Development and vascular application of shape memory stents
By developing PCL-ACPCL shape memory polymers suitable for the vascular system, the problems of high melting temperature and material rigidity of existing SMPs in the treatment of vascular diseases have been solved, and the shape memory and anti-neointimal therapeutic effects at physiological temperatures have been achieved. Reduces treatment pain and cost.
Patent Information
- Application Number
- CN201680036337.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-04-15
- Filing Date
- 2016-04-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2036-04-15
AI Technical Summary
Existing shape memory polymers (SMPs) have high melting temperatures and are invasive when treating vascular conditions, resulting in painful and costly treatment procedures, and the material rigidity of external mesh supports used for hemodialysis leads to neointima formation and Risk of restenosis, difficulty controlling external supports and venous septa.
A new shape memory polymer (SMP) based on poly(ε-caprolactone) (PCL), PCL-co-(α-allyl carboxylate ε-caprolactone) (x%PCL- y% ACPCL), designed to have suitable melting points and mechanical compliance for custom-fitting vascular grafts that provide localized sustained delivery of anti-neointimal therapeutics without sutures or small incisions through shape memory properties Molded external supports.
It achieves SMP with higher elastic recovery at physiological temperature, reduces operation time and infection risk, reduces neointimal formation and restenosis risk, provides more uniform outward remodeling and anti-neointimal treatment effect, and is suitable for For the treatment of hemodialysis and other vascular conditions.
Smart Images

Figure CN107735049B_ABST
Abstract
Description
[0001] Government interests
[0002] This invention was made with government support under Grant No. CBET1219573 awarded by the National Science Foundation. The government has certain rights in this invention. Technical Field
[0003] The presently disclosed subject matter relates to shape memory polymers. In particular, the presently disclosed subject matter relates to vascular grafts comprising allyl-functionalized shape memory polymers and methods of using the vascular grafts to treat vascular conditions.
[0004] introduction
[0005] Vascular disorders can often lead to serious complications or even death. Such vascular disorders include, but are not limited to, hemorrhage, aneurysms, occlusions, and ischemic tissue. Vascular disorders also present unique treatment challenges. This is especially true when treating small or difficult-to-access blood vessels. For example, traditional surgical treatment techniques are invasive to surrounding tissues and can be costly, cause a great deal of pain, and can require a lengthy recovery.
[0006] In this regard, thermoresponsive shape memory polymers (SMPs) have attracted great interest in a wide range of applications, including biomedical, aerospace, self-healing, and textile applications. See, for example, Xue et al. in "J Material Chemistry, 2012: 22 (15)" for a description of the synthesis and characterization of elastic star-shaped memory polymers as self-expanding drug eluting stents. This SMP can recover its original shape after being programmed into a unique temporary shape. Poly(ε-caprolactone) (PCL) is an exemplary biocompatible, biodegradable polymer approved by the FDA for specific biomedical applications, which can be chemically modified and cross-linked to form SMPs. However, its melting temperature (T ) of 45°C to 60°C is too high for physiological applications (37°C). m ) is too high. Therefore, SMPs such as PCL have limited clinical capabilities in treating vascular and other conditions. In addition, the use of other SMPs for therapeutic purposes has been hampered by the need for additional methacrylate functionalization steps or multi-step monomer synthesis schemes.
[0007] Thus, there remains a need for relatively non-invasive, painless and economical compositions and methods for treating vascular disorders.There is also a need for SMPs that can be used in such applications and have a melting point suitable for physiological applications.
[0008] One embodiment of the present invention is a mechanically compliant, moldable shape memory outer support that can be custom fit around a vascular graft anastomosis to prevent neointimal formation. This embodiment can also provide local sustained delivery of therapeutic agents with anti-neointimal effects.
[0009] Other embodiments include anastomotic stents using the compositions disclosed herein, which include a new type of poly(ε-caprolactone) (PCL)-based shape memory polymer (SMP), PCL-co-(α-allyl carboxylate ε-caprolactone) (x% PCL-y% ACPCL) [x% and y%: molar percentage], and are designed to meet the design criteria developed for external stenting of vascular and hemodialysis grafts. Anti-neointimal therapeutic agents can also be incorporated into the matrix for local sustained release and may have a more significant therapeutic effect.
[0010] External mesh supports applied to vein grafts have shown promise in inhibiting intimal hyperplasia by promoting "outward remodeling" (arterialization) with adventitial microvascular growth (i.e., neovascularization). However, in contrast to the compliant nature of arteries, the materials used to date are highly rigid and hard. This precludes application to anastomoses where failures frequently occur, especially in hemodialysis access patients receiving PTFE access grafts. Rigidity also increases the risk of restenosis and makes it difficult to control the spacing between the external support and the vein. Previous studies have shown that these meshes should fit loosely around the graft, and that asymmetric wrapping leads to uneven neovascularization, turbulence, and neointimal formation, especially around the anastomotic site. The present invention overcomes this problem by developing a new type of shape memory external support that can be custom-fitted to each vein anastomosis to promote more uniform outward remodeling rather than inward remodeling, and to locally deliver anti-neointimal therapeutic agents over time.
[0011] Embodiments of the present invention are biocompatible, biodegradable SMPs and can be custom fitted to promote uniform vein-to-stent spacing and outward remodeling that favors neointimal elimination.
[0012] Embodiments of the present invention encompass novel SMPs that maintain a healthy vascular cell phenotype and possess a modulated redox potential for improved venous patency.
[0013] Embodiments of the present invention include SMPs that are mechanically compliant, thereby enabling venous constriction and providing arterial-mimicking mechanical support in the arterial circulation, thereby mitigating neointimal formation caused by compliance mismatch and arterial hemodynamic effects.
[0014] Embodiments of the present invention encompass slowly degrading SMPs that enable sustained mechanical support during the critical period of venous adaptation.
[0015] Embodiments of the present invention encompass SMPs that are easily deployed over PTFE grafts onto venous anastomoses and thus are capable of providing site-directed therapeutic interventions.
[0016] Adventitial administration of therapeutic materials and drugs allows for more effective minimization of intimal hyperplasia by achieving closer contact with myofibroblasts / vascular smooth muscle cells (VSMCs) and maintaining higher drug concentrations with fewer toxicity issues.
[0017] Embodiments of the present invention may encompass anti-neointimal therapeutic agents that may be incorporated into the matrix (see table below).
[0018] Anti-neointimal agents Molecular Target Therapeutic function Anti-neoplastic peptide MK2 Fibrosis, inflammation, migration, proliferation Rapamycin mTOR Hyperplasia Tacrolimus FKB Inflammation Marimastat MMPs migrate Dexamethasone GR Inflammation, migration, proliferation Pioglitazone PPARy Hyperplasia AZX HSP20 Migration, fibrosis Cilostazol Adenylate cyclase Migration, inflammation
[0019] Other embodiments are described herein, including specifically Annexes 1-4. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figures 1A-1E include:( Figure 1A ) Synthesis of α-allyl carboxylate ε-caprolactone (ACCL), ( Figure 1B )ACCL 1 H-NMR spectrum, ( Figure 1C )x%PCL-y%ACPCL SMP network synthesis scheme, ( Figure 1D )96% PCL-04% ACPCL copolymer 1 H-NMR spectrum and ( Figure 1E ) Plot of ACCL:CL feed ratio versus actual x%PCL-y%ACCPCL molar composition.
[0021] Figure 2A and 2B include:( Figure 2A ) Synthesis scheme of 100% PCL-dimethacrylate control and ( Figure 2B ) 100% PCL (top) and 100% PCL-dimethacrylate (bottom) 1 H-NMR spectrum.
[0022] Figure 3 Included are graphs showing the correlation between y% ACPCL and thermal properties of the cross-linked SMP networks.
[0023] Figures 4A-4C include( Figure 4A ) cross-linked 96% PCL-4% ACPCL, ( Figure 4A) cross-linked 89% PCL-11% ACPCL and ( Figure 4C ) Stress-controlled thermomechanical cycling of 100% PCL-dimethacrylate SMP networks, where the SMP film: (1) was heated above T m And by being subjected to tensile stress (0.004MPa min -1 to 0.039MPa) programmed into an elongated shape, (2) cooled (2℃min -1 to 0℃) to obtain the maximum strain ε1(N), (3) stress relief (0.004MPa min -1 to 0MPa) to obtain a temporary shape ε u (N), and (4) heated (2℃min -1 ) to exceed T m And get the original shape ε p (N).
[0024] Figures 5A-5F Includes shape memory demonstration for 88% PCL-12% ACPCL, showing ( Figure 5A ) tubular original shape, its ( Figure 5B ) was deformed into a linear shape by heating at 50°C, applying strain, and fixing in an ice bath, ( Figure 5C ) heated at 37°C to restore the original tube shape, and ( Figure 5D )94% PCL-06% ACPCL guitar shape, ( Figure 5E ) which were heated to 50°C, strained, twisted and fixed at 4°C, and then ( Fig. 5F ) at 48°C and finally restored to its original guitar shape.
[0025] Figure 6 Included are graphs showing the covariance between the physicochemical properties and the thermal, mechanical, and shape memory properties of the photocrosslinked SMP library, where the degree of covariance between the properties is represented by color and annotated values indicating the correlation between the variables (y% = y% ACPCL; Xg = X G ; Mn=M n ; Mw=M w ; Tm=T m ; Hm=ΔH m ; Tc=T c ; E tn =E'(37℃); Snmax=ε max ; Ssmax=σ max ; Rr=R r (N); Rf = R f (N)).
[0026] Figure 7Included are graphs showing the viability of HUVECs seeded directly on polymer surfaces at specific time points (@ = significantly different from TCPS; * = significantly different from 1% agarose; and ** = significantly different from both 100% PCL and 1% agarose, or if located above a 1% agarose bar, significantly different from 100% PCL only).
[0027] Figures 8A-8E Included in ( Fig. 8A )TCPS,( Figure 8B )100%PCL、( Figure 8C )96%PCL-04%ACPCL、( Fig.8D )89% PCL-11% ACPCL and ( Fig. 8E ) Confocal microscopy images of human coronary artery endothelial cells (hCAEC) 3 days after seeding on 88% PCL-12% ACPCL.
[0028] Figures 9A-9C Included are images of the 88% PCL-12% ACPCL shape memory arterial bypass graft: Fig.9A ) original tubular shape, ( Fig. 9B ) after being heated, deformed and fixed into its temporary wire-like shape, and ( Fig. 9C ) after recovering the original tubular shape at 37 °C.
[0029] Figures 10A-10E include( Fig. 10A ) Schematic diagram of minimally invasive bypass grafting of occluded vessels (e.g., bilateral carotid artery ligation), showing ( Fig. 10B ) SMP is implanted and sutured with its linear geometry, ( Fig. 10C ) by embedding collagen hydrogel with C16 and Ac-SDKP peptides for functionalization, ( Fig. 10D ) restore the original tubular shape of the SMP and ( Fig.10E ) blood perfusion through the tubes and functional biomolecules, which over time induce angiogenesis for regeneration and reperfusion of the occluded area.
