A method for producing a glass disk, a method for producing a glass substrate for a magnetic disk, a method for producing a magnetic disk, and an apparatus for a glass disk manufacturing process

LAP910AUndetermined Publication Date: 2026-01-09HOYA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP910
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-01-28
Filing Date
2022-01-28
Publication Date
2026-01-09

AI Technical Summary

Technical Problem

The existing methods for manufacturing glass substrates for magnetic disks face challenges in efficiently chamfering the inner peripheral end surfaces of annular glass plates, leading to complications in device configuration and reduced productivity due to the need for complex moving mechanisms and reflective mirrors.

Method used

A method involving the irradiation of the inner peripheral end surface of an annular glass plate with a laser beam, where the laser light is focused and converted into diffused light inclined relative to the main surface, allowing for chamfering of the corners between the main surfaces and the inner peripheral end surface without the need for reflective mirrors, using a simpler device configuration.

Benefits of technology

This approach enables efficient chamfering of the glass substrates with improved surface roughness and axisymmetric cross-sectional shapes, enhancing the stability and usability of the glass substrates for magnetic disks, while simplifying the device configuration and increasing productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
  • Figure 00000000_0001_ABST
    Figure 00000000_0001_ABST
  • Figure 00000000_0002_ABST
    Figure 00000000_0002_ABST
Patent Text Reader

Abstract

A method for manufacturing a glass plate includes a process for illuminating a circular surface extending along a circular hole in a circular glass plate with a laser beam focused by a condenser lens and formed as diffuse light, and the surface of the circular surface is illuminated with diffuse light from an oblique direction relative to the main surface of the glass plate.
Need to check novelty before this filing date? Find Prior Art

Description

Glass plate manufacturing method, magnetic disk glass substrate manufacturing method, magnetic disk manufacturing method, and glass plate processing apparatus

[0001] The present invention relates to a method for manufacturing a glass plate, which includes irradiating the inner peripheral edge surface of a circular glass plate with laser light, a method for manufacturing a glass substrate for a magnetic disk using this glass plate manufacturing method, a method for manufacturing a magnetic disk, and a glass plate processing device.

[0002] Hard disk drive (HDD) devices for data recording use magnetic disks in which a magnetic layer is provided on a circular non-magnetic magnetic disk glass substrate. When manufacturing a magnetic disk glass substrate, it is preferable to smooth the edge surface of the circular glass plate that forms the final magnetic disk glass substrate, where particles are likely to be generated, to prevent fine particles from adhering to the main surface and adversely affecting the performance of the magnetic disk. Furthermore, in order to accurately incorporate the magnetic disk into the HDD device, and further, to make the edge surface of the glass plate suitable for gripping by a jig that grips the outer peripheral edge surface of the glass substrate when forming a magnetic film on the main surface of the glass substrate, it is preferable to align the edge surface of the glass plate to a target shape.

[0003] As a method for forming the edge of an annular glass plate into a target shape, a method of chamfering the edge of the glass plate using a laser beam is known. For example, a technology is known that can easily and inexpensively smooth the inner and outer edge surfaces of a glass substrate for an information recording medium using a laser beam (Patent Document 1). Specifically, when chamfering the inner edge surface, a reflecting mirror is placed in the inner hole of the annular glass plate, and laser light is irradiated onto the reflecting mirror from above the main surface of the glass plate, and the laser light reflected by the reflecting mirror is irradiated onto the inner edge surface.

[0004] Japanese Patent Application Laid-Open No. 2002-150546

[0005] However, when using the above technology to irradiate the inner peripheral edge surfaces of multiple glass plates with laser light, it is necessary to retract the reflecting mirror from the inner hole and move it into the inner hole of the next glass plate to be processed, for example, every time a glass plate is replaced, to prevent the glass plate from colliding with the reflecting mirror. In this case, a movement mechanism is required to move the reflecting mirror, and it takes time to move the reflecting mirror. On the other hand, even if the glass plate is moved without moving the reflecting mirror, the movement path becomes complicated. As a result, the configuration of a laser light irradiation device using a reflecting mirror becomes complex and productivity deteriorates.

[0006] Therefore, an object of the present invention is to provide a method for manufacturing a glass plate, a method for manufacturing a glass substrate for a magnetic disk, and a method for manufacturing a magnetic disk, which are capable of irradiating the inner peripheral edge surface of a circular glass plate with laser light using a simple device configuration when manufacturing the glass plate.

[0007] One aspect of the present invention is a method for manufacturing a glass plate, comprising: irradiating a laser beam along an inner peripheral edge surface of an annular glass plate that is aligned with an inner hole of the glass plate; In the process, when irradiating the inner peripheral edge surface with the laser beam, the laser beam is focused by a focusing lens and then converted into diffused light, and the diffused light is irradiated onto the inner peripheral edge surface from a direction inclined with respect to the main surfaces of the glass plate; It is preferable that the process chamfers corners between the inner peripheral edge surface and each of the main surfaces on both sides of the glass plate.

