AI Technical Summary
The increasing demand for higher storage capacity in hard disk drives (HDDs) due to big data analysis has led to challenges in miniaturizing magnetic particles, resulting in larger magnetic disk substrates with increased diameters and decreased thickness, which causes vibrations and particle generation from external impacts, leading to potential damage and data loss.
A magnetic disk substrate with a diameter of 85 mm or more and a plate thickness of 0.6 mm or less, made from materials with a Young's modulus of 90 GPa or more, such as glass or metal alloys, is designed to minimize vibrations and particle generation by using specific glass compositions and surface treatments like chamfering, ensuring the substrate can withstand impacts without chipping or generating debris.
The solution effectively suppresses particle generation and substrate damage from external impacts, maintaining data integrity and storage capacity while preventing contact with other components within the HDD, thus enhancing the reliability and durability of magnetic disks.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Magnetic disk substrate and magnetic disk
[0001] The present invention relates to a magnetic disk substrate and a magnetic disk.
[0002] Glass substrates and aluminum alloy substrates have traditionally been used as magnetic disk substrates. Magnetic disks are formed on the main surfaces of these substrates, with magnetic films formed on them. It is desirable for magnetic disks to have few surface defects, to have no problems with reading and writing information, and to be able to read and write large amounts of information. Furthermore, in response to demands for increased storage capacity in hard disk drive devices (hereinafter referred to as HDDs), efforts are being made to increase the density of magnetic recording.
[0003] For example, when increasing the density of magnetic recording, a method for manufacturing a glass substrate for a magnetic disk is known in which the surface roughness (arithmetic mean roughness Ra) of the glass substrate for a magnetic disk is reduced so that reading and writing can be performed without hindrance using a magnetic head (DFH head) equipped with a DFH (Dynamic Flying Height) mechanism (Patent Document 1).
[0004] International Publication No. 2014 / 051153
[0005] In recent years, the hard disk drive industry has been reaching the limits of miniaturization of magnetic particles in magnetic disks, slowing the pace of conventional improvements in recording density. Meanwhile, demand for increased storage capacity for HDDs is becoming increasingly intense due to big data analysis and other factors. As a result, increasing the number of magnetic disks installed in a single HDD is being considered. To store such large amounts of data, HDDs with a nominal size of 3.5 inches are typically used. Increasing storage capacity by increasing the number of magnetic disks installed in a HDD requires reducing the thickness of the magnetic disk substrate, which accounts for the majority of the thickness of the magnetic disk within the limited space within the HDD. Furthermore, increasing the size of magnetic disks is also desired to increase storage capacity.
[0006] However, it has been found that increasing the diameter and thinning the thickness of magnetic disk substrates reduces the substrate's rigidity, making it more susceptible to large vibrations and making it difficult to contain those vibrations. For example, cloud data centers use a huge number of HDDs, and HDDs are frequently replaced due to failure. It has been found that the impact of installing a new HDD in a rack can cause failure or shorten the time until failure. Further detailed investigation revealed that when an HDD is subjected to external impact, it can be damaged even though the magnetic disk is not yet rotating because power is not yet being supplied to the HDD.
[0007] Unlike steady-state flutter vibrations that occur during steady rotation due to the rotating magnetic disk and the surrounding airflow, vibrations caused by external impacts decay over time. However, if the amplitude of these vibrations is large, they are more likely to come into contact with the ramp inside the HDD and with adjacent magnetic disks. Furthermore, the magnetic disk located at the top of multiple magnetic disks arranged at regular intervals may come into contact with the ceiling surface of the magnetic disk storage container of the HDD. Such contact can cause the magnetic disk to chip at the contacted portion, generating particles. Particles can also be generated by rubbing or abrasion. The generated particles often scatter within the storage container and adhere to the large read / write area (main surface) of the magnetic disk. As such, by increasing the diameter and thinning the thickness of magnetic disk substrates, vibrations caused by external impacts and the resulting particles, which were previously not a problem, can no longer be ignored. In particular, in the case of a large magnetic disk substrate having a nominal magnetic disk of 3.5 inches (for example, 95 mm diameter) or more, the problem of particles generated by the contact caused by vibration of the substrate cannot be ignored.
[0008] Therefore, an object of the present invention is to provide a magnetic disk substrate and a magnetic disk that can suppress the generation of particles caused by external impacts even when the diameter of the magnetic disk substrate is increased and the plate thickness is reduced.
[0009] One aspect of the present invention is a disk-shaped magnetic disk substrate, the substrate having a diameter D of 85 mm or more and a thickness T of 0.6 mm or less, and made of a material having a Young's modulus E of 90 GPa or more.
[0010] It is preferable that the diameter D is 90 mm or more. When an impact of 70 [G] is applied to the substrate for 2 [ms] in the normal direction of the main surface of the substrate with the inner peripheral edge of the substrate fixed, it is preferable that the maximum amplitude due to vibration of the outer peripheral edge of the substrate in the plate thickness direction is 0.25 mm or less.
[0011] Another aspect of the present invention is a disk-shaped magnetic disk substrate, the substrate having a diameter D of 85 mm or more and a thickness T of 0.6 mm or less, wherein when an impact of 70 G is applied to the substrate for 2 ms in a direction normal to a main surface of the substrate while the inner peripheral edge of the substrate is fixed, the maximum amplitude of vibration in the thickness direction of the outer peripheral edge of the substrate is 0.25 mm or less.
[0012] The diameter D is preferably 90 mm or more. The substrate is preferably a glass substrate made of glass having a glass transition point of 650° C. or more.
[0013] It is preferable that the change in flatness of the substrate after heating at 730° C. and the flatness of the substrate before heating is 4 μm or less.
[0014] The substrate has a linear expansion coefficient of 70×10 -7 It is preferable that the material is [1 / K] or less.
[0015] The Vickers hardness Hv of the substrate is 650 [kgf / mm 2 ] or more.
[0016] The Knoop hardness Hk of the substrate is 600 [kgf / mm 2 ] or more.
[0017] At least a chamfered surface is provided on the surface of the outer peripheral end of the substrate, and the chamfered surface has a width W along the radial direction of the substrate. 1the ratio W to the radius R of the substrate 1 It is preferable that / R is 0.0025 or less.
[0018] The width W of the chamfered surface along the thickness direction of the substrate 2 The ratio of the thickness T to the thickness T is twice (2.W 2 ) / T is preferably 0.4 or less.
[0019] With respect to the Young's modulus E and the thickness T of the substrate, E·T 3 The value is 3 to 18 [GPa mm 3 ] is preferable.