[0030] Figures 11A-11C Confocal images from fluorescence microangiography are included, showing ( Fig.11A ) "polymer + peptide", ( Fig. 11B ) "peptide only" and ( Fig. 11C ) “Untreated” group.
[0031] Fig. 12A and Fig. 12B Included are images of hematoxylin-eosin (H&E) staining two weeks after in vivo implantation, showing capillary connections between the polymer tube and the native artery.
[0032] Fig.13 Included are fluorescence microscopy images showing CD31 staining as a marker for vascular endothelial cells and leukocytes in the "polymer + peptide" group after 2 weeks. Scale bar = 200 μm.
[0033] Fig.14 Examples of extravascular grafts or supports of the present invention and their optional features are shown, including shape memory properties and anti-neointimal therapeutic agent features.
[0034] Fig.15 A and Fig.15 B shows the properties of x% PCL-y% ACPCL polymer. 15A. Three consecutive thermomechanical (TM) cycles with highly repeatable shape fixity and shape recovery, and 15B. Macroscopic shape memory demonstration showing excellent shape memory capability.
[0035] Fig.16 An embodiment of the present invention is shown and the average stress distribution of an end-to-side Dacron graft-artery anastomosis is shown. The stress along the suture is approximately 8 times the stress along the distal host artery. Similar results were obtained for arterial and venous grafts in this geometry.
[0036] Fig.17 MK2i was shown to inhibit MAPKAP kinase II (MK2). MK2 is in the stress activated protein kinase cascade. Stress, injury, TGFβ, cytokines and lysophosphatidic acid (LPA) activate p38MAP kinase, which in turn activates MK2. MK2 activates the fibrotic pathway via LIM kinase and small heat shock protein HSPB1, which leads to myofibroblast formation and ECM deposition. MK2 also activates the transcription factors hnRNPA0 and TTP that lead to cytokine production. Therefore, MK2i inhibits fibrosis and inflammation, both of which are essential for neointimal formation.
[0037] Fig.18 is a graph showing the effect of MK2i on intimal thickening. HSV rings cultured for 14 days in RPMI medium (30% FBS) were either untreated (control) or treated with MK2i 2 hours before culture. Intimal thickening was measured morphometrically. *p<0.01 (N=4-5).
[0038] Fig.19 is a graph showing the effect of MK2i on wall thickness in vivo. Mouse inferior vena cava to aorta interposition grafts were performed. Prior to implantation, the grafts were incubated in MK2i (100 μM) for 20 minutes. Weekly duplex ultrasound measurements showed that the effect of MK2i was mainly in the first week of treatment.
[0039] Fig. 20 A-20F shows a 3D printing method for prototyping. Fig. 20 A. Male mold design and Fig. 20 B.Print. Fig. 20 C (side view) negative PDMS / glass and Fig. 20 D. (Top view). Fig. 20 E. Porous 89% PCL-11% ACPCL. Fig. 20 F. Final Y-shaped CAD design.
[0040] Fig.21 AB show MK2i release from reservoir gel layers on scaffolds with different gel integrity. Fig.21 A. Schematic illustration of poly(DOPA) coating and heparin immobilization on the outer membrane surface of the SMP scaffold for unidirectional sustained release of MK2i. Fig.21 B. Reservoir layers with higher integrity (cross-link density) release MK2i (100 μM loading) at a more sustained rate compared to reservoir layers with lower integrity.
[0041] Fig. 22 A scheme for vascular access establishment is shown. DETAILED DESCRIPTION
[0042] Details of one or more embodiments of the subject matter of the present disclosure are set forth in this document. Modifications to the embodiments described in this document and other embodiments will be apparent to one of ordinary skill in the art after studying the information provided in this document. The information provided in this document and in particular the specific details of the exemplary embodiments are provided primarily for clear understanding and should not be construed as containing unnecessary limitations. In the event of a conflict, the present document, including definitions, shall prevail.
[0043] The subject matter of the present disclosure includes compounds and methods for treating vascular disorders. In some embodiments, the compounds of the present disclosure include novel allyl-functionalized shape memory polymers (SMPs) that can be cross-linked via side chain allyl groups. In some embodiments, the materials of the present disclosure (e.g., vascular grafts) include SMPs, and in certain embodiments include thermally responsive SMPs that are activated at physiological temperatures (e.g., about 37° C.) or near physiological temperatures. The materials and grafts of the present disclosure are advantageous because they can have relatively high elastic recovery, are easy to manufacture and program, are low in cost, are compatible with the vascular system, are adjustable and / or biodegradable. Therefore, embodiments of the materials of the present disclosure that possess some or all of these features are advantageous for manufacturing simple and minimally invasive implantable devices for various biomedical applications.
[0044] In this regard, the subject matter of the present disclosure includes compounds that can form SMP materials. In some embodiments, the compound comprises an allyl functionalized and cross-linkable first monomer and a non-cross-linkable second monomer. In a specific embodiment, the first monomer is photo-cross-linkable. The method for preparing the compound of the present disclosure is not particularly limited, and in some embodiments, the compound is prepared via a process including ring-opening polymerization.
[0045] Hemodialysis is a major lifeline for patients with end-stage renal disease (ESRD), but arteriovenous graft (AVG) failure results in significant morbidity, mortality, and economic burden. Stenosis at the venous anastomosis ultimately leads to impaired blood flow, requiring vascular intervention. Failure rates of 50% after 1 year and 75% after 2 years have been reported in hemodialysis patients using polytetrafluoroethylene (PTFE) dialysis grafts.
[0046] AVG failure remains an unmet clinical need. External mesh supports used in other settings (e.g., saphenous vein grafts in the heart or peripheral bypass grafting) have been shown to inhibit neointimal formation. These materials have limited success in the hemodialysis setting due to the geometric complexity of the venous anastomosis and complications such as infection and suture dehiscence. Embodiments of the present invention include a mechanically compliant, moldable external support that can be custom-fitted around each dialysis graft anastomosis without the need for suturing to prevent neointimal formation. The device of the present invention provides local sustained delivery of a therapeutic agent with anti-neointimal effects to further eliminate neointimal formation.
[0047] Improvements in AVG failure would significantly impact clinical outcomes and economic impact in hemodialysis patients. This proposal provides a unique platform to improve adventitial drug delivery methods and, if successful, could lead to therapeutic solutions in other clinical settings such as coronary and peripheral bypass grafting.
[0048] Arteriovenous graft (AVG) failures cause considerable morbidity, mortality, and economic burden in patients with end-stage renal disease (ESRD) undergoing hemodialysis. Stenosis at the venous anastomosis leads to impaired blood flow, requiring repeated vascular interventions. AVG failure occurs at the venous anastomosis 90% of the time. In hemodialysis patients with polytetrafluoroethylene (PTFE) AVGs, failure rates of 50% after 1 year and 75% after 2 years have been reported.
[0049] There are no available treatments that effectively prevent AVG failure. Several approaches to local treatment of venous anastomoses initially showed promise only to fail clinically due to adverse complications (e.g., infection, suture dehiscence) or lack of patency benefit. The approach closest to market, sirolimus-eluting collagen membrane (Coll-R TM), are susceptible to infection due to the immunosuppressant activity of sirolimus and the long operative time required for suturing.
[0050] Embodiments of the present invention are custom-fit external supports that do not require suturing, and in further embodiments, can elute therapeutic agents such as anti-neointimal pleiotropic peptides. The support can be custom-fit around the venous anastomosis to prevent neointimal formation and associated AVG failure via promoting outward remodeling rather than inward remodeling and local sustained delivery of therapeutic agents (Figure 1).
[0051] In 2011, kidney disease was the ninth leading cause of death in the United States. An estimated 31 million people have chronic kidney disease and 615,899 people have kidney failure (end-stage renal disease: ESRD). ESRD patients require a transplant or dialysis to survive. In 2012, an estimated 408,711 people were on hemodialysis, an increase of about 12,632 people per year since 2000.
[0052] PTFE AVGs are a common form of hemodialysis vascular access, but have a failure rate of approximately 50% after 1 year and 75% after 2 years, primarily due to neointima formation. Once an AVG fails, either an interventional technique (i.e., balloon angioplasty + / - stent) or a re-entry procedure is required. The cost of treating patients with graft failure is even more expensive, at approximately $87,895 per patient-year, with direct costs exceeding $4.8 billion and growing annually.
[0053] The main cause of failure is neointimal formation at the venous anastomosis, which is triggered by the venous response to surgical injury caused by PTFE implantation, arterial flow and other factors. These events lead to inflammation, accompanied by phenotypic regulation, migration and proliferation of vascular smooth muscle cells (VSMCs); and subsequent deposition of excess matrix to form the neointima.
[0054] Systemic pharmacological approaches have shown little efficacy in preventing venous collapse, suggesting the need for more local approaches. Past attempts have involved treatments from the outer adventitia layer and include: i) gel foams loaded with allogeneic endothelial cells (Vascugel TM , Shire Pharmaceuticals), which was subsequently discontinued due to lack of open-label benefit; ii) a collagen collar loaded with an adenoviral vector containing the vascular endothelial growth factor D gene (Trinam TM , Ark Therapeutics Group), whose Phase III clinical trial was terminated for "strategic reasons"; and iii) paclitaxel-eluting ethylene vinyl acetate coating (Vascular Wrap TM, Angiotech Pharmaceuticals) 6 , whose Phase III clinical trial was terminated due to a high infection rate in the paclitaxel treatment group.
[0055] As the method closest to the market, sirolimus eluted collagen membrane (Coll-R TM , vascular therapy) showed safety and technical feasibility in a phase I / II clinical trial. However, the trial was conducted with only 12 patients, which is not representative of the hemodialysis population (all Caucasians, only one diabetic patient, and no common comorbidities such as coronary or peripheral artery disease) and lacked a control group. In addition, a precise suturing process is required to cover the venous anastomosis, which not only increases surgical time and cost, but also increases the risk of suture dehiscence, patient discomfort and infection, especially for a more representative population. The immunosuppressant sirolimus may also increase the risk of these adverse complications.
[0056] To address this long-felt need, embodiments of the present invention include a sutureless, custom-fit outer support that optionally elutes multi-potent, non-immunosuppressive anti-neointimal peptides. For patients who rely on hemodialysis, coronary artery bypass graft (CABG), peripheral bypass graft (PVBG), or other arteriovenous shunts for survival, combining new shape memory polymers (SMPs) with promising peptides should ultimately reduce neointimal formation, re-operations, or other adverse events.
