Polyester elastomer resin composition

The thermoplastic polyester elastomer resin composition with naphthalene dicarboxylic acid and aliphatic diols in the hard segment, and aliphatic polyethers, addresses the limitations of conventional polyester elastomers by enhancing fuel barrier properties and heat aging resistance, ensuring improved performance in tubular molded products.

WO2024203743A1PCT designated stage expired Publication Date: 2024-10-03TOYOBO MC CORP

Patent Information

Application Number
PCT/JP2024/011085
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional polyester elastomers used in tubular molded products, such as hoses and tubes, face challenges with poor water resistance, heat aging resistance, and flexibility, particularly when exposed to high temperature oils and chemicals, failing to meet recent market demands for improved fuel barrier properties and low-temperature flexibility.

Method used

A thermoplastic polyester elastomer resin composition is developed with a hard segment containing naphthalene dicarboxylic acid and specific aliphatic and alicyclic diols, along with aliphatic polyethers, which adjusts the soft segment ratio and melt flow rate within a predetermined range to enhance fuel barrier properties, heat aging resistance, and flexibility.

Benefits of technology

The composition achieves improved fuel evaporative gas barrier properties, heat aging resistance, and flexibility, making it suitable for tubular molded products like fuel tubes, addressing the limitations of conventional polyester elastomers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a polyester elastomer resin composition from which a tubular molded body that suppresses the permeation of a fuel evaporation gas and has excellent heat aging resistance, oil resistance, and flexibility can be formed. A polyester elastomer resin composition according to the present invention that solves the above problem contains a thermoplastic polyester elastomer (A) in which a hard segment composed of a polyester containing an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol as constituent components is bonded to at least one soft segment selected from among aliphatic polyethers, aliphatic polyesters, and aliphatic polycarbonates, and is characterized in that: the hard segment contains a naphthalene dicarboxylic acid component as the aromatic dicarboxylic acid component; the content of the soft segment is 5-22 mass% of the thermoplastic polyester elastomer (A); and the melt flow rate is at most 15 g / 10 min.
Need to check novelty before this filing date? Find Prior Art

Description

Polyester elastomer resin composition

[0001] The present invention relates to a thermoplastic polyester elastomer having excellent fuel barrier properties, heat aging resistance, oil resistance, and flexibility, and a molded article thereof, and relates to a thermoplastic polyester elastomer used for tubular molded articles such as tubes and hoses.

[0002] Polyester elastomers have excellent flexibility, heat resistance, oil resistance, chemical resistance, mechanical properties, electrical properties, etc., and are therefore widely used in a variety of applications, such as electrical and electronic parts, automobile and other machine parts, office equipment, home appliances, and other products and parts. In particular, polyester elastomers are used in applications for tubular molded articles such as tubes and hoses, because in addition to the above properties, they also have the ease of molding that takes advantage of their thermoplastic properties.

[0003] For example, hoses / tubes formed by laminating an inner layer, a reinforcing layer, and an outer layer into a tubular shape, or tubular hoses / tubes formed by a single layer, have the inner layer, outer layer, or single layer constructed of vulcanized rubber or thermoplastic resin, and the reinforcing layer is made of fiber or steel wires such as steel or stainless steel braided in a braided or spiral shape, optionally subjected to a rubber coating or other adhesive treatment. However, when rubber is used for the inner and outer layers, a vulcanization process is required, making the manufacturing process complicated. Furthermore, when a thermoplastic resin is used for the inner and outer layers, there are problems such as poor flexibility and, depending on the resin, a low melting point and poor heat resistance. Proposals to solve these problems include a hose (Patent Document 1) in which the inner layer is constructed of a thermoplastic elastomer in which a vulcanized composition of an acrylic group-containing rubber is dispersed in a copolymer elastomer having polybutylene terephthalate as a hard segment and polytetramethylene glycol and / or polycaprolactone as a soft segment, and a hydraulic piping hose constructed of a polyamide elastomer or polyester elastomer inner layer, a reinforcing layer, and a urethane elastomer outer layer.

[0004] However, conventional polyester elastomers have poor water resistance and heat aging resistance, and polyester elastomers with a surface hardness of 60A to 60D suffer from significant swelling and deterioration due to high-temperature oil and chemicals. Polyamide elastomers have poor flexibility and suffer from significant swelling due to high-temperature oil and chemicals. Furthermore, polyurethane elastomers, while slightly less prone to swelling due to oil than other elastomers, have the problem of a low softening temperature. Therefore, conventional thermoplastic elastomers have been unable to meet the demands of the market in recent years.

[0005] As a solution to this problem, a hose using a polyester elastomer containing naphthalenedicarboxylic acid as the acid component in the hard segment has been proposed (Patent Document 2).

[0006] Japanese Patent Laid-Open No. 6-64102 Japanese Patent Laid-Open No. 2000-95848

[0007]

[0003] In recent years, with the tightening of VOC emission regulations, fuel hose materials are increasingly required to suppress the permeation of fuel vapors, while at the same time, the demand for heat aging resistance is becoming stricter to prevent fuel leakage from deteriorated hoses. Furthermore, further performance improvements, including suppression of swelling due to fuel, are required. However, the polyester elastomers mentioned above have not been sufficiently studied to address these issues.

[0008] The present invention has been made in consideration of the current state of the prior art, and its object is to provide a polyester elastomer resin composition capable of forming a tubular molded article that suppresses the permeation of fuel evaporative gas and has excellent heat aging resistance, oil resistance, and flexibility (particularly low-temperature flexibility).

[0009] Means for Solving the Problems As a result of intensive investigations into solving the above-mentioned problems, the present inventors have found that all of the above-mentioned problems can be solved by adjusting the soft segment ratio and MFR within predetermined ranges in a polyester elastomer resin composition containing a naphthalenedicarboxylic acid component in the hard segment, and have thus completed the present invention.

[0010] That is, the present invention has the following features. [1] A polyester elastomer resin composition containing a thermoplastic polyester elastomer (A) having hard segments composed of a polyester having an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol as constituent components, and at least one soft segment selected from an aliphatic polyether, an aliphatic polyester, and an aliphatic polycarbonate bonded thereto, wherein the hard segments contain a naphthalene dicarboxylic acid component as the aromatic dicarboxylic acid component, and the content of the soft segments is 5 to 22 mass% in the thermoplastic polyester elastomer (A). [2] The polyester elastomer resin composition according to [1], which has a melt flow rate (MFR) of 15 g / 10 min or less when measured at a measurement temperature of 250°C and a load of 2.16 kg. [3] The polyester elastomer resin composition according to [1] or [2], wherein the hard segments contain a 2,6-naphthalenedicarboxylic acid component as the aromatic dicarboxylic acid component, and the amount of the 2,6-naphthalenedicarboxylic acid component is 85 mol % or more relative to the total 100 mol % of all dicarboxylic acid components constituting the hard segments. [4] The polyester elastomer resin composition according to any one of [1] to [3], wherein the aliphatic and / or alicyclic diol component constituting the hard segments is an aliphatic diol component, and the aliphatic diol component is an alkylene glycol component having 2 to 8 carbon atoms. [5] The polyester elastomer resin composition according to any one of [1] to [4], wherein the hard segments contain butylene naphthalate units, and the content of the butylene naphthalate units in the polyester constituting the hard segments is 80 mass % or more. [6] The polyester elastomer resin composition according to any one of [1] to [5], wherein the soft segments are aliphatic polyether. [7] The polyester elastomer resin composition according to [6], wherein the aliphatic polyether is at least one selected from the group consisting of poly(tetramethylene oxide) glycol and ethylene oxide adducts of poly(propylene oxide) glycol.[8] The polyester elastomer resin composition according to any one of [1] to [7], wherein the resin composition contains a thickener (B), and the thickener (B) has at least one functional group capable of reacting with an end group of the thermoplastic polyester elastomer (A). [9] The polyester elastomer resin composition according to [8], wherein the functional group is at least one selected from the group consisting of an epoxy group, an acid anhydride group, a carbodiimide group, and an isocyanate group.

