Electrostatic chuck
The electrostatic chuck with a ceramic sintered body and optimized surface features effectively addresses heat transfer inefficiencies by enhancing contact and gas flow, ensuring rapid heat removal and uniform temperature distribution for higher power semiconductor processes.
Patent Information
- Application Number
- JP2023044419
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing electrostatic chucks face challenges in efficiently transferring heat from substrates due to low contact ratios and non-uniform gas flow paths, which can lead to temperature inconsistencies and insufficient heat removal, especially with increased power densities in semiconductor processes.
The electrostatic chuck features a ceramic sintered body with a high contact ratio of 30% to 99.5% and a surface roughness of 0.2 μm or less, along with skewness Rsk less than -1.0, combined with pin-shaped and island-shaped protrusions to enhance heat conduction and gas transfer, ensuring uniform heat distribution and improved adsorption.
This design allows for rapid heat removal from substrates, maintaining temperature uniformity and suppressing dechucking performance deterioration, making it suitable for higher power semiconductor processes.
Smart Images

Figure 2024134222000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrostatic chuck. [Background technology]
[0002] Electrostatic chucks are used as a means for holding substrates in film formation devices such as plasma CVD in which a substrate (wafer) is placed in a reduced pressure chamber, raw material gas is supplied onto the substrate, the raw material gas is converted into plasma using radio frequency (RF) current or the like, and a thin film is formed by depositing a substance generated by a chemical reaction on the substrate, and in etching devices such as plasma etching in which plasma is used to remove the substrate surface to form grooves, patterns, etc.
[0003] In the above-mentioned plasma processing steps, the temperature of the substrate also rises due to the generated heat. In this case, various methods are used to adjust the temperature of the substrate so that it is suitable for each processing temperature. For example, the temperature of the substrate is kept constant by joining a base member made of a metal such as aluminum having a flow path for circulating a medium such as cooling water to the surface facing the substrate holding surface of the electrostatic chuck, or by providing a heat transfer structure for introducing an inert gas such as He into the space between the back surface of the substrate and the substrate holding surface of the electrostatic chuck.
[0004] In recent years, advances in manufacturing process technology have led to an increase in the power density of plasma, which has led to an increase in the amount of heat incident on the substrate. The increase in the amount of heat incident on the substrate can cause the substrate temperature to rise excessively, which can affect each manufacturing process, such as causing defects in the pattern formation process, so it is necessary to improve the cooling performance of the substrate more than ever before. In addition, in order to improve manufacturing yields, it is necessary to adjust the substrate temperature to an appropriate temperature early on. For example, although the appropriate process temperature differs depending on the manufacturing process, it needs to be controlled to around 100°C to 400°C (up to around 200°C for aluminum-based substrates).
[0005] Patent document 1 discloses a substrate cooling device having a substrate contact plate having a protruding portion provided on the peripheral portion, a recessed portion forming a cavity, a central portion having a plurality of convex portions each terminating at a contact surface and each of the contact surfaces being generally on the same plane as the surface of the protruding portion provided on the peripheral portion, and at least one gas inlet groove for supplying gas into the cavity, and a cooling plate thermally connected to the substrate contact plate and having a groove for passing a cooling liquid.
[0006] Patent Document 2 discloses an electrostatic chuck in which the gas grooves of the electrostatic chuck are composed of a plurality of radial grooves arranged at equal intervals, a plurality of annular grooves connected to the radial grooves and arranged concentrically, and at least one partition groove extending in the radial direction that divides each mounting surface surrounded by two adjacent annular grooves and two adjacent radial grooves into two or more parts in the region from the first annular groove from the center onwards, so that the mounting surface surrounded by two adjacent annular grooves and two adjacent radial grooves, the mounting surface surrounded by two adjacent annular grooves, the radial grooves and the partition groove, and the mounting surface surrounded by two adjacent annular grooves and two adjacent partition grooves each have approximately the same area. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 9-232415 [Patent Document 2] JP 2002-170868 A Summary of the Invention [Problem to be solved by the invention]
[0008] The multiple protrusions described in Patent Document 1 have a contact surface with the substrate that is roughened to about Ra 0.35 μm to 3.0 μm, and the contact rate between the substrate and the multiple protrusions is about 2 to 20%. The main part of the cooling means described in Patent Document 1 is heat transfer by the substrate and the gas in the cavity, but the contact rate is low and the gas pressure is also low (20 Torr or less). Therefore, the substrate cooling device of Patent Document 1 may be insufficient to transfer a large amount of heat quickly.
[0009] In the technology described in Patent Document 2, the heat transfer gas is introduced from a gas inlet formed only in the center of the substrate, flows in the radial grooves in the radial direction, and then flows while merging with the annular groove. Because the gas flow path described in Patent Document 2 is a complex flow path, there is a risk that it will be insufficient to equalize the temperature of the entire substrate or to transfer a larger amount of heat due to unevenness in the flow of the heat transfer gas at the branching point of the flow path and a time lag in the gas flow from the center of the substrate to the outer diameter. In addition, the pressure of the helium gas introduced from the gas inlet was low (about 10 Torr).
[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide an electrostatic chuck that can quickly remove heat input to a substrate, can accommodate the increasing power required for semiconductor processes, and can suppress deterioration of dechucking performance. [Means for solving the problem]
[0011] (1) In order to achieve the above object, the present invention provides the following means: That is, an electrostatic chuck according to an embodiment of the present invention is an electrostatic chuck comprising a base made of a sintered ceramic body, an electrostatic attraction electrode embedded in the base, and a plurality of gas introduction holes opening in an upper surface of the base, the base having a surface with a contact rate with a substrate placed thereon of 30% or more and 99.5% or less, the surface roughness Ra of the surface being 0.2 μm or less, and the skewness Rsk calculated from a roughness curve of the surface being negative.
[0012] In this way, by increasing the contact rate with the substrate and by controlling the surface condition of the surface in contact with the substrate to fall within the above range, the contact condition between the substrate and the surface of the base body is improved, the heat input to the substrate can be removed early, and the semiconductor process can be made more powerful. In addition, the heat transfer from the substrate to the electrostatic chuck can be improved while preventing the deterioration of the dechucking performance.
[0013] (2) In the electrostatic chuck according to the application example of (1) above, the skewness Rsk is less than −1.0.
[0014] This makes it possible to further suppress deterioration of the dechucking performance while maintaining heat transfer from the substrate to the electrostatic chuck.
[0015] (3) Furthermore, the electrostatic chuck according to the application example of (1) or (2) above is characterized by further comprising a base member joined to a lower surface of the substrate opposite to the upper surface thereof, the base member having a gas flow passage connected to the gas inlet hole.