[0057] Therefore, embodiments of the present invention include a new type of poly(ε-caprolactone) (PCL)-based SMP, PCL-co-(α-allyl carboxylate ε-caprolactone) (x% PCL-y% ACPCL) [x% and y%: molar percentages] to fully meet the design criteria established for extra-stenting of hemodialysis grafts.
[0058] Previously studied polymers and shape memory alloys have shown promising anti-intimal hyperplasia effects in vein grafts in various CABG and PVBG preclinical models, but are difficult to apply to the various geometrically complex anastomoses encountered clinically and require suturing.
[0059] Thermally responsive SMPs solve this problem. SMPs can be heated above their shape transition temperature (T) (e.g., melting temperature T m ) to recover from a different temporary shape to its original permanent shape. Heating the SMP beyond its T during hemodialysis access surgery m , enabling the easy molding of external supports around geometrically complex anastomoses without sutures or large incisions, thereby reducing surgical time and the associated risk of infection while completely avoiding the risk of suture dehiscence.
[0060] One aspect of the invention is an implantable vascular graft. Embodiments include a graft having at least one cross-linked polymer, wherein the polymer comprises a first monomer that is cross-linkable and a second monomer that is not cross-linkable. The graft is capable of transitioning between an original shape and an implanted shape.
[0061] Another aspect of the present invention is an implantable tissue support device in the form of a biodegradable polymer scaffold that surrounds tissue, wherein the polymer scaffold comprises at least one cross-linked polymer, wherein the polymer comprises at least one cross-linkable monomer and / or at least one shape memory polymer; wherein the device is capable of transforming between an original shape and an implanted shape; and wherein the device is mechanically compliant at about 20 to about 50°C.
[0062] In embodiments of the foregoing aspects of the invention, the first monomer is allyl functionalized and comprises an allyl carboxylate group. In addition, the first monomer, the second monomer, or both are esters. In other embodiments, the first monomer, the second monomer, or both comprise ε-caprolactone (CL). In addition, the plurality of cross-linked polymers may comprise poly(ε-caprolactone)-co-(α-allyl carboxylate ε-caprolactone) polymers. In other embodiments, the plurality of cross-linked polymers may comprise about 1 mol % to about 30 mol % of the first monomer. In other embodiments, the plurality of cross-linked polymers comprise a shape transition temperature of about 20° C. to about 50° C.
[0063] Embodiments of the present invention may be configured to transform from the original shape to the graft shape when heated to a shape transition temperature exceeding the plurality of cross-linked polymers. The original shape may be a compressed form of the graft shape. The original shape may be a linear, sheet-like, tubular shape, a shape corresponding to a blood vessel, a vascular patch, a vascular bypass graft, a vascular stent, and a combination thereof. The graft shape may be a shape corresponding to a blood vessel, a vascular patch, a vascular bypass graft, a vascular stent, and a combination thereof.
[0064] Embodiments of the present invention may optionally further comprise a bioactive agent. The bioactive agent may be at least one of the following: a pleiotropic agent, a growth factor, a peptide, a nucleic acid, a pharmacological agent, an MK2 inhibitor, an antiproliferative agent, an anti-migratory agent, an anti-inflammatory agent, or an anti-fibrotic agent. The bioactive agent may also be at least one of the following: rapamycin, tacrolimus, paclitaxel, marimastat, dexamethasone, pioglitazone, AZX, or cilostazol.
[0065] Embodiments of the present invention may have a shape fixity of 50-100% and / or a shape recovery of 50-100%.The Young's modulus at 37°C may be about 0.05-200 MPa.
[0066] As described above, embodiments of the present invention surround tissue. In preferred embodiments, the tissue may be a vein or an artery. Furthermore, the embodiments may be external to the vein or artery. Preferably, the embodiments may be external to a vascular graft anastomosis.
[0067] Once implanted, embodiments of the present invention may form a seamless and sutureless sheath. The sheath is a mesh or netting. Additionally, once implanted, embodiments of the present invention preferably have an elastic radial behavior in a manner that mimics the compliant nature of the tissue. They may deform to conform to the shape of the tissue by at least one of extending or bending along their length.
[0068] Embodiments of the present invention provide a unique ability to provide a custom fit for each anastomosis. This spatial control between the stent and the vein critically affects adventitial microvascularization and outward remodeling which can mitigate neointimal formation. It can also help minimize asymmetric wall thickening which leads to turbulent, irregular flow and subsequent thrombosis and proliferation, especially around anastomoses (see Fig.14 ).
[0069] Because the copolymerization of ε-caprolactone (CL) with the novel CL derivative α-allyl carboxylate-ε-caprolactone (ACCL) produced a T m and a library of polymers with unusual shape memory properties, making it possible to customize the fit at vascular access operating temperatures (e.g., 28-37°C). Given its shape memory capability at 37°C, the geometry of the outer support can be customized by the surgeon to fit asymmetric distal anastomoses with relative ease (see Fig. 22 ).
[0070] This unique copolymeric form also enables fine-tuning of thermomechanical properties, allowing for the fabrication of SMP scaffolds with mechanical properties that mimic those of arteries. This is important because the mismatch in compliance between veins and synthetic grafts or arteries is another factor involved in neointimal formation. For example, a 68% decrease in mechanical compliance from vessel to graft (equivalent to switching from artery to Dacron) resulted in a 40% increase in mean anastomotic stress along the suture line and subsequent neointimal formation in an end-to-side geometry ( Fig.16 The material properties of this SMP library are highly tunable, as the molar composition, molecular weight, and crosslink density can all be varied to provide a wide range of elastic moduli (1-100 MPa at 37°C) that are stiffer than arteries. Therefore, this SMP library provides a unique opportunity to generate mechanically compliant, custom-fit external supports.
[0071] Porosity is also critical for cultured adventitial microvascularization and can be controlled during scaffold fabrication.
[0072] Embodiments of the present invention may be slowly biodegradable (>1 year) and bioresorbable, ensuring that their mechanical properties are maintained until venous remodeling stabilizes, while ultimately being resorbed to avoid potential long-term complications.
[0073] As described above, embodiments of the present invention include the addition of anti-neointimal peptides. With their anti-fibrotic and anti-inflammatory properties ( Fig.17 ), peptide inhibitors of MK2 (MK2i) show promise as agents to prevent neointimal formation. MK2 is downstream of the TGFβ-p38 stress-activated protein kinase pathway, conferring specificity and limiting off-target toxicity.
[0074] MK2i has been shown to inhibit VSMC proliferation, migration, and, most importantly, synthetic phenotype regulation. Treatment of human saphenous vein (HSV) with MK2i in an ex vivo organ culture model resulted in a reduction in intimal thickening ( Fig.18 In an in vivo rat inferior vena cava interposition model, a single 20-min ex vivo MK2i treatment of vein grafts prior to implantation reduced wall thickness by 72% at 28 days ( Fig.19 These data suggest that MK2i is one of the most comprehensive therapeutic approaches to prevent the cascade of events that lead to neointima formation. Furthermore, external support may further abrogate neointima formation by prolonging its action ( Fig.19 ).
[0075] The ratio of the first monomer to the second monomer is not particularly limited either. In some embodiments, the compound comprises about 1 mol %, 5 mol %, 10 mol %, 15 mol %, 20 mol %, 25 mol %, 30 mol %, 35 mol %, 40 mol %, 45 mol % or 50 mol % of the first monomer. In other embodiments, the compound comprises about 1 mol % to about 50 mol % of the first monomer, about 1 mol % to about 30 mol % of the first monomer or about 1 mol % to about 15 mol % of the first monomer. In such an embodiment, the remainder of the polymer may include the second monomer.
[0076] In other embodiments, the first monomer, the second monomer, or both comprise an ester. As used herein, the term "ester" is represented by the formula R1OC(O)R2 or R1C(O)OR2, wherein R1 and R2 can be independently selected from, but not limited to, optionally substituted alkyl, alkenyl, alkynyl, etc. The term ester includes "polyesters" or compounds comprising two or more ester groups.
[0077] In some embodiments, the allyl functionalized first monomer comprises an allyl carboxylate group. In such embodiments, the monomer may comprise a carboxylate group that is subsequently functionalized with an allyl group, or the monomer may be functionalized with an allyl carboxylate group. The allyl carboxylate group described herein may be represented by the formula:
[0078]
[0079] In other embodiments, the first monomer, the second monomer, or both comprise ε-caprolactone (CL) and / or derivatives thereof. For example, the first monomer comprising ε-caprolactone may comprise an α-allyl carboxylate ε-caprolactone (ACCL) monomer. In some embodiments, the compound is based on polycaprolactone (PCL) because PCL has desirable properties for vascular applications, including biocompatibility, suitable biodegradation rates, and mechanical compliance. Therefore, in certain embodiments, the compound comprises poly(ε-caprolactone)-co-(α-allyl carboxylate ε-caprolactone) copolymer (PCL-ACPCL), and some embodiments of the compounds of the present disclosure may comprise the following formula: Wherein x and y are integers without particular limitation. Embodiments of the polymers disclosed herein may also be characterized as x% poly(ε-caprolactone)-co-y%(α-allyl carboxylate ε-caprolactone) (x% PCL-y% ACPCL), wherein x% and y% correspond to molar ratios and are not particularly limited.
[0080] In some embodiments, the compound is a block copolymer. A "block" copolymer refers to a structure comprising one or more sub-combinations of constituent units or monomeric units. In some embodiments, the constituent units are derived from one or more polymerizable monomers via an additional process. There is no limit to the number of blocks, and unless otherwise explicitly stated, in each block, the constituent units can be arranged in a configuration of pure random, alternating random, regular alternating, regular blocks, or random blocks.
[0081] As described above, the compounds of the present disclosure may include cross-linkable allyl functional monomers. The terms "cross-linkable", "cross-linked", etc. used herein refer to a portion of a polymer chain connected to a portion of the same polymer chain or a portion of another polymer chain by a chemical bond, wherein the chemical bond connects one or more atoms of one or more polymer chains. Exemplary chemical bonds that can form cross-links include covalent bonds and hydrogen bonds, as well as hydrophobic, hydrophilic, ionic or electrostatic interactions. In some cases, covalently cross-linked SMP materials exhibit excellent shape memory properties and thermal stability compared to SMP materials cross-linked by non-covalent bonds.
[0082] Crosslinking can be done naturally and artificially. For example, in some embodiments, the first monomer is photo-crosslinkable, wherein the term "photo-crosslinking" and the like are used herein to refer to crosslinks formed when exposed to electromagnetic radiation (e.g., visible light and / or ultraviolet radiation). In some embodiments, photo-crosslinks can be formed by exposure to ultraviolet light having a wavelength of about 100 nm to about 300 nm. The terms "crosslinking" and the like used herein may include the terms "photo-crosslinking" and the like.
[0083] In some embodiments, the allyl-functional monomer comprises a pendant allyl-containing group (eg, an allyl carboxylate group) that can be crosslinked. In some embodiments, the allyl-containing group can be photocrosslinked to another allyl-containing group of the same compound or another compound.