[10] The polyester elastomer resin composition according to [8], wherein the thickener (B) is a polyfunctional epoxy compound and / or a polycarbodiimide compound.

[11] The polyester elastomer resin composition according to [8], wherein the thickener (B) is at least one selected from the group consisting of a difunctional epoxy compound, a trifunctional epoxy compound, and a polycarbodiimide compound containing 5 to 30 carbodiimide groups per molecule.

[12] A tubular molded article having at least one layer formed from the polyester elastomer resin composition according to any one of [1] to

[11] .

[13] The tubular molded article according to

[12] , further comprising a layer formed from a thermoplastic polyester elastomer (C) other than the thermoplastic polyester elastomer (A), wherein the thermoplastic polyester elastomer (C) is a thermoplastic polyester elastomer comprising a hard segment formed from a polyester having terephthalic acid and an aliphatic and / or alicyclic diol as constituent components, and at least one soft segment selected from an aliphatic polyether, an aliphatic polyester, and an aliphatic polycarbonate bonded thereto.

[14] A hose having at least one layer formed from the polyester elastomer resin composition according to any one of [1] to

[11] .

[15] A fuel tube having at least one layer formed from the polyester elastomer resin composition according to any one of [1] to

[11] .

[16] A hose made from the polyester elastomer resin composition according to any one of [1] to

[11] .

[17] A fuel tube made from the polyester elastomer resin composition according to any one of [1] to

[11] .

[0011] The polyester elastomer resin composition of the present invention has improved barrier properties against fuel evaporative gases (hereinafter, may be simply referred to as "fuel barrier properties"), heat aging resistance, oil resistance, and flexibility (particularly low-temperature flexibility), and therefore can be used for tubular molded articles such as fuel tubes.

[0012] The polyester elastomer resin composition of the present invention will be described in detail below.

[0013] [Thermoplastic polyester elastomer (A)] The thermoplastic polyester elastomer (A) is formed by bonding hard segments and soft segments. The hard segments are made of a polyester having, as constituent components, an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol.

[0014] The hard segment contains a naphthalenedicarboxylic acid component as an aromatic dicarboxylic acid component. This enhances fuel barrier properties, as well as heat resistance, water resistance, heat aging resistance, oil resistance, and chemical resistance. Specific examples of the naphthalenedicarboxylic acid that constitutes the hard segment include 2,3-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid, with 2,6-naphthalenedicarboxylic acid being preferred.

[0015] The content of the naphthalenedicarboxylic acid (preferably 2,6-naphthalenedicarboxylic acid) component is, for example, 50 mol% or more, preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, and particularly preferably 90 mol% or more, relative to 100 mol% in total of all dicarboxylic acid components constituting the polyester of the hard segment.

[0016] The naphthalenedicarboxylic acid component is introduced by ester synthesis using, for example, naphthalenedicarboxylic acid, a salt thereof, or a naphthalenedicarboxylic acid ester as a raw material. As the raw material, a naphthalenedicarboxylic acid ester is preferably used. Examples of the naphthalenedicarboxylic acid ester include a monoalkyl ester of naphthalenedicarboxylic acid and a dialkyl ester of naphthalenedicarboxylic acid. A diester of naphthalenedicarboxylic acid and an alkyl alcohol having 1 to 4 carbon atoms is preferred, and dimethyl naphthalenedicarboxylic acid ester is more preferred.

[0017] The hard segment may contain a dicarboxylic acid component other than naphthalenedicarboxylic acid (hereinafter referred to as "other dicarboxylic acid"). Examples of the other dicarboxylic acid component include aromatic dicarboxylic acids other than naphthalenedicarboxylic acid, such as terephthalic acid, diphenyldicarboxylic acid, isophthalic acid, and 5-sodium sulfoisophthalic acid; alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid and cyclohexenedicarboxylic acid; and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, dimer acid, and hydrogenated dimer acid. These can be used within a range that does not significantly lower the melting point of the thermoplastic polyester elastomer (A). The dicarboxylic acid (component) constituting the polyester may be used alone or in combination of two or more. The other dicarboxylic acid component may be introduced, for example, by ester synthesis using other dicarboxylic acids, other dicarboxylic acid esters, other dicarboxylic acid salts, or other dicarboxylic acid anhydrides as raw materials.

[0018] In the thermoplastic polyester elastomer (A), the aliphatic or alicyclic diol that constitutes the polyester of the hard segment is generally aliphatic or alicyclic diols. Examples of the aliphatic diol include, but are not limited to, aliphatic glycols such as alkylene glycols (e.g., ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol). Examples of the alicyclic diol include, but are not limited to, alicyclic glycols such as 1,4-cyclohexanedimethanol and 1,4-cyclohexanediol. These diols (components) may be used alone or in combination of two or more.

[0019] The aliphatic and / or alicyclic diol (component) is preferably an aliphatic diol, more preferably an alkylene glycol having 2 to 8 carbon atoms, and even more preferably an alkylene glycol having 2 to 4 carbon atoms. More specifically, at least one selected from the group consisting of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol is preferred, at least one selected from the group consisting of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol is more preferred, and ethylene glycol and / or 1,4-butanediol is even more preferred.

[0020] As the unit constituting the polyester of the hard segment, one composed of butylene naphthalate units (e.g., units composed of 2,6-naphthalenedicarboxylic acid and 1,4-butanediol) is particularly preferred in terms of physical properties, moldability, and cost performance. The content of the butylene naphthalate units in the polyester constituting the hard segment is preferably 50 to 100% by mass, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0021] The thermoplastic polyester elastomer (A) may be produced by first preparing an aromatic polyester suitable as a polyester constituting the hard segment, and then copolymerizing it with a soft segment component. In this case, the aromatic polyester can be easily obtained according to a conventional polyester production method. Such an aromatic polyester preferably has a number average molecular weight of 4,000 to 100,000.

[0022] The soft segment of the thermoplastic polyester elastomer (A) is at least one selected from the group consisting of aliphatic polyethers, aliphatic polyesters, and aliphatic polycarbonates.

[0023] Examples of aliphatic polyethers constituting the soft segment include polyethers having one or more alkanediols having 2 to 10 carbon atoms as structural units, such as poly(ethylene oxide) glycol, poly(propylene oxide) glycol, poly(tetramethylene oxide) glycol (sometimes referred to as polytetramethylene glycol), poly(hexamethylene oxide) glycol, a copolymer of ethylene oxide and propylene oxide, an ethylene oxide adduct of poly(propylene oxide) glycol, and a copolymer of ethylene oxide and tetrahydrofuran. Among these, at least one selected from poly(tetramethylene oxide) glycol and an ethylene oxide adduct of poly(propylene oxide) glycol is preferred from the viewpoint of elastic properties.

[0024] The number average molecular weight of the aliphatic polyether (preferably poly(tetramethylene oxide) glycol) constituting the soft segment is preferably 500 or more, more preferably 800 or more, and even more preferably 1000 or more, from the viewpoint of imparting good elastomeric properties. Furthermore, if the compatibility with the hard segment component decreases, block copolymerization may become difficult. Therefore, from the viewpoint of improving compatibility with the hard segment component, the number average molecular weight of the aliphatic polyether (preferably poly(tetramethylene oxide) glycol) is preferably 4000 or less, more preferably 3000 or less, and even more preferably 2500 or less. That is, the number average molecular weight of the aliphatic polyether (preferably poly(tetramethylene oxide) glycol) is preferably 500 to 4000, more preferably 800 to 3000, and even more preferably 1000 to 2500.