[0008] The tilt angle of the central axis of the laser beam with respect to the main surface is preferably 20 degrees or less.

[0009] The diffusion angle of the laser light is preferably 20 degrees or less.

[0010] It is preferable that the treatment chamfers corners between the inner peripheral edge face and each of the main surfaces on both sides of the glass plate, and that the cross-sectional shape of the inner peripheral edge face with the chamfered corners is symmetrical with respect to a center line that passes through the center of the glass plate in the thickness direction and is parallel to the main surface.

[0011] It is preferable that the position at which the laser light is focused by the focusing lens is above a plane including the main surface that is radially outward of the position of the inner end face that faces the irradiation position of the laser light on the inner end face across the center of the inner hole.

[0012] The glass plate is preferably a glass substrate that will be used as a base for a magnetic disk glass substrate.

[0013] After the irradiation of the laser light, it is preferable to grind or polish the main surfaces of the glass plate without polishing the inner peripheral end face.

[0014] Another aspect of the present invention is a method for manufacturing a glass substrate for a magnetic disk, which includes manufacturing a glass plate by the above-described method for manufacturing a glass plate, and then grinding or polishing a main surface of the glass plate to manufacture the glass substrate for a magnetic disk.

[0015] Yet another aspect of the present invention is a method for producing a magnetic disk, comprising forming a magnetic film on a main surface of a glass plate produced by the method for producing a magnetic disk glass substrate.

[0016]

[0013] Yet another aspect of the present invention is a glass plate processing apparatus that performs a process of irradiating a laser beam along an inner peripheral edge surface of an annular glass plate that is aligned with an inner hole. In the process, when the laser beam is irradiated onto the inner peripheral edge surface, the laser beam is focused by a focusing lens and then converted into diffused light, and the diffused light is irradiated onto the inner peripheral edge surface from a direction inclined with respect to the main surfaces of the glass plate. It is preferable that the process chamfers corners between the inner peripheral edge surface and each of the main surfaces on both sides of the glass plate.

[0017] According to the above-described glass plate manufacturing method, magnetic disk glass substrate manufacturing method, magnetic disk manufacturing method, and glass plate processing apparatus, in an apparatus for manufacturing a glass plate by irradiating the inner peripheral edge surface of a circular ring-shaped glass plate with laser light, laser light irradiation can be performed with a simple apparatus configuration.

[0018] 1A is a perspective view of an example of a glass plate manufactured by a glass plate manufacturing method according to an embodiment, FIG. 1B is a diagram showing an example of the cross-sectional shape of the end face of the glass plate after the formation of a chamfered surface, and FIG. 1C is a diagram showing an example of the cross-sectional shape of the end face of the glass plate before the formation of a chamfered surface. FIG. 1C is a diagram explaining the irradiation of laser light performed in a glass plate manufacturing method according to an embodiment. FIG. 1D is a diagram explaining the irradiation of laser light performed in a glass plate manufacturing method using diffused light.

[0019] Hereinafter, a method for manufacturing a glass plate, a processing apparatus for a glass plate, a method for manufacturing a magnetic disk glass substrate, and a method for manufacturing a magnetic disk according to an embodiment will be described in detail.

[0020] The glass plate manufactured by the glass plate manufacturing method of one embodiment is a circular glass plate having chamfered edges, and is used, for example, as a glass substrate for a magnetic disk. Fig. 1(a) is a perspective view of an example of a circular glass plate manufactured by the glass plate manufacturing method of one embodiment. The circular glass plate is a glass plate having a circular outer periphery. The circular glass plate has an inner periphery with an inner hole concentric with the circular circle. The circular glass plate also has a pair of main surfaces.

[0021] The glass plate 1 shown in FIG. 1( a) can be used as a magnetic disk glass substrate. When the glass plate 1 is used as a magnetic disk glass substrate, the size of the magnetic disk glass substrate is not limited, but may be, for example, a magnetic disk glass substrate having a nominal diameter of 2.5 inches or 3.5 inches. In the case of a magnetic disk glass substrate having a nominal diameter of 2.5 inches, the outer diameter (diameter) is 55 to 70 mm, for example, 65 mm or 67 mm, the inner hole diameter (diameter) is 20 mm, and the plate thickness is 0.3 to 1.3 mm. In the case of a magnetic disk glass substrate having a nominal diameter of 3.5 inches, the outer diameter is 85 to 100 mm, for example, 95 mm, 96 mm, or 97 mm, the inner hole diameter is 25 mm, and the plate thickness is 0.3 to 1.3 mm.