[0020] The Q value of the material at 3000 Hz at room temperature is preferably 1500 or less.
[0021] ρ is the density of the material at room temperature [g / cm 3 ], Q is the Q value of the material at room temperature at 3000 Hz, E is the Young's modulus [GPa] of the material at room temperature, and ν is the Poisson's ratio of the material at room temperature, and ρ (1-ν) of the material 2 ・Q / E value is 25 [g / cm 3 / GPa] or less.
[0022] Another aspect of the present invention is a magnetic disk having at least a magnetic film on the surface of the magnetic disk substrate.
[0023] According to the magnetic disk substrate and magnetic disk described above, even if the diameter of the magnetic disk substrate is increased and the plate thickness is reduced, the generation of particles caused by external impact can be suppressed.
[0024] 1A and 1B are diagrams illustrating an example of an external shape of a magnetic disk substrate according to an embodiment, a diagram illustrating an example of vibration of a magnetic disk substrate according to an embodiment, and a diagram illustrating an example of an outer peripheral edge of a magnetic disk according to an embodiment.
[0025] The magnetic disk substrate of the present invention will be described in detail below. In the following description, a magnetic disk glass substrate will be used. However, the magnetic disk substrate may be a non-magnetic metal substrate in addition to a glass substrate. In the case of a glass substrate, aluminosilicate glass, soda-lime glass, borosilicate glass, etc. can be used as the glass. Amorphous aluminosilicate glass is particularly suitable because it can be chemically strengthened as needed and can produce a magnetic disk glass substrate with excellent main surface flatness and substrate strength. Examples of materials that can be used for the metal substrate include aluminum alloys, titanium alloys, and single-crystal silicon. A magnetic disk is produced by forming at least a magnetic film on the surface of this magnetic disk substrate.
[0026] FIG. 1 is a diagram showing the external shape of a magnetic disk substrate according to this embodiment. As shown in FIG. 1 , the magnetic disk substrate 1 (hereinafter simply referred to as substrate 1) according to this embodiment is a thin, disk-shaped substrate having an inner hole 2 formed therein. A magnetic disk is produced by forming films such as a magnetic film, an underlayer, and a soft magnetic layer on this substrate 1. The size of the substrate 1 is not limited as long as the diameter D is 85 mm or more, preferably 90 mm or more. However, the substrate 1 is suitably applicable to a magnetic disk substrate having a nominal diameter of, for example, 3.5 inches. For a magnetic disk substrate having a nominal diameter of 3.5 inches, the diameter D (outer diameter) of the disk shape is 85 mm or more, preferably 90 mm or more. Specifically, the nominal value of the outer diameter of the disk shape is 95 mm or 97 mm. As described above, the amplitude of vibration of the magnetic disk caused by an external impact, which is different from flutter vibration, increases with the outer diameter of the substrate 1, and is therefore less susceptible to attenuation. Therefore, the substrate 1 of this embodiment is preferable when used for a magnetic disk with a nominal size of 3.5 inches or larger.
[0027] In this embodiment, the diameter D of the substrate 1 is 85 mm or more, preferably 90 mm or more, and the thickness T of the substrate 1 is 0.6 mm or less. Furthermore, the substrate 1 is made of a material with a Young's modulus E of 90 GPa or more. The substrate 1 has a larger diameter D and a thinner thickness T than conventional substrates. This allows for a larger number of magnetic disks to be incorporated into the HDD, thereby increasing storage capacity. Because the diameter D of the substrate 1 is large and the thickness T is thin, as described above, vibrations of the substrate 1 caused by impacts during installation of the HDD can cause the magnetic disks to come into contact with the ramp inside the HDD and with adjacent magnetic disks within the HDD. Furthermore, the magnetic disk located at the top of the magnetic disks may come into contact with the ceiling surface of the magnetic disk storage container of the HDD. The upper limit of the diameter D of the substrate 1 is, for example, 100 mm, in consideration of the standard size of a nominal 3.5-inch HDD. The lower limit of the thickness T of the substrate 1 is, for example, 0.30 mm from the viewpoint of suppressing arcing when a bias voltage is applied during the film formation process. There is no particular need to set an upper limit for the Young's modulus E, but from the viewpoint of ease of processing, it is, for example, 120 GPa.
[0028] FIG. 2 shows an example of vibration of the substrate 1 caused by the impact. This vibration differs from steady-state flutter vibration, which occurs during steady rotation due to the rotating magnetic disk and the surrounding airflow. Impact-induced vibration is vibration in which the main surface of the substrate 1 is displaced out of plane relative to the main surface. In particular, in a HDD, the inner peripheral edge is fixed to the spindle, while the outer peripheral edge is free and displaces out of plane relative to the main surface. This vibration displaced out of plane relative to the main surface (vibration in the thickness direction) can cause contact with the ramp inside the HDD, adjacent magnetic disks, and even the ceiling of the magnetic disk storage container. This contact can chip the magnetic disk at the contacted portion, generating particles. These particles often scatter within the storage container and adhere to the read / write area of the magnetic disk. For this reason, in this embodiment, a material with a Young's modulus of 90 GPa or greater is used for the substrate 1.
[0029] When the substrate 1 is a glass substrate, for example, the following glass composition can provide an amorphous oxide glass having a Young's modulus of 90 GPa or more.
[0030] (Glass 1) SiO2 56 to 80 mol%, Li2O 1 to 10 mol%, B2O3 0 to 4 mol%, MgO and CaO total content (MgO + CaO) 9 to 40 mol%. The specific gravity of Glass 1 is 2.75 g / cm 3 Hereinafter, the glass transition temperature Tg is 650° C. or higher.
[0031] (Glass 2) SiO2 56 to 80 mol%, Li2O 1 to 10 mol%, BO 3 0 to 4 mol%, the total content of MgO and CaO (MgO + CaO) is 9 to 40 mol%, and AlO 3 The molar ratio of the total content of SiO and ZrO to the total content of AlO ((SiO + ZrO) / AlO 3 ) is 2 to 13. The glass transition temperature Tg of glass 2 is 650°C or higher.