[0025] Examples of the aliphatic polyester constituting the soft segment include aliphatic polyesters in which an ester group and an alkylene group having 2 to 12 carbon atoms are repeated, such as poly(ε-caprolactone), polyenantholactone, polycaprylolactone, and polybutylene adipate. Among these, at least one selected from poly(ε-caprolactone) and polybutylene adipate is preferred from the viewpoint of elastic properties.

[0026] From the viewpoint of imparting good elastomer properties, the number average molecular weight of the aliphatic polyester is preferably 300 or more, more preferably 500 or more, and even more preferably 700 or more. Furthermore, from the viewpoint of improving compatibility with the hard segment component, the number average molecular weight of the aliphatic polyester is preferably 5,000 or less, more preferably 4,000 or less, and even more preferably 2,000 or less. That is, the number average molecular weight of the aliphatic polyester is preferably 300 to 5,000, more preferably 500 to 4,000 or more, and even more preferably 700 to 2,000.

[0027] The aliphatic polycarbonate constituting the soft segment may be a resin composed of a carbonate unit and an aliphatic diol unit, and preferably contains an aliphatic diol residue mainly having 2 to 12 carbon atoms. Examples of these aliphatic diols include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,9-nonanediol, and 2-methyl-1,8-octanediol. In particular, aliphatic diols having 5 to 12 carbon atoms are preferred in terms of further enhancing the flexibility and low-temperature properties of the resulting thermoplastic polyester elastomer (A). These components may be used alone, or two or more types may be used in combination as necessary.

[0028] The number-average molecular weight of the aliphatic polycarbonate is preferably 5,000 or more, more preferably 7,000 or more, and even more preferably 10,000 or more. From the viewpoint of compatibility between the hard segment and the soft segment, the upper limit of the number-average molecular weight of the aliphatic polycarbonate is preferably 80,000 or less, more preferably 70,000 or less, and even more preferably 60,000 or less. If the molecular weight of the aliphatic polycarbonate is too high, compatibility decreases, causing phase separation, which significantly affects the mechanical properties of the molded article and may reduce the strength and elongation of the molded article. That is, the number-average molecular weight of the aliphatic polycarbonate is preferably 5,000 to 80,000, more preferably 7,000 to 70,000, and even more preferably 10,000 to 60,000.

[0029] From the viewpoint of further improving low-temperature properties, the aliphatic polycarbonate constituting the soft segment of the thermoplastic polyester elastomer (A) preferably has a low melting point (e.g., 70°C or lower) and a low glass transition temperature (e.g., -40°C or lower). In general, aliphatic polycarbonates composed of carbonate units and 1,6-hexanediol units, which are used to form the soft segment of a thermoplastic polyester elastomer, have a low glass transition temperature of around -60°C and a melting point of around 50°C, and therefore have good low-temperature properties. In addition, aliphatic polycarbonates obtained by copolymerizing, for example, an appropriate amount of 3-methyl-1,5-pentanediol with the above-mentioned aliphatic polycarbonates have a slightly higher glass transition point than the original aliphatic polycarbonate, but have a lower melting point or become amorphous, and therefore have good low-temperature properties. Furthermore, for example, an aliphatic polycarbonate consisting of a carbonic acid unit, a 1,9-nonanediol unit, and a 2-methyl-1,8-octanediol unit has a melting point of about 30° C. and a glass transition temperature of about −70° C., which are sufficiently low, and therefore has good low-temperature properties.

[0030] The soft segment of the thermoplastic polyester elastomer (A) is preferably an aliphatic polyether from the viewpoint of further improving fuel barrier properties, heat aging resistance, oil resistance, and flexibility.

[0031] The soft segment content in the thermoplastic polyester elastomer (A) is 5% by mass or more, preferably 10% by mass or more. Adjusting the soft segment content within the above range prevents excessive crystallinity, further enhances flexibility (particularly low-temperature flexibility), and reduces the likelihood of permanent deformation. The soft segment content in the thermoplastic polyester elastomer (A) is 22% by mass or less, preferably 20% by mass or less, more preferably 18% by mass or less, and may even be 17.0% by mass or less. Adjusting the soft segment content within the above ranges can further enhance fuel barrier properties and oil resistance, and further impart appropriate crystallinity. That is, the soft segment content in the thermoplastic polyester elastomer (A) is 5 to 22% by mass, preferably 10 to 20% by mass, more preferably 10 to 18% by mass, and may even be 10 to 17.0% by mass.

[0032] On the other hand, in order to achieve particularly excellent heat resistance and tear strength, the content of the hard segment in the thermoplastic polyester elastomer (A) is preferably 78 to 95 mass%, more preferably 80 to 90 mass%, even more preferably 82 to 90 mass%, and may be 83.0 to 90 mass%.

[0033] The thermoplastic polyester elastomer (A) may be used alone or in combination of two or more.

[0034] The lower limit of the melting point of the thermoplastic polyester elastomer (A) is not particularly limited, but from the viewpoint of improving properties in the high temperature range (e.g., tensile strength at break, tear strength, puncture strength, etc.), it is generally preferably 150°C or higher, more preferably 180°C or higher. The upper limit of the melting point of the thermoplastic polyester elastomer (A) is also not particularly limited, but from the viewpoint of moldability, it is preferably 260°C or lower, more preferably 240°C or lower. That is, the melting point of the thermoplastic polyester elastomer (A) is preferably 150 to 260°C, more preferably 180 to 240°C. The melting point can be measured by the method described in the Examples below.

[0035] When the thermoplastic polyester elastomer (A) contains two or more thermoplastic polyester elastomers, multiple melting points may be observed. In such cases, the melting point of the thermoplastic polyester elastomer (A) may be determined as follows. That is, when the thermoplastic polyester elastomer (A) contains two or more thermoplastic polyester elastomers and has multiple melting points, and the difference between the maximum and minimum of the multiple melting points is within 15°C, the melting point of the thermoplastic polyester elastomer (A) may be the weighted average of the melting points. When the thermoplastic polyester elastomer (A) contains two or more thermoplastic polyester elastomers and has multiple melting points, and the difference between the maximum and minimum of the multiple melting points is more than 15°C, the highest melting point may be determined as the melting point of the thermoplastic polyester elastomer (A).

[0036] The reduced viscosity of the thermoplastic polyester elastomer (A) is preferably 1.0 dl / g or more, more preferably 1.2 dl / g or more, from the viewpoint of improving durability such as heat aging resistance. Furthermore, from the viewpoint of processability, it is preferably 4.0 dl / g or less, more preferably 3.7 dl / g or less. That is, the reduced viscosity of the thermoplastic polyester elastomer (A) is preferably 1.0 to 4.0 dl / g, more preferably 1.2 to 3.7 dl / g. The reduced viscosity can be measured by the method described in the Examples below.

[0037] The polyester elastomer resin composition of the present invention preferably contains the thermoplastic polyester elastomer (A) as a main component. The content of the thermoplastic polyester elastomer (A) in the polyester elastomer resin composition is preferably 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit of the content is not particularly limited, but may be 100% by mass or 99% by mass or less.

[0038] The composition and composition ratio of the polyester elastomer resin composition may be determined by calculation from the amounts of raw materials used, or by dissolving a sample in a solvent such as deuterated chloroform and measuring the composition. 1 It can also be calculated from the proton integral ratio of H-NMR.

[0039] The thermoplastic polyester elastomer (A) can be produced by any known method, including, for example, a method of transesterifying a diester of a dicarboxylic acid and a lower alcohol, a diol, and a soft segment component in the presence of a catalyst and polycondensing the resulting reaction product, a method of esterifying a dicarboxylic acid, a diol, and a soft segment component in the presence of a catalyst and polycondensing the resulting reaction product, a method of preparing a hard segment polyester in advance, adding a soft segment component to the polyester, and randomizing the polyester through a transesterification reaction, a method of linking hard segments and soft segments with a chain linking agent, and, when poly(ε-caprolactone) is used for the soft segment, a method of adding an ε-caprolactone monomer to the hard segment.