[0022] In the glass plate 1 shown in FIG. 1( a), corners between the end faces (inner peripheral end faces and / or outer peripheral end faces) and the main surfaces are chamfered to form chamfered surfaces (or chamfered portions). In the present invention, even if the chamfered portion, which is the region after chamfering, is not a flat surface, as described below, the chamfered portion is referred to as a chamfered surface. FIG. 1( b) is a diagram showing an example of the cross-sectional shape of the entire end face whose corners have been chamfered according to the present invention. The end face with two chamfered corners has two chamfered surfaces 5. The cross-sectional shape is the shape of the glass plate 1 passing through the center of the annular shape of the glass plate 1 along the radial direction and the plate thickness direction. As shown in FIG. 1( b), the cross-sectional shape of the chamfered surface 5 forms a curved surface shape formed by a smooth curve that convex outward on the surface of the glass plate. The cross-sectional shape of the end face after chamfering (after chamfering) may be such that the chamfered surfaces 5 connecting to the two main surfaces and the side wall surfaces 6 between the two chamfered surfaces 5 form a single curved surface as a whole, as shown in the example of FIG. 1( b). As another example of the cross-sectional shape shown in FIG. 1( b), the chamfered surfaces connecting to the two main surfaces may be formed in two curved shapes, and the side wall surfaces between the two chamfered surfaces may be formed in a linear shape perpendicular to the main surfaces or in a curved shape different from the chamfered surfaces. The radial chamfer length of the glass plate 1 after the chamfering process is defined as the difference between the radius at the position where the end face protrudes most in the radial direction and the radius at the position where the main surface begins to slope toward the end face, and can be, for example, 30 to 200 μm. In the case of a glass substrate for a magnetic disk, the main surfaces of the glass plate 1 are ground and / or polished as necessary, and then a magnetic film is formed on the main surface of the glass plate 1 to produce a magnetic disk.

[0023] FIG. 1( c ) shows an example of the cross-sectional shape of the inner peripheral edge 7 of a glass plate (hereinafter also referred to as a raw glass plate) before chamfering. By irradiating this inner peripheral edge 7 with a laser beam (described later), the corners at the boundaries between the main surfaces of the glass plate and the inner peripheral edge 7 are heated to a temperature above their softening point and partially melted, forming a curved surface, as shown in FIG. 1( b ), thereby completing the chamfering process. The inner peripheral edge 7 of the glass plate before chamfering is a surface that is approximately perpendicular to the main surfaces of the glass plate. Like the inner peripheral edge 7, the outer peripheral edge also has a surface that is approximately perpendicular to the main surfaces of the glass plate. By irradiating such a surface with a laser beam (described later), the corners between the main surfaces and the inner peripheral edge 7 can be chamfered, forming, for example, the chamfered surface 5 shown in FIG. 1( b ). The cross-sectional shape of the inner peripheral end face 7 shown in FIG. 1( c) is one example, and is not limited to a shape that is approximately perpendicular to the main surface. The shape may have slightly rounded corners or may be inclined relative to the main surface. However, if the cross-sectional shape of the inner peripheral end face 7 is line-symmetric (as described below) with respect to a center line that passes through the center of the thickness of the glass plate in the thickness direction and is parallel to the main surface before the chamfered surface 5 is formed, this is preferable because the cross-sectional shape of the inner peripheral end face after irradiation with laser light, i.e., the inner peripheral end face after the chamfered surface 5 is formed, is also likely to be line-symmetric.

[0024] 2 and 3 are diagrams illustrating the laser beam irradiation performed in one embodiment of the method for manufacturing a glass plate 1. Irradiation with laser beam L forms a chamfered surface 5 on the inner peripheral edge surface 7 and reduces the surface roughness of the inner peripheral edge surface 7 or the chamfered surface 5. The surface roughness of the inner peripheral edge surface (chamfered surface 5 and / or side wall surface 6) after irradiation with laser beam L is 50 nm or less in arithmetic mean roughness Ra (JIS B0601 2001) and / or 500 nm or less in maximum height Rz (JIS B0601 2001). The surface roughness can be measured, for example, with a laser microscope. As shown in FIGS. 2 and 3 , when irradiating the inner peripheral edge surface 7 along the inner hole 3 of the annular glass plate (i.e., the annular glass plate 2) with laser beam L before laser beam irradiation, the laser beam L is irradiated onto the inner peripheral edge surface 7 so that the laser beam L moves relative to the inner peripheral edge surface 7 in the circumferential direction of the glass plate 2. In other words, the laser beam L passes through the focusing position 12 of the focusing lens 10 to change from converging beam L1 to diverging beam L2, and this diverging beam L2 is irradiated onto the inner peripheral end face 7 from a direction oblique to the main surface of the raw glass plate 2. That is, in the embodiment shown in FIGS. 2 and 3 , the laser beam L is focused by the focusing lens 10 and then converted into diverging beam L2, and this diverging beam L2 is irradiated onto the inner peripheral end face 7 from a direction oblique to the main surface. Irradiating the diverging beam L2 from a direction oblique to the main surface means irradiating the diverging beam L2 with the central axis of the beam of the diverging beam L2 being inclined relative to the main surface. In other words, in the embodiment shown in FIGS. 2 and 3 , the laser beam L focused by the focusing lens 10 passes the focusing position (focus) 12 and becomes diverging beam L2, and is then irradiated onto the inner peripheral end face 7. It is sufficient that the convergence and divergence of the laser beam L occur at least in the thickness direction of the raw glass plate.