[0032] (Glass 3) In mol %, SiO 2 56-65%, Al 2 O 3 5-20%, B 2 O 3 0-4%, MgO 3-28%, Li 2 O 1-10%, and SiO 2 and Al 2 O 3 The total content (SiO 2 +Al 2 O 3 ) 65 to 80%, total content of MgO and CaO (MgO + CaO) 11 to 30%, total content of MgO, CaO, SrO and BaO (MgO + CaO + SrO + BaO) 12 to 30%, MgO content, 0.7 x CaO content, Li 2 O content, TiO 2 Content and ZrO 2 Sum of contents (MgO+0.7CaO+Li 2 O+TiO 2 + ZrO 2 ) 16% or more, 5xLi2 O content, 3×Na 2 O content, 3×K 2 O content, 2×B 2 O 3 Content, MgO content, 2×CaO content, 3×SrO content, and the sum of BaO content (5Li) 2 O+3Na 2 O+3K 2 O+2B 2 O 3 +MgO+2CaO+3SrO+BaO) 32~58%, SiO 2 Content, Al 2 O 3 Content, B 2 O 3 Content, P 2 O 5 Content, 1.5 × Na 2 O content, 1.5 × K 2 O content, 2 × SrO content, 3 × BaO content, およびZnO content and (SiO 2 +Al 2 O 3 +B 2 O 3 +P 2 O 5 +1.5 Na 2 O+1.5K 2 O+2SrO+3BaO+ZnO) 86% or less, and びSiO 2 Content, Al 2 O 3 Content, B 2 O 3 Content, P 2 O 5 Content, Na 2 O content, K 2 O content, CaO content, 2 × SrO content and 3 × BaO content (SiO 2 +Al 2 O 3 +B 2 O 3 +P 2 O 5 +Na 2 O+K 2 O+CaO+2SO+3BaO) 92% or less, であり, The MgO content ratio is 2.5 or less, and the CaO content ratio (CaO / MgO) is 2.5 or less, Li 2Na content relative to O content 2 Molar ratio of O content (Na 2 O / Li 2 O) is 5 or less, and the ratio of Li to the total content of MgO and CaO 2 Molar ratio of O content (Li 2 O / (MgO+CaO)) is 0.03 to 0.4, Li 2 O, Na 2 O and K 2 SiO relative to the total content of O 2 Molar ratio of content (SiO 2 / (Li 2 O + Na 2 O+K 2 O)) is 4 to 22, Al 2 O 3 SiO 2 and ZrO 2 The molar ratio of the total content of (SiO 2 + ZrO 2 ) / Al 2 O 3 ) is 2 to 10, TiO relative to the total content of MgO and CaO 2 and Al 2 O 3 The molar ratio of the total content of (TiO 2 +Al 2 O 3 ) / (MgO+CaO)) is 0.35 to 2; the molar ratio of the total content of MgO and CaO to the total content of MgO, CaO, SrO and BaO ((MgO+CaO) / (MgO+CaO+SrO+BaO)) is 0.7 to 1; the molar ratio of the content of BaO to the total content of MgO, CaO, SrO and BaO (BaO / (MgO+CaO+SrO+BaO)) is 0.1 or less; B 2 O 3 , SiO 2 , Al 2 O 3 and P 2 O 5 P relative to the total content of 2 O 5 Molar ratio of content (P 2 O 5 / (B 2 O 3 +SiO 2 +Al 2 O3 +P 2 O 5 )) is 0.005 or less, the glass transition temperature is 670°C or more and the Young's modulus is 90 GPa or more, the specific gravity is 2.75 or less, and the average linear expansion coefficient at 100 to 300°C is 40 x 10 -7 ~70 x 10 -7 / °C range.
[0033] In this case, when an impact (acceleration) of 70 G is applied to the substrate 1 in the normal direction to the main surface of the substrate 1 while the inner peripheral edge of the substrate 1 is fixed for 2 ms, the maximum amplitude of vibration of the outer peripheral edge of the substrate 1 in the thickness direction is preferably 0.25 mm or less. By setting the maximum amplitude to 0.25 mm or less, the above-mentioned contact can be prevented. The impact test was conducted using an AVEX-SM-110-MP testing machine manufactured by Air Brown Co., Ltd. Therefore, in one embodiment, the substrate 1 has a diameter D of 85 mm or more, preferably 90 mm or more, a thickness T of 0.6 mm or less, and when an impact of 70 G is applied to the substrate 1 in the normal direction to the main surface of the substrate 1 while the inner peripheral edge of the substrate 1 is fixed for 2 ms, the maximum amplitude of vibration of the outer peripheral edge of the substrate 1 in the thickness direction is 0.25 mm or less.
[0034] According to one embodiment, the substrate 1 is preferably made of glass having a glass transition temperature Tg of 650°C or higher, and more preferably, a glass transition temperature Tg of 680°C or higher. The higher the glass transition temperature Tg, the higher the thermal durability, and the more effectively the substrate deformation, e.g., flatness, that occurs when the substrate 1 is heat-treated can be suppressed. Considering the heat treatment required to form the magnetic film of the magnetic disk on the substrate 1, the glass transition temperature Tg is preferably set to 650°C or higher to suppress thermal deformation. Specifically, when a metal film containing a magnetic film or the like is formed to a thickness of approximately 30 nm on the substrate 1 to produce a magnetic disk, the substrate 1 is heated. During this heat treatment, the substrate 1 is susceptible to deformation due to thermal history. Therefore, according to one embodiment, the change in flatness of the substrate 1 after heating at 730°C and the flatness of the substrate 1 before heating (flatness after heating - flatness before heating) is preferably 4 μm or less. By limiting the change in flatness in this manner, a flat magnetic disk can be obtained, and micro-vibrations during rotation of the magnetic disk can be reduced.
[0035] According to one embodiment, the substrate 1 has a linear expansion coefficient of 70×10 -7 It is preferable that the material has a linear expansion coefficient of 60×10 -7 The lower limit of the linear expansion coefficient of the substrate 1 is, for example, 40×10 -7 [1 / K]. The linear expansion coefficient here is the linear expansion coefficient calculated from the difference in thermal expansion between 100°C and 300°C. By using such a linear expansion coefficient, it is possible to suppress thermal expansion during the heat treatment when forming a magnetic film or the like, and when the gripping member of the film forming apparatus fixes and grips the substrate 1 at the surface of the outer periphery end (hereinafter referred to as the outer periphery end face), it is possible to suppress thermal distortion of the substrate 1 around the gripped portion. For example, the linear expansion coefficient of a conventional aluminum alloy substrate is 242 x 10 -7 [1 / K], and for a conventional glass substrate, it is 95×10 -7 [1 / K] or more, whereas the linear expansion coefficient of the glass substrate 1 of one embodiment is 51×10 -7On the other hand, there is no need to set a lower limit for the linear expansion coefficient of the substrate 1, but if the linear expansion coefficient of the substrate 1 becomes too small, when the temperature inside the HDD rises, the spindle may expand and come into contact with and press against the circular hole in the substrate, causing deformation of the substrate. Therefore, for example, it is preferable to set the lower limit for the linear expansion coefficient to 20×10 -7 It is more preferable to set it to [1 / K].