[0016] This allows heat to be conducted from the substrate to the base member, and allows heat to be transferred more efficiently from the substrate to the substrate.
[0017] (4) Furthermore, in the electrostatic chuck according to any one of the application examples of (1) to (3) above, the electrostatic chuck is characterized in that it comprises a plurality of pin-shaped convex portions formed so as to protrude upward from the upper surface of the base, and an annular convex portion formed so as to protrude upward from the upper surface of the base so as to surround the plurality of pin-shaped convex portions, and the surface is constituted by upper end surfaces of the pin-shaped convex portions and an upper end surface of the annular convex portion.
[0018] This allows the substrate to be evenly adsorbed even if it is warped or wavy, and the incident heat to the substrate can be transferred evenly through thermal conduction through contact with the pin-shaped protrusions and the heat transfer effect of the gas.
[0019] (5) Furthermore, in the electrostatic chuck of any of the application examples described above in (1) to (3), the electrostatic chuck is characterized in that it comprises a plurality of island-shaped convex portions formed so as to protrude upward from the upper surface of the base, and an annular convex portion formed so as to protrude upward from the upper surface of the base so as to surround the plurality of island-shaped convex portions, and the surface is constituted by upper end surfaces of the island-shaped convex portions and an upper end surface of the annular convex portion.
[0020] This allows the substrate to be evenly adsorbed even if it is warped or wavy, and the incident heat to the substrate can be transferred evenly through thermal conduction through contact with the island-shaped protrusions and the heat transfer effect of the gas.
[0021] (6) In the electrostatic chuck according to the application example of (4) above, the height of the pin-shaped protrusion is not less than 5 μm and not more than 10 μm.
[0022] This makes it possible to increase the electrostatic attraction force at the non-contact surface portion that is not in contact with the substrate, thereby improving the attraction force of the entire substrate. Also, the space can be filled with gas quickly.
[0023] (7) In the electrostatic chuck according to the application example of (5) above, the island-shaped protrusions have a height of 25 μm or more and 1000 μm or less.
[0024] This allows the amount of gas introduced into the space to be increased, and the heat transfer effect of the gas to be improved. Effect of the Invention
[0025] According to the electrostatic chuck of the present invention, the contact state between the substrate and the surface of the base body is improved, the heat input to the substrate can be removed early, and the electrostatic chuck can be adapted to high-power semiconductor processes. In addition, the deterioration of dechucking performance can be suppressed while improving the heat transfer from the substrate to the electrostatic chuck. [Brief description of the drawings]
[0026] [Figure 1]FIG. 1 is a schematic cross-sectional view showing an example of an electrostatic chuck according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of the upper surface of an electrostatic chuck according to an embodiment of the present invention. [Diagram 3] FIG. 11 is a schematic cross-sectional view showing a modified example of an electrostatic chuck according to an embodiment of the present invention. [Figure 4] 10A and 10B are schematic diagrams illustrating modified examples of the upper surface of the electrostatic chuck according to the embodiment of the present invention. [Diagram 5] FIG. 11 is a schematic cross-sectional view showing a modified example of an electrostatic chuck according to an embodiment of the present invention. [Figure 6] 10A and 10B are schematic diagrams illustrating modified examples of the upper surface of the electrostatic chuck according to the embodiment of the present invention. [Figure 7] FIG. 11 is a schematic partial cross-sectional view showing a modified example of an electrostatic chuck according to an embodiment of the present invention. [Figure 8] 1 is a table showing the production conditions and the results of various tests of Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Next, an embodiment of the present invention will be described with reference to the drawings. In order to facilitate understanding of the description, the same reference numerals are used for the same components in each drawing, and duplicated descriptions will be omitted. In the configuration diagrams, the size of each component is conceptually shown, and does not necessarily represent the actual dimensional ratio.
[0028] [Embodiment] (Structure of electrostatic chuck) An electrostatic chuck according to an embodiment of the present invention will be described with reference to Figs. 1 and 2. Fig. 1 is a schematic cross-sectional view showing an example of an electrostatic chuck according to an embodiment of the present invention. Fig. 2 is a schematic view showing an example of the upper surface of an electrostatic chuck according to an embodiment of the present invention. Fig. 1 shows a cross section taken along line AA in Fig. 2. An electrostatic chuck 100 according to an embodiment of the present invention includes a base 110 and at least one electrostatic attraction electrode 120.
[0029] The base 110 is made of a ceramic sintered body. The base 110 may be in various shapes such as a substantially circular plate, a polygonal plate, or an elliptical plate. The base 110 is flat except for protrusions formed on the upper surface 112. Materials for the ceramic sintered body include aluminum nitride, aluminum oxide, silicon carbide, and silicon nitride.
[0030] The base 110 has a plurality of gas introduction holes 118 opening on the upper surface 112 of the base 110. The gas introduction holes 118 are preferably formed in a plurality of locations in order to introduce a heat transfer gas uniformly and at high pressure to the rear surface of the substrate W. For example, it is preferable that the diameter of the gas introduction hole is 0.05 mm to 3 mm, one is arranged at a position corresponding to the center 116 of the base 110, and a plurality of gas introduction holes are arranged at equal intervals on one or more concentric circles increasing at equal intervals in the radial direction from the center. Alternatively, a plurality of gas introduction holes may be arranged at predetermined intervals in a regular pattern such as an equilateral triangle or square. In order to obtain uniform heat transfer, it is preferable to arrange the gas introduction holes 118 as symmetrically as possible.
[0031] However, depending on the arrangement of lift pin holes, convex portions, etc., it is not necessary for all gas introduction holes 118 to be arranged regularly. Also, even when surface 130 is composed of the upper end faces of pin-shaped convex portions or island-shaped convex portions described later, it is preferable to arrange gas introduction holes 118 as symmetrically as possible according to the shape of the concave portions and groove portions.
[0032] The base 110 has a surface 130 with a contact rate with the substrate W placed thereon of 30% or more and 99.5% or less. The surface 130 of the base 110 refers to the surface that actually comes into contact with the substrate W. In this way, by setting the contact rate between the surface 130 of the base 110 that actually comes into contact with the substrate W and the substrate W to be 30% or more and 99.5% or less, thermal conduction is improved and heat can be efficiently transferred from the substrate W to the base 110, thereby improving heat transfer. As a result, the contact state between the substrate W and the surface 130 of the base 110 is improved, the amount of heat input to the substrate W can be removed early, and it is possible to respond to the increasing power of semiconductor processes.