[0025] The luminous flux of the diffused light L2 is small near the focusing position 12. If the luminous flux is large, the portion of the glass plate 2 that faces the irradiation position 14 of the laser light L on the inner peripheral end face 7 across the center of the annular glass plate 2 becomes an obstacle in the optical path, causing the light to scatter, or even if the light passes through the opposing portion, the intensity of the transmitted light decreases, making it difficult to form the chamfered surface 5 or making it impossible to ensure sufficient light intensity to make the cross-sectional shape of the inner peripheral end face line-symmetrical.

[0026] In this embodiment, the diffused light L2 after passing through the focusing position 12 is used to reduce the beam flux near the location where the glass plate 2 is likely to become an obstacle (position A, described below). This allows the laser light L to easily avoid the location of the glass plate 2 that is likely to become an obstacle. This reduces the inclination angle of the diffused light L2 with respect to the main surface of the glass plate 2. By irradiating the diffused light L2 with a small inclination angle with respect to the main surface of the glass plate 2, the temperatures of both corners of the inner peripheral edge surface 7 in the thickness direction at the focusing position 12 approach approximately the same temperature during irradiation. This facilitates the formation of a line-symmetrical cross-sectional shape of the inner peripheral edge surface with a target shape. That is, the cross-sectional shape of the inner peripheral edge surface can be formed line-symmetrically with respect to a centerline passing through the center of the glass plate 1 in the thickness direction and parallel to the main surface.

[0027] Here, the term "axisymmetric shape" refers to a case where the maximum deviation in the direction parallel to the main surface between the contour lines of the end faces at each position in the thickness direction when the contour line of the cross-sectional shape is folded back relative to a centerline passing through the center of the thickness direction of the glass plate 1 and parallel to the main surface is 30 μm or less. The maximum deviation is preferably 20 μm or less. If the maximum deviation exceeds 30 μm, the orientation of the glass plate 1 becomes unstable when the inner hole 3 is held in a film-forming device that deposits a magnetic film or the like to function as a magnetic disk, making the glass plate 1 more susceptible to cracking or dropping. Furthermore, the term "axisymmetric shape" with respect to the cross-sectional shape of the inner peripheral end face of the glass plate 2 refers to a case where the maximum deviation is 30 μm or less when the glass plate 2 is used instead of the glass plate 1.

[0028] To prevent the opposing portion 20 of the irradiation position 14 on the inner peripheral end face 7 across the center of the inner bore 3 from obstructing the optical path, the focusing position 12 is preferably set in an area centered above the position on the inner peripheral end face 7 that faces the irradiation position 14 on the inner peripheral end face 7 of the diffused light L2 across the center of the inner bore 3 (hereinafter also referred to as "position A"). The focusing position 12 may be adjusted in various ways, taking into account the specifications of the laser light L (such as the inclination angle θ and the diffusion angle φ), the thickness of the glass plate 2, and the diameter of the inner bore 3. The focusing position 12 is preferably set above a plane that includes the main surface radially outward of position A. This also has the effect of sufficiently widening the area (spot diameter) of the beam of diffused light L2 at the irradiation position 14. In other words, the focusing position 12 is preferably located radially outward from position A by a distance of more than 0 mm in a plan view. The distance is more preferably 10 mm or more, and even more preferably 20 mm or more. There is no particular upper limit to the distance, but it may be, for example, 300 mm or less to avoid an increase in the size of the device. In this specification, "planar view" means a view from a direction perpendicular to the main surface of the glass plate.