[0084] In some embodiments, the compounds of the present disclosure may further include a bioactive agent. The term "bioactive agent" is used herein to refer to a compound or entity that changes, promotes, accelerates, prolongs, inhibits, activates or otherwise affects the biological or chemical events of an individual (e.g., a person). The manner in which the bioactive agent is incorporated into the compound is not particularly limited. In some embodiments, the bioactive agent can be incorporated (e.g., mixed with it) into the compound. In some embodiments, the bioactive agent can be covalently bound to the allyl group containing the first monomer via thiol-ene click chemistry.
[0085] Exemplary biologically active agents may include, but are not limited to, anticancer substances, antibiotics, immunosuppressants, antiviral agents, enzyme inhibitors, neurotoxins, opioids, hypnotics, antihistamines, lubricants, sedatives, anticonvulsants, muscle relaxants, antispasmodics and muscle contractants (including channel blockers), growth factors, miotics and anticholinergics, antiparasitics, antiprotozoal agents and / or antifungal agents, modulators of cell-extracellular matrix interactions (including cell growth inhibitors and anti-adhesion molecules), vasodilators, inhibitors of DNA, RNA or protein synthesis, antihypertensives, analgesics, antipyretics, steroidal anti-inflammatory agents and nonsteroidal anti-inflammatory agents, antiangiogenic factors, angiogenic factors, antisecretory factors, anticoagulants and / or antithrombotic agents, local anesthetics, ophthalmic medications, prostaglandins, cellular response modifiers, cells, peptides (including polypeptides as used herein), viruses and vaccines.
[0086] In some embodiments, the compounds of the present disclosure are biocompatible. In fact, as shown by higher levels of long-term cell viability and healthy cell morphology, certain embodiments of the compounds of the present disclosure and transplants are more biocompatible with endothelial cells (EC) compared to 100% PCL. The term "biocompatible" used herein is intended to describe the properties of a material that does not usually cause undesirable or adverse side effects when administered in vivo. For example, a biocompatible material may not cause side effects such as significant inflammation and / or acute rejection. It should be recognized that "biocompatibility" is a relative term, and some side effects can be expected even for some biocompatible materials. In some embodiments, a biocompatible material does not cause irreversible side effects, and in some embodiments, if a material does not cause long-term side effects, the material is biocompatible. One test for determining a material is to measure whether a cell dies when exposed to a material in vitro. For example, a biocompatible compound or transplant can cause less than about 30%, 20%, 10% or 5% cell death.
[0087] Additionally or alternatively, some embodiments of the compounds of the present disclosure are biodegradable. As used herein, the term "biodegradable" describes the properties of a substance that degrades under physiological conditions to form a substance that can be metabolized or excreted without damaging an individual. In certain embodiments, the product can be metabolized or excreted without permanent damage to the individual. Biodegradable substances also include substances that decompose within the cell. Degradation can occur by hydrolysis, oxidation, enzymatic processes, phagocytosis, other processes and combinations thereof. The degradation rate of a substance can vary and may be a few hours, days, weeks, months or years, depending on the material.
[0088] Embodiments of the disclosed compounds may further include additional functional groups and / or monomers to impart desired properties to the compounds. Adding functional groups or monomers to the compounds may impart desired functionality to the compounds and / or affect the melting temperature of the compounds. Therefore, certain functional groups or monomers may be incorporated into the compounds to adjust the thermomechanical properties of the compounds.
[0089] The subject matter of the present disclosure also includes shape memory polymer (SMP) materials comprising any of the compounds of the present disclosure. In some cases, the materials are used to form a graft, such as a vascular graft for a blood vessel (e.g., a vein, an artery). Exemplary vascular grafts can include a plurality of cross-linked polymers, the polymers including an allyl-functionalized and cross-linkable first monomer and a non-cross-linkable second monomer, and the graft is capable of switching between a temporary shape and an original shape.
[0090] The term "implanted shape" refers to a shape given to a material by applying a force on the material and / or exposing the material to a temperature (i.e., a programming step). Although the material can maintain its temporary shape for any length of time, the shape is called temporary because the shape only exists when an external force is applied to the material. In addition, as described below, in some embodiments, the material may lose its temporary shape when exposed to a temperature exceeding the melting temperature of the material.
[0091] The term "original shape" refers to the shape of the material when the polymers of the material are in their natural, pre-implantation, unstrained state. Once the material is in its original shape, the material will generally maintain the original shape unless an external force, etc. is applied to the material. Some embodiments of the material, when exposed to a temperature exceeding the melting temperature of the material in a physically stress-free state (i.e., a recovery step), recover and / or maintain the original shape. The crosslinks (chemical or physical in nature) between the multiple polymers that make up the material help prevent irreversible plastic deformation during the programming and recovery steps.
[0092] There is no particular limitation on what shape the temporary shape or original shape of the material can take. In some embodiments, the temporary shape is selected from a linear, sheet-like, tubular shape and a shape corresponding to a blood vessel, a vascular patch, a vascular bypass graft, a vascular stent, and a combination thereof. Similarly, in some embodiments, the original shape can be selected from a linear, sheet-like, tubular shape and a shape corresponding to a blood vessel, a vascular patch, a vascular bypass graft, a vascular stent, and a combination thereof. As discussed further below, certain shapes may be advantageous for certain therapeutic uses of the materials disclosed herein.
[0093] Therefore, the embodiments of the material of the present disclosure can be classified as thermomechanical SMP, whereby, when transitioning at a melting temperature exceeding and / or below the compound, the polymer can present a transition from a temporary shape to an original shape. For example, the material may initially have an original shape, and a temporary shape may be caused by heating the material to a temperature exceeding its melting temperature while applying to the material a force that molds or bends the material into a desired temporary shape. If the material is subsequently cooled to a temperature below the melting point of the material while the material is maintained in the temporary shape, the material can maintain its temporary shape, and as long as the material is maintained at a temperature below the melting temperature of the material, the material can substantially maintain the temporary shape. Subsequently, by heating the material to a temperature above its melting temperature, the material can be restored to its original shape.
[0094] The compounds of the present disclosure and materials comprising the compounds of the present disclosure may include a wide range of melting temperatures. In some embodiments, the compounds and materials comprising the compounds include a melting temperature of about 20°C to about 50°C, including melting temperatures of about 20°C, 25°C, 30°C, 35°C, 40°C, 45°C and 50°C. In some embodiments, the compounds and materials include a melting temperature at or substantially close to physiological temperature (e.g., about 37°C) so that when implanted in an individual, the material can undergo a switch-like shape transition. The materials of the present disclosure may also include higher elastic recovery. In some embodiments, the materials of the present disclosure include a strain recovery rate (R) of 90% or more. r ) and / or strain fixation ratio (R f ), and in some embodiments, R r and R f Can be about 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or more independently. The materials of the present disclosure can also have properties that make them similar to blood vessels and therefore suitable for use in conjunction with blood vessels and / or as blood vessel substitutes. For example, some embodiments of the material have compliance and ductility suitable for use with vascular systems. Some embodiments can also include an elastic modulus of about 1.0 to about 200.0 MPa at 37°C, which can be suitable for certain vascular applications.
[0095] The shape memory properties of the material of the present disclosure can be adjusted by modifying the compound of the present disclosure. The melting temperature and other properties of the material can be changed by modifying the compound in a manner that affects the allyl groups of the allyl functionalized first monomer. Not subject to the constraints of theory or mechanism, this is due to the fact that the allyl group of the compound can affect the crystallinity and grid point spacing of the compound and any material comprising the compound. Therefore, the molar concentration of the first monomer and / or the concentration and arrangement of the allyl groups on the first monomer can provide effective means for adjusting the thermomechanical, shape memory and biological functions of the material of the present disclosure. In some cases, the properties of the material of certain embodiments can be further adjusted by changing the molecular weight or gel content of the material.
[0096] Therefore, the compounds and materials disclosed herein have excellent and unexpected advantages, i.e., have adjustable properties, and can be adjusted to have physiologically relevant melting temperatures in some cases. The method for adjusting the properties of the compounds and materials includes but is not limited to changing the molar concentration of the allyl functionalized first monomer in the polymer, changing the concentration of the allyl groups in the allyl functionalized first monomer, and changing the size and molecular weight of the first monomer, the second monomer, or other monomers in the polymer, or a combination thereof. Can be adjusted to imitate a series of soft tissues in certain embodiments.
[0097] The subject matter of the present disclosure further includes methods for treating vascular conditions. In some embodiments, the methods include administering to an individual in need thereof a vascular graft in a temporary shape, the graft comprising a plurality of cross-linked polymers comprising an allyl-functionalized, cross-linkable first monomer and a non-cross-linkable second monomer. The methods of the embodiments further include the step of allowing the vascular graft to transform from the temporary shape to an original shape. The transformation from the temporary shape to the original shape can be initiated by heating the graft to a temperature exceeding the melting point of the plurality of polymers, and in some embodiments, the heating is passively accomplished by heat emanating from the individual.
[0098] The step of applying the graft may include coupling the graft to a vessel of interest. As used herein, the term "coupling" and the like refer to connecting the graft to a vessel by any means. In some cases, coupling refers to wrapping a sheet graft around a vessel. In other cases, coupling refers to suturing a linear graft to a vessel. In still other cases, coupling may refer to inserting the graft into a vessel through an opening in a tubular graft. Thus, the term "coupling" broadly refers to a variety of methods of configuring a graft relative to a vessel or other therapeutic target.
[0099] The term "treatment" or "treatment" refers to the medical management of an individual with the intention of curing, alleviating, stabilizing or preventing a disease, pathological condition. The term "condition" includes diseases, disorders, etc. "Treatment" includes active treatment, i.e., treatment specifically aimed at improving a condition, and also includes etiological treatment, i.e., treatment aimed at removing the cause of the relevant disease, pathological condition or disorder. In addition, the term includes palliative treatment, i.e., treatment used to relieve symptoms rather than cure the disease, pathological condition or disorder; preventive treatment, i.e., treatment used to minimize or partially or completely inhibit the formation of the relevant disease, pathological condition or disorder; and supportive treatment, i.e., treatment used to supplement other specific therapies for improving the relevant disease, pathological condition or disorder.
[0100] In addition, the term "subject" or "subject in need thereof" refers to a target of administration, which optionally shows symptoms associated with a specific disease, pathological condition, disorder, etc. The subject of the methods disclosed herein can be a vertebrate, such as a mammal, fish, bird, reptile, or amphibian. Therefore, the subject of the methods disclosed herein can be a human, non-human primate, horse, pig, rabbit, dog, sheep, goat, cow, cat, guinea pig, or rodent. The term does not indicate a specific age or gender. Therefore, adult and newborn subjects, whether male or female, are included therein. A patient refers to an individual suffering from a disease or disorder. The term "subject" includes human and animal subjects.