[0033] The contact rate can be calculated by (area of the surface of the base) / (area of the substrate to be attached)×100(%). The area of the surface 130 of the base 110 can be calculated by subtracting the area of holes of the substrate W that are not in contact with the base 110, such as the gas introduction holes 118 and lift pin holes, from the area of the upper surface 112 of the base 110. When the base 110 is present outside the outer periphery of the substrate W, that is, when the base 110 is larger than the substrate W, the area of the upper surface 112 of the base 110 when calculating the area of the surface 130 of the base 110 is to exclude the upper surface 112 of the base 110 that is outside the outer periphery of the substrate W. The area of the surface 130 of the base 110 may be measured using a laser interferometer. The area of the substrate W to be attached is to be a substrate that meets the standard of SEMI (Semiconductor Equipment and Materials International). For example, the area of the substrate W with a diameter Φ of 300 mm can be used as a reference.
[0034] The surface roughness (center line average roughness) Ra of the surface 130 is 0.2 μm or less. In this way, by making the surface roughness Ra of the surface 130 close to a mirror finish of 0.2 μm or less, the contact state with the substrate W is improved and the chucking force is increased. This allows a heat transfer gas such as He gas at a higher pressure to be introduced from the multiple gas introduction holes 118, improving the heat transfer of the substrate W by gas heat transfer. In addition, the improved chucking force can suppress unexpected detachment of the substrate W from the electrostatic chuck 100 due to high gas pressure. For example, even under a pressure of 100 Torr, the substrate W can be suppressed from being detached from the base 110, and the heat of the substrate W can be cooled early. The lower limit of the surface roughness Ra of the surface 130 does not need to be particularly limited, but it is preferable that it is 0.01 μm or more in consideration of processing time, etc.
[0035] The skewness Rsk obtained from the roughness curve of the surface 130 is negative. In this way, by increasing the contact rate with the substrate W and then making the skewness Rsk obtained from the roughness curve of the surface 130 negative, it is possible to improve heat transfer from the substrate W to the base 110 while suppressing deterioration of the dechucking performance of the substrate W. It is preferable that the skewness Rsk is less than -1.0. By making the skewness Rsk less than -1.0, it is possible to further suppress deterioration of the dechucking performance while maintaining heat transfer from the substrate to the electrostatic chuck.
[0036] The skewness Rsk is an index showing the symmetry of the height distribution, and is an index showing the ratio of the peaks and valleys to the average height of the roughness curve, which is defined in JIS B 0601. A negative skewness Rsk indicates that the surface has many fine valleys. When the skewness Rsk is negative, the valleys allow the heat transfer gas to enter, and the gas heat transfer is improved. In addition, the improved contact rate can prevent the chucking force from becoming too large, which leads to a deterioration in the dechucking performance. The lower limit of the skewness Rsk is not particularly limited, but it is preferable that it is, for example, -5.0 or more.
[0037] The surface roughness Ra and the skewness Rsk can be measured in accordance with JIS B 0601 using a commercially available non-contact surface roughness meter. As a method for making the skewness Rsk and the surface roughness Ra within the range of the present invention, a ceramic sintered body (base 110) can be manufactured by a known manufacturing method, followed by sandblasting or grinding with a grindstone having a large mesh (small grain size), and then polishing the top surface. As a method for making the skewness Rsk less than 0 (i.e. negative), for example, the following can be used. After processing the outer shape of the base 110, the surface that will become the surface 130 is ground with a grindstone having a grit size higher than #170. Then, polishing is performed using free abrasive grains (diamond slurry) with a grain size larger than 3 μm, and finally, finish polishing is performed using small free abrasive grains with a grain size of 3 μm or less. Polishing is performed for a total of 3 hours or more. Also, by shortening the time for finish polishing, the skewness Rsk can be made less than -1.0.
[0038] From the viewpoint of suppressing particle shedding in the valleys of the surface 130 and ensuring the adsorption force, it is preferable to design the maximum valley depth Rv in the reference length of the surface 130 to be 2 μm or more and 8 μm or less. The maximum valley depth Rv can also be measured by a measurement method conforming to JIS B 0601.
[0039] The electrostatic attraction electrode 120 is embedded in the base 110. The electrostatic attraction electrode 120 is embedded in a shape that corresponds to the design of the electrostatic chuck 100. The electrostatic attraction electrode 120 is preferably made of W, Mo, or an alloy containing these as main components.
[0040] The base 110 may have an electrode embedded therein other than the electrostatic attraction electrode 120. For example, by embedding the electrostatic attraction electrode 120 and a heater electrode in the base 110, the base 110 can exhibit the electrostatic attraction function of the substrate, as well as the temperature control and heating functions, thereby making the semiconductor manufacturing process more sophisticated.
[0041] Fig. 3 is a schematic cross-sectional view showing a modified example of the electrostatic chuck 100 according to the embodiment of the present invention. Fig. 4 is a schematic view showing a modified example of the upper surface of the electrostatic chuck 100 according to the embodiment of the present invention. Fig. 3 shows a cross section taken along line BB in Fig. 4. As shown in Fig. 3 or 4, the electrostatic chuck 100 preferably includes a plurality of pin-shaped protrusions 140 and an annular protrusion 150. In this case, the surface 130 is formed by upper end surfaces 142 of the pin-shaped protrusions and an upper end surface 152 of the annular protrusion.
[0042] When the pin-shaped protrusions 140 are formed on the base 110, a plurality of the pin-shaped protrusions 140 are formed protruding upward from the upper surface 112 of the base 110. The pin-shaped protrusions 140 are formed surrounded by a recess 144. That is, the bottom surface of the recess 144 becomes the upper surface 112 of the base 110. The shape of the pin-shaped protrusions 140 is appropriately selected from among pillar shapes such as a cylindrical shape or a rectangular pillar, pyramid shapes such as a cone shape or a pyramid shape, and shapes in which the upper part of a pyramid shape such as a truncated cone shape or a truncated pyramid shape is cut off.
[0043] The arrangement of the pin-shaped protrusions 140 is not particularly limited. It may be in a known form or a form similar thereto. For example, it is preferable that they are arranged regularly, such as in a triangular lattice form as shown in FIG. 4, a concentric circle form, or a square lattice form. It is preferable that the distance (pitch) between the centers of adjacent pin-shaped protrusions 140 is 4 mm or more and 20 mm or less. It is preferable that the maximum diameter of the upper end surface 142 of the pin-shaped protrusions is 0.1 mm or more and 5 mm or less. The surface roughness Ra of the upper end surface 142 of the pin-shaped protrusions is 0.2 μm or less. It is preferable that the surface roughness Ra of the upper end surface 142 of the pin-shaped protrusions is 0.01 μm or more.
