubber have no bonding properties, and the inner tube 2, the middle layer 3 and the outer tube 1 are pressed together.

[0061] Preferably, there is hot melt adhesive, plastic or rubber between the end surface of the socket portion 13 and the inner tube 2 and between the outer wall of the socket portion 13 and the socket sleeve 21 .

[0062] like Figure 2 As shown, the thickness of the socket portion 13 is equal to the thickness of the straight tube portion 12. At this time, after the manufacturing is completed, the socket sleeve 21 protrudes from the outer wall of the straight tube portion 12. Figure 1 As shown, the sum of the thickness of the socket portion 13, the thickness of the socket sleeve 21, and the thickness of the medium between the outer wall of the socket portion 13 and the socket sleeve 21 is equal to the thickness of the straight tube portion 12. In this way, after manufacturing is completed, the outer wall of the straight tube portion 12 and the outer wall of the socket sleeve 21 are flush, the appearance is more beautiful, and the socket portion 13 is not easily damaged during transportation.

[0063] like Figure 1 , 2As shown, the socket portion 11 is provided with a sealing ring limiting end 111, a sealing ring containing end 112, a sealing ring limiting protrusion 113, a first step 114 and a second step 115 in order from the end away from the straight pipe portion 12 to the end close to the straight pipe portion 12. The inner diameter of the sealing ring limiting end 111 is smaller than the inner diameter of the sealing ring containing end 112, the inner diameter of the sealing ring limiting protrusion 113 is larger than the inner diameter of the sealing ring limiting end 111 and smaller than the inner diameter of the sealing ring containing end 112, and the inner diameter of the first step 114 is substantially equal to the inner diameter of the sealing ring containing end 112. The inner wall of the first step 114 is a cylindrical wall surface. The inner wall of the second step 115 is the outer side surface of a truncated cone, that is, from the first step 114 toward the direction of the straight pipe portion 12, the inner diameter of the second step 115 gradually increases, which is equivalent to a bell mouth. Preferably, the maximum inner diameter of the second step 115 is smaller than the inner diameter of the first step 114. The minimum inner diameter of the second step 115 is greater than the inner diameter of the straight tube portion 12. Thus, an end of the straight tube portion 12 close to the second step 115 forms a third step.

[0064] The inner wall bell mouth of the second step 115 is provided to provide a deflection angle for the adjacent composite pipe connected thereto, i.e., to allow the center line of one composite pipe and the center line of the adjacent composite pipe connected thereto to be in an intersecting state rather than an overlapping state, in order to allow a certain installation error and facilitate actual operation.

[0065] Preferably, the inner tube 2 covers the inner wall of the first step 114 and the inner wall of the second step 115 , and does not cover the inner wall of the sealing ring limiting end 111 , the inner wall of the sealing ring containing end 112 , and the inner wall of the sealing ring limiting protrusion 113 .

[0066] In this embodiment, the outer diameter of the inner sleeve 22 is slightly smaller than the inner diameter of the outer tube 1, and the thickness of the inner sleeve 22 is not less than 0.1 mm.

[0067] The main function of the inner tube 2 is corrosion protection, so its thickness should not be too large. A large number of welding tests have shown that under the conditions of fiber laser welding, a stainless steel plate with a minimum wall thickness of 0.1 mm can obtain a weld with high welding strength and small deformation. Taking into account the complexity of the welding process equipment, the investment cost, and the fact that the middle layer 3 shrinks at low temperatures due to its large thermal expansion coefficient, and generates internal stress that separates it from the outer tube 1, it is necessary to give full play to the supporting role of the inner tube 2 on the middle layer 3 to offset the internal stress of the outer tube 1 and the middle layer 3. The preferred thickness of the inner sleeve 22 is 0.1 mm-2 mm.

[0068] The wall thickness of the middle layer 3 is not less than 0.2 mm. The inner diameter of the middle layer 3 is slightly larger than the outer diameter of the inner sleeve 22 , and the outer diameter of the middle layer 3 is slightly smaller than the inner diameter of the outer tube 1 . The length of the middle layer 3 is substantially the same as that of the inner sleeve 22 .

[0069] When the middle layer 3 is hot melt adhesive, it serves as an adhesive layer. When the inner wall roughness of the outer tube 1 is relatively large during compounding, the middle layer 3 is heated and melted to fill the pits on the inner wall of the outer tube 1. If the thickness of the middle layer 3 is too small, poor adhesion may occur in areas with large local roughness. At the same time, the middle layer 3 also serves as an insulating layer, and a certain thickness is required to produce an insulating effect between the outer tube 1 and the inner tube 2. The electric spark test and the peel strength test show that when the thickness of the middle layer 3 reaches more than 0.2mm, the peel strength and insulation performance with good performance can be stably obtained. The optimal thickness of the middle layer 3 is 0.2mm-2mm.