[0101] Vascular disorders that can be treated by the grafts of the present disclosure include, but are not limited to, stroke, aneurysm, ischemic vessels, hemorrhage, occlusion, ruptured vessels, vulnerable vessels, stenosis, atherosclerosis, peripheral arterial disease, arteriovenous fistula, or a combination thereof. A person of ordinary skill in the art will appreciate other vascular disorders and non-vascular disorders that can be treated with the materials of the present disclosure upon reading this application.
[0102] The implant may be implanted in its temporary shape or in its original shape. Where the implant is implanted in a temporary shape, embodiments of the method of treatment may further comprise the step of cooling the implant in the temporary shape to a temperature below the melting temperature prior to the step of applying.
[0103] The mechanical and thermal properties of the grafts disclosed herein can be adjusted within the system to more closely match the mechanical and thermal properties of natural blood vessels. In some embodiments, the grafts disclosed herein can include elasticity similar to that of natural arteries. This biomimetic can allow the grafts disclosed herein to achieve excellent results when compared to vein grafts or other synthetic grafts. For example, veins are not designed for and do not work well under the sinusoidal flow conditions that arteries typically experience, and do not contain a muscle layer similar to that of arteries. Therefore, vein grafts such as saphenous vein grafts can experience atherosclerosis, intimal hyperplasia, thrombosis, and restenosis. In addition, the process of grafting and treating veins can itself lead to ischemic damage to the veins. On the other hand, due to elasticity and other mechanical properties that mimic arteries, the grafts disclosed herein can be used as arterial grafts with fewer or no side effects that vein grafts typically experience.
[0104] In addition, surgical procedures (e.g., traditional bypass surgeries) for treating vascular conditions are typically highly invasive, which can prolong patient recovery time and hospital stays and limit treatment options for patients suffering from arterial occlusions. However, embodiments of the graft disclosed herein may include temporary shapes that facilitate surgery and make it less invasive. For example, in some embodiments, the graft can be programmed into a thin line-like temporary shape that allows administration via a small-caliber catheter and can allow the graft to be manipulated along the artery. Alternatively, an exemplary graft can be tunneled along the artery via a connection to a tunneling device. One of ordinary skill in the art will appreciate other temporary shapes and methods for administering the graft that can reduce the invasiveness of surgery for treating vascular conditions.
[0105] In specific embodiments, the graft can be used for bypass procedures. In some embodiments, the graft includes an original shape, which is a stent that generally takes the form of an elongated tubular. The graft can be coupled to the outside of a vein graft by wrapping or placing the graft around the vein graft. This configuration can improve the adaptability of the vein to the high pressure, high flow environment of the arterial circulation. In such an embodiment, the graft can include a temporary shape of a sheet, so that the graft is used to support the vein graft by coupling (i.e., wrapping) the sheet around the vein graft and then allowing the graft to transform into its original stent shape.
[0106] Some embodiments of the treatment methods disclosed herein also provide bypass surgery that does not require transecting a natural artery. For example, the graft may include a temporary shape of a linear (i.e., an elongated line) to facilitate insertion of the graft into an individual and manipulation of the graft along an artery. The graft may then be coupled to the artery by tying the graft to the artery with sutures, etc., and the graft may then be converted into its original vascular bypass graft shape. Subsequently, capillary ingrowth from the artery into an adjacent graft may be achieved, so that the occluded area portion of the adjacent artery may be regenerated and reperfused over time. In addition, in some embodiments, the graft may include and / or may be administered in combination with a bioactive agent (e.g., peptide, growth factor, etc.) that promotes angiogenesis.
[0107] Treatment may also refer to placing a graft in or on a blood vessel that has ruptured or is prone to rupture. The graft may then include the original shape of a vascular patch that seals and protects the rupture or potential rupture.
[0108] Thus, the compounds and grafts of the present disclosure provide several advantages for methods of treating vascular conditions. First, the graft can include an original shape that provides a custom fit graft that avoids flow-mediated thrombosis and hyperplasia. The ability to customize the original shape of the graft also makes it suitable for use in unusual vascular systems such as branching arteries, as well as for treating other non-vascular conditions. The ability to customize a temporary shape also allows the grafts of the present disclosure to be robust and easily placed surgically via minimally invasive techniques.
[0109] Once implanted, the grafts of the present disclosure can provide mechanical compliance to withstand vascular pulsations similar to arteries. In addition, embodiments of the grafts of the present disclosure can be biocompatible and optionally can exhibit sufficiently slow biodegradable properties to allow the vascular system to heal. The grafts of the present disclosure can also have porosity that promotes microvascular growth to repair damaged vascular tissue. Therefore, the grafts of the present disclosure can provide a treatment method that is easy to implement, cost-effective, and less invasive to an individual.
[0110] In addition, the subject matter of the present disclosure further includes a kit that can include materials comprising embodiments of the compounds of the present disclosure, the materials packaged together with a device for applying the materials. As will be appreciated by those of ordinary skill in the art, the appropriate application aid will depend on the temporary shape of the implant and / or the desired site of application.
[0111] Example
[0112] The presently disclosed subject matter is further illustrated by the following specific but non-limiting examples.The following examples may include data compilations representing data collected at various times during the development and experimentation process associated with the presently disclosed subject matter.
[0113] Example 1
[0114] This example describes the synthesis and characterization of an exemplary x% PCL-y% ACPCL copolymer library. To prepare the copolymer library, a novel α-carboxylic acid allyl ester ε-caprolactone (ACCL) monomer ( ) was first synthesized in a single reaction via lithium diisopropyl amine (LDA)-mediated carbanion formation at the α-carbon of ε-caprolactone (CL) and subsequent allyl chloroformate addition. Figure 1A). More specifically, in a 250 mL round-bottom flask, distilled CL (13.9 mL, 125 mmol) was added dropwise to LDA (125 mL of 2 M in THF / n-heptane / ethylbenzene, 250 mmol) in anhydrous THF (200 mL) at -78°C. After 1 hour, the temperature was raised to -30°C and allyl chloroformate (13.3 mL, 125 mmol) was added dropwise. After 30 minutes, the temperature was raised to 0°C and the reaction was quenched with saturated NH4Cl (30 mL). The crude ACCL was diluted with H2O (100 mL), extracted with ethyl acetate (300 mL×3), dried over Na2SO4, filtered, evaporated, and purified by column chromatography using Silica Gel Premium Rf (Sorbent Technologies, Norcross, GA) and 10% ethyl acetate in hexane. Yield: 58% (14.3 g, 72 mmol). 1 H-NMR confirmed the formation of the desired ACCL product, as evidenced by the characteristic allyl group (5.92 (G i )、5.31(H ii ) and 4.63(F ii )ppm) and CL peaks ( Figure 1B ).
[0115] The ring-opening (co)polymerization (ROP) of ACCL and CL using diethylzinc catalyst and 1,6-hexanediol initiator generated a library of novel x% PCL-y% ACPCL (x and y: molar ratio) copolymers, where y = 4.16-14.50%, which is due to the allylic CH protons (G i , δ = 5.92 ppm) and the CH2 protons (ε ii , δ=4.15ppm) ratio to determine ( Figure 1C and 1D , Table 1). To form these polymers, different molar ratios of dried ACCL and CL (100 mmol in total) were introduced into a pre-dried test tube containing 1,6-hexanediol (0.5 mmol). The polymerization mixture was degassed with two freeze-purge-freeze-thaw cycles, immersed in a 140°C oil bath, and catalyzed by dropwise addition of Zn(Et)2 (1 mmol, 15 wt% in toluene) for 1 hour. The solution was precipitated in cold diethyl ether and dried in vacuo.
[0116] As a control, 100% PCL (Table 1, M 257) was synthesized similarly by adding 2-isocyanatoethyl methacrylate (0.22 g, 1.42 mmol) to 100% PCL (1.0 g, 86.0 μMol) in anhydrous THF (20 mL) in a 100 mL round-bottom flask. n=11600Da, PDI=1.54). The reaction mixture was heated to 60°C and catalyzed with dibutyltin dilaurate (10 μL, 17 nmol) for 1 hour. The product was washed with 100% hexane and 90% hexane / 10% methanol and then dried in vacuo. 6.12 ) and 5.61ppm(I 5.61 The normalized methacrylate proton integrals of the peaks were summed and then divided by 3.66 ppm (I) from the terminal hydroxyl groups adjacent to the unmodified 100% PCL. 3.66,notfunc ) The normalized integral of CH2 protons was used to calculate the conversion of terminal hydroxyl groups to methacrylate or the degree of methacrylate esterification (D M PCL showed a 90.5% conversion rate of terminal hydroxyl groups to methacrylate (D M )(Figure 2).
[0117] Due to the lower reactivity of ACCL monomer, the obtained allyl compounds were lower than the ACCL:CL feed ratio (Table 1, Figure 1E ). Molecular weight (M n =12-19 kDa, polydispersity index (PDI) = 1.78-2.50) was controlled by the 1,6-hexanediol initiator:total monomer ratio, but was also affected by the feed ratio of the less reactive ACCL monomer. The higher PDI and lower yields (22.6-56.6%) obtained for these copolymers may be due to transesterification reactions involving the polyester backbone and the pendant carboxylic acid allyl esters. There was an inverse relationship between thermal properties and allyl composition, probably because ACPCL disrupted PCL crystallinity, thereby reducing T m and percentage crystallinity (X c )(Table 1).
[0118] Table 1. Characterization of x% PCL-y% ACPCL copolymers
[0119]
[0120]
[0121] a) y%ACCPCL is integrated from 5.90ppm (I 5.90 ) and 4.15ppm integral (I 4.15 ) ratio
[0122] Rate to determine: b)Molecular weight properties were determined by gel permeation chromatography using a Phenogel 10E3A column (Phenomenex Inc., Torrance, CA) in THF versus PMMA standards (Agilent Technologies, Inc., Santa Clara, CA). c) in Melting enthalpy of 100% crystalline PCL.
[0123] Example 2
[0124] This example describes the preparation and characterization of crosslinked x% PCL-y% ACPCL and 100% PCL-dimethacrylate SMP films using the polymers synthesized in Example 1. A subset of the x% PCL-y% ACPCL copolymers and a 100% PCL-dimethacrylate control were photocrosslinked to produce a shape memory effect and evaluated for gel content, thermal properties, mechanical properties, and shape memory properties. The films were photocured using a thin film coater (Precision Gage & Tool Co., Dayton, OH) and a Novacure 2100 Spot Curing System (Exfo Photonic Solutions, Inc., Mississauga, Ontario, Canada) at 365 nm radiation (4.89 J cm -2 , 18.1mW cm -2 ), cross-linked x% PCL-y% ACPCL and 100% PCL-dimethacrylate SMP films with uniform thickness (0.2-0.3 mm) were prepared from 10 wt% polymer solutions containing 3 wt% 2,2-dimethoxy-2-phenylacetophenone. After drying, the samples were incubated in DCM for 2 days to determine the gel content. Thermal properties were measured on a TA Instruments (New Castle, DE) Q1000 differential scanning calorimeter. Mechanical properties and shape memory properties were determined using a TA Instruments Q2000 dynamic mechanical analyzer in tensile mode.