[0044] The height of the pin-shaped protrusions 140 is preferably 5 μm or more and 10 μm or less. This makes it possible to increase the electrostatic adsorption force in the non-contact surface portion that is not in contact with the substrate W, and improve the adsorption force of the entire substrate W. In addition, the space can be filled with gas quickly. It is difficult to form the pin-shaped protrusions 140 with a height of less than 5 μm. In addition, if the height of the pin-shaped protrusions 140 exceeds 10 μm, an excessively large voltage is required to obtain a sufficient adsorption force, which is not industrially preferable. The height of the pin-shaped protrusions 140 is defined as the distance between the upper surface 112 of the base 110 and the upper end surface 142 of the pin-shaped protrusions.
[0045] When the pin-shaped protrusions 140 are formed on the base 110, an annular protrusion 150 is formed. The annular protrusion 150 is formed to protrude upward from the upper surface 112 of the base 110 so as to surround the multiple pin-shaped protrusions 140. The outer diameter of the annular protrusion 150 is set to be the same as or smaller than the outer diameter of the base 110. The width of the annular protrusion 150 is preferably 0.3 mm or more and 5 mm or less in order to function as a sealing portion. In addition, the annular protrusion 150 may be formed in multiple layers (for example, double layers) as a measure against gas leakage caused by increasing the gas pressure.
[0046] The height of the annular convex portion 150 is preferably the same as the height of the pin-shaped convex portions 140. This allows the gas to be sealed in. However, if the amount of gas that escapes from the gap between the upper end surface 152 of the annular convex portion and the substrate W is an amount that does not affect the heat transfer by the gas, the height of the annular convex portion 150 may be lower than the height of the pin-shaped convex portions 140. Specifically, it is permissible for the height to be lower by about 1 μm to 3 μm. The height of the annular convex portion 150 is the distance between the upper surface 112 of the base 110 (the bottom surface of the recess) and the upper end surface 152 of the annular convex portion. The surface roughness Ra of the upper end surface 152 of the annular convex portion is 0.2 μm or less. The surface roughness Ra of the upper end surface 152 of the annular convex portion is preferably 0.01 μm or more.
[0047] The upper end faces 142 of the multiple pin-shaped protrusions and the upper end face 152 of the annular protrusion collectively define a plane or curved surface (substrate mounting surface 132) of a predetermined shape on which the substrate W is mounted. As a result, the multiple pin-shaped protrusions 140 and the annular protrusion 150 support the substrate W. That is, in this modification, the upper end faces 142 of the pin-shaped protrusions and the upper end face 152 of the annular protrusion that are in actual contact with the substrate W of the substrate mounting surface 132 are the surface 130. Note that, among the multiple pin-shaped protrusions 140, there may be some whose upper end faces do not come into contact with the substrate W. This is because, even if such pin-shaped protrusions 140 exist, it is possible to support the substrate W depending on the arrangement of the surrounding pin-shaped protrusions 140. 3, the entire upper end faces 142 of the pin-shaped convex portions and the upper end face 152 of the annular convex portion are in contact with the substrate W, but only a portion of the upper end faces 142 of the pin-shaped convex portions or the upper end face 152 of the annular convex portion may be in contact with the substrate W. In such a case, the area of the surface 130 is defined as the area of the upper end faces 142 of the pin-shaped convex portions and the upper end face 152 of the annular convex portion that actually contacts the substrate W.
[0048] Fig. 5 is a schematic cross-sectional view showing a modified example of the electrostatic chuck 100 according to the embodiment of the present invention. Fig. 6 is a schematic view showing a modified example of the upper surface of the electrostatic chuck according to the embodiment of the present invention. Fig. 5 shows a cross section taken along line CC in Fig. 6. As shown in Fig. 5 or 6, the electrostatic chuck 100 preferably includes an island-shaped protrusion 160 and an annular protrusion 150. In this case, the surface 130 is formed by an upper end surface 162 of the island-shaped protrusion and an upper end surface 152 of the annular protrusion.
[0049] When the island-shaped protrusions 160 are formed on the base 110, the island-shaped protrusions 160 are formed by protruding upward from the upper surface 112 of the base 110. The island-shaped protrusions 160 are formed surrounded by the grooves 164. That is, the bottom surface of the grooves 164 becomes the upper surface 112 of the base 110. The shape and arrangement of the island-shaped protrusions 160 are not particularly limited. The shape of the grooves 164 is preferably a linear shape combining straight lines and arcs, or a wide shape without abruptly narrowing portions, so that the heat transfer gas can be quickly distributed inside the grooves 164. When the grooves 164 are formed linearly, they can be, for example, a checkerboard-shaped groove combining linear grooves, a radial groove passing through the center, or a doughnut-shaped groove combining annular grooves. A shape combining these may also be used. When the grooves 164 are formed linearly, the width of the grooves 164 is preferably 0.5 mm or more and 5.0 mm or less. A gas introduction hole 118 may be formed in the upper end surface 162 of the island-shaped protrusion.
[0050] In this specification, a convex portion whose upper end surface has an area equal to or less than the area of a circle with a diameter of 5000 μm is referred to as a pin-shaped convex portion 140, and a convex portion whose upper end surface has an area greater than the area of a circle with a diameter of 5000 μm is referred to as an island-shaped convex portion 160. The area of each island-shaped convex portion 160 is preferably designed to be approximately the same for the purpose of uniforming the amount of heat transfer. The surface roughness Ra of the upper end surface 162 of the island-shaped convex portion is 0.2 μm or less. The surface roughness Ra of the upper end surface 162 of the island-shaped convex portion is preferably 0.01 μm or more.
[0051] The height of the island-shaped protrusion 160 is preferably 25 μm or more and 1000 μm or less. In the case of the island-shaped protrusion 160, the flow path of the heat transfer gas is the groove 164, so that the volume is smaller than that of the recess 144 of the pin-shaped protrusion 140. Therefore, by increasing the height of the island-shaped protrusion 160, that is, by deepening the groove 164, the amount of gas introduced into the space can be increased, and the heat incident on the substrate W can be uniformly transferred by the solid heat transfer and gas heat transfer effects. To ensure the electrostatic adsorption force, the island-shaped protrusion 160 may also be provided in a multi-layer structure in which the electrostatic adsorption electrode 120 is arranged inside the island-shaped protrusion 160.
[0052] When the island-shaped protrusions 160 are formed on the base 110, an annular protrusion 150 is formed. The annular protrusion 150 is formed to protrude upward from the upper surface 112 of the base 110 so as to surround the multiple island-shaped protrusions 160. The outer diameter of the annular protrusion 150 is set to be the same as or smaller than the outer diameter of the base 110. The width of the annular protrusion 150 is preferably 0.3 mm or more and 5 mm or less in order to function as a sealing portion. In addition, the annular protrusion 150 may be formed in multiple layers (for example, double layers) as a measure against gas leakage caused by increasing the gas pressure.
