A kind of mildew-proof and antibacterial weather-resistant water-based interior wall paint and preparation method thereof
An interior wall coating, anti-mildew and anti-bacterial technology, applied in anti-fouling/underwater coatings, coatings, paints containing biocides, etc., can solve the problems of poor mechanical properties, poor weather resistance, and poor coating properties and other problems, to achieve the effects of excellent impact resistance of the coating film, improved dispersion performance, and low equipment requirements
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2021-01-01
Abstract
Description
Technical field:
[0001] The invention relates to the application of building materials, in particular to a mildewproof and antibacterial weather-resistant water-based interior wall paint. Background technique:
[0002] Harmful substances in interior wall coatings mainly include volatile organic compounds (VOC), heavy metals and suspended particles, which together constitute indoor pollution sources and damage human health. Therefore, it is extremely important to carry out research on interior wall coatings, improve the pollution of interior wall coatings to the indoor environment, create a good living and working environment for people, and protect the health of the crowd. In recent years, a large number of scholars have participated in the research of interior wall coatings, improved various performances of interior wall coatings on the basis of the original, and developed some new coatings at the same time.
[0003] Water-based interior wall paint is a kind of interior wa...
Examples
Embodiment 1
[0034] A mildewproof and antibacterial weather-resistant water-based interior wall paint, in parts by weight, comprises the following components:
[0035] 18 parts of acrylate monomer, 3 parts of eucalyptus eucalyptus powder,
[0036] 1 part of nano-montmorillonite, 1 part of emulsifier,
[0037] 0.8 part of initiator, 1 part of white carbon black,
[0038] 1 part of film-forming aid, 0.5 part of defoamer,
[0039] 0.5 parts of thickener, 0.5 parts of leveling agent, 20 parts of deionized water;
[0040] Its preparation method comprises the following steps:
[0041] (1) Dry the leaves of Eucalyptus macrocephalus, then dry them at 90-100° C. for 10 h, grind to obtain Eucalyptus macrocephalus powder, then place it in a 30% nitric acid solution for immersion treatment for 3 hours, take it out, and dry it in the air Drying, microwave treatment for 5min under 200-300W power; make pretreated Eucalyptus macrophylla powder;
[0042] (2) Soak the nano-montmorillonite in nitric aci...
Embodiment 2
[0047] A mildewproof and antibacterial weather-resistant water-based interior wall paint, in parts by weight, comprises the following components:
[0048] 35 parts of acrylate monomer, 6 parts of eucalyptus eucalyptus powder,
[0049] 3 parts of nano-montmorillonite, 2 parts of emulsifier,
[0050] 1 part of initiator, 5 parts of white carbon black,
[0051] 2 parts of film-forming aid, 1.5 parts of defoamer,
[0052] 1 part of thickener, 1 part of leveling agent, 30 parts of deionized water;
[0053] Its preparation method comprises the following steps:
[0054] (1) Dry the leaves of Eucalyptus macrocephalus, then dry them at 90-100°C for 20 hours, grind them to obtain Eucalyptus macrocephala powder, then place it in a 50% nitric acid solution for soaking treatment for 6 hours, take it out, and dry it in the air Dry, microwave treatment for 15min under 200-300W power; make pretreated Eucalyptus macrophylla powder;
[0055] (2) Soak nano-montmorillonite in nitric acid solut...
Embodiment 3
[0060] A mildewproof and antibacterial weather-resistant water-based interior wall paint, in parts by weight, comprises the following components:
[0061] 20 parts of acrylate monomer, 5 parts of eucalyptus eucalyptus powder,
[0062] 1.5 parts of nano-montmorillonite, 1.6 parts of emulsifier,
[0063] 0.85 parts of initiator, 2 parts of white carbon black,
[0064] 1.3 parts of film-forming aids, 0.7 parts of defoamers,
[0065] 0.6 parts of thickener, 0.5 parts of leveling agent, 25 parts of deionized water;
[0066] Its preparation method comprises the following steps:
[0067] (1) Dry the leaves of Eucalyptus macrocephalus, then dry them at 90-100° C. for 12 hours, grind them to obtain Eucalyptus macrocephala powder, then place it in a 35% nitric acid solution for soaking for 4 hours, take it out, and let it dry in the air Dry, microwave treatment for 10min under 200-300W power; make pretreated Eucalyptus macrophylla powder;
[0068] (2) Soak nano-montmorillonite in n...