[0036] According to one embodiment, the Vickers hardness Hv of the substrate 1 is 650 [kgf / mm 2 According to one embodiment, the Knoop hardness Hk of the substrate 1 is preferably 600 [kgf / mm 2 ] or more. By increasing the Vickers hardness Hv or Knoop hardness Hk, it is possible to prevent the substrate 1 from chipping and generating particles even when the substrate 1 comes into contact with another substrate 1 or with another member due to vibration caused by an external impact. Furthermore, when the outer peripheral end face is gripped by a gripping member of a film-forming device during film formation, a part of the outer peripheral end face is chipped due to gripping, generating particles, and it is possible to prevent these particles from adhering to the main surface of the substrate 1. For example, the Vickers hardness Hv of an aluminum alloy substrate is 128 [kgf / mm 2 ], and for a conventional glass substrate, it is 620 [kgf / mm 2 ], whereas the glass substrate 1 of one embodiment has a strength of 741 [kgf / mm 2 ].
[0037] FIG. 3 is an enlarged view illustrating an example of the edge of a magnetic disk. This figure shows two adjacent magnetic disks in a HDD. In FIG. 3, the thickness of the magnetic film and other components is significantly smaller than the thickness of the substrate 1, on the order of several tens of nanometers, and therefore the magnetic film and other components are not shown. The substrate 1 has a pair of main surfaces 3, sidewall surfaces 4 arranged in a direction perpendicular to the pair of main surfaces 3, and a pair of chamfered surfaces 5 arranged between the pair of main surfaces 3 and the sidewall surfaces 4. The sidewall surfaces 4 and the chamfered surfaces 5 are formed at the outer peripheral edge and inner peripheral edge of the substrate 1, respectively.
[0038] In a HDD, magnetic disks 10, each having a magnetic film or the like (not shown) formed on the surface of a substrate 1, are arranged adjacent to one another as shown in FIG. 3 . When the magnetic disks 10 vibrate in the normal direction of their main surfaces 3 and come into contact with adjacent magnetic disks 10, corners 6, which are the connection points between the main surfaces 3 at the outer periphery and the chamfered surfaces 5, tend to come into contact. This contact causes a large impact on the chamfered surfaces 5 near the corners 6. The chamfered surfaces 5 are formed by grinding with a shaped grinding wheel and then polishing the edges with a brush or the like. However, it has been found that substrates made of glass materials with a Young's modulus E of 90 GPa or greater have more latent cracks or microcracks on the surface of the chamfered surfaces 5 than conventional glass substrates with a lower Young's modulus. While the cause of this is not entirely clear, it is presumed that, for example, high-Young's modulus glass is generally hard, which increases the load during grinding, resulting in deeper cracks than conventional glass substrates, some of which remain as latent cracks or microcracks after polishing. In this state, if the corner 6 is subjected to an impact due to contact with a ramp member or the like, latent cracks or fine cracks may develop, resulting in chipping of the corner 6 or part of the chamfered surface 5 of the substrate 1 in the magnetic disk 10, which may cause particles to be generated together with the magnetic film thereon. 1 The larger the difference, the more likely it is that the corner 6 or the chamfered surface 5 will chip. Particles generated at the corner 6 or the chamfered surface 5 will scatter inside the HDD housing and often adhere to the read / write area of the magnetic disk 10.
[0039] For this reason, according to one embodiment, it is preferable to reduce the machining allowance when forming the chamfered surface 5 in the chamfering process. When the magnetic disk 10 has a diameter of 85 mm or more, preferably 90 mm or more, and a thickness of 0.600 mm or less, the corner 6 is prone to contact due to vibration. Therefore, it is preferable to reduce the machining allowance when forming the chamfered surface 5 to reduce the number of latent cracks and microcracks. This reduces the machining allowance when forming the chamfered surface 5 to reduce the number of latent cracks and microcracks. Even if the corner 6 of the magnetic disk 10 comes into contact with a ramp or other component due to strong vibration, particle generation can be suppressed. Here, the machining allowance when forming the chamfered surface 5 refers to the width W1, which will be described later. Alternatively, the outer diameter may be adjusted by removing a certain amount of the outer periphery at the beginning of grinding. However, research by the present inventors has shown that such initial machining allowance does not affect latent cracks, etc. This is presumably because latent cracks, etc., generated by the initial machining allowance are eliminated by the final machining allowance. Specifically, the chamfered surface 5 is provided at least on the outer peripheral edge of the substrate 1. At this time, the width W of the chamfered surface 5 along the radial direction of the substrate 1 1 (See FIG. 3) is preferably 120 μm or less. 1 It is more preferable that the width W is 90 μm or less. 1 By adjusting the removal amount when forming the chamfered surface 5 so that the width W is 120 μm or less, it is possible to reduce the number of latent cracks or fine cracks on the chamfered surface 5 even when the magnetic disk 10 using a high Young's modulus glass substrate has a large diameter and a thin plate thickness, making the corners 6 more likely to come into contact due to vibration. Therefore, even if the corners 6 come into contact, it is possible to prevent parts of the corners 6 or the chamfered surface 5 from chipping off and generating particles. 1 The lower limit of the width W is, for example, 20 μm. 1If the chamfered surface 5 is less than 20 μm, the chamfered surface 5 is too small, and chipping may occur during the substrate manufacturing process or film formation process after shaping. As shown in FIG. 3, the chamfered surface 5 may have a linear shape in a cross section cut along the radial direction through the center of the magnetic disk 10, or may have an arc or curved shape that is convex outward. In this case, the chamfered surface 5 refers to the portion where the inclination angle of the tangent at each position with respect to the side wall surface 4 and the main surface 3 is 5 to 85 degrees. FIG. 3 shows the inclination angle θ with respect to the main surface 3. 1 A chamfered surface 5 is shown where σ is constant.
[0040] According to one embodiment, the width W of the chamfered surface 5 at the outer periphery of the substrate 1 along the thickness direction of the substrate 1 2 (See Figure 3) twice the ratio of the thickness T (2.W 2 ) / T is preferably 0.4 or less. 2 It is more preferable that the ratio (2.W) / T is 0.3 or less. 2 If ) / T exceeds 0.4, the side wall surface 4 becomes too small, and the outer peripheral edge may be chipped or cracked due to gripping or bias voltage application when forming a magnetic film or the like.