[0070] Compared with the thickness of the inner lining stainless steel required by the standard "Inner lining stainless steel composite steel pipe (CJ / T 192-2017)", when the middle layer 3 uses hot melt adhesive, the inner lining stainless steel thickness is thinner and the cost is lower. When the inner diameter of the outer pipe 1 is the same, the inner diameter of the composite pipe is larger and the transportation efficiency is higher.

[0071] When the inner diameter of the outer tube 1 is 100-300mm, the inner lining is stainless steel, and the thickness of the stainless steel is 0.5-0.9mm, the bonding strength between the inner lining stainless steel and the outer tube 1 does not meet the requirements of the standard "Lined Stainless Steel Composite Steel Pipe (CJ / T 192-2017)". During use, the composite part is prone to peeling and the inner lining is easily washed away by the liquid.

[0072] The conclusions of the lining peel strength test (this test uses an outer tube with an inner diameter of 100-300mm and an inner lining stainless steel thickness of 0.1mm-0.3mm) are as follows:

[0073] When the rust removal grade of the inner wall surface of the metal outer tube 1 reaches Sa2.5, the surface roughness is Ra12.5-Ra25, and the thickness of the intermediate layer 3 is not less than 0.2mm, the peel strength between the hot melt adhesive and the outer tube can stably reach more than 70N / cm; the peel strength between the hot melt adhesive and the inner lining can stably reach more than 50N / cm;

[0074] When the rust removal grade of the inner wall surface of the metal outer tube 1 reaches Sa2.5, the surface roughness is Ra25-Ra50, and the thickness of the intermediate layer 3 is above 0.2mm, the peel strength between the hot melt adhesive and the outer tube can stably reach above 120N / cm; the peel strength between the hot melt adhesive and the inner lining can stably reach above 50N / cm;

[0075] When the rust removal level of the inner wall surface of the metal outer tube 1 reaches Sa2.5, the surface roughness is greater than Ra50, and the thickness of the intermediate layer 3 is above 0.2 mm, the peel strength between the hot melt adhesive and the outer tube can stably reach above 150 N / cm; the peel strength between the hot melt adhesive and the inner lining can stably reach above 50 N / cm.

[0076] According to hydraulic calculations, in existing liquid transport pipelines, the maximum lateral liquid scouring force is 1.15 MPa. The peel strength of the hot melt adhesive and the lining of this solution can reach 50 N / cm, and the corresponding bonding strength is 5 MPa, that is, the pipe of this solution can withstand a lateral liquid scouring force of 5 MPa.

[0077] When the middle layer 3 is hot melt adhesive, the thickness of the middle layer 3 is preferably 0.2 mm to 0.5 mm. When the thickness of the middle layer 3 is greater than 0.5 mm, the peel strength remains substantially unchanged.

[0078] Based on the above structure, when two adjacent composite pipes are connected, Figure 3 and 4 As shown, the spigot 13 of a composite pipe is inserted into the socket 11 of the adjacent composite pipe and sealed by the sealing ring 4. The outer ring of the sealing ring 4 contacts the inner wall of the inner tube 2 at one end of the socket 11 of the composite pipe, and the inner ring of the sealing ring 4 contacts the outer wall of the spigot sleeve 21 on the outer wall of the spigot 13 of the adjacent composite pipe. Preferably, the end face of one end of the sealing ring 4 contacts the end face of the sealing ring limiting end 111, a part of the sealing ring 4 is accommodated on the sealing ring accommodating end 112, the sealing ring limiting protrusion 113 is stuck in the middle of the sealing ring 4, and the other part of the sealing ring 4 is located on the first step 114. At the same time, there is a gap between the end face of one end of the spigot 13 of a composite pipe and the end face of the straight pipe 12 of the adjacent composite pipe, and the existence of this gap is also to allow the existence of a deflection angle when two adjacent composite pipes are installed.

[0079] From the above, the length of the spigot 13 is greater than the length of the socket 11, so that when two adjacent pipes are connected by spigot, the inner and outer rings of the sealing ring 4 can contact the stainless steel, avoiding the straight pipe 12 made of metal from partially extending between the sealing ring 4 and the end face of the spigot 13, causing this part of the straight pipe 12 to contact the liquid and rust. At the same time, the inner pipe 2 on the end face of the composite pipe prevents the liquid in the pipeline from contacting the middle layer of the end face of the spigot 13, and the tension of the water causes the composite pipe to be delaminated.