[0053] The height of the annular convex portion 150 is preferably the same as the height of the island-shaped convex portions 160. This allows the gas to be sealed in. However, if the amount of gas that escapes from the gap between the upper end surface 152 of the annular convex portion and the substrate W is an amount that does not affect the heat transfer by the gas, the height of the annular convex portion 150 may be lower than the height of the island-shaped convex portions 160. Specifically, it is permissible for the height to be lower by about 1 μm to 3 μm. The height of the annular convex portion 150 is the distance between the upper surface 112 of the base 110 (the bottom surface of the groove portion 164) and the upper end surface 152 of the annular convex portion. The surface roughness Ra of the upper end surface 152 of the annular convex portion is 0.2 μm or less. The surface roughness Ra of the upper end surface 152 of the annular convex portion is preferably 0.01 μm or more.
[0054] The upper end faces 162 of the island-shaped convex portions and the upper end face 152 of the annular convex portion together define a plane or curved surface (substrate mounting surface 132) of a predetermined shape on which the substrate W is mounted. As a result, the island-shaped convex portions 160 and the annular convex portion 150 support the substrate W. That is, in this modification, the upper end faces 162 of the island-shaped convex portions and the upper end face 152 of the annular convex portion that are actually in contact with the substrate W of the substrate mounting surface 132 are the surface 130. Note that in FIG. 5, the entire upper end faces 162 of the island-shaped convex portions and the upper end face 152 of the annular convex portion are in contact with the substrate W, but only a part of the upper end face 162 of the island-shaped convex portions or the upper end face 152 of the annular convex portion may be in contact with the substrate W. In such a case, the area of the surface 130 is the area of the upper end faces 162 of the island-shaped convex portions and the upper end face 152 of the annular convex portion that are actually in contact with the substrate W. In a modified example in which a pin-shaped protrusion 140 or an island-shaped protrusion 160 is formed, the area of the surface 130 can be calculated by subtracting the areas of the gas inlet holes 118 and lift pin holes inside the substrate W, the recesses 144 that form the pin-shaped protrusions 140 and annular protrusions 150, and the grooves 164 that form the island-shaped protrusions 160 and annular protrusions 150 from the area of the substrate W.
[0055] The height of the pin-shaped protrusion 140, the island-shaped protrusion 160, or the annular protrusion 150, and the three-dimensional position of the upper end surface 142 of the pin-shaped protrusion, the upper end surface 162 of the island-shaped protrusion, or the upper end surface 152 of the annular protrusion can be measured using a three-dimensional measuring device or a laser interferometer.
[0056] The base 110 may have both the pin-shaped protrusions 140 and the island-shaped protrusions 160. This improves the suction force in the portion where the island-shaped protrusions 160 are formed, and reduces the risk of particles getting caught in the portion where the pin-shaped protrusions 140 are formed, allowing the warped substrate W to be appropriately sucked according to the warpage. When the base 110 has both the pin-shaped protrusions 140 and the island-shaped protrusions 160, the depths of the recesses 144 and the grooves 164 may be different, that is, the upper surface 112 of the base 110 may differ depending on the position.
[0057] Fig. 7 is a schematic cross-sectional view showing a modified example of the electrostatic chuck 100 according to the embodiment of the present invention. As shown in Fig. 7, the electrostatic chuck 100 preferably includes a base member 170 that is joined to a lower surface 114 facing an upper surface 112 of a substrate 110 and has a gas flow passage 172 connected to a gas introduction hole 118. This allows heat to be conducted from the substrate 110 to the base member 170, and allows heat to be transferred more efficiently from the substrate W to the substrate 110.
[0058] The base member 170 functions as a cooling member used to transfer the heat input to the substrate W during the semiconductor process through the base body 110 and maintain the substrate W at a predetermined temperature. The base member 170 is made of metal or ceramics. As such metals, Al and Al alloys, which have good workability and high thermal conductivity, are most preferable, and other materials such as alloys containing copper, titanium, and nickel, and SUS may also be used. As ceramics, ceramics with a thermal conductivity of 100 W / m·K or more are particularly preferable, and examples thereof include aluminum nitride.
[0059] The base member 170 preferably has a coolant flow path 174 therein. The coolant flow path 174 is formed, for example, in a tubular shape. This can further improve the heat transfer performance from the substrate W. The coolant can be water, ethylene glycol, freon, or the like. The width of the coolant flow path 174 is preferably 1 mm or more and 60 mm or less. The cross-sectional shape of the coolant flow path 174 is not limited to a rectangle, and may be any shape that can be manufactured, such as a circle, an ellipse, a semicircle, or a stepped shape.
[0060] The substrate 110 and the base member 170 are preferably bonded by adhesion, as this is simple. The bonding method may be selected depending on the operating temperature of the semiconductor process used; for example, silicone resin bonding, In bonding, or bonding using Al foil may be used. A stress relaxation structure may be provided between the substrate 110 and the base member 170. Since the substrate 110 and the base member 170 generally have different thermal expansion coefficients, there is a risk of peeling between the substrate 110 and the base member 170 due to warping or deformation caused by thermal stress that occurs during use, but the risk of peeling can be suppressed by the stress relaxation layer.
[0061] The electrostatic chuck 100 may include a terminal 180 and a terminal hole 182, if necessary. The electrostatic chuck 100 may also include a lift pin hole (not shown) and the like.
[0062] [Electrostatic chuck manufacturing method] Next, a method for manufacturing an electrostatic chuck according to an embodiment of the present invention will be described. The electrostatic chuck according to an embodiment of the present invention is manufactured by, for example, a powder hot pressing method. The powder hot pressing method is a method in which ceramic raw material powder and a predetermined electrode are alternately stacked to embed the electrodes inside the ceramic, and then uniaxial hot pressing and firing the resulting material. By employing the powder hot pressing method, the electrostatic chuck can be manufactured in a short period of time. Note that the manufacturing method is not limited to this method, and may be, for example, a molded body hot pressing method disclosed in Japanese Patent No. 6148845, a green sheet lamination method, a CIP molding method, or other conventional manufacturing methods.
[0063] For example, additives such as sintering aids, binders, plasticizers, and dispersants are appropriately added to and mixed with ceramic powder to prepare ceramic raw material powder (slurry), and the granulated powder is granulated by a spray-drying method or the like. For example, when AlN is used as the raw material, 0.3 to 6 wt% of Y is added as a sintering aid to the AlN ceramic raw material powder. 2 O 3The mixture is mixed in a wet or dry manner, and a mixer such as a ball mill or a vibration mill can be used. As the ceramic powder used as the raw material, aluminum nitride, aluminum oxide, silicon carbide, silicon nitride, etc. are used.