[0040] The catalyst used in the reaction of the thermoplastic polyester elastomer (A) is preferably at least one selected from antimony catalysts, germanium catalysts, and titanium catalysts. Titanium catalysts, more specifically tetraalkyl titanates such as tetrabutyl titanate and tetramethyl titanate, and metal oxalates such as potassium titanium oxalate are particularly preferred. Other catalysts are not particularly limited as long as they are known catalysts, and examples include tin compounds such as dibutyltin oxide and dibutyltin dilaurate, and lead compounds such as lead acetate.

[0041] The polyester elastomer resin composition of the present invention may contain one or more resins (hereinafter, sometimes referred to as "other resins") different from the thermoplastic polyester elastomer (A). Examples of the other resins include polyolefin resins, polyvinyl chloride resins, polyamide resins, polyester resins, and thermoplastic elastomer resins other than the thermoplastic polyester elastomer (A), and among these, polyester resins are preferred.

[0042] The polyester resin is preferably a polyester containing an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol as constituent components.

[0043] Examples of the aromatic dicarboxylic acid include terephthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, isophthalic acid, and 5-sodium sulfoisophthalic acid. Among these, terephthalic acid and naphthalenedicarboxylic acid are preferred, and naphthalenedicarboxylic acid is more preferred. The polyester resin may contain a dicarboxylic acid component other than the aromatic dicarboxylic acid. Examples of the dicarboxylic acid component include alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid and cyclohexenedicarboxylic acid; and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, dimer acid, and hydrogenated dimer acid. The content of the aromatic dicarboxylic acid component is, for example, 50 mol% or more, preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, and particularly preferably 90 mol% or more, based on a total of 100 mol% of all dicarboxylic acid components constituting the polyester resin.

[0044] The aliphatic or alicyclic diol is the same as the aliphatic or alicyclic diol that constitutes the polyester of the hard segment in the thermoplastic polyester elastomer (A), and preferred embodiments thereof are also the same. The content of the aliphatic and alicyclic diol components is, for example, 50 mol% or more, preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, and particularly preferably 90 mol% or more, based on 100 mol% of the total of all diol components that constitute the polyester resin.

[0045] In particular, the polyester resin preferably contains a butylene terephthalate unit (e.g., a unit composed of terephthalic acid and 1,4-butanediol) and / or a butylene naphthalate unit (e.g., a unit composed of naphthalenedicarboxylic acid and 1,4-butanediol), and more preferably contains a butylene naphthalate unit.

[0046] When the polyester elastomer resin composition of the present invention contains another resin, the content of the other resin is preferably 1 to 50 parts by mass, more preferably 5 to 35 parts by mass, per 100 parts by mass of the thermoplastic polyester elastomer (A).

[0047] [Thickener (B)] The polyester elastomer resin composition of the present invention may further contain a thickener (B). The thickener (B) is a reactive compound having a functional group capable of reacting with a hydroxy group or a carboxy group of the thermoplastic polyester elastomer (A). When the thickener (B) has a functional group capable of reacting with a hydroxy group or a carboxy group, the molecular chain of the thermoplastic polyester elastomer (A) can be extended, thereby reducing the melt flow rate of the polyester elastomer resin composition.

[0048] The functional group is preferably at least one selected from an epoxy group (preferably a glycidyl group), an acid anhydride group, a carbodiimide group, and an isocyanate group, more preferably at least one selected from an epoxy group (preferably a glycidyl group) and a carbodiimide group, and even more preferably an epoxy group (preferably a glycidyl group).The thickener (B) preferably contains two or more functional groups per molecule, more preferably 2 to 50 functional groups, and even more preferably 2 to 20 functional groups.

[0049] When the thickener (B) is a compound having an epoxy group, the thickener (B) is preferably a polyfunctional epoxy compound having two or more epoxy groups. Specific examples of the polyfunctional epoxy compound include bifunctional epoxy compounds having two epoxy groups per molecule, such as 1,6-dihydroxynaphthalene diglycidyl ether and 1,3-bis(oxiranylmethoxy)benzene; trifunctional epoxy compounds having three epoxy groups per molecule, such as 1,3,5-tris(2,3-epoxypropyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione and diglycerol triglycidyl ether; and tetrafunctional epoxy compounds having four epoxy groups per molecule, such as 1-chloro-2,3-epoxypropane-formaldehyde-2,7-naphthalene diol polycondensate and pentaerythritol tetraglycidyl ether. Among these, from the viewpoint of heat resistance, difunctional or tetrafunctional epoxy compounds having a naphthalene structure in the skeleton, or trifunctional epoxy compounds having a triazine structure in the skeleton are preferred. In consideration of the effect of appropriately increasing the solution viscosity of the thermoplastic polyester elastomer (A) to a level that does not cause gelation, the effect of efficiently reducing the acid value of the thermoplastic polyester elastomer (A), and the effect of suppressing gel formation due to aggregation and solidification of the epoxy itself, difunctional or trifunctional epoxy compounds are preferred.

[0050] Other examples of the thickener (B) having an epoxy group include a copolymer containing two or more glycidyl groups per molecule, having a weight-average molecular weight of 4,000 to 25,000, and comprising (X) 20 to 99% by mass of a vinyl aromatic monomer, (Y) 1 to 80% by mass of an epoxy group-containing (meth)acrylate, and (Z) 0 to 79% by mass of a vinyl group-containing monomer other than (X) that does not contain an epoxy group.

[0051] The copolymer is preferably a copolymer containing 20 to 99% by mass of (X), 1 to 80% by mass of (Y), and 0 to 79% by mass of (Z), more preferably a copolymer containing 20 to 99% by mass of (X), 1 to 80% by mass of (Y), and 0 to 40% by mass of (Z), and even more preferably a copolymer containing 25 to 90% by mass of (X), 10 to 75% by mass of (Y), and 0 to 35% by mass of (Z). These compositions affect the concentration of functional groups that contribute to the reaction with the thermoplastic polyester elastomer (A), so it is preferable to appropriately control them within the above ranges.

[0052] Examples of the vinyl aromatic monomer (X) include styrene-based monomers such as styrene and α-methylstyrene; (meth)acrylic acid aryl esters such as phenyl (meth)acrylate; (meth)acrylic acid aralkyl esters such as benzyl (meth)acrylate; and (meth)acrylic acid phenoxyalkyl esters such as phenoxyethyl (meth)acrylate. Using a styrene-based monomer as the vinyl aromatic monomer (X) is preferable in that it improves compatibility with the thermoplastic polyester elastomer (A) and broadens the molecular weight distribution of the resulting polyester elastomer resin composition. Examples of the epoxy group-containing (meth)acrylate (Y) include glycidyl (meth)acrylate, (meth)acrylic acid esters having a cyclohexene oxide structure, and (meth)acrylic glycidyl ethers. Among these, glycidyl (meth)acrylate is preferred due to its high reactivity. Examples of the (Z) other vinyl group-containing monomer include alkyl (meth)acrylate esters having an alkyl group having 1 to 22 carbon atoms (the alkyl group may be linear or branched), such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, stearyl (meth)acrylate, and methoxyethyl (meth)acrylate, as well as polyalkylene glycol (meth)acrylate esters, alkoxyalkyl (meth)acrylate esters, hydroxyalkyl (meth)acrylate esters, dialkylaminoalkyl (meth)acrylate esters, isobornyl (meth)acrylate esters, and alkoxysilylalkyl (meth)acrylate esters. Furthermore, (meth)acrylamide, (meth)acryldialkylamide, vinyl esters such as vinyl acetate, vinyl ethers, and α-olefin monomers such as ethylene and propylene can also be used as the (Z) other vinyl group-containing monomer.