[0029] The laser light L can be obtained by emitting it from a laser oscillator (not shown). Furthermore, to move the laser light L (diffused light L2) relative to the inner peripheral end face 7 in the circumferential direction of the glass plate 2, for example, a method can be used in which the center of the annular shape of the glass plate 2 is aligned with and fixed to the center of rotation of a turntable (not shown), and the glass plate 2 is rotated. For example, the laser light L can be irradiated onto the inner peripheral end face 7 of the glass plate 2, which rotates together with the turntable, so that the laser light L scans along the inner peripheral end face 7 of the glass plate 2. The relative movement speed of the laser light L and the inner peripheral end face 7 of the glass plate 2 can be, for example, 0.7 to 100 mm / sec. The laser light L can be, for example, CO 2 Laser light can be used. 2 The wavelength of the laser light is preferably 3 μm or more. The laser light L may be CO 2 if it has an oscillation wavelength that is absorbed by glass. 2Other than laser light, for example, CO laser light (oscillation wavelength: approximately 5 μm or approximately 10.6 μm), Er-YAG laser light (oscillation wavelength: approximately 2.94 μm), etc. may also be used. The size and shape of the light beam (irradiation spot) of the laser light L at the irradiation position on the inner peripheral end face 7 may be, for example, a circle with a diameter of 1 to 10 mm, but may also be an ellipse with an equivalent area. The size and shape of the irradiation spot may be selected appropriately depending on the thickness of the glass plate 2 to be chamfered, but from the viewpoint of making the cross-sectional shape of the inner peripheral end face 7 line-symmetrical, it is preferable that the size be larger than the thickness of the glass plate 2 at least in the thickness direction. The average power density of the light beam L at the irradiation position may be, for example, 1 to 30 [W / mm 2 The average power density can be calculated by multiplying the total power [W] of the laser light L by the area [mm 2 ] (that is, if a part of the light beam protrudes from the inner peripheral end face 7, the area of ​​the protruding part is also included). The total power of the laser light L may be set to, for example, 10 to 300 [W].

[0030] When irradiating the inner peripheral end face 7 with the diffused light L2, it is preferable to irradiate the laser light L so that the central axis of the luminous flux of the diffused light L2 passes above the center of the annular shape of the raw material glass plate 2 (a position above the raw material glass plate 2 on the central axis of the raw material glass plate 2 that is perpendicular to the main surface). In this way, the angle of incidence of the laser light L on the inner peripheral end face 7 approaches perpendicularity, minimizing energy loss due to reflection of the laser light L and enabling the chamfered surface 5 to be formed efficiently.

[0031] It is also preferable to heat the glass plate 2 before and / or during irradiation with the laser beam L. This reduces residual strain that occurs near the inner peripheral edge after chamfering with the laser beam L. For example, a heater or the like may be disposed around the glass plate 2 to raise the temperature of the entire glass plate 2. For example, a halogen lamp heater, a carbon heater, an infrared heater such as a sheath heater, or the like may be used as the heater.

[0032] In this way, by irradiating the diffused light L2 of the laser light L that has passed through the focusing position 12 onto the inner end surface 7, there is no longer any need to place a reflective mirror in the inner hole 3 as in the conventional method, so the transport path of the glass raw material 2 and the glass plate 1 is not restricted and the device configuration can be simplified.

[0033] 4 is a diagram illustrating the irradiation of laser light in a method for manufacturing a glass plate 1 that is different from the present invention. Fig. 4 shows an example in which converging light L1 is irradiated onto the inner peripheral edge surface 7. The beam of converging light L1 spreads the further away from the irradiation position 14 on the inner peripheral edge surface 7. Therefore, the opposing portion 20 of the glass plate 2 that faces the irradiation position 14 of the inner peripheral edge surface 7 becomes an obstacle, causing some of the light to scatter. Even if the light is transmitted, the intensity of the transmitted light is reduced, making it difficult to form the chamfered surface 5 or preventing sufficient light intensity from being obtained to achieve an axisymmetric cross-sectional shape on the inner peripheral edge surface.

[0034] As described above, the inclination angle θ (see FIG. 3 ) of the central axis of the diffused light L2 (laser light) relative to the main surface is preferably small to achieve line-symmetrical cross-sectional shape of the inner peripheral end face. Specifically, it is preferably 20 degrees or less, more preferably 15 degrees or less, and even more preferably 10 degrees or less. Furthermore, it is preferable to irradiate the diffused light L2 only from one main surface of the glass plate 2, from a direction inclined relative to this main surface. In this case, the glass plate 2 can be firmly fixed from the other main surface opposite to the one main surface, thereby preventing misalignment of the glass plate 2. This enables precise shape control, making it easier to achieve the aforementioned line-symmetrical shape over the entire inner peripheral end face. Furthermore, the device configuration can be significantly simplified. The minimum value of the inclination angle θ is not particularly limited, but is preferably 1 degree or greater. If the inclination angle θ is less than 1 degree, adjustment of the optical system during mass production may be difficult. Furthermore, the diffusion angle φ of the laser light L (see FIG. 4; the angle indicating the narrowing or widening of the light beam when focused or diffused) is preferably 20 degrees or less in full-width, more preferably 10 degrees or less, and even more preferably 5 degrees or less, in order to facilitate the reduction of the tilt angle θ. Furthermore, the smaller the diffusion angle φ, the easier it is to position the laser oscillator and / or optical components such as lenses relatively farther from the glass plate 2 to be processed, thereby providing the advantage of greater design flexibility for, for example, ancillary devices for loading and unloading the glass plate 2 into the laser beam irradiation device. The minimum value of the diffusion angle φ is not particularly limited, but is preferably 0.5 degrees or more in full-width. A diffusion angle φ of less than 0.5 degrees may result in an increased device size.