[0125] Hope to prepare T m SMPs slightly above and below 37°C, as the surgical preference for the onset of shape recovery depends on the specific biomedical application. For use in a variety of vascular applications, it is also desirable that the SMP library exhibits tunable mechanical properties with adequate compliance and extensibility. In addition, in order to tightly control the shape memory behavior after shape programming and recovery and maintain the integrity and functionality of the implant, a complete and repeatable shape recovery with an on-off "switch-like" response to small temperature changes is sought. Gel content (X G) relates to the percentage crosslinking of the material, and in some SMP networks a minimum X of 10%-30% is required G To achieve shape memory effect. -2 , 18.1mW cm -2 ) after that, the x% PCL-y% ACPCL films had a x% PCL-y% ACPCL content of 72.0±17.3% compared to the 100% PCL-dimethacrylate control. G The average T of all materials except 85% PCL-15% ACPCL was 57.3±7.2% before cross-linking. m The crosslinking of the material resulted in a T value of y = 4.16-14.50% for the copolymer film due to the restricted mobility of the crosslinked polymer chains. m The reduced chain mobility also disrupts the post-melting chain arrangement, as shown by the percentage crystallinity (X c ) is shown by the decrease in T. m , X c , crystallization temperature (T c ) and crystallization enthalpy (ΔH C ), so except for T g In addition, the thermal properties are dependent on the molar composition of the cross-linked polymer ( Figure 3 ). The generated X c Similar to the branched PCL cross-linked films, it was shown that switchable shape recovery is possible for these SMPs. Cross-linking produced a library of SMPs with a transition temperature (T) close to 37 °C. m ) and X sufficient for full shape recovery and switchable behavior in physiological applications c .
[0126] Table 2. Gel content and thermal properties of cross-linked x% PCL-y% ACPCLSMP films
[0127]
[0128] a) Where m extracted is the mass after 2 days of incubation in dichloromethane and subsequent drying, while minitial is the initial mass; b) in Melting enthalpy of 100% crystalline PCL.
[0129] The mechanical properties of the SMP test films were evaluated isothermally at 37°C to determine suitability for vascular applications. Compared with 100% PCL-dimethacrylate (Table 3, for y = 4.16-14.50%): Tensile modulus at 37°C (E tn Compared with the cross-linked copolymer membranes with y% ACPCL, the elasticity is of the same order of magnitude or one order lower, which can be considered as the desired compliance for vascular applications. tn '(37°C), which more closely matches that of native arteries and is primarily a result of these materials partially or completely melting at 37°C. max The fracture strain ε of each test film is between 3.3 and 0.12 MPa, and most materials have good ductility at 37 °C. max More than 85%, but 85% PCL-15% ACPCL ε max These experiments demonstrate that the cross-linked SMP library has appropriate extensibility and compliance for vascular applications.
[0130] Table 3. Mechanical properties and shape memory properties of cross-linked SMP films
[0131]
[0132] a) The pressure was measured at 37 °C at 0.1 MPa min -1 The mechanical properties are determined by performing tensile tests with a stress ramp. b) Shape memory properties determined by stress-controlled thermomechanical cycling. Describes the relationship between the deformation to the maximum strain ε1(N) and the Nth cycle (ε p How well the shape is recovered compared to the beginning of (N-1)); c) It is defined that the programmed shape ε1(N) is maintained after stress unloading to obtain the temporary shape ε u (N) ability. f) 96% PCL-04% ACPCL test film (where X G =36.7±8.6%) with R r (1) = 99.9 ± 0.2, R r (N) = 99.8 ± 0.4% and R f (N) = 99.8 ± 0.1%.
[0133] Example 3
[0134] This example describes the preparation of SMP shapes for evaluating shape memory properties via stress-controlled thermomechanical cycling ( Figures 4A-4C ). End-capped polymer tubes (length 1.0-2.0 cm, ID 0.90 mm, OD 1.0-1.6 mm) were prepared by immersing polyvinyl alcohol (PVA) coated 0.90 mm O.D. glass capillaries into the polymer film prep solution and UV cross-linked as above. The capillary containing the tube was dried and immersed in deionized H2O and 100% ethanol, and the tube was then manually pulled out of the capillary. The tube was washed with H2O, dried, and sealed by immersing the open side of the tube into the polymer solution and UV cross-linked. A 2 mm PDMS mold containing the CAD designed guitar was prepared by first laser etching (Epilog Laser, Golden, CO), then pouring a 94% PCL-06% ACPCL polymer solution into the mold and UV cross-linking on a 48°C hot plate (365 nm, 26.1 J cm -2 , 290mW cm -2 ), to prepare a guitar shape containing 94% PCL-06% ACPCL.
[0135] Shape recovery after the first cycle R r (N), which indicates the quantitative ability of the material to recover its original shape (e.g., tubular shape), was over 98% for the tested films of each material composition, 85% PCL-15% ACPCL (R r (N) = 86.9 ± 4.7%) (Table 3). f ) represents the ability of a material to be fixed in a temporary shape (e.g., a thread-like shape), and was over 98% for the selected films for each material composition. Illustration of three consecutive thermomechanical cycles of 96% PCL-04% ACPCL and 89% PCL-11% ACPCL ( Figure 4B and 4C ) illustrates the repeatability of shape programming and recovery of these SMPs. The demonstration of shape memory further confirms the usefulness of the materials in biomedical applications ( Figures 5A-5F and Figures 9A-9C ), including the desired wire-to-tube transition for minimally invasive catheters or laparoscopic deployment in arterial bypass grafting at 37° C. Most copolymers possess excellent, tightly controllable shape memory capabilities.
[0136] Example 4
[0137] This example evaluates structure-function relationships to better elucidate material properties (T m , ΔH m , T c 、E tn ′(37℃),σ max , ε max , Rr (N), R f (N)) and physical and chemical properties (y%ACPCL, M n 、M w , PDI, X G ). Briefly, a 13 × 10 matrix was constructed containing the mean values ( Figure 6 ). Matrix values were normalized to their z-scores for easier comparison between variables, and covariance matrices were calculated and plotted using MATLAB (MathWorks Inc., Natick, MA).
[0138] Covariances (covs) closest to an absolute value of 1 indicate the strongest correlation between the variables, while positive and negative values indicate positive and negative correlations, respectively. tn ′(37℃) and σ max The close correlation with y%ACCPCL (cov = -0.80-0.94) indicates a dominant effect of molar composition on these properties. Without being bound by theory or mechanism, the dominance of molar composition on certain material properties can be explained by the fact that changing the allyl content simultaneously changes the crystallinity and grid point spacing of the crosslinked network. r (N) is also affected by the molar composition (cov = -0.60), however it is conceivable that programming parameters (e.g., cure and deformation temperature, stress or strain rate) can be adjusted to improve the R of higher y% ACPCL copolymers. r (N) M n With ε max There is a strong correlation (cov = 0.78), indicating that M n To improve the elongation of these SMPs. In addition, X G To increase R f (N)(cov=-0.54) and ΔH m (cov = -0.46). Thus, a variety of material properties are affected by molar composition, and many can be tuned via adjustment of other physicochemical properties to include PCL-ACPCLSMPs with certain thermal, mechanical, and shape memory properties.
[0139] Example 5
[0140] This example describes a vascular compatibility study used to evaluate the biocompatibility of the membranes. Human umbilical vein endothelial cells (HUVECs) were seeded on the polymer membranes and their viability was measured over the course of four days using the resazurin assay ( Figure 7To prevent cells from attaching to the tissue culture polystyrene (TCPS) underneath the test membrane, the wells were coated with a 1% agarose solution. The agarose-coated wells were dried, washed with 100% ethanol, UV sterilized, and washed with MesoEndo Endothelial Cell Growth Medium (Cell Applications, Inc., San Diego, CA). The ethanol-soaked, medium-soaked polymer disks (approximately 31 mm 2 , about 50 μM thick) were placed on the agarose-coated wells, and 5th generation red fluorescent protein-expressing HUVEC (P5 RFP-HUVEC) (470 cells mm -2 ) were inoculated directly on the membrane surface, TCPS (positive control) and 1% agarose (negative control). After 1.5 hours, 150 μL of culture medium was added.
[0141] Viability was assessed via the resazurin assay at 9, 35, and 91 hour time points. Briefly, resazurin (5 μM in MesoEndo) was added to each well, incubated for 4 hours at 37°C, and Supernatants were read on a M1000Pro plate reader (Tecan Group Ltd, San Jose, CA) at 560 / 590 nm excitation / emission. Live cell numbers were calculated based on a standard curve of RFP-HUVEC fluorescence on TCPS, and % cell viability was normalized to TCPS control. All samples were tested in biological quadruplicate assays.
[0142] It is known that 100% PCL (Sigma-Aldrich, M n =70-90 kDa) is biocompatible and was therefore selected as a control membrane. At 9 hours post-inoculation, there was no statistically significant difference in HUVEC viability on the experimental SMP membranes (60.0-65.2% relative to TCPS) compared to 100% PCL (59.4±4.9%). At later time points, HUVEC viability on all copolymer membranes (102.9-106.7% at 35 hours and 85.0-103.0% at 91 hours) was greater than that on 100% PCL (66.0±14.4% and 64.1±32.0%, respectively).
[0143] Additionally, cell morphology was assessed by seeding P5 human coronary artery endothelial cells (hCAEC) (Cell Applications, Inc., San Diego, CA) directly onto polymer disks. After 3 days of incubation on disks or TCPS controls, cells were fixed with 4% paraformaldehyde (15 minutes), permeabilized with 0.5% Triton X-100 (10 minutes), and blocked with 10% bovine serum albumin (30 minutes). Cells were then incubated with 2 μM Ethidium Homodimer-1 (10 minutes) and 50 μM Alexa Fluor 488 Phalloidin (Molecular Probes, Eugene, OR) (20 minutes) were incubated together. Cells on polymer surfaces were imaged on an LSM510META inverted confocal microscope (CarlZeiss, LLC, Thormwood, NY), while TCPS controls were imaged using a Nikon Eclipse Ti inverted fluorescence microscope (Nikon Instruments Inc. Melville, NY). Images were post-processed and analyzed using ImageJ software (NIH, Bethesda, MD). Confocal microscopy of hCAECs on all membranes after 3 days showed labeled cobblestone morphology ( Figures 8A-8E ). Therefore, SMPs are compatible with vascular ECs and may be endothelialized when used as arterial bypass grafts.