[0064] The ceramic powder is preferably of high purity, and the purity is preferably 96% or more, more preferably 98% or more. The average particle size of the ceramic powder varies depending on the type of ceramic powder used as the raw material, but for example, when AlN is used as the raw material, the average particle size is preferably 0.1 μm to 1.0 μm, and more preferably 0.3 μm to 0.8 μm.
[0065] The material of the electrostatic adsorption electrode embedded in the ceramic sintered compact is preferably Mo, W, or an alloy thereof. The electrostatic adsorption electrode can be formed of a mesh, foil, coil, or thin film of these materials. For example, Mo mesh (wire diameter 0.1 mm, 50 mesh, plain weave) is cut into a predetermined shape to form the electrostatic adsorption electrode. The outer diameter is smaller than the outer diameter of the base so that it is not exposed from the outer surface of the base. A terminal for connection to an external power source may be embedded at the same time. A heater electrode may also be embedded for the purpose of local temperature control, etc.
[0066] For sintering, uniaxial hot press sintering or atmospheric sintering can be used. In uniaxial hot press sintering, a granulated powder that forms the base is filled into a bottomed carbon mold, and an electrostatic adsorption electrode cut into a predetermined shape after uniaxial pressing is placed on the compact. The same granulated powder is filled on top of it, a carbon punch is placed on it, and after molding, it is sintered under predetermined sintering conditions. For example, when AlN is used as the raw material, it is preferable to perform hot press sintering under temperature conditions of 1700°C to 2000°C, pressure conditions of 1 MPa to 20 MPa, and for 0.1 hours to 20 hours.
[0067] After firing, the gas inlet holes are formed, the front and back surfaces are processed, terminal holes are formed, and grinding and polishing are performed to a predetermined shape. The formation method can be blasting, milling, laser processing, etc. Also, multiple pin-shaped convex portions, multiple island-shaped convex portions, annular convex portions, etc. may be formed depending on the design of the electrostatic chuck. At this time, the gas inlet holes, multiple pin-shaped convex portions, multiple island-shaped convex portions, annular convex portions, etc. are formed so that the contact rate of the surface is within a predetermined range.
[0068] The surface that will become the substrate mounting surface is processed to a predetermined surface condition. First, the surface is shaped (formed into a flat surface, pin-shaped convex portions, or island-shaped convex portions) by laser processing, sandblasting, or grinding with a grindstone. This makes it possible to make the skewness Rsk of the surface negative after polishing, which will be described later. Then, the top surface that will become the substrate mounting surface is polished to have a surface roughness Ra within a predetermined range.
[0069] After polishing, terminals are connected to the terminal holes with brazing material etc. Ni etc. can be used for the terminals. Au brazing material etc. can be used for the brazing material.
[0070] In this manner, it is possible to manufacture an electrostatic chuck that can quickly remove the heat input to the substrate, can accommodate the increasing power required for semiconductor processes, and can suppress deterioration of dechucking performance.
[0071] [Examples and Comparative Examples] Example 1 Example 1 is an example of an electrostatic chuck with a flat surface. The AlN raw material powder contains 5 wt% Y as a sintering aid. 2 O 3A slurry was prepared by adding a binder, a dispersant, etc., and mixing the mixture to prepare a slurry, which was then granulated by a spray-drying method. In addition, an electrode was prepared by cutting a Mo mesh to a wire diameter of 0.1 mm and a mesh size of #50 as an electrostatic adsorption electrode. Next, the granulated powder was filled into a carbon mold, the electrode was embedded, and the mixture was uniaxially hot-pressed in a nitrogen atmosphere at a firing temperature of 1800°C and a hot-press pressure of 5 MPa. The firing time was 6 hours. The obtained ceramic sintered body was machined to produce a ceramic sintered body with a diameter of 310 mm and a thickness of 25 mm.
[0072] A plurality of gas introduction holes of Φ0.5 mm were formed on the surface of the ceramic sintered compact whose outer shape was processed so that the contact rate with the substrate to be placed was 99.4%. The surface was then ground and polished with free abrasive grains to obtain a predetermined surface condition. Then, a cooling member (base member) made of an Al alloy was prepared on the surface (lower surface) opposite the surface, which was formed to the same diameter and thickness as the ceramic sintered compact and had a rectangular coolant flow path with a width of 10 mm and a height of 10 mm in cross section, and was bonded with a silicone adhesive to produce the electrostatic chuck of Example 1. The surface roughness Ra of the surface confirmed after production was 0.18 μm, and the skewness Rsk calculated from the surface roughness curve was -1.2.
[0073] Example 2 Examples 2 to 6 are examples of electrostatic chucks with pin-shaped convex portions and annular convex portions on the surface. In Example 2, the surface of the ceramic sintered body with its outer shape processed as in Example 1 was blasted to form a plurality of pin-shaped convex portions and annular convex portions so that the contact rate of the surface with the substrate to be placed after polishing was 30%. In addition, a plurality of gas introduction holes of Φ0.5 mm were formed in the concave portion. Then, the upper end surface (surface) of the pin-shaped convex portions and the annular convex portions was ground and polished with free abrasive grains to obtain a predetermined surface state, thereby producing the electrostatic chuck of Example 2. The diameter of the plurality of pin-shaped convex portions after polishing was Φ1.0 mm, the height was 10 μm, and the width of the annular convex portion was 1.0 mm and the height was 10 μm. The surface roughness Ra of the surface confirmed after production was 0.08 μm, and the skewness Rsk obtained from the surface roughness curve was -2.5.
[0074] Example 3 In Example 3, a plurality of pin-shaped convex portions and annular convex portions were formed so that the contact rate of the surface after polishing with the substrate to be placed thereon was 45%. Except for this, the electrostatic chuck of Example 3 was produced under the same conditions as those of Example 2. The surface roughness Ra of the surface confirmed after production was 0.11 μm, and the skewness Rsk calculated from the surface roughness curve was -1.8.
[0075] Example 4 In Example 4, the height of the plurality of pin-shaped convex portions and the annular convex portion was set to 5 μm. Except for that, the electrostatic chuck of Example 4 was produced under the same conditions as those of Example 2. The surface roughness Ra of the surface confirmed after production was 0.08 μm, and the skewness Rsk calculated from the surface roughness curve was −2.1.
[0076] Example 5 In Example 5, the height of the plurality of pin-shaped convex portions and the annular convex portion was set to 20 μm. Except for that, the electrostatic chuck of Example 5 was produced under the same conditions as those of Example 2. The surface roughness Ra of the surface confirmed after production was 0.08 μm, and the skewness Rsk calculated from the surface roughness curve was −1.9.