[0035] The method for manufacturing the raw glass plate 2 to be irradiated with the laser beam L is not particularly limited, but may be, for example, a float process, a down-draw process, or a press process. A plurality of disk-shaped glass plates with internal holes can be cut out from a wide sheet-like glass plate manufactured by the float or down-draw process. The disk-shaped glass plates can be cut out from the wide sheet-like glass plate by cutting using a known scriber, or by irradiating the glass plate with laser beam to form a circular defect and then cutting out an annular glass plate.

[0036] A glass plate processing apparatus according to one embodiment is configured to perform the above-described glass plate manufacturing method. The glass plate processing apparatus includes a laser beam irradiation device. The laser beam irradiation device has a laser oscillator and optical components. The optical components include lenses including a condenser lens 10. The glass plate processing apparatus may also include a holding unit that holds the raw glass plate by fixing or placing it, and a rotation mechanism for rotating the holding unit. The glass plate processing apparatus may also include a turntable that integrates the functions of the holding unit and the rotation mechanism.

[0037] When a magnetic disk glass substrate is manufactured from the glass plate 1 having the chamfered surface 5 formed thereon, various processes described below are carried out so that the final product, a magnetic disk glass substrate, has properties suitable for the glass plate 1.

[0038] The glass plate 1 undergoes grinding and polishing of its main surfaces. In the grinding and polishing process, the glass plate 1 is ground and / or polished. If both processes are performed, polishing is performed after grinding. In the grinding process, a double-side grinding machine equipped with a planetary gear mechanism is used to grind the pair of main surfaces of the glass plate 1. Specifically, both main surfaces of the glass plate 1 are ground while the outer peripheral edge of the glass plate 1 is held in a holding hole provided in a holding member (grinding carrier) of the double-side grinding machine. The double-side grinding machine has a pair of upper and lower surface plates (upper and lower surface plates), and the glass plate 1 is sandwiched between the upper and lower surface plates. Then, by moving either the upper or lower surface plate, or both, and moving the glass plate 1 relative to each other while supplying coolant, both main surfaces of the glass plate 1 can be ground. For example, grinding can be performed by attaching a grinding member formed of a sheet of fixed abrasive grains formed by fixing diamond particles with a resin to the surface plate.

[0039] Next, a first polishing is performed on the pair of main surfaces of the ground glass plate 1. Specifically, both main surfaces of the glass plate 1 are polished while the outer peripheral edge surface of the glass plate 1 is held in a holding hole provided in a polishing carrier of a double-side polishing machine. The purpose of the first polishing is to remove scratches and distortions remaining on the main surfaces after the grinding process or to adjust minute surface irregularities (microwaviness, roughness).

[0040] In the first polishing process, a double-sided polishing machine having a configuration similar to that of the double-sided polishing machine used in the above-described fixed abrasive grinding process is used to polish the glass plate 1 while applying a polishing slurry. In the first polishing process, a polishing slurry containing loose abrasive grains is used. The loose abrasive grains used in the first polishing process include abrasive grains such as cerium oxide or zirconia. As with the double-sided polishing machine, the glass plate 1 is sandwiched between a pair of upper and lower platens. Flat polishing pads (e.g., resin polishers) having an overall annular shape are attached to the top and bottom surfaces of the lower platen. Either the upper or lower platen, or both, are then moved to move the glass plate 1 relative to the respective platens, thereby polishing both main surfaces of the glass plate 1. The size of the polishing abrasive grains is preferably within the range of 0.5 to 3 μm in average particle size (D50).

[0041] After the first polishing, the glass plate 1 may be chemically strengthened. In this case, a mixed molten liquid of potassium nitrate and sodium nitrate, for example, is used as a chemical strengthening liquid, and the glass plate 1 is immersed in the chemical strengthening liquid. This allows a compressive stress layer to be formed on the surface of the glass plate 1 by ion exchange.