[0053] The weight-average molecular weight of the copolymer is preferably 4,000 to 25,000, more preferably 5,000 to 15,000. Adjusting the weight-average molecular weight to 4,000 or more can prevent unreacted copolymer from volatilizing during the molding process or bleeding out onto the surface of the molded article, thereby preventing contamination of the molded article surface. On the other hand, adjusting the weight-average molecular weight to 25,000 or less not only improves the reaction with the thermoplastic polyester elastomer (A) and enhances the molecular weight increasing effect, but also improves the compatibility between the copolymer and the thermoplastic polyester elastomer (A), thereby preventing a decrease in the inherent properties of the thermoplastic polyester elastomer (A), such as heat resistance.

[0054] The epoxy value of the copolymer is 400 to 2500 equivalents / 1×10 6 g, and more preferably 500 to 1500 equivalents / 1×10 6 g, more preferably 600 to 1000 equivalents / 1×10 6 g. The epoxy value is 400 equivalents / 1 x 10 6 g or more, the thickening effect can be further enhanced. 6 By adjusting the viscosity to 1000 ppm or less, it is possible to prevent the thickening effect from becoming excessive and adversely affecting moldability.

[0055] When the thickener (B) is a compound having a carbodiimide group, a polycarbodiimide compound can be preferably used. The polycarbodiimide compound is advantageous in that it can efficiently reduce the acid value.

[0056] The polycarbodiimide compound may be any polycarbodiimide having two or more carbodiimide groups (—N═C═N— structure) in one molecule, and examples thereof include aliphatic polycarbodiimides derived from aliphatic diisocyanates, alicyclic polycarbodiimides derived from alicyclic diisocyanates, aromatic polycarbodiimides derived from aromatic diisocyanates, and copolymers thereof. Preferred are aliphatic polycarbodiimides or alicyclic polycarbodiimides.

[0057] The polycarbodiimide compound can be obtained, for example, by the carbon dioxide removal reaction of a diisocyanate compound. Examples of diisocyanate compounds that can be used herein include aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, and 1,3,5-triisopropylphenylene-2,4-diisocyanate; aliphatic diisocyanates such as tetramethylene diisocyanate and hexamethylene diisocyanate; and alicyclic diisocyanates such as dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, isophorone diisocyanate, and methylcyclohexane diisocyanate. These may be used alone or in the form of copolymers of two or more. A branched structure may be introduced, or a functional group other than a carbodiimide group or an isocyanate group may be introduced by copolymerization. Terminal isocyanates may be used as they are, but the degree of polymerization may be controlled by reacting the terminal isocyanates, or a portion of the terminal isocyanates may be blocked.

[0058] As the polycarbodiimide compound, alicyclic polycarbodiimides derived from dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, isophorone diisocyanate, etc. are particularly preferred, and polycarbodiimides derived from dicyclohexylmethane diisocyanate or isophorone diisocyanate are particularly preferred.

[0059] From the viewpoints of stability and ease of handling, the polycarbodiimide compound preferably contains 2 to 50 carbodiimide groups per molecule, and more preferably 5 to 30 carbodiimide groups per molecule. The number of carbodiimide groups per molecule of the polycarbodiimide compound (i.e., the number of carbodiimide groups) corresponds to the degree of polymerization in the case of a polycarbodiimide compound obtained from a diisocyanate compound. For example, a polycarbodiimide compound obtained by linking 21 diisocyanate compounds in a chain has a degree of polymerization of 20, and the number of carbodiimide groups in the molecular chain is 20. Typically, a polycarbodiimide compound is a mixture of molecules of various lengths, and the number of carbodiimide groups is expressed as an average value. Having a number of carbodiimide groups within the above range makes the compound more likely to solidify near room temperature, thereby enabling it to be powdered. This results in excellent workability and compatibility when mixed with the thermoplastic polyester elastomer (A), and is also preferred in terms of uniform reactivity and bleed-out resistance. The number of carbodiimide groups can be measured, for example, by a conventional method (a method in which a compound is dissolved in an amine and then back-titrated with hydrochloric acid).

[0060] From the viewpoints of stability and ease of handling, the polycarbodiimide compound preferably has an isocyanate group at its terminal, more preferably a polycarbodiimide compound having an isocyanate group content of 0.5 to 4 mass%, and even more preferably a polycarbodiimide compound having an isocyanate group content of 1 to 3 mass%. In particular, polycarbodiimides derived from alicyclic diisocyanates such as dicyclohexylmethane diisocyanate and isophorone diisocyanate and having an isocyanate group content within the above range are preferred. The isocyanate group content can be measured using a standard method (a method in which a compound is dissolved in an amine and then back-titrated with hydrochloric acid).

[0061] When the thickener (B) is a compound having an isocyanate group, examples of the thickener include the above-mentioned polycarbodiimide compounds containing an isocyanate group at the terminal, and isocyanate compounds such as aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates, which are raw materials for the above-mentioned polycarbodiimide compounds.

[0062] When the thickener (B) is a compound having an acid anhydride group, a compound containing 2 to 4 anhydrides per molecule is preferred in terms of stability and ease of handling. Examples of such compounds include phthalic anhydride, trimellitic anhydride, and pyromellitic anhydride.

[0063] The thickener (B) may be used alone or in combination of two or more kinds.

[0064] The content of the thickener (B) is preferably 0.1 parts by mass or more per 100 parts by mass of the thermoplastic polyester elastomer (A). By adjusting the amount of the thickener (B) within the above range, the targeted molecular chain extension effect can be achieved. Note that, as long as the melt flow rate of the polyester elastomer resin composition is within a predetermined range, the content of the thickener (B) may be 0 parts by mass. Furthermore, the content of the thickener (B) is preferably 4.5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, and particularly preferably 2 parts by mass or less per 100 parts by mass of the thermoplastic polyester elastomer (A). By adjusting the amount of the thickener (B) within the above range, the thickening effect can be prevented from becoming excessive, thereby improving moldability and mechanical properties. Furthermore, when the thickener (B) is a compound having an epoxy group, adjusting the amount of the thickener (B) within the above range can prevent the occurrence of unevenness on the surface of the molded product due to aggregation and curing of the compound having an epoxy group. Furthermore, when the thickener (B) is a compound having a carbodiimide group, adjusting the amount of the thickener (B) within the above range can prevent the basicity of the compound having a carbodiimide group from causing hydrolysis of the thermoplastic polyester elastomer (A), which would adversely affect the mechanical properties. That is, the content of the thickener (B) is preferably 0 to 4.5 parts by mass, more preferably 0.1 to 4 parts by mass, even more preferably 0.1 to 3 parts by mass, and particularly preferably 0.1 to 2 parts by mass, per 100 parts by mass of the thermoplastic polyester elastomer (A).

[0065] [Additives] One or more known additives may be added to the polyester elastomer resin composition of the present invention, as long as the effects of the present invention are not impaired. Examples of the additives include hindered phenol-based, sulfur-based, and phosphorus-based antioxidants; hindered amine-based, triazole-based, benzophenone-based, benzoate-based, nickel-based, and salicylic acid-based light stabilizers; mold release agents; antistatic agents; lubricants; molecular weight modifiers such as peroxides, metal deactivators; organic and inorganic nucleating agents; neutralizing agents; antacids; antibacterial agents; fluorescent brighteners; inorganic fibrous substances such as glass fiber, carbon fiber, silica fiber, and alumina fiber; powdery and granular fillers such as carbon black, silica, quartz powder, glass beads, glass powder, silicates (e.g., calcium silicate, kaolin, talc, clay, diatomaceous earth, and wollastonite), metal oxides (e.g., iron oxide, titanium oxide, zinc oxide, and alumina), metal carbonates (e.g., calcium carbonate and barium carbonate), and various other metal powders; plate-like fillers such as mica, glass flakes, and various metal powders; flame retardants; flame retardant assistants; and organic and inorganic pigments. The amount of the additive may be adjusted appropriately depending on the type of additive, and is, for example, 0.01 part by mass or more or 0.5 part by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 3 parts by mass or less, relative to 100 parts by mass of the thermoplastic polyester elastomer (A). That is, the amount of the additive may be 0.01 to 10 parts by mass, 0.5 to 5 parts by mass, or 0.5 to 3 parts by mass, relative to 100 parts by mass of the thermoplastic polyester elastomer (A).