[0080] A method for manufacturing a multi-layer composite pipe with a socket coating, for manufacturing the composite pipe, comprises the following steps:

[0081] Step S1: processing the inner wall and the outer wall of the outer tube 1, making the inner sleeve 22, and making the socket sleeve 21.

[0082] In this step, the method for processing the inner wall and outer wall of the outer tube 1 is to first grind the inner wall of the outer tube 1, and then sandblast or shot blast the inner wall and outer wall. Use an internal grinder to grind the inner wall of the outer tube 1 made of ductile iron, grind the inner wall of the tube flat, and remove surface oxide scale, scum and rust. Alternatively, after the inner wall is polished flat, use a laser cleaning machine to clean the inner wall of the tube to deeply remove the oxide scale and rust on the inner wall of the tube. When sandblasting or shot blasting, remove dust, oxide scale, and rust on the inner and outer walls, and sandblast the inner and outer walls of the tube into a frosted surface.

[0083] Making the inner sleeve 22 comprises the following steps:

[0084] S11: Process the stainless steel sheet into a ring shape or a thin cylindrical shape to complete the rolling. In this step, the rolling is performed by a rolling machine (the technical solution of the rolling machine in the patent 2020114372537 of the applicant can be used).

[0085] S12: Cut the rolled stainless steel sheet and weld it into a cylindrical shape. In this step, if a single roll is obtained in step S11, a straight seam welding is performed using a argon arc welder or a laser welder, and the weld extends from one end of the inner sleeve 22 to the other end. If multiple spirally connected rolls are obtained in step S11, a spiral seam welding machine is used to weld the multiple spirally connected rolls in sequence to form a thin cylinder.

[0086] Preferably, the length of the stainless steel round tube obtained in step S12 is greater than the length of the inner sleeve 22 of the composite tube that is finally processed. Specifically, the length of the stainless steel round tube obtained in step S12 is greater than the sum of the length of the socket portion 11, the length of the straight pipe portion 12 and the length of the socket portion 13.

[0087] The steps of making the socket sleeve 21 are the same as the steps of making the inner sleeve 22. The thickness of the socket sleeve 21 is substantially equal to the thickness of the inner sleeve 22, and the length of the socket sleeve 21 is greater than the length of the socket portion 13.

[0088] Step S2: The inner sleeve 22 , the middle layer 3 and the outer tube 1 are arranged in sequence from the inside to the outside, and the socket sleeve 21 is sleeved on the outer wall of the socket part 13 .

[0089] In this step, when the material of the middle layer 3 is hot melt adhesive or plastic, step S3 can be completed in the following three ways:

[0090] The first way is as follows:

[0091] First, the hot melt adhesive or plastic is formed into a round tube by extrusion molding, vacuum sizing, pulling, and cutting. Extrusion molding, vacuum sizing, pulling, and cutting can be performed by an extruder, a vacuum box, a tractor, and a cutting machine in the prior art. The extrusion molding is a prior art and will not be described in detail here.

[0092] Then, the obtained shaped intermediate layer 3 is sleeved on the outer wall of the inner sleeve 22. In this step, the sleeve can be made manually or by a sleeve machine.

[0093] Next, the inner wall of the bell mouth 11 and the outer wall of the socket 13 are sprayed. After the outer walls of the bell mouth 11 and the socket 13 are heated, powdered hot melt adhesive or plastic is rotomolded or sprayed on the inner wall of the bell mouth 11 and the outer wall of the socket 13 by a roller coater or a plastic coating machine.

[0094] Finally, the intermediate layer 3 and the inner sleeve 22 are inserted into the outer tube 1 as a whole, and the socket sleeve 21 is inserted into the outer wall of the socket part 13. Similarly, in this step, the sleeve can be completed manually or by a pipe threading machine.

[0095] The second way is as follows:

[0096] First, after the inner wall of the outer tube 1 and the outer wall of the insertion part 13 are heated, a roller coating machine or a plastic coating machine is used to roll-coat or spray-coat the powdered hot melt adhesive on the inner wall of the outer tube 1 and the outer wall of the insertion part 13. The thickness of the roll-coating or spray-coating is greater than 0.2 mm.

[0097] Then, the inner sleeve 22 is inserted into the outer tube 1 with the middle layer 3 on the inner wall, and the socket sleeve 21 is inserted into the outer wall of the socket part 13 .