[0042] Next, the glass plate 1 is subjected to a second polishing process. The second polishing process aims to mirror-polish the main surfaces. A double-sided polishing machine having the same configuration as the double-sided polishing machine used in the first polishing process is also used in the second polishing process. Specifically, the outer peripheral edge of the glass plate 1 is held in a holding hole provided in a polishing carrier of the double-sided polishing machine, and both main surfaces of the glass plate 1 are polished. In the second polishing process, the type and particle size of the free abrasive grains are different from those in the first polishing process, and the hardness of the resin polisher is different. The hardness of the resin polisher is preferably lower than that in the first polishing process. For example, a polishing liquid containing colloidal silica as free abrasive grains is supplied between the polishing pad of the double-sided polishing machine and the main surfaces of the glass plate 1, and the main surfaces of the glass plate 1 are polished. The size of the abrasive grains used in the second polishing process is preferably within the range of 5 to 50 nm in average particle size (d50). The roughness of the pair of main surfaces of the glass plate 1 after the second polishing is preferably 0.2 nm or less in terms of arithmetic mean roughness Ra (JIS B0601 2001). The surface roughness can be measured, for example, by AFM.

[0043] The necessity of chemical strengthening treatment can be appropriately selected based on the glass composition and other requirements. In addition to the first and second polishing treatments, another polishing treatment may be performed, or the two main surfaces may be polished in a single polishing treatment. The order of the above treatments may also be changed as appropriate. After producing the glass plate 1 having the chamfered end surface 5 formed by irradiating the end surface with the laser light L (diffused light L2) described above, the main surfaces of the glass plate 1 are ground or polished to produce a magnetic disk glass substrate that meets the requirements for a magnetic disk glass substrate. Then, a magnetic disk is produced by forming at least a magnetic film on the main surface of the magnetic disk glass substrate.

[0044] After forming the chamfered surface 5 by irradiating the end surface with the laser light L (diffused light L2), edge polishing may be performed to polish the end surface (inner peripheral edge surface and / or outer peripheral edge surface) of the glass plate 1. Even when such edge polishing is performed, the arithmetic mean roughness Ra of the end surface of the glass plate 1 on which the chamfered surface 5 is formed by irradiating the laser light L can be set to 50 nm or less and / or Rz can be set to 500 nm or less, thereby shortening the time required for edge polishing. The edge polishing may be performed using an abrasive brush method in which abrasive brushes are used to polish the end surface while supplying free abrasive grains to the end surface. However, to improve production efficiency, it is preferable to grind or polish the main surfaces of the glass plate 1 without edge polishing. That is, it is preferable to grind or polish the main surfaces of the glass plate 1 while maintaining the surface roughness of the end surface obtained by irradiating the laser light L. In this embodiment, the surface roughness of the end surface formed by irradiating the laser light L is small, so the formation of the chamfered surface 5 can sometimes be considered to also serve as edge polishing. In this case, the above-mentioned end face polishing refers to additional end face polishing other than the end face polishing performed simultaneously with the formation of the chamfered surface 5. The additional end face polishing is preferably performed before the first polishing. If the additional end face polishing is performed after the first polishing, scratches may be caused on the polished main surface. The additional end face polishing may also be performed before or after the grinding process of the main surface.

[0045] Amorphous glass such as aluminosilicate glass, soda-lime glass, or borosilicate glass can be used as the glass material for the glass plate 1 and its precursor, the raw glass plate 2. Amorphous glass is preferred as the glass material, as it allows the production of a magnetic disk glass substrate with excellent main surface flatness and substrate strength. Furthermore, the glass transition temperature Tg of the glass plate 1 and the raw glass plate 2 is preferably 450 to 850°C so that they can withstand the heating required for forming the magnetic film.

[0046] Experimental Example 1 When the conditions for irradiating the inner peripheral end face of a circular glass plate with laser light L were changed in various ways, a simulation was carried out to confirm whether the light beam was blocked by the glass plate.

[0047] Simulation Conditions: The shape of the annular glass plate was 97 mm outer diameter, 25 mm inner diameter, and 1 mm thickness. The cross section of the inner peripheral edge was the same as that shown in Figure 1(c). The laser beam was irradiated onto the inner peripheral edge of the glass plate with various settings, such as the tilt angle θ, diffusion angle φ, irradiation spot diameter, irradiation method (convergent or divergent), and distance (in plan view) from the irradiation position 14 to the focusing position 12, as shown in Table 1. To simplify the calculation, the irradiation spot diameter was defined as the maximum length of the beam cross section in the thickness direction of the glass plate at the irradiation position on the inner peripheral edge (i.e., not the length obtained from a cross section perpendicular to the central axis of the laser beam L with the tilt angle θ). The center of the irradiation spot diameter was aligned with the center of the thickness of the inner peripheral edge. Evaluation Results: A case in which the beam was blocked by the glass plate even slightly was rated as BAD (i.e., the case shown in Figure 4), and a case in which no beam was blocked at all was rated as GOOD (i.e., the case shown in Figure 3).