[0066] The polyester elastomer resin composition of the present invention has a melt flow rate (MFR) of 15 g / 10 min or less, preferably 12 g / 10 min or less, and more preferably 10 g / 10 min or less, when measured at a temperature of 250°C and a load of 2.16 kg. By adjusting the MFR of the polyester elastomer resin composition within the above range, heat aging resistance can be improved and moldability into a tubular molded article can also be improved. The MFR of the polyester elastomer resin composition can be reduced by increasing the molecular weight or reduced viscosity of the thermoplastic polyester elastomer (A) contained therein or by adding a thickener (B) to the resin composition. While there is no particular lower limit for the MFR of the polyester elastomer resin composition of the present invention, a lower MFR of 1 g / 10 min or more is preferred, since an MFR that is too low tends to make extrusion molding difficult.

[0067] The polyester elastomer resin composition of the present invention can be obtained by mixing a thermoplastic polyester elastomer (A), a thickener (B), additives, and other resins, which are used as needed. The mixing is preferably performed by melt-kneading using a twin-screw extruder. After mixing, the mixture may be pelletized.

[0068] The polyester elastomer resin composition of the present invention can be suitably used for tubular molded articles such as hoses, tubes, etc. The tubular molded article of the present invention may have at least one layer formed from the polyester elastomer resin composition, and may have a single-layer structure or a multi-layer structure.

[0069] For example, a polyester elastomer resin composition can be extruded using an extruder, and the resulting molten tube can be passed through a sizing die to produce a tubular molded article having a single-layer structure.

[0070] Alternatively, a two-layer tubular molded article can be produced by separately preparing an inner layer material and an outer layer material, co-extruding the materials for each layer using, for example, an extruder, and passing the resulting molten tube through a sizing die, thereby forming an outer layer on the outer peripheral surface of the inner layer. Alternatively, a three-layer tubular molded article can be produced by co-extruding one or more intermediate layer materials together with the inner layer material and the outer layer material in the same manner as above, and passing the resulting molten tube through a sizing die, thereby forming one or more intermediate layers on the outer peripheral surface of the inner layer, and then forming an outer layer on the outer peripheral surface of the intermediate layer. This melt extrusion (co-extrusion) molding ensures good adhesion between the layers.

[0071] In the case of a tubular molded article having a multi-layer structure, the polyester elastomer resin composition of the present invention may be used as a material for forming any of the inner layer, outer layer, and intermediate layer of the tubular molded article, but is preferably used as a material for forming the inner layer and / or outer layer, and more preferably as a material for forming at least the inner layer. In the case of a tubular molded article having a multi-layer structure, the tubular molded article may have only a layer formed from the polyester elastomer resin composition of the present invention, or may have a layer formed from the polyester elastomer resin composition of the present invention and other layers. Note that when multiple layers are formed from the polyester elastomer resin composition of the present invention, the respective polyester elastomer resin compositions may be the same or different from each other. For example, the thermoplastic polyester elastomer (A) contained in each resin composition may have different soft segment ratios or different components constituting the soft segments and / or hard segments.

[0072] When the tubular molded article of the present invention has a layer other than the layer formed from the aforementioned polyester elastomer resin composition, the layer can be formed using a resin composition containing a resin such as a polyolefin resin, a polyvinyl chloride resin, a polyamide resin, a polyester resin, or a thermoplastic elastomer resin other than the thermoplastic polyester elastomer (A) (hereinafter, sometimes referred to as "other resin composition"). In particular, from the viewpoint of further improving gas barrier properties and low-temperature flexibility, it is preferable for the tubular molded article to have a multilayer structure in which the inner layer is formed from the polyester elastomer resin composition of the present invention and the outer layer is formed from a resin composition containing a thermoplastic elastomer resin other than the thermoplastic polyester elastomer (A) (particularly a thermoplastic polyester elastomer other than the thermoplastic polyester elastomer (A)).

[0073] The thermoplastic elastomer resin other than the thermoplastic polyester elastomer (A) is preferably a thermoplastic polyester elastomer other than the thermoplastic polyester elastomer (A) (hereinafter, may be referred to as a thermoplastic polyester elastomer (C)). The thermoplastic polyester elastomer (C) is preferably a thermoplastic polyester elastomer in which a hard segment made of a polyester containing, as constituent components, an aromatic dicarboxylic acid other than naphthalenedicarboxylic acid and an aliphatic and / or alicyclic diol is bonded to at least one soft segment selected from aliphatic polyethers, aliphatic polyesters, and aliphatic polycarbonates.

[0074] Examples of aromatic dicarboxylic acids constituting the hard segments of the thermoplastic polyester elastomer (C) include terephthalic acid, diphenyldicarboxylic acid, isophthalic acid, and 5-sodium sulfoisophthalic acid, with terephthalic acid being preferred. The hard segments may contain dicarboxylic acid components other than aromatic dicarboxylic acids. Examples of such dicarboxylic acids include alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid and cyclohexenedicarboxylic acid; and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, dimer acid, and hydrogenated dimer acid. The content of the aromatic dicarboxylic acid component is, for example, 50 mol% or more, preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, and particularly preferably 90 mol% or more, based on a total of 100 mol% of all dicarboxylic acid components constituting the polyester of the hard segments of the thermoplastic polyester elastomer (C).

[0075] In the thermoplastic polyester elastomer (C), the aliphatic or alicyclic diol that is a component constituting the polyester of the hard segment is the same as the aliphatic or alicyclic diol that is a component constituting the polyester of the hard segment described in the thermoplastic polyester elastomer (A), and preferred embodiments thereof are also the same.

[0076] As the unit constituting the polyester of the hard segment, one composed of butylene terephthalate units (e.g., units composed of terephthalic acid and 1,4-butanediol) is particularly preferred in terms of physical properties, moldability, and cost performance. The content of the butylene naphthalate units in the polyester constituting the hard segment is preferably 50 to 100% by mass, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0077] In the thermoplastic polyester elastomer (C), the aliphatic polyether, aliphatic polyester, or aliphatic polycarbonate constituting the soft segment is the same as the aliphatic polyether, aliphatic polyester, or aliphatic polycarbonate constituting the soft segment in the thermoplastic polyester elastomer (A), and preferred embodiments thereof are also the same.

[0078] The other resin composition preferably contains the resin (preferably the thermoplastic polyester elastomer (C)) as a main component. The content of the resin in the polyester elastomer resin composition is preferably 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit of the content is not particularly limited, but may be 100% by mass or 99% by mass or less.