[0041] Furthermore, according to one embodiment, the Young's modulus E [GPa] and the plate thickness T [mm] are expressed as follows: 3 The value is 3 to 18 [GPa / mm 3 ], and 3 to 16 [GPa / mm 3 ], and more preferably 5 to 15 [GPa / mm 3 It is particularly preferred that E.T. 3 If the value of E·T is in this range, contact of the magnetic disk 10 due to vibration can be suppressed. 3 The value is 3 [GPa / mm 3 If the value is less than E·T, contact of the magnetic disk 10 due to vibration is likely to occur. 3 The value is 18 [GPa / mm 3], the plate thickness cannot be increased in order to ensure the number of magnetic disks 10 that can be built into the HDD, so Young's modulus E is increased. In this case, as Young's modulus E increases, the substrate 1 tends to become harder than necessary, which lengthens the polishing time for the main surface 3, and is undesirable in terms of the production efficiency of the magnetic disk substrate 1. Furthermore, according to one embodiment, the Young's modulus E [GPa] and density ρ [g / cm 3 ], the specific elastic modulus calculated by E / ρ is 36 [GPa cm 3 / g] or more. Even if the Young's modulus is high, if the density is high, the weight of the substrate itself may cause large vibrations. There is no particular need to set an upper limit for the specific modulus, but from the viewpoint of productivity, it is preferable that the upper limit be, for example, 41 [GPa cm]. 3 / g] may also be used.
[0042] When such substrates 1 are mounted in an HDD, the number of substrates 1 mounted in the HDD depends on the thickness T of the substrates 1. The film thickness of the magnetic film formed on the substrate 1 is several tens of nanometers, which is thin enough to be ignored compared to the thickness T of the substrate 1. For example, if the thickness T of the substrate 1 is 0.635 mm, nine or more substrates 1 can be mounted; if the thickness T of the substrate 1 is 0.5 mm, ten or more substrates 1 can be mounted; and if the thickness T of the substrate 1 is 0.38 mm, twelve or more substrates 1 can be mounted. Thus, the number of substrates 1 mounted varies depending on the thickness T of the substrate 1. Therefore, by reducing the thickness T of the substrate 1 and increasing the number of substrates mounted, the storage capacity can be increased. In this case, as described above, the substrate 1 of this embodiment is less likely to come into contact with other substrates 1 or components due to vibration, even when the thickness T is thin. Furthermore, according to one embodiment, it is preferable that the substrate 1 does not break in an impact test in which the inner peripheral edge of the substrate 1 is fixed to reproduce the clamping of a magnetic disk and an impact of 600 G is applied to the substrate 1 for 2 ms. Such a substrate 1 is preferable from the viewpoint of improved durability, since the substrate 1 does not break even when a large impact is applied to the HDD. This substrate 1 can be achieved, for example, using the above-mentioned glasses 1 to 3.
[0043] According to one embodiment, the Q value (Quality Factor) of the material of the substrate 1 at 3000 Hz at room temperature (25°C) is preferably 1500 or less. The Q value is calculated by dividing the vibration energy stored in the vibrating substrate 1 during one cycle by the energy dissipated from the vibrating substrate 1; the smaller this value, the greater the vibration damping. Therefore, the smaller the Q value of a material used, the faster the vibration damping can be. This reduces the number of contacts with adjacent substrates 1 or lamps in the HDD and also mitigates the impact at the time of contact, making it possible to suppress adverse effects such as particle generation due to contact. The Q value at room temperature and 3000 Hz is more preferably 1300 or less. The Q value at 3000 Hz was obtained as follows. First, a laser Doppler vibrometer (LDV) was used to generate vibrations on the substrate 1 rotated by a spin stand, and a laser was applied to the approximate outer peripheral edge of the substrate 1 to measure the vibrations. The obtained data was then appropriately Fourier transformed to obtain a frequency response function (horizontal axis: frequency (unit: Hz), vertical axis: NRRO (Non Repeatable Runout) Amplitude (unit: nm)). Next, for each peak observed in the frequency response function, the Q value (= f0 / (f2-f1)) was calculated using the half-width method (a calculation method using frequencies f1 and f2 (> f1) corresponding to values 3 dB lower than the NRRO peak value and the frequency f0 (resonance frequency) corresponding to the peak value). The obtained measurement results were plotted on an XY plane with frequency on the horizontal axis and Q value on the vertical axis, and a linear approximation was performed by the least squares method to obtain an approximate straight line. The Q value at 3000 Hz was obtained on the obtained approximate straight line, or by extrapolating the approximate straight line as necessary. The substrates 1 used for evaluation using the laser Doppler vibrometer were all 95 mm in outer diameter, 25 mm in inner diameter, and 0.635 mm in thickness. The substrate rotation speed was 6900 rpm, and the measurement position was 46.5 mm radially from the center of the substrate (1 mm inward from the outer periphery), and the measurement was performed at room temperature.
[0044] According to one embodiment, ρ is the density at room temperature of the material of the substrate 1 [g / cm 3], Q is the Q value of the material of substrate 1 at room temperature at 3000 Hz, E is the Young's modulus [GPa] of the material of substrate 1 at room temperature, and ν is the Poisson's ratio of the material at room temperature, and ρ (1-ν) of the material of substrate 1 2 ・Q / E value is 25 [g / cm 3 The amplitude at the outer peripheral edge of the substrate 1 is preferably less than ρ (1-ν) 2 The amplitude is proportional to / E / ξ (ξ is the damping ratio of the material of the substrate 1), and the damping ratio ξ is expressed as 1 / (2·Q) (Q is the Q value), so the amplitude is 2·ρ·(1−ν) 2 ・Proportional to Q / E, where 2 ・ρ(1-ν) 2 ・Q / E is 25 [g / cm 3 / Gpa], it was found that the amplitude of vibration in a specific frequency band can be efficiently reduced, that is, the RSS (root of sum of squares) of flutter vibration in the range of 1000 to 4000 Hz can be made less than 80 nm. Specifically, the RSS in the range of 1000 to 4000 Hz is the square root of the integrated value of the square of the amplitude of flutter vibration in the range of 1000 to 4000 Hz. That is, 2·ρ(1−ν) 2 ・Q / E is 25 [g / cm 3 / GPa], the RSS in the range from 1000 Hz to 4000 Hz can be reduced. 2 ・Q / E is 20 [g / cm 3 / Gpa] or less, the RSS in the 1000 Hz to 4000 Hz range can be set to 68 nm or less, which is even more preferable. Note that the impact of flutter vibration in the frequency band below 1000 Hz has been reduced due to recent advances in head servo technology, while flutter vibration in the band above 4000 Hz is already small. Therefore, it is important to reduce flutter vibration in the 1000 to 4000 Hz band. The substrate 1 of this embodiment has these characteristics.