[0048]

[0049] As can be seen from Table 1, even in cases where the light beam would be blocked under conventional conditions using convergent light, the use of diffused light enabled laser light irradiation without blocking the light beam. When the distance from the irradiation position to the focusing position exceeds 25 mm, the focal point is located radially outward from the inner diameter end of the glass workpiece in a planar view. In other words, it is located radially outward from the aforementioned "position A." In such cases, it becomes easier to position the laser oscillator and / or optical components such as lenses relatively far away from the glass workpiece. This is preferable because it increases the design flexibility of, for example, ancillary devices for loading and unloading glass workpieces into the laser beam irradiation device.

[0050] (Experimental Example 2) The inner peripheral edge of a glass plate was actually chamfered using conditions 10, 12, and 14 in Table 1. The shape of the annular glass plate was the same as in Experimental Example 1, except that the thickness was changed to 0.7 mm. The glass plate was made of amorphous aluminosilicate glass with a glass transition point of approximately 500°C. The laser light L was CO 2A laser was used. The entire main surface of the glass plate 2 was heated by an infrared heater before irradiation with the laser light L. Other irradiation conditions and methods were appropriately adjusted with reference to the above-described embodiment so that the inner peripheral edge after chamfering had a cross-sectional shape similar to that shown in FIG. 1(b).

[0051] As a result, under all conditions, the inner peripheral edge surfaces of the obtained glass plates had a cross-sectional shape similar to that shown in Figure 1(b), and a chamfered surface was formed. Furthermore, the surface roughness of these inner peripheral edge surfaces was 50 nm or less in terms of arithmetic mean roughness Ra (measured with a laser microscope). Furthermore, the shape was line-symmetrical with respect to a center line passing through the center of the glass plate in the thickness direction and parallel to the main surface.

[0052] The method for manufacturing a glass plate, the method for manufacturing a glass substrate for a magnetic disk, the method for manufacturing a magnetic disk, and the processing apparatus for a glass plate of the present invention have been described in detail above. However, the present invention is not limited to the above-described embodiments, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.

[0053] REFERENCE SIGNS LIST 1 glass plate 2 raw glass plate 3 inner hole 5 chamfered surface 6 side wall surface 7 inner peripheral end surface 10 condenser lens 12 condensing position 14 irradiation position 20 opposing portion

Claims

1. A method for manufacturing a glass plate including a process of irradiating a laser beam along an inner peripheral end face along an inner hole of an annular glass plate, wherein in the process, when irradiating the inner peripheral end face with the laser beam, the laser beam is condensed by a condenser lens and then diffused, and the diffused light is irradiated onto the inner peripheral end face from a direction inclined with respect to a main surface of the glass plate. A method for manufacturing a glass plate, characterized in that.

2. The method for manufacturing a glass plate according to claim 1, wherein an inclination angle of a central axis of the laser beam with respect to the main surface is 20 degrees or less.

3. The method for manufacturing a glass plate according to claim 1 or 2, wherein a diffusion angle of the laser beam is 20 degrees or less.

4. By the process, corners between each of the main surfaces on both sides of the glass plate and the inner peripheral end face are chamfered, and a cross-sectional shape of the inner peripheral end face with the chamfered corners is symmetric with respect to a center line passing through a center in a thickness direction of the glass plate and parallel to the main surface. The method for manufacturing a glass plate according to any one of claims 1 to 3.

5. A position where the laser beam is condensed by the condenser lens is above a plane including the main surface on a radially outer side of a position of the inner peripheral end face on the inner peripheral end face of the laser beam across the center of the inner hole with respect to an irradiation position on the inner peripheral end face. The method for manufacturing a glass plate according to any one of claims 1 to 4.

6. The method for manufacturing a glass plate according to any one of claims 1 to 5, wherein the glass plate is a glass substrate that is a base for a glass substrate for a magnetic disk.

7. After irradiation of the laser beam, the main surface of the glass plate is ground or polished without polishing the inner peripheral end face. The method for manufacturing a glass plate according to any one of claims 1 to 6.

8. A method for manufacturing a glass substrate for a magnetic disk, characterized in that after manufacturing a glass plate by the method for manufacturing a glass plate according to any one of claims 1 to 6, the main surface of the glass plate is ground or polished to manufacture the glass substrate for a magnetic disk.

9. A method for manufacturing a magnetic disk, characterized in that a magnetic film is formed on a main surface of a glass plate manufactured by the method for manufacturing a glass substrate for a magnetic disk according to claim 8.

10. A glass plate processing apparatus that performs a process of irradiating a laser beam along an inner peripheral end face along an inner hole of an annular glass plate, wherein in the process, when irradiating the inner peripheral end face with the laser beam, the laser beam is condensed by a condenser lens and then diffused, and the diffused light is irradiated onto the inner peripheral end face from a direction inclined with respect to the main surface of the glass plate. A glass plate processing apparatus characterized by the above.