[0079] The other resin composition may contain one or more known additives within the range that does not impair the effects of the present invention. Examples of the additives include thickeners; hindered phenol-based, sulfur-based, and phosphorus-based antioxidants; hindered amine-based, triazole-based, benzophenone-based, benzoate-based, nickel-based, and salicylic acid-based light stabilizers; release agents; antistatic agents; lubricants; molecular weight modifiers such as peroxides, metal deactivators; organic and inorganic nucleating agents; neutralizing agents; antacids; antibacterial agents; fluorescent brighteners; inorganic fibrous substances such as glass fiber, carbon fiber, silica fiber, and alumina fiber; powdery and granular fillers such as carbon black, silica, quartz powder, glass beads, glass powder, silicates (e.g., calcium silicate, kaolin, talc, clay, diatomaceous earth, and wollastonite), metal oxides (e.g., iron oxide, titanium oxide, zinc oxide, and alumina), metal carbonates (e.g., calcium carbonate and barium carbonate), and various other metal powders; plate-like fillers such as mica, glass flakes, and various metal powders; flame retardants; flame retardant assistants; and organic and inorganic pigments. The amount of the additive may be adjusted appropriately depending on the type of additive, but is, for example, 0.01 parts by mass or more or 0.5 parts by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, relative to 100 parts by mass of the resin. That is, the amount of the additive may be 0.01 to 10 parts by mass, 0.5 to 5 parts by mass, or 0.5 to 3 parts by mass, relative to 100 parts by mass of the resin.

[0080] For the purpose of improving the adhesion between the inner layer and the outer layer, between the inner layer and the intermediate layer, between the intermediate layer and the outer layer, etc., alloy materials or adhesives such as isocyanate-based, phenolic resin-based, epoxy resin-based, and urethane-based adhesives may be used. Furthermore, when strict dimensional accuracy is required for the tubular molded body, a mandrel may be used, but it is not necessary to use one.

[0081] The tubular molding of the present invention may further include a reinforcing layer formed from a reinforcing material, as needed. The reinforcing layer is preferably formed between the inner layer and the outer layer. That is, when the tubular molding of the present invention includes a reinforcing layer, the reinforcing layer is preferably formed on the outer peripheral surface of the inner layer, and the outer layer is further formed on the outer peripheral surface of the reinforcing layer. The reinforcing material may be formed in either a braided or spiral shape, and the material used may be a reinforcing thread or a reinforcing wire. Examples of reinforcing threads include threads made of vinylon fiber, rayon fiber, polyester fiber, nylon fiber, aromatic polyamide fiber, etc. Examples of reinforcing wires include hard steel wires, and more specifically, steel wires plated with brass or zinc for rust prevention and adhesion. Furthermore, adhesives may be used to improve the adhesiveness of these reinforcing layers without any particular problems. Examples of such adhesives include isocyanate-based, phenolic resin-based, epoxy resin-based, and urethane-based adhesives.

[0082] When the tubular molding is to be formed into a bellows shape, the co-extruded molten tube can be passed through a corrugating machine to produce a bellows-shaped tubular molding of a predetermined size.

[0083] The tubular molded article of the present invention has excellent chemical liquid permeation resistance and is therefore suitable as a chemical liquid transport tube. Examples of such a tube include fuel tubes (e.g., feed tubes, return tubes, evaporative tubes, fuel filler tubes, ORVR tubes, reserve tubes, and vent tubes), oil tubes, oil drilling tubes, brake tubes, windshield washer fluid tubes, engine coolant (LLC) tubes, reservoir tank tubes, urea solution transport tubes, coolant cooler tubes, refrigerant cooler tubes, air conditioner refrigerant tubes, heater tubes, road heating tubes, floor heating tubes, infrastructure supply tubes, tubes for fire extinguishers and fire extinguishing equipment, tubes for medical cooling equipment, ink spray tubes, paint spray tubes, and other chemical liquid tubes. In particular, the tubular molded article of the present invention has enhanced fuel barrier properties, heat aging resistance, oil resistance, and flexibility, making it suitable as a fuel tube.

[0084] When the tubular molded article of the present invention is used as a fuel tube, it can be used as a fuel tube for a fuel injection system, etc. It is suitably used as a fuel tube for automobiles that use gasoline, alcohol-blended gasoline, diesel fuel, CNG (compressed natural gas), LPG (liquefied petroleum gas), etc., but is not limited thereto, and can also be used as a fuel tube for fuel cell automobiles that use methanol, hydrogen, dimethyl ether (DME), etc.

[0085] This application claims the benefit of priority based on Japanese Patent Application No. 2023-057165, filed on March 31, 2023. The entire contents of the specification of Japanese Patent Application No. 2023-057165, filed on March 31, 2023, are incorporated herein by reference.

[0086] The present invention will be explained in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0087] In the following examples and comparative examples, the following raw materials were used.

[0088] <Thermoplastic Polyester Elastomer (A)> (Polyester Elastomer (A-1)) 481 parts by mass of dimethyl naphthalate (DMN), 165 parts by mass of 1,4-butanediol (BD), 142 parts by mass of polytetramethylene glycol (number average molecular weight 1000) (PTMG), 1.6 parts by mass of Irganox 1330 (manufactured by BASF), and 0.8 parts by mass of tetrabutyl titanate (TBT) were charged into a 4 L autoclave, and the temperature was raised from room temperature to 220°C over 3 hours to carry out a transesterification reaction. The pressure inside the autoclave was then gradually reduced and the temperature was raised, and the pressure was lowered to 250°C and 1 torr or less over 45 minutes to carry out an initial polymerization reaction. The polymerization reaction was further carried out for 2 hours at 250°C and 1 torr or less, and the resulting molten polyester resin was withdrawn in the form of a strand from the outlet at the bottom of the polymerization vessel, cooled in a water bath, and then cut into chips to obtain polyester elastomer (A-1). The soft segment content was 18% by mass, the melting point was 232°C, and the reduced viscosity was 1.21 dl / g.

[0089] (Polyester elastomer (A-2)) Polyester elastomer (A-2) was obtained in the same manner as Polyester elastomer (A-1), except that 495 parts by mass of dimethyl naphthalate, 172 parts by mass of 1,4-butanediol, and 118 parts by mass of polytetramethylene glycol (number average molecular weight 1,000) were used. The soft segment content was 15% by mass, the melting point was 236°C, and the reduced viscosity was 1.15 dl / g.

[0090] (Polyester elastomer (A-3)) Polyester elastomer (A-3) was obtained in the same manner as Polyester elastomer (A-1), except that 513 parts by mass of dimethyl naphthalate, 181 parts by mass of 1,4-butanediol, and 94 parts by mass of polytetramethylene glycol (number average molecular weight 1,000) were used. The soft segment content was 12% by mass, the melting point was 239°C, and the reduced viscosity was 1.11 dl / g.

[0091] (Polyester elastomer (A-4)) Polyester elastomer (A-4) was obtained in the same manner as Polyester elastomer (A-1), except that 533 parts by mass of dimethyl naphthalate, 191 parts by mass of 1,4-butanediol, and 63 parts by mass of polytetramethylene glycol (number average molecular weight 1,000) were used. The soft segment content was 8% by mass, the melting point was 243°C, and the reduced viscosity was 1.06 dl / g.

[0092] (Polyester elastomer (A-5)) Polyester elastomer (A-5) was obtained in the same manner as Polyester elastomer (A-1), except that 452 parts by mass of dimethyl naphthalate, 151 parts by mass of 1,4-butanediol, and 180 parts by mass of polytetramethylene glycol (number average molecular weight 1,000) were used. The soft segment content was 23% by mass, the melting point was 228°C, and the reduced viscosity was 1.26 dl / g.

[0093] (Polyester elastomer (A-6)) Polyester elastomer (A-6) was obtained in the same manner as for polyester elastomer (A-1), except that 556 parts by mass of dimethyl naphthalate, 203 parts by mass of 1,4-butanediol, and 23 parts by mass of polytetramethylene glycol (number average molecular weight 1,000) were used. The soft segment content was 3% by mass, the melting point was 249°C, and the reduced viscosity was 1.00 dl / g.