[0045] Such a substrate 1 is fabricated, for example, as follows. Here, as an example, a case where a glass substrate is used as the substrate 1 will be described. First, a glass blank, which will be the material for a plate-shaped magnetic disk substrate having a pair of main surfaces, is formed. Next, the glass blank is roughly ground. The glass blank is then shaped and its edge polished. The main surfaces of the substrate obtained from the glass blank are then finely ground using fixed abrasive grains. The substrate is then subjected to first polishing of the main surfaces, chemical strengthening, and second polishing of the main surfaces. Note that, in this embodiment, the substrate is fabricated in the above-described order; however, the above processes do not always need to be performed, and the order of these processes may be reversed or omitted as appropriate. For example, among the above processes, the fine grinding, first polishing, and chemical strengthening may not be performed. Each process will be described below.
[0046] (a) Forming of Glass Blank For forming a glass blank, for example, a press molding method can be used. A circular glass blank can be obtained by the press molding method. Furthermore, it can be manufactured using known manufacturing methods such as a down-draw method, a re-draw method, and a fusion method. A disk-shaped substrate that serves as the base of a magnetic disk substrate can be obtained by appropriately shaping a plate-shaped glass blank manufactured by these known manufacturing methods.
[0047] (b) Rough grinding In rough grinding, grinding is performed on both main surfaces of the glass blank. For example, loose abrasive grains are used as the abrasive. In rough grinding, the glass blank is ground so as to approximate the target thickness dimension and flatness of the main surfaces. Note that rough grinding is performed depending on the dimensional accuracy or surface roughness of the formed glass blank, and may not be performed in some cases.
[0048] (c) Shape Processing Next, shape processing is performed. In shape processing, first, after molding the glass blank, a circular hole and an outer periphery are formed using a known processing method to obtain a disk-shaped substrate with a circular hole (circular hole forming process). Then, the edge surface of the substrate is chamfered (chamfering process). As a result, on the edge surface of the substrate, side wall surfaces 4 perpendicular to the main surface 3 and chamfered surfaces 5 inclined with respect to the main surface 3 are formed between the side wall surfaces 4 and both main surfaces 3. In the chamfering process, the side wall surfaces 4 and two chamfered surfaces 5 may be formed simultaneously by grinding the edge surface of the substrate using a forming grindstone.
[0049] (d) Edge Polishing Next, the edge of the substrate is polished. Edge polishing is a process in which a polishing liquid containing free abrasive grains is supplied between the polishing brush and the outer peripheral edge (side wall surface 4 and chamfered surface 5) and inner peripheral edge (side wall surface 4 and chamfered surface 5) of the substrate, and the polishing brush and the substrate are moved relative to each other. In edge polishing, the inner peripheral edge and the outer peripheral edge of the substrate are polished to a mirror finish.
[0050] (e) Precision grinding Next, the main surface of the substrate is subjected to precision grinding. For example, a double-side grinding device with a planetary gear mechanism is used to grind the main surface 3 of the substrate. In this case, for example, a fixed abrasive is provided on a surface plate for grinding. Alternatively, grinding can be performed using loose abrasive. Note that precision grinding may not be performed in some cases.
[0051] (f) First Polishing Next, the main surface 3 of the substrate is subjected to the first polishing. The first polishing uses a polishing pad attached to a surface plate with loose abrasive grains. The first polishing removes cracks and distortions remaining on the main surface 3 after precision grinding with a fixed abrasive grains, for example. The first polishing can reduce the surface roughness of the main surface 3, such as the arithmetic mean roughness Ra, while preventing the edge shape of the main surface 3 from excessively recessing or protruding. The loose abrasive grains used in the first polishing are not particularly limited, but examples include cerium oxide abrasive grains or zirconia abrasive grains. Note that the first polishing may not be performed in some cases.
[0052] (g) Chemical Strengthening Depending on the embodiment, the substrate 1 may be chemically strengthened as appropriate. For chemical strengthening, a molten solution obtained by heating, for example, potassium nitrate, sodium nitrate, or a mixture thereof, can be used as the chemical strengthening liquid. By immersing the substrate in the chemical strengthening liquid, lithium ions and sodium ions in the glass composition on the surface of the substrate are replaced by sodium ions and potassium ions, respectively, which have relatively large ionic radii in the chemical strengthening liquid, forming a compressive stress layer in the surface layer and strengthening the substrate. The timing of chemical strengthening can be determined as appropriate, but polishing after chemical strengthening is particularly preferred because it smooths the surface and removes foreign matter adhered to the surface of the substrate by chemical strengthening.
[0053] (h) Second Polishing (Mirror Polishing) Next, the chemically strengthened substrate is subjected to second polishing. The second polishing aims to mirror-polish the main surface 3. The second polishing is also performed using a polishing device with the same configuration as the first polishing. In the second polishing, the type and particle size of the free abrasive grains are changed from those in the first polishing, and a softer resin polisher is used as the polishing pad to perform mirror polishing. This reduces the roughness of the main surface 3 while preventing excessive depression or protrusion of the edge shape of the main surface 3. The roughness of the main surface 3 is preferably 0.2 nm or less in terms of arithmetic mean roughness Ra (JIS B 0601 2001). The substrate is then washed to obtain the substrate 1.
[0054] (Examples, Comparative Examples, Conventional Examples) Various substrates were prepared to examine the effect of substrate 1 (Conventional Examples 1 and 2, Comparative Examples 1 and 2, Examples 1 to 12, Examples 61 to 67, Examples 81 to 84, Examples 111 to 114, and Examples 121 to 124). Glass substrates or aluminum alloy substrates were used. Glass 4 having the following composition was used for the substrates of Conventional Example 1 and Comparative Example 1. Glass 1 described above was used for the substrate 1 of Examples 1 and 2. Glass 2 described above was used for the substrate 1 of Examples 3 to 5. Glass 3 described above was used for the substrate 1 of Examples 6 to 10. Glasses 5 and 6, which are amorphous aluminosilicate glasses with a Young's modulus E of 100 GPa or more and have a different composition from Glasses 1 to 4, were used for the substrate 1 of Examples 11 and 12. Glass 3 described above was used for the substrate 1 of Examples 61 to 67 and Examples 81 to 84. Glass 5 was used for the substrate 1 in Examples 111 to 114, and Glass 6 was used for the substrate 1 in Examples 121 to 124. Chemical strengthening was not performed on any of the substrates. Glasses 1 to 3, 5, and 6 had specific elastic moduli of 36 GPa cm 3 / g] or more. Glass 4 is less than 36.