[0144] Example 6
[0145] This example describes an in vivo arterial bypass graft performed to evaluate the therapeutic activity of the compounds and grafts disclosed herein. The SMP tubular graft was used to provide a conduit for blood flow through the occluded area in an in vivo rat carotid artery ligation model. 89% PCL-11% ACPCL copolymer was selected as the tubular structure because it possesses shape memory properties (R f and R r >99%), close to the body's T m temperature (37.9°C) and high EC biocompatibility (103.0%) after 91 hours ( Figures 9A to 9C ).
[0146] Immediately before surgery, a capped SMP graft (ID 0.9 cm, OD 1.2 cm, length 1.5 cm) containing 89% PCL-11% ACPCL was UV sterilized and a collagen gel containing C16 and Ac-SDKP was prepared. Sprague Dawley rats were subjected to double ligation of the left common carotid artery as a model of complete blood arrest ( Fig. 10A). The experimental groups included "polymer + peptide", "peptide only" and "untreated" experimental groups. In the "polymer + peptide" group, an SMP tube with two closed ends was placed over the entire occluded area immediately after ligation, each tube end was tied to the native artery by suture, and the structure and artery were buried in collagen gel containing pro-angiogenic C16 and anti-inflammatory Ac-SDKP peptides by cotton swab application. In the "peptide only" group, only the peptide-containing collagen gel was applied immediately after ligation. No polymer or peptide was applied in the "untreated" group. All incisions were sutured closed using non-degradable sutures. Rats were given buprenorphine 0.05mg / kg SQ every 8-12 hours as needed for pain and monitored for two weeks.
[0147] Two weeks after implantation, 0.1 μM diameter Fluorescent microangiography was performed using carboxylate-modified red fluorescent microspheres (Life Technologies Corp., Carlsbad, CA) to assess the area of capillary growth and blood perfusion. The beads were observed using an LSM 510META inverted confocal microscope (Carl Zeiss, LLC, Thormwood, NY) within a 3-hour perfusion event. Rat tissues around the polymer-artery interface were embedded in optical cutting temperature (OCT), frozen at -80°C for 24 hours, and sectioned using a cryostat (5 μM sections).
[0148] To identify vascular cells around the polymer-artery interface, cryosections were stained with mouse anti-rat phycoerythrin (PE)-conjugated CD31 antibody (clone TLD-3A12, BD Biosciences) as an endothelial and leukocyte cell marker, followed by counterstaining with Hoechst 33258 nuclear stain (Life Technologies, Inc.). Images of IF-stained OCT sections were captured using a Nikon Eclipse Ti inverted fluorescence microscope (Nikon Instruments Inc. Melville, NY).
[0149] After 2 weeks, the extremely strong fluorescence signal from the fluorescent beads detected by fluorescent microangiography in the “polymer+peptide” group ( Fig.11A ) showed that blood flowed through the tubular structure. Fig. 11B and Fig. 11C ) showed almost no visible fluorescence, indicating almost complete occlusion in the absence of this combined treatment. Observation of the purple / pink microvascular network from H&E staining ( Fig. 12A and Fig. 12B ) and CD31 in the “polymer+peptide” group + Fluorescence of vascular cells ( Fig.13 ) illustrates the anastomosis between a polymer tube and a native artery interconnected via capillaries.
[0150] Example 7
[0151] This example demonstrates the characteristics of an embodiment of the present invention.
[0152] One embodiment of the present invention is a composition of x% PCL-y% ACPCL (y=10-15%) that is cross-linked to achieve custom fit capabilities, modulation of healthy VSMC phenotype, and surface coating-mediated sustained unidirectional MK2i delivery.
[0153] This embodiment includes SMPs having at least one of the following (in any combination): high shape fixity and shape recovery (>95%) (see Fig.15 ) to ensure effective coating of the external support; melting temperature <37℃( Fig.15 ), enabling shape molding at approximately body temperature; tensile modulus E of 1-100 MPa at 37°C tn '(37℃), thereby providing mechanical support for the healthy adaptation of the vein graft in the arterial circulation while eliminating any adverse effects caused by the compliance mismatch between the graft and the vein; high porosity (>50%) with a diameter of approximately 750μM ( Fig. 20 ), thereby promoting neoadventitia growth and extension beyond the outside of the stent for efficient nutrient and oxygen transport; slow degradation (at least several months) to maintain adequate mechanical support during the critical adaptation period from venous to arterial circulation; heparin coating ("reservoir") to achieve unidirectional sustained release of MK2i. Positively charged MK2i can be loaded into heparin-containing hydrogels in a manner similar to other heparin-binding peptides and released based on heparin concentration; and a desired MK2i release profile (50 μg MK2i / day) to achieve 100 μM / day in 28 days at a volume equivalent to a typical venous anastomosis. Heparin concentration controls the density of anionic charges and the porosity of the heparin layer, providing a variable "release window" for drugs such as cationic MK2i. MK2i concentration can also be controlled to change the release amount and kinetics.
[0154] Example 8
[0155] This embodiment shows the custom-fitting process of the SMP of the present invention. The present invention has excellent shape memory at body temperature. Examples of the SMP outer stent of the present invention may include 5 different x% PCL-y% ACPCL copolymers (y = 10%, 11%, 12%, 13%, 14% and 15%, with a melting temperature of 28-37°C). First, the stent can be made to have an 8mm diameter to fit loosely around a typical human saphenous vein (HSV) (about 2mm intervals to allow new adventitia growth), with a 0.5mm thickness to allow significant deformability, with a 3.1cm long arm and a 1cm side arm to fully cover the vein anastomosis. Similar to other external meshes, large pores with a diameter of 750μM and a porosity of> 50% can be made to prevent ischemia and promote adventitia growth and outward remodeling.
[0156] The present invention includes an SMP outer mesh having a melting temperature within the vascular access operating temperature range (28-37°C) and containing macropores: the positive mold can be 3D printed ( Fig. 20 ab) and assembled, and then embedded with polydimethylsiloxane (PDMS) to make a negative mold containing channels (pore generators) ( Fig. 20 cd). The PDMS mold can then be placed in the glass mold ( Fig. 20 d). The space between the PDMS and the glass negative mold can then be filled with a polymer solution [25 (wt / vol)% of x% PCL-y% ACPCL (y=10%, 11%, 12%, 13%, 14, and 15%) in dichloromethane, 1 (wt / vol)% of 2,2-dimethoxy-2-phenylacetophenone] and UV crosslinked (4.89 J / cm 2 , 18.1mW / cm 2 ) 4 The PDMS was then mechanically cut to retain the SMP scaffold ( Fig. 20 e). These molds can be adjusted to y-shaped forms ( Fig. 20 f).
[0157] Heparin coating can be achieved by first forming a thin layer of poly(3,4-dihydroxy-1-phenylalanine) (poly(DOPA)) on the luminal surface of the SMP. The amine groups of heparin can then be covalently conjugated to the poly(DOPA) ( Fig.21 a). The cavity surface of the SMP support can be immersed in Tris (pH 8.5) and ethanol (V tris :V 乙醇=7:3) and I-DOPA mixture for 12 hours. The DOPA coated surface can then be immersed in a heparin solution (pH 7.4) with different concentrations (1, 10 and 50 g / L) for 24 hours. Then AlexaFluor568 conjugated MK2i (10, 100 or 1000 μM in 100 μL PBS) can be incubated with the heparin coated stent sample at 37°C for 2 hours. Then, fresh PBS is added at each time point (0.25, 0.5, 1, 2, 4, 8, 12 and 24 hours, then every day and for 28 days) to mimic the in vivo "infinite sedimentation" state, as we have shown previously. The collected supernatant can be read on a plate reader (excitation / emission 578 / 603nm) and compared with controls without SMP / heparin loading and drug-AlexaFluor568 only to derive a standard curve.
[0158] MK2i doses within this range should allow 50 μg / day of MK2i to be released over 28 days to reach 100 μM / day, which is an effective dose for preventing neointimal hyperplasia in vein grafts equivalent in volume to a typical antecubital vein (3 mm diameter, 230 microns thickness). Although vein wall thickening persists beyond 12 weeks into arterial exposure, a 2-4 week sustained release profile of MK2i may be ideal, as the majority of VSMC proliferation and migration occurs within this window, and MK2i inhibits VSMC action through its antiproliferative potency.
[0159] As expected ( Fig.21 b), the most complete reservoir layer (highest cross-linking with the smallest mesh size) produces the most sustained release, while the most incomplete stent (largest mesh size) exhibits the most sudden release. The data suggest that when neointimal formation is accelerated most rapidly due to VSMC proliferation and migration, the integrity of the reservoir layer can be altered to achieve a sustained release profile over a critical 2-4 week period. However, because accelerated in vivo degradation of the reservoir material used (gelatin gel) is expected, an anionic heparin coating can be used instead of the cationic MK2i.
[0160] Without being bound by theory or mechanism, capillary formation is due to the pro-angiogenic, anti-inflammatory activity of the C16 and Ac-SDKP peptides distributed throughout the polymer-artery interface, thereby providing a means for blood to be transferred to the polymer structure and back to the native artery via a pressure gradient generated in the direction of blood stasis. Therefore, a tubular structure connected to the native vascular system via a capillary connection can provide an additional conduit for occluded arteries and can eliminate the need for arterial transection during arterial bypass grafting.
[0161] It should be understood that various details of the subject matter of the present disclosure may be changed without departing from the scope of the subject matter disclosed herein.In addition, the description provided herein is for illustrative purposes only and not for limiting purposes.
[0162] While the terms used herein are believed to be well understood by one of ordinary skill in the art, the definitions set forth herein are provided to facilitate explanation of the subject matter of the present disclosure.
[0163] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the subject matter of the present disclosure belongs. Although any methods, devices, and materials similar or equivalent to those described herein can be used in the practice or testing of the subject matter of the present disclosure, representative methods, devices, and materials are now described.
[0164] The terms “comprising,” “including,” and “having” are intended to be inclusive and mean that there may be additional elements other than the listed elements.
[0165] In accordance with long-standing patent law convention, the English terms "a," "an," and "the" are used in this application to mean "one or more." Thus, for example, reference to "a polymer" includes a plurality of such polymers, and so on.
[0166] Unless otherwise indicated, all numbers expressing quantities of ingredients, properties (e.g., reaction conditions), and so forth used in the specification and claims are to be understood as being modified in all instances by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth in the specification and claims are approximations that may vary depending upon the desired properties sought to be obtained by the presently disclosed subject matter.
[0167] As used herein, the term "about" when referring to a value or amount of mass, weight, time, volume, concentration, or percentage means that in some embodiments, ±50% variations are encompassed, in some embodiments, ±40% variations are encompassed, in some embodiments, ±30% variations are encompassed, in some embodiments, ±20% variations are encompassed, in some embodiments, ±10% variations are encompassed, in some embodiments, ±5% variations are encompassed, in some embodiments, ±1% variations are encompassed, in some embodiments, ±0.5% variations are encompassed, and in some embodiments, ±0.1% variations are encompassed, as these variations are suitable for performing the disclosed methods.