[0077] Example 6 The polishing method was changed in Example 6. Otherwise, an electrostatic chuck of Example 6 was produced under the same conditions as those of Example 2. The surface roughness Ra of the surface confirmed after production was 0.15 μm, and the skewness Rsk calculated from the surface roughness curve was −0.33.
[0078] Example 7 Examples 7 to 12 are examples of electrostatic chucks with island-shaped convex portions and annular convex portions on the surface. In Example 7, a surface of a ceramic sintered body with a processed outer shape produced in the same manner as in Example 1 was blasted to form a plurality of island-shaped convex portions and annular convex portions so that the contact rate of the surface with the substrate to be placed after polishing was 60%. At this time, the areas of the plurality of island-shaped convex portions were made to be approximately the same, and a groove portion with a width of 3.0 mm was formed. In addition, a plurality of gas introduction holes with a diameter of 0.5 mm were formed in the groove portion. Thereafter, the upper end surfaces (surfaces) of the island-shaped convex portions and annular convex portions were ground and polished with free abrasive grains to obtain a predetermined surface state, thereby producing the electrostatic chuck of Example 7. The height of the plurality of island-shaped convex portions after polishing was 500 μm, the width of the annular convex portion was 1.0 mm, and the height was 500 μm. After preparation, the surface roughness Ra was confirmed to be 0.12 μm, and the skewness Rsk calculated from the surface roughness curve was −2.1.
[0079] Example 8 In Example 8, a plurality of island-shaped convex portions and annular convex portions were formed so that the contact rate of the surface after polishing with the substrate to be placed thereon was 75%. Except for this, the electrostatic chuck of Example 8 was produced under the same conditions as those of Example 7. The surface roughness Ra of the surface confirmed after production was 0.15 μm, and the skewness Rsk calculated from the surface roughness curve was −3.0.
[0080] Example 9 In Example 9, the height of the plurality of island-shaped convex portions and the annular convex portion was set to 50 μm. Except for this, the electrostatic chuck of Example 9 was produced under the same conditions as those of Example 7. After production, the surface roughness Ra of the surface confirmed was 0.13 μm, and the skewness Rsk calculated from the surface roughness curve was −1.8.
[0081] Example 10 In Example 10, the height of the plurality of island-shaped convex portions and the annular convex portion was set to 950 μm. Except for this, the electrostatic chuck of Example 10 was produced under the same conditions as those of Example 7. After production, the surface roughness Ra of the surface confirmed was 0.11 μm, and the skewness Rsk calculated from the surface roughness curve was −1.5.
[0082] Example 11 In Example 11, the height of the plurality of island-shaped convex portions and the annular convex portion was set to 20 μm. Except for this, the electrostatic chuck of Example 9 was produced under the same conditions as those of Example 7. After production, the surface roughness Ra of the surface confirmed was 0.12 μm, and the skewness Rsk calculated from the surface roughness curve was −2.6.
[0083] Example 12 In Example 12, the height of the plurality of island-shaped convex portions and the annular convex portion was set to 1100 μm. Except for this, the electrostatic chuck of Example 12 was produced under the same conditions as those of Example 7. After production, the surface roughness Ra of the surface confirmed was 0.12 μm, and the skewness Rsk calculated from the surface roughness curve was −1.5.
[0084] Comparative Example 1 Comparative Example 1 is a comparative example of an electrostatic chuck with a flat surface. In Comparative Example 1, a plurality of gas introduction holes were formed so that the contact rate of the surface after polishing with the substrate to be placed thereon was 99.6%. In addition, the surface grinding and polishing methods were changed. The electrostatic chuck of Comparative Example 1 was produced under the same conditions as in Example 1 except for the above. The surface roughness Ra of the surface confirmed after production was 0.17 μm, and the skewness Rsk calculated from the surface roughness curve was -1.3.
[0085] Comparative Example 2 Comparative Example 2 and Comparative Example 3 are comparative examples of electrostatic chucks whose surfaces have pin-shaped convex portions and annular convex portions. In Comparative Example 2, the polishing method was changed. Otherwise, the electrostatic chuck of Comparative Example 2 was produced under the same conditions as in Example 2. After production, the surface roughness Ra of the surface confirmed was 0.24 μm, and the skewness Rsk calculated from the surface roughness curve was -1.1.
[0086] Comparative Example 3 In Comparative Example 3, a plurality of pin-shaped protrusions and annular protrusions were formed so that the contact rate of the surface after polishing with the substrate to be placed was 20%. Except for that, the electrostatic chuck of Example 3 was produced under the same conditions as Example 2. The surface roughness Ra of the surface confirmed after production was 0.10 μm, and the skewness Rsk calculated from the surface roughness curve was -1.9.
[0087] (Preparation for temperature measurement) The electrostatic chucks of the examples and comparative examples were installed in a chamber, a silicon wafer was placed on the surface as a measurement substrate, and a voltage of ±1.0 kV was applied to the electrostatic adsorption electrode to adsorb and fix the silicon wafer. He gas was also introduced from multiple gas inlet holes to fill the gap between the substrate mounting surface and the silicon wafer. At this time, the He gas pressure was adjusted to 100 Torr. A mixture of water and ethylene glycol was prepared in the coolant flow path, and the coolant temperature was set to 20°C and circulated at a flow rate of 3 L / min.
[0088] (Surface temperature measurement) Next, heat input was performed by irradiating the silicon wafer with plasma at an output of 3 kW. The silicon wafer used was a thermocouple (TC) wafer with 17 points (1 at the center, 8 at the middle radius, and 8 at the periphery), and the temperature at the measurement points was measured.
[0089] (Temperature difference measurement) In addition, to evaluate temperature uniformity, the temperature difference ΔT was calculated by subtracting the minimum temperature from the maximum temperature at the measurement points, and a temperature difference ΔT of 5.0°C or less was rated as particularly good (O), a temperature difference ΔT of more than 5.0°C but not exceeding 7.0°C was rated as good (△), and a temperature difference ΔT greater than that was rated as poor (×).
[0090] Fig. 8 is a table showing the manufacturing conditions and the results of various tests for the examples and comparative examples. Note that * in the columns for substrate surface temperature and temperature difference in the table of Fig. 8 indicates that the temperature measurement conditions were different. It was found that the electrostatic chucks of Examples 1 to 4 and 6 to 10 had their surface temperatures controlled to 100°C or less at all measurement points under the conditions for preparing the temperature measurement, and the temperature difference ΔT was also controlled to 5°C or less, and thus had excellent heat transfer efficiency and temperature distribution uniformity.
[0091] The electrostatic chuck of Example 5, which has a high pin-shaped protrusion, was unable to obtain sufficient clamping force at the voltage used for the preparation of the temperature measurement, and the substrate was detached by the gas pressure of 100 Torr, making it impossible to measure. However, by increasing the clamping voltage, it became possible to prevent the substrate from being detached by the gas pressure of 100 Torr. At this time, the surface temperature was controlled to 100°C or less at all measurement points, and the temperature difference ΔT could also be controlled to 5°C or less.