[0094] <Thickener (B)> (Thickener (B-1)) Polyethylene glycol diglycidyl ether ("Denacol EX-850", manufactured by Nagase ChemteX Corporation, epoxy valence (average number of epoxy groups per molecule): 2)

[0095] (Thickener (B-2)) Triglycidyl isocyanurate compound ("TEPIC-S", manufactured by Nissan Chemical Industries, Ltd., epoxy valence (average number of epoxy groups per molecule): 3)

[0096] (Thickener (B-3)) Polycarbodiimide ("Carbodilite HMV-8CA", manufactured by Nisshinbo Chemical Inc., carbodiimide valence (average number of carbodiimide groups per molecule): 11)

[0097] <Other Additives> (Stabilizer) Hindered phenol-based antioxidant ("Irganox 1010", manufactured by BASF) (Mold Release Agent) Mold Release Agent ("Licorb WE40", manufactured by Clariant Japan Co., Ltd.)

[0098] [Examples 1 to 5, Comparative Examples 1 to 4] <Preparation of Polyester Elastomer Resin Compositions> Various components were melt-kneaded using a twin-screw extruder according to the formulations shown in Table 1, and then pelletized to obtain pellets of Examples 1 to 5 and Comparative Examples 1 to 3. The resulting polyester elastomer resin compositions and molded articles obtained from the resin compositions were evaluated for the following material properties. The results are shown in Table 1.

[0099] <Preparation of Fuel Tube> The polyester elastomer resin compositions obtained in the Examples and Comparative Examples were used as inner layer materials, and Pelprene P-180BD (manufactured by Toyobo Co., Ltd., a polyester elastomer in which the hard segment polyester is composed of polybutylene terephthalate and the soft segment is composed of PTMG) was used as the outer layer material. These materials were melt extruded (co-extruded) into a hose using an extruder to prepare laminated hoses (fuel tubes) with an inner diameter of 12 mm. The inner layer had a thickness of 0.2 mm, and the outer layer had a thickness of 0.8 mm. In Comparative Example 4, P-180BD was used for both the inner and outer layers of the fuel tube. The resulting fuel tubes were evaluated for the following fuel tube properties. The results are shown in Table 1.

[0100] [Melting Point] A differential scanning calorimeter "DSC220" manufactured by Seiko Instruments Inc. was used. Specifically, 5 mg of the thermoplastic polyester elastomer (A) was placed in an aluminum pan, the pan was sealed with a lid, and the pan was melted in nitrogen at 250°C for 2 minutes. The pan was then cooled to 50°C at a rate of 20°C / min, and the pan was then heated from 50°C to 250°C at a rate of 20°C / min, and a thermogram curve was measured. The endothermic peak due to melting was determined from the obtained thermogram curve, and this was taken as the melting point.

[0101] [Reduced Viscosity] 0.05 g of the thermoplastic polyester elastomer (A) was dissolved in 25 ml of a mixed solvent (phenol / tetrachloroethane=60 / 40 (mass ratio)), and the reduced viscosity was measured at 30° C. using an Ostwald viscometer.

[0102] [MFR] The melt flow rate (MFR, unit: g / 10 min) of the polyester elastomer resin composition pellets obtained in the examples and comparative examples was measured at a temperature of 250°C and a load of 2160 g in accordance with the test method (Method A) described in JIS K7210 (ASTM D1238). Polyester elastomer resin compositions with a moisture content of 0.1 wt% or less were used for the measurement.

[0103] [Tensile Breaking Strength] The tensile breaking strength was measured in accordance with JIS K6251: 2010. Test specimens were prepared by injection-molding a polyester elastomer resin composition dried under reduced pressure at 100°C for 8 hours into a 100 mm x 100 mm x 2 mm flat plate using an injection molding machine (manufactured by Yamashiro Seiki Seisakusho Co., Ltd., model-SAV) at a cylinder temperature (melting point of the thermoplastic polyester elastomer (A) used + 20°C) and a mold temperature of 30°C, and then punching out a dumbbell-shaped No. 3 test specimen from the flat plate.

[0104] [Oil resistance (weight gain)] A simulated alcohol-added gasoline was prepared as the gasoline for evaluation test, which was a mixture of toluene, isooctane, and ethanol in a volume ratio of 40:40:20. The weight gain of the above-mentioned dumbbell-shaped No. 3 test piece when immersed in this gasoline for evaluation test for 48 hours was calculated using the following formula: Weight gain (%) = (weight of test piece after immersion / weight of test piece before immersion) x 100

[0105] [Fuel Barrier Properties] Using a pressure-constant hose permeability measuring device (GTR-TUBE3-TG, manufactured by GTR Tech Co., Ltd.), the permeability coefficient (unit: mg / m / day) of the gasoline for evaluation sealed in each fuel tube was measured for one month at 40°C. The evaluation was carried out as follows: a value of less than 10 (mg / m / day) was rated as ⊚, a value of 10 (mg / m / day) or more but less than 20 (mg / m / day) was rated as ○, and a value of 20 (mg / m / day) or more was rated as ×.

[0106] [Low temperature flexibility] After cooling the fuel tube for 3 hours and 4 hours at -40°C, the tube was immediately bent 180° and checked for the presence or absence of cracks. Tubes that did not develop cracks after either 3 or 4 hours of cooling were marked with "◯", tubes that developed cracks only after 4 hours of cooling were marked with "△", and tubes that developed cracks after either cooling time were marked with "X".

[0107] [Heat Aging Resistance] The fuel tube was left in an environment of 135°C for 500 hours and then bent 180°. Heat aging resistance was evaluated by assigning a grade of "○" to tubes that showed no cracks or breaks when bent, and a grade of "×" to tubes that showed cracks or breaks.

[0108]

[0109] As is clear from Table 1, all of Examples 1 to 5 within the scope of the present invention are excellent in fuel barrier properties, oil resistance, heat aging resistance, and low-temperature flexibility.

[0110] The polyester elastomer resin composition of the present invention has improved fuel vapor barrier properties, heat aging resistance, oil resistance, and flexibility, and can therefore be used for tubular molded articles such as fuel tubes, making a significant contribution to industry.

Claims

1. A polyester elastomer resin composition containing a thermoplastic polyester elastomer (A) having a hard segment made of a polyester having an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol as its constituent components, and at least one soft segment selected from an aliphatic polyether, an aliphatic polyester, and an aliphatic polycarbonate bonded thereto, wherein the hard segment contains a naphthalene dicarboxylic acid component as an aromatic dicarboxylic acid component, the content of the soft segment is 5 to 22 mass% in the thermoplastic polyester elastomer (A), and the melt flow rate (MFR) measured at a measurement temperature of 250°C and a load of 2.16 kg is 15 g / 10 min or less.

2. The polyester elastomer resin composition according to claim 1, wherein the hard segments contain a 2,6-naphthalenedicarboxylic acid component as an aromatic dicarboxylic acid component, and the amount of the 2,6-naphthalenedicarboxylic acid component is 85 mol % or more out of a total of 100 mol % of all dicarboxylic acid components constituting the hard segments.

3. The polyester elastomer resin composition according to claim 1, wherein the resin composition contains a thickener (B), and the thickener (B) has at least one functional group capable of reacting with an end group of the thermoplastic polyester elastomer (A).

4. The polyester elastomer resin composition according to claim 3, wherein the functional group is at least one selected from the group consisting of an epoxy group, an acid anhydride group, a carbodiimide group and an isocyanate group.

5. A tubular molded article having at least one layer formed from the polyester elastomer resin composition according to any one of claims 1 to 4.

6. A fuel tube having at least one layer formed from the polyester elastomer resin composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Hose

    JP1994064102A

  • Polyester-type block copolymer

    JP2000095848A

  • Semiconductor Devices

    JP2023057165A

  • Tube for fuel pipe

    JP2000154890A

  • Thermoplastic polyester resin composition and molded article comprising the same

    JP2011241265A

Cited By

  • Resin composition

    WO2026127562A1

  • Resin composition

    WO2026127565A1

  • Thermoplastic elastomer resin and preparation method therefor

    WO2026230666A1