[0055] (Glass 4) SiO 2 , Al 2 O 3 And Li 2 O, Na 2 O, and K 2 one or more alkali metal oxides selected from the group consisting of MgO, CaO, SrO, and BaO; one or more alkaline earth metal oxides selected from the group consisting of ZrO 2 , HfO 2 , Nb 2 O 5 , Ta 2 O 5 , La 2 O 3 , Y 2 O 3、 and TiO 2 and one or more oxides selected from the group consisting of SiO 2 50 mol% or more of Al 2 O 3 3 mol % or more, and SiO 2 and Al2 O 3 The total content of 70 to 85 mol%, Li 2 O and Na 2 Contains O and Li 2 O 4.3 mol% or more, Na 2 O 5 mol% or more and Li 2 O and Na 2 a total content of the alkali metal oxide and the alkaline earth metal oxide of 24 mol % or less, a total content of the alkali metal oxide and the alkaline earth metal oxide of 8 mol % or more, and a molar ratio of the total content of the oxides to the total content of the alkali metal oxide and the alkaline earth metal oxide (ZrO 2 +HfO 2 +Nb 2 O 5 +Ta 2 O 5 +La 2 O 3 +Y 2 O 3 + TiO 2 ) / (Li 2 O + Na 2 O+K 2 an amorphous glass containing MgO and CaO, wherein MgO is less than 3 mol % and CaO is 4 mol % or less, and the molar ratio of the MgO content to the CaO content (MgO / CaO) is 0.130 to 0.700.
[0056] The size of the fabricated substrate is an outer diameter (diameter) of 85 mm to 97 mm and an inner diameter (circular hole diameter) of 25 mm. 1 is 60 μm to 150 μm, and the width W along the plate thickness direction 2 Specifically, in Conventional Examples 1 and 2, where the plate thickness exceeds 0.6 mm, the width W along the radial direction of the chamfered surface is 1 is 150 μm, and the width W along the plate thickness direction 2 In Comparative Examples 1 and 2 and Examples 1 to 12, the plate thickness of which is 0.6 mm or less, the width W 1 is 100 μm, and the width W 2 The width W of Examples 61 to 67 and 81 to 84 was set to 100 μm. 1and width W 2 is shown in Tables 3A to 3D below. Therefore, the width W 1 and width W 2 If these are equal, the tilt angle θ 1 The angle (see Figure 3) was 45 degrees. In the shaping process, when forming the outer periphery of the substrate, a diamond scriber was used to make a vertical cut, which was then extended to the opposite surface and cut. In the subsequent chamfering process, a chamfered surface was formed using a grinding wheel.
[0057] (Experiment 1) The fabricated substrates of Conventional Examples 1 and 2, Comparative Examples 1 and 2, and Examples 1 to 12 were attached to an evaluation device equipped with a high-speed camera to measure the maximum amplitude. This evaluation device is capable of applying an external impact (acceleration) of any magnitude and capturing the resulting movement (vibration) of the outer edge of the substrate as a video. The video can then be analyzed to measure the displacement of the outer edge in the normal direction to the main surface. Using this evaluation device, an impact test was conducted in which a 70 G impact was applied to the substrate for 2 ms in the normal direction to the main surface of the substrate, and the vibration of the outer edge in the normal direction to the main surface was measured. The measurement results are represented as waveform data such as those shown in FIG. 2. From this waveform data, the maximum displacement of the outer edge of the substrate in either direction normal to the center of the displacement amount of 0 was calculated as the maximum amplitude.
[0058] Actual HDDs incorporate ramps for the magnetic head ramp load mechanism, which, when each magnetic disk is installed, leave a gap of 0.25 mm from both main surfaces. In other words, the gap between the ramps for the magnetic disk to fit is the thickness of the magnetic disk plus 0.5 mm. Actual HDDs are designed to maintain this gap constant even when the thickness of the substrate changes. On the other hand, the evaluation device does not include such ramps. Therefore, determining whether the vibration of the substrate will cause contact with other components such as ramps (adjacent substrates, ramps, or HDD containers) in actual HDDs is determined by the maximum amplitude of the substrate vibration. If the maximum amplitude is 0.25 mm or less, it can be determined that contact with the ramp will not occur. If the maximum amplitude exceeds 0.25 mm, there is a very high possibility of contact with other components. The maximum amplitude was measured for three substrates, and the average of the maximum amplitudes was used. In this evaluation, the substrates were not rotating but were stationary. The thickness of the magnetic film formed in the media process is approximately 100 nm or less on the main surface, and can therefore be substantially ignored.
[0059] The evaluation results of maximum amplitude are shown in Tables 1, 2A, and 2B below. The aluminum alloys ("Al alloys") of Conventional Example 2 and Comparative Example 2 are Al-Mg alloys having the following composition: Mg: 3.5-5%, Si: 0-0.05%, Fe: 0-0.1%, Cu: 0-0.12%, Mn: 0-0.3%, Cr: 0-0.1%, Zn: 0-0.5%, Ti: 0-0.1%, and the balance being Al. Furthermore, a film of Ni-P alloy (P: 10% by mass, balance Ni) was formed on the surface of an Al-Mg alloy substrate by electroless plating so as to cover the entire surface of the substrate. The plate thickness of the substrate on which the plated film is formed refers to the plate thickness including the film.
[0060]
[0061] According to Table 1, in Conventional Examples 1 and 2, in which the plate thickness T exceeds 0.6 mm, even if the Young's modulus is less than 90 GPa, the plate thickness T is large, so the maximum amplitude is small and the substrate does not come into contact with other members. However, as shown in Comparative Examples 1 and 2, when the plate thickness T is 0.6 mm or less, the maximum amplitude exceeds 0.25 mm, making it highly likely that the substrate will come into contact with other members. In contrast, in Examples 1 and 2, even if the plate thickness T is 0.6 mm or less, the Young's modulus is 90 GPa or more, so the maximum amplitude is 0.25 mm or less.
[0062]
[0063]
[0064] In Examples 3 to 12, similarly to Examples 1 and 2, even if the plate thickness T is 0.6 mm or less, the Young's modulus is 90 GPa or more, so the maximum amplitude is 0.25 mm or less.
[0065] From the above, according to Tables 1, 2A, and 2B, even if the diameter D of substrate 1 is 85 mm or more and the thickness T of substrate 1 is 0.6 mm or less, if the Young's modulus E of the material of substrate 1 is 90 GPa or more, the maximum amplitude will be 0.25 mm or less, so that vibrations caused by external impacts will not cause substrate 1 to come into contact with other components. This makes it possible to suppress the generation of particles inside the HDD.