[0168] As used herein, ranges can be expressed as from "about" one particular value and / or to "about" another particular value. It should also be understood that a number of numerical values are disclosed herein, and that each value is also disclosed herein as "about" a particular value in addition to the value itself. For example, if the value "10" is disclosed, then "about 10" is also disclosed. It should also be understood that each unit between two particular units is also disclosed. For example, if 10 and 15 are disclosed, then 11, 12, 13, and 14 are also disclosed.
[0169] Throughout this document, references are cited. All of these references are incorporated herein by reference.
[0170] References
[0171] 1.A.Lendlein,S.Kelch,Angewandte Chemie International Edition 2002,41,2034.
[0172] 2.W.Small,P.Singhal,TSWilson,DJMaitland,Journal of materialschemistry 2010,20,3356.
[0173] 3.A.Lendlein,M.Behl,B.Hiebl,C.Wischke,Expert review of medical devices 2010,7,357.
[0174] 4.MCSerrano,GAAmeer,Macromolecular bioscience 2012,12,1171.
[0175] 5.C.Liu,H.Qin,PTMather,Journal of materials chemistry 2007,17,1558.
[0176] 6.A.Lendlein,S.Kelch,Angew Chem Int Ed Engl 2002,41,2035.
[0177] 7.M.Behl,A.Lendlein,Materials Today 2007,10,20.
[0178] 8.J.Leng,X.Lan,Y.Liu,S.Du,Progress in Materials Science 2011,56,1077.
[0179] 9.I.A.Rousseau,Polymer Engineering&Science 2008,48,2075.
[0180] 10.A.Lendlein,R.Langer,Science 2002,296,1673.
[0181] 11.M.Ebara,K.Uto,N.Idota,J.M.Hoffman,T.Aoyagi,Advanced Materials2012,24,273.
[0182] 12.A.Garle,S.Kong,U.Ojha,B.M.Budhlall,ACS applied materials&interfaces 2012.
[0183] 13.M.Uygun,M.A.Tasdelen,Y.Yagci,Macromolecular Chemistry and Physics2010,211,103.
[0184] 14.X.Xu,K.A.Davis,P.Yang,X.Gu,J.H.Henderson,P.T.Mather,MacromolecularSymposia 2011,309-310,162.
[0185] 15.X.Wang,T.C.Boire,C.Bronikowski,A.L.Zachman,S.W.Crowder,H.-J.Sung,Tissue Engineering Part B:Reviews 2012,18,396.
[0186] 16.M.A.Woodruff,D.W.Hutmacher,Progress in Polymer Science 2010,35,1217.
[0187] 17.H.Jeong,B.Kim,Y.Choi,Polymer 2000,41,1849.
[0188] 18.M.A.Woodruff,D.W.Hutmacher,Progress in Polymer Science 2010,35,1217.
[0189] 19.D.L.Safranski,K.E.Smith,K.Gall,Polymer Reviews 2013,53,76.
[0190] 20.G.Mani,M.D.Feldman,D.Patel,C.Agrawal,Biomaterials 2007,28,1689.
[0191] 21.S.J.Head,J. R.L.J.Osnabrugge,T.M.Kieser,V.Falk,D.P.Taggart,J.D.Puskas,J.F.Gummert,A.P.Kappetein,European heart journal 2013,34,2873.
[0192] 22.A.L.Zachman,S.W.Crowder,O.Ortiz,K.J.Zienkiewicz,C.M.Bronikowski,S.S.Yu,T.D.Giorgio,S.A.Guelcher,J.Kohn,H.-J.Sung,Tissue Engineering Part A2012,19,437.
[0193] 23.X.Hu,X.Chen,S.Liu,Q.Shi,X.Jing,Journal of Polymer Science Part A:Polymer Chemistry 2008,46,1852.
[0194] 24.A.Mahmud,X.-B.Xiong,A.Lavasanifar,Macromolecules 2006,39,9419.
[0195] 25.A.S.Karikari,W.F.Edwards,J.B.Mecham,T.E.Long,Biomacromolecules2005,6,2866.
[0196] 26.A.Lendlein,AMSchmidt,M.Schroeter,R.Langer,Journal of PolymerScience Part A:Polymer Chemistry 2005,43,1369.
[0197] 27.CGPitt,FIChasalow,YMHibionada,DMKlimas,A.Schindler,Journalof applied polymer science 1981,26,3779.
[0198] 28.CMYakacki,R.Shandas,J.Lanning,B.Rech,A.Eckstein,K.Gall,Biomaterials 2007,28,2255.
[0199] 29.L.Xue,S.Dai,Z.Li,Macromolecules 2009,42,964.
[0200] 30.G.Zhu,G.Liang,Q.Xu,Q.Yu,Journal of applied polymer science 2003,90,1589.
[0201] 31.F.Li,W.Zhu,X.Zhang,C.Zhao,M.Xu,Journal of applied polymer science1999,71,1063.
[0202] 32.B.Guo,Y.Chen,Y.Lei,L.Zhang,WYZhou,ABRabie,J.Zhao,Biomacromolecules 2011,12,1312.
[0203] 33.DMFeldkamp,IARousseau,Macromol Mater Eng 2010,295,726.
[0204] 34.AWMcClung,G.Tandon,J.Baur,Mech Time-Depend Mater 2013,17,39.
[0205] 35.K.Gall,CMYakacki,Y.Liu,R.Shandas,N.Willett,KSAnseth,Journal ofBiomedical Materials Research Part A 2005,73A,339.
[0206] 36.MVLancaster,US Patent 5 501 959,1996.
[0207] 37.MCSerrano,R.Pagani,M.Vallet-Regí,J. A.Rámila,I.Izquierdo,MTPortolés,Biomaterials 2004,25,5603.
[0208] 38.CXFLam,DWHutmacher,J.-T.Schantz,MAWoodruff,SHTeoh,Journalof Biomedical Materials Research Part A 2009,90A,906.
[0209] 39.WPWilliamson IV,PASpence,GAKeller,CRRobinson,TJWard,USPatent 7 722 642,2010.
[0210] 40.M.Song,H.Jang,J.Lee,JHKim,SHKim,K.Sun,Y.Park,Biomaterials2014,35,2436.
Claims
1. An implantable tissue support device in the form of a biodegradable polymer scaffold capable of surrounding and supporting tissue, the biodegradable polymer scaffold having a porosity that promotes microvascular growth to promote outward growth and remodeling of the tissue, wherein the tissue is a vein, artery or synthetic graft and the device is external to a vascular anastomosis, and the biodegradable polymer scaffold comprises at least one cross-linked polymer, the at least one cross-linked polymer comprising at least one cross-linkable monomer and at least one shape memory polymer; wherein the biodegradable polymer scaffold is configured to have a melting temperature and can be transformed from an original shape to an implanted shape by an external force when the melting temperature is reached or exceeded, and wherein the biodegradable polymer scaffold has a shape fixity of 50-100% and a shape recovery of 50-100%.
2. The device of claim 1, wherein the melting temperature is 20°C to 50°C.
3. The device of claim 1, wherein the melting temperature is 25°C to 45°C.
4. The device of claim 1, wherein the melting temperature is 30°C to 40°C.
5. The device of claim 1, wherein the melting temperature is 37°C.
6. The device of claim 1, wherein the implant shape forms a seamless and sutureless sheath and includes an elastic radial performance that mimics the compliant properties of the tissue.
7. The device of claim 1, wherein the implant shape forms a seamless and sutureless sheath and is deformable to conform to the shape of the tissue by at least one of extending or bending along the length of the biodegradable polymer scaffold.
8. The device of claim 1, wherein the implanted shape provides for outward tissue remodeling and delivery of an anti-neointimal therapeutic agent.
9. The device of claim 1, wherein the biodegradable polymer scaffold further comprises a Young's modulus of 0.05-200 MPa at 37°C.
10. The device of claim 1, wherein the biodegradable polymer stent is degradable for more than one year after implantation.
11. The device of claim 1, wherein the biodegradable polymer stent further comprises at least one bioactive agent, wherein the bioactive agent is a pharmacological agent.
12. The device of claim 1, wherein the biodegradable polymer scaffold further comprises at least one bioactive agent, wherein the bioactive agent is at least one of the following: a pleiotropic agent, a growth factor, a peptide, a nucleic acid, an anti-proliferative agent, an anti-migratory agent, an anti-inflammatory agent, or an anti-fibrotic agent.
13. The device of claim 1, wherein the biodegradable polymer scaffold further comprises at least one bioactive agent, wherein the bioactive agent is at least one of the following: a pleiotropic agent, a growth factor, a peptide, a nucleic acid, an MK2 inhibitor, an anti-migratory agent, an anti-inflammatory agent, or an anti-fibrotic agent.
14. The device of claim 1, wherein the biodegradable polymer scaffold has a shape fixity of at least 98% and a shape recovery of at least 98%.
15. An implantable tissue support device, wherein include: A biodegradable polymer scaffold capable of surrounding and supporting tissue, wherein the tissue is a vein, artery or synthetic graft and the device is outside of a vascular anastomosis, the biodegradable polymer scaffold comprising a composition of x% PCL-y% ACPCL cross-linked, wherein y=10%-15%, and wherein the biodegradable polymer scaffold is configured to have: at least 95% or greater shape fixity and 95% or greater shape recovery, a melting temperature of 37°C or less, a Young's modulus of 1-100 MPa at 37°C, a porosity of greater than 50% pores of 750 μM in diameter, such that the biodegradable polymer scaffold is biodegradable at a degradation rate of at least several months after implantation.
16. The device of claim 15, wherein the biodegradable polymer stent further comprises a heparin coating comprising MK2i.
17. The device of claim 15, wherein the biodegradable polymer stent is configured to transform from an original shape to an implanted shape, the transformation occurring when the melting temperature is reached or exceeded and an external force is applied to the stent.
18. The device of claim 17, wherein the implant shape is configured to surround tissue.
19. The device of claim 17, wherein the implant shape forms a seamless and sutureless sheath and is deformable to conform to the shape of the tissue by at least one of extending or bending along the length of the biodegradable polymer scaffold.
20. The device of claim 17, wherein the implanted shape provides for outward tissue remodeling and delivery of an anti-neointimal therapeutic agent.
21. The device of claim 16, wherein the heparin coating is configured to release MK2i at a rate of 50 μg / day.
Citation Information
Patent Citations
Polymer compositions and methods for their use
CN101420991A
Bioabsorbable elastomeric polymer networks, cross-linkers and methods of use
CN101678041A
Preparation method of macromolecular crosslinking agent for ultraviolet light crosslinking polyolefin
CN104194001A
Implantable Tissue Compositions and Method
US20070254005A1
Implantable tissue compositions and method
US20090130162A2