Low-grade non-oriented silicon steel produced in continuous casting and rolling processes of sheet billet and preparation method thereof
A thin slab continuous casting, oriented silicon steel technology, applied in metal rolling and other directions, can solve the problems of large rolling mill load, increased burden, difficult plate shape control, etc., to achieve good magnetic properties, reduce production costs, and reduce production processes.
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2015-04-29
Smart Images
Figure 1
Abstract
Description
technical field
[0001] The invention belongs to the field of metallurgy, and relates to a low-grade non-oriented silicon steel produced by a thin slab continuous casting and rolling process and a preparation method thereof. Background technique
[0002] The thin slab continuous casting and rolling production process is short, the slab is thin, and the heat loss in the process is small, which can save a lot of energy and reduce costs. Moreover, due to the short rolling line length and small temperature drop, high-temperature final rolling and high-temperature coiling can be realized, and non-oriented silicon steel with excellent magnetic properties can be produced.
[0003] The non-oriented silicon steel slab produced by thin slab continuous casting and rolling is thin, with fast casting speed and well-developed columnar crystals. In the production process of 50W470 grade non-oriented silicon steel, the content of Si and Al in the steel is generally Si+Al>1.5%. When the c...
Examples
Embodiment 1
[0034] Prepare raw materials according to the following chemical composition in mass percentage: C: 0.0029%, Si: 1.48%, Al: 0.39%, Mn: 0.79%, P: 0.021%, N: 0.0035%, S: 0.0039%, the rest is iron and To avoid impurities, carry out smelting and vacuum refining.
[0035] Afterwards, thin slab continuous casting is carried out, and the liquid core reduction process is adopted to reduce the thickness of the slab from 90mm at the exit of the crystallizer to 60mm. %, the average grain size of the equiaxed grains is about 1.62mm, and the distance between the primary dendrite arms of the columnar grains in the slab is about 380μm; after soaking at 1130°C, it is hot-rolled, and the first-pass rolling reduction rate is 49% ; After pickling, the hot-rolled sheet is cold-rolled to a thickness of 0.5 mm, and then annealed and coated in a continuous annealing and coating unit.
[0036] Finished iron loss P 15 / 50 3.27W / kg, magnetic induction B 50 It is 1.70T, and there are no corrugated def...
Embodiment 2
[0038] Raw materials are prepared according to the chemical composition of the following mass percentages: C: 0.0036%, Si: 1.25%, Al: 0.90%, Mn: 0.31%, P: 0.07%, N: 0.0038%, S: 0.0038%, and the rest is iron and To avoid impurities, carry out smelting and vacuum refining.
[0039] Afterwards, thin slab continuous casting is carried out, and the liquid core reduction process is adopted to reduce the thickness of the slab from 90mm at the exit of the crystallizer to 60mm. %, the average grain size of equiaxed grains is about 1.50mm, and the primary dendrite arm spacing of columnar grains in the slab is about 340μm; after soaking at 1120°C, hot rolling is performed, and the reduction rate of the first rolling pass is 48% ; After pickling, the hot-rolled sheet is cold-rolled to a thickness of 0.5 mm, and then annealed and coated in a continuous annealing and coating unit.
[0040] Finished iron loss P 15 / 50 3.44W / kg, magnetic induction B 50 It is 1.72T, and there are no corrugat...
Embodiment 3
[0042]Raw materials are prepared according to the chemical composition of the following mass percentages: C: 0.0051%, Si: 1.36%, Al: 0.69%, Mn: 0.50%, P: 0.03%, N: 0.0036%, S: 0.0040%, and the rest is iron and To avoid impurities, carry out smelting and vacuum refining.
[0043] Afterwards, thin slab continuous casting is carried out, and the liquid core reduction process is adopted to reduce the thickness of the slab from 90mm at the exit of the crystallizer to 55mm. %, the average grain size of equiaxed grains is about 1.47mm, and the primary dendrite arm spacing of columnar grains in the slab is about 355μm; after soaking at 1140°C, hot rolling is carried out, and the rolling reduction rate of the first pass is 45% ; After pickling, the hot-rolled sheet is cold-rolled to a thickness of 0.5 mm, and then annealed and coated in a continuous annealing and coating unit.
[0044] Finished iron loss P 15 / 50 3.39W / kg, magnetic induction B 50 It is 1.71T, and there are no corruga...