[0098] The third way is as follows:

[0099] First, after heating the outer wall of the inner sleeve 22 and the outer wall of the socket part 13, a powdered hot melt adhesive is roto-molded or spray-molded on the outer wall of the inner sleeve 22 and the outer wall of the socket part 13 made of stainless steel by a roller coating machine or a plastic coating machine. The thickness of the roto-molding or spray-molding is greater than 0.2 mm. Then, the inner sleeve 22 with the intermediate layer 3 on the outer wall is inserted into the outer tube 1, and the socket sleeve 21 is inserted into the outer wall of the socket part 13.

[0100] When the material of the middle layer 3 is rubber, first roll the rubber sheet on the outer wall of the inner tube 2, then use adhesive to bond the rubber seam, and then insert the inner tube 2 with rubber into the outer tube 1. Alternatively, put the rubber tube on the outer wall of the inner tube 2 and then put the whole tube into the outer tube 1. The length of the rubber should be enough to cover the inner wall of the socket part 11, the inner wall of the straight tube part 12, the inner wall of the plug part 13, the end face of the plug part 13 and the outer wall of the plug part 13. The rubber tube that exceeds the end face of the plug part 13 is turned outward and put on the outer wall of the plug part 13, and then the plug sleeve 21 is put on the rubber pad on the outer wall of the plug part 13.

[0101] Step S3: Press the inner sleeve 22 and the middle layer 3 onto the outer tube 1 , and press the socket sleeve 21 onto the outer wall of the socket sleeve 21 .

[0102] This step can be completed by spin forming or hydraulic forming. During spin forming, the inner sleeve 22 of the socket part 13, the straight pipe part 12 and the socket part 11 are respectively spin-formed by a pipe spinning machine. When the socket part 11 is spun, it is spun from the inside to the outside, so that the inner sleeve 22 lined with stainless steel material, the middle layer 3, and the outer tube 1 are closely attached in sequence. During hydraulic forming, the two ends of the inner sleeve 22 of stainless steel material inserted into the outer tube 1 are sealed, and water is injected into the tube to pressurize it, so that the inner sleeve 22, the middle layer 3, and the outer tube 1 are closely attached in sequence.

[0103] Step S4: welding the inner sleeve 22 and the socket sleeve 21, wherein the welding point is located on the end surface of one end of the socket portion 13 of the composite pipe.

[0104] In this step, first, the inner sleeve 22 and / or the socket sleeve 21 at one end of the socket part 13 are spun by using a pipe mouth spinning machine, so that one end of the inner sleeve 22 and / or one end of the socket sleeve 21 covers the end surface of the socket part 13 of the composite pipe. Then, the excess burrs are trimmed to facilitate subsequent welding. Finally, the inner sleeve 22 and the socket sleeve 21 are welded together, and the welding point is located at the end surface of the socket part 13 of the composite pipe.

[0105] Step S5: Compounding.

[0106] In this step, the pipe is heated by a medium frequency inductor or a heating furnace, the hot melt adhesive is melted, and after cooling, the outer pipe 1 and the inner sleeve 22 are bonded together, and the socket sleeve 21 and the socket part 13 are bonded together.

[0107] When the material of the middle layer 3 is plastic or rubber, there is no step S5.

[0108] After completing the above steps, the outer wall of the pipe is sprayed with paint or plastic coated or other methods are used for external anti-corrosion treatment.

[0109] Embodiment 2

[0110] The difference between this embodiment and the first embodiment lies in the structure of the socket portion 11 and the number of sealing rings 4 .

[0111] like Figures 5 to 8 As shown, from the direction away from the straight pipe part 12 toward the direction close to the straight pipe part 12, the socket part 11 includes a sealing ring installation part 116 and a transition part 117 which are integrally connected and arranged in sequence on the same center line. The sealing ring installation part 116 is a cylindrical structure, and the inner wall of the sealing ring installation part 116 is provided with at least two annular grooves arranged at intervals, the annular ring and the composite pipe have the same center line, and the groove is a sealing ring installation groove 118. The transition part 117 includes a cylindrical part and a truncated cone part, and the sealing ring installation part 116, the cylindrical part, the truncated cone part and the straight pipe part 12 are connected in sequence. The inner diameter of the cylindrical part is larger than the inner diameter of the straight pipe part 12.

[0112] In this embodiment, two sealing ring installation grooves 118 are provided on the inner wall of the socket portion 11. The inner tube 2 covers the inner wall of the cylindrical portion of the socket portion 11, the inner wall of the truncated cone portion, and the inner wall of a sealing ring installation groove 118 close to the cylindrical portion, and the inner tube 2 does not cover the inner wall of a sealing ring installation groove 118 away from the cylindrical portion.