[0092] In the electrostatic chuck of Example 11 in which the height of the island-shaped convex portions was short, the amount of gas introduced into the space was small, and therefore there were measurement points where the surface temperature was higher than in the above examples, and a slight temperature difference was confirmed.
[0093] In addition, the electrostatic chuck of Example 12, which had a high island-shaped convex portion, had a similar surface temperature to the other examples, but the risk of discharge between the bottom of the groove and the substrate increased, resulting in a problem in the stability of the process. This is presumably because the grooves were too deep and the gas pressure, temperature, and other conditions increased the probability that gas molecules in the grooves would collide with other molecules.
[0094] The electrostatic chuck of Comparative Example 1, which had a high contact rate with the substrate, had excellent solid-state heat transfer and the surface temperature was controlled to 100° C. or less, but the temperature difference ΔT was higher than 7.0° C. This is presumably because the number of gas introduction holes formed was small, which resulted in inappropriate gas heat transfer in some locations, and because the substrate was warped and therefore the electrostatic chuck could not be uniformly adsorbed over the entire substrate mounting surface.
[0095] In addition, in the electrostatic chuck of Comparative Example 2, which has a high surface roughness Ra of the substrate mounting surface, sufficient clamping force could not be obtained at the voltage of the preparation conditions for temperature measurement, and the substrate was detached by the gas pressure of 100 Torr, making measurement impossible. By increasing the clamping voltage, it was possible to prevent the substrate from being detached by the gas pressure of 100 Torr. At this time, the substrate could be clamped, but the contact with the substrate was poor, and although the surface temperature was controlled to be 100°C or less, the temperature difference ΔT was higher than 7.0°C.
[0096] In addition, the electrostatic chuck of Comparative Example 3, which had a low contact rate with the substrate, was unable to exhibit sufficient solid thermal conductivity performance, and the surface temperature could not be controlled to 100° C. or less. In addition, the temperature difference ΔT was higher than 7.0° C.
[0097] In Example 6, in which the skewness Rsk was negative but larger than -1.0, the surface temperature was controlled to 100°C or less at all measurement points, and the temperature difference ΔT was also controlled to 5°C or less, and the heat transfer efficiency and temperature distribution uniformity were excellent. However, the dechucking performance was slightly worse than that of Example 2. This is presumably because Example 2 has a small skewness value and a surface state with more fine valleys than Example 6, so that gas also enters the substrate mounting surface, improving the detachment performance between the substrate mounting surface and the substrate, while Example 6 has fewer fine valleys and reduces the area into which gas enters, maintaining a high chucking force and resulting in worse detachment performance than Example 2. Therefore, it was confirmed that in order to further suppress the deterioration of the dechucking performance while maintaining the heat transfer from the substrate to the electrostatic chuck, it is preferable that the skewness Rsk is less than -1.0.
[0098] From the above results, it was confirmed that the electrostatic chuck of the present invention can improve the contact state between the substrate and the surface of the base body, can quickly remove the heat input to the substrate, and can accommodate high-power semiconductor processes. It was also confirmed that the electrostatic chuck can improve the heat transfer from the substrate to the electrostatic chuck while suppressing the deterioration of the dechucking performance.
[0099] The present invention is not limited to the above-described embodiment, and it goes without saying that various modifications and equivalents are included within the spirit and scope of the present invention. In addition, the structure, shape, number, position, size, etc. of the components shown in each drawing are for convenience of explanation and may be changed as appropriate. [Explanation of symbols]
[0100] 100 Electrostatic Chuck 110 Base 112 Top surface 114 Bottom surface 116 center 118 Gas inlet hole 120 Electrostatic Adsorption Electrode 130 Surface 132 Substrate mounting surface 140 Pin-shaped protrusion 142 Upper end surface of pin-shaped protrusion 144 Recess 150 Annular protrusion 152 Upper end surface of annular protrusion 160 Island-shaped protrusion 162 Upper end surface of island-shaped convex part 164 Groove 170 Base material 172 Gas flow path 174 Coolant flow path 180 Terminals 182 Terminal hole
Claims
1. 1. An electrostatic chuck comprising: A substrate made of a ceramic sintered body; an electrostatic attraction electrode embedded in the base; a plurality of gas introduction holes opening on the upper surface of the substrate; the base has a surface with a contact rate with a substrate placed thereon of 30% or more and 99.5% or less; The surface roughness Ra of the surface is 0.2 μm or less, The electrostatic chuck according to claim 1, wherein the skewness Rsk calculated from the surface roughness curve is negative.
2. 2. The electrostatic chuck of claim 1, wherein the skewness Rsk is less than −1.
0.
3. 2. The electrostatic chuck according to claim 1, further comprising a base member joined to a lower surface of the substrate opposite to the upper surface, the base member having a gas flow passage connected to the gas inlet hole.
4. 3. The electrostatic chuck according to claim 2, further comprising a base member joined to a lower surface of the substrate opposite to the upper surface, the base member having a gas flow passage connected to the gas inlet hole.
5. A plurality of pin-shaped protrusions formed to protrude upward from the upper surface of the base body; an annular protrusion formed to protrude upward from the upper surface of the base so as to surround the plurality of pin-shaped protrusions, 5. The electrostatic chuck according to claim 1, wherein the surface is constituted by upper end faces of the pin-shaped protrusions and an upper end face of the annular protrusion.
6. a plurality of island-shaped protrusions formed to protrude upward from the upper surface of the base; an annular protrusion formed to protrude upward from the upper surface of the base so as to surround the plurality of island-shaped protrusions, 5. The electrostatic chuck according to claim 1, wherein the surface is constituted by an upper end surface of the island-shaped convex portion and an upper end surface of the annular convex portion.
7. 6. The electrostatic chuck according to claim 5, wherein the height of the pin-shaped protrusion is not less than 5 [mu]m and not more than 10 [mu]m.
8. 7. The electrostatic chuck according to claim 6, wherein the height of the island-shaped protrusions is 25 μm or more and 1000 μm or less.
Citation Information
Patent Citations
Corrosion resistant member and its production method
JP2008156160A
Substrate mounting stage and its surface processing method
JP2008198843A
Electrostatic chuck with a shape-adaptive coating layer
JP2012511832A
Electrostatic chuck
JP2018101705A
Electrostatic chuck device
WO2017069238A1
Cited By
Retaining member
JP7943463B1
Composite sintered body and electrostatic chuck
WO2026140496A1
Electrostatic chuck device
WO2026196914A1