[0066] (Experiment 2) Furthermore, using the substrates 1 of Examples 6, 8, 11, and 12 as a reference, the width W of the chamfered surface 5 1 , W 2 The quality of the substrate 1 was evaluated after the impact test using the substrate 1 (Examples 61 to 67, Examples 81 to 84, Examples 111 to 114, Examples 121 to 124) in which the width W 1 , W 2 The width W of the substrate 1 in Example 6 was changed by changing the grindstone shape and processing conditions when performing chamfering using a shaped grindstone. 1 , W 2 In Examples 81 to 84, the width W of the substrate 1 in Example 8 is changed. 1 , W 2In Examples 111 to 114, the width W of the substrate 1 in Example 11 is changed. 1 , W 2 In Examples 121 to 124, the width W of the substrate 1 in Example 12 is changed. 1 , W 2 Therefore, the material, Young's modulus E, plate thickness, and outer diameter of Examples 61 to 67 are the same as those of Example 6, the material, Young's modulus E, plate thickness, and outer diameter of Examples 81 to 84 are the same as those of Example 8, the material, Young's modulus E, plate thickness, and outer diameter of Examples 111 to 114 are the same as those of Example 11, and the material, Young's modulus E, plate thickness, and outer diameter of Examples 121 to 124 are the same as those of Example 12.
[0067] The quality of the fabricated substrates 1 was evaluated by disassembling a commercially available HDD. The substrates 1 and spacers of each example were attached to a spindle, and a simulated ramp member made of engineering plastic was attached so that it protruded from the substrate surface. A 0.25 mm gap was maintained between the ramp member and the substrate. Then, while the substrate 1 was still attached, an impact test was conducted in which a 200 G impact was applied for 2 ms in the normal direction to the main surface of the substrate 1. This test was an accelerated test in which the outer edge of the substrate 1 was deliberately collided with the ramp member several times or more. The particle distribution around the area where the ramp member contacted the surface of the substrate 1 was then observed. Due to the difficulty of quantifying the results, a relative evaluation was used. Rank 1: Almost no particles; Rank 2: Medium number of particles; Rank 3: Large number of particles. The evaluation results are shown in Tables 3A to 3D below. A lower rank indicates better quality, with Rank 1 representing the highest rating.
[0068]
[0069]
[0070]
[0071]
[0072] According to Tables 3A to 3D, the width W 1 It can be seen that the number of particles can be reduced by setting the width W1 Therefore, when the diameter D of the substrate 1 is 85 mm or more, the thickness T of the substrate 1 is 0.6 mm or less, and the substrate 1 is made of a material having a Young's modulus E of 90 GPa or more, the width W 1 By making the thickness 120 μm or less, the number of particles adhering to the main surface of the substrate 1 in the HDD can be further reduced.
[0073] The magnetic disk substrate and magnetic disk of the present invention have been described in detail above, but the present invention is not limited to the above-mentioned embodiments and examples, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.
[0074] REFERENCE SIGNS LIST 1 magnetic disk substrate 2 inner hole 3 main surface 4 side wall surface 5 chamfered surface 6 corner 10 magnetic disk
Claims
1. A disk-shaped magnetic disk substrate, wherein the diameter D of the substrate is 85 mm or more, the thickness T of the substrate is 0.6 mm or less, and the substrate is made of a material with a Young's modulus E of 90 GPa or more.
2. The magnetic disk substrate according to claim 1, wherein the diameter D is 90 mm or more.
3. A magnetic disk substrate according to claim 1 or 2, wherein when an impact of 70 G is applied to the substrate for 2 ms in the normal direction to the main surface of the substrate while the inner peripheral edge of the substrate is fixed, the maximum amplitude of vibration in the thickness direction of the outer peripheral edge of the substrate is 0.25 mm or less.
4. A disk-shaped magnetic disk substrate, wherein the diameter D of the substrate is 85 mm or more, and the thickness T of the substrate is 0.6 mm or less, and when an impact of 70 G is applied to the substrate for 2 ms in the normal direction of the main surface of the substrate while the inner peripheral edge of the substrate is fixed, the maximum amplitude of vibration in the thickness direction of the outer peripheral edge of the substrate is 0.25 mm or less.
5. The magnetic disk substrate according to claim 4, wherein the diameter D is 90 mm or more.
6. A magnetic disk substrate according to any one of claims 1 to 5, wherein the substrate is a glass substrate made of glass having a glass transition point of 650°C or higher.
7. A magnetic disk substrate according to any one of claims 1 to 6, wherein the change in flatness of the substrate after heating at 730°C and the flatness of the substrate before heating is 4 μm or less.
8. The substrate has a linear expansion coefficient of 70 x 10 -7 8. The magnetic disk substrate according to claim 1, which is made of a material having a viscosity of not more than [1 / K].
9. The Vickers hardness Hv of the substrate is 650 [kgf / mm 2 9. The magnetic disk substrate according to claim 1, wherein the thickness of the magnetic disk substrate is 100 nm or more.
10. The Knoop hardness Hk of the substrate is 600 [kgf / mm 2 10. The magnetic disk substrate according to claim 1, wherein the thickness of the magnetic disk substrate is 100 nm or more.
11. A chamfered surface is provided on at least the surface of the outer peripheral end of the substrate, and the width W of the chamfered surface along the radial direction of the substrate 1 The magnetic disk substrate according to any one of claims 1 to 10, wherein the thickness is 120 µm or less.
12. Width W of the chamfered surface along the thickness direction of the substrate 2 The ratio of the thickness T to the thickness T is twice (2.W 2 12. The magnetic disk substrate according to claim 1, wherein ) / T is 0.4 or less.
13. Regarding the Young's modulus E of the substrate and the plate thickness T, E·T 3 The value is 3 to 18 [GPa mm 3 13. The magnetic disk substrate according to claim 1, wherein:
14. A magnetic disk substrate according to any one of claims 1 to 13, wherein the material has a Q value of 1500 or less at 3000 Hz at room temperature.
15. ρ is the density of the material at room temperature [g / cm 3 ], Q is the Q value of the material at room temperature at 3000 Hz, E is the Young's modulus [GPa] of the material at room temperature, and ν is the Poisson's ratio of the material at room temperature, and ρ (1-ν) of the material 2 ・Q / E value is 25 [g / cm 3 15. The magnetic disk substrate according to claim 1, wherein the surface tension is less than [0.1 GPa / GPa].
16. A magnetic disk having at least a magnetic film on the surface of the magnetic disk substrate according to any one of claims 1 to 15.