[0113] Based on the above structure, Figure 7 , 8 As shown, when two adjacent composite pipes are connected, the spigot 13 of one composite pipe is inserted into the socket 11 of the adjacent composite pipe and sealed by at least two sealing rings 4, each of which is installed in each sealing ring installation groove 118. Similarly, the inner ring of at least one sealing ring 4 contacts the outer wall of the spigot sleeve 21 on the outer wall of the spigot 13 of one composite pipe, and the outer ring of at least one sealing ring 4 contacts the inner wall of the inner pipe 2 at one end of the socket 11 of the adjacent composite pipe. Compared with the first embodiment, the socket structure of this embodiment is simpler and easier to manufacture.

[0114] Embodiment 3

[0115] The difference between this embodiment and the first or second embodiment is the method of forming the socket sleeve 21 .

[0116] In this embodiment, the socket sleeve 21 and the inner sleeve 22 are not made separately, but the circular tubular inner tube 2 is made as a whole. After the inner tube 2 is inserted into the outer tube 1, one end of the inner tube 2 extends beyond the end face of the socket part 13, and the portion of the inner tube 2 that extends beyond the end face of the socket part 13 is flanged by spin forming and pressed against the outer wall of the socket part 13 to form the socket sleeve 21.

[0117] Finally, it is necessary to explain here that the above embodiments are only used to further illustrate the technical solution of the utility model in detail and cannot be understood as limiting the protection scope of the utility model. Some non-essential improvements and adjustments made by technicians in this field based on the above content of the utility model belong to the protection scope of the utility model.

Claims

1. A multi-layer composite pipe with a socket coating, characterized in that: The invention comprises an inner tube (2), an intermediate layer (3) and an outer tube (1); the inner tube (2), the intermediate layer (3) and the outer tube (1) are bonded together to form a composite tube or compressed to form a composite tube; the material of the intermediate layer (3) is non-metallic; the outer tube (1) comprises a socket portion (11), a straight tube portion (12) and a plug portion (13) which are connected in sequence; the inner tube (2) is made of a corrosion-resistant metal material; one section of the inner tube (2) covers part of the inner wall of the socket portion (11) and the inner wall of the straight tube portion (12); and the other section of the inner tube (2) completely covers the plug portion (13).

2. The composite pipe according to claim 1, characterized in that: The inner tube (2) comprises an inner sleeve (22) and a socket sleeve (21), and the inner sleeve (22), the middle layer (3) and the outer tube (1) are sleeved in sequence from the inside to the outside.

3. The composite pipe according to claim 2, characterized in that: The inner sleeve (22) and the socket sleeve (21) are integrally formed.

4. The composite pipe according to claim 3, characterized in that: The socket sleeve (21) is formed by spinning and turning one end of the inner tube (2) outward.

5. The composite pipe according to claim 3, characterized in that: The socket sleeve (21) and the inner sleeve (22) are welded together.

6. The composite pipe according to claim 5, characterized in that: The welding point of the socket sleeve (21) and the inner sleeve (22) is located on the end surface of the socket part (13), and the inner tube (2) area covering the end surface of the socket part (13) is formed by welding after flanging the socket sleeve (21) and / or flanging the inner sleeve (22).

7. The composite pipe according to claim 1, characterized in that: The material of the middle layer (3) is hot melt adhesive, plastic or rubber.

8. The composite pipe according to any one of claims 1 to 7, characterized in that: The material of the outer tube (1) is metal.

9. The composite pipe according to any one of claims 1 to 7, characterized in that: The thickness of the middle layer (3) is not less than 0.2 mm, and the thickness of the inner sleeve (22) is not less than 0.1 mm.

10. The composite pipe according to claim 1, characterized in that: When two adjacent composite pipes are connected, the spigot portion (13) of one composite pipe is inserted into the socket portion (11) of the adjacent composite pipe and sealed by a sealing ring (4); the outer ring of the sealing ring (4) contacts the inner wall of the inner pipe (2) of the socket portion (11) of one composite pipe, and the inner ring of the sealing ring (4) contacts the outer wall of the spigot sleeve (21) on the outer wall of the spigot portion (13) of the adjacent composite pipe.

Citation Information

Cited By

  • Multi-layer composite pipe coated with bell and spigot and manufacturing method of multi-layer composite pipe

    CN119353504A

  • A multi-layer composite pipe with socket and spigot covering and its manufacturing method

    CN119353504B