A high light transmittance energy-saving glass that can be used in a single piece

By depositing composite film layers on the glass, optimizing the thickness and structure of each layer, the problems of low light transmittance and easy damage in the prior art are solved, and the high light transmittance and low heat transfer coefficient are achieved, ensuring that the glass is Product stability and thermal insulation.

CN108774006BActive Publication Date: 2024-11-05WUJIANG CSG HUADONG ARCHITECTURAL GLASS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201810857136.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-07-31
Publication Date
2024-11-05
Estimated Expiration
2038-07-31

AI Technical Summary

Technical Problem

While ensuring a low heat transfer coefficient, the light transmittance is difficult to reach more than 40%. In particular, silver-based low-radiation coating glass is prone to oxidation, resulting in easy damage to the film surface and transparent when the thickness of the niobium functional layer is insufficient. The light rate is less than 30%.

Method used

A composite film layer structure is adopted, including a first anti-reflective dielectric film layer deposited on the glass substrate, a first high-temperature flame retardant film layer, a first metal isolation film layer, a functional film layer (metal niobium or niobium nitride layer), The dimetal isolation film layer, the second anti-reflective dielectric film layer, the second high-temperature flame retardant film layer and the protective film layer optimizes the thickness and structure of each layer to ensure high light transmittance and low heat transfer coefficient of the glass product.

Benefits of technology

It achieves the high light transmittance (greater than 50%) and low heat transfer coefficient of glass products. The product stability is improved, the appearance is clear, and it has good heat insulation and insulation effects, which meets the natural and environmental protection needs, and reduces the appearance after tempering. defect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108774006B_ABST
    Figure CN108774006B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of glass production, and in particular to an energy-saving glass with high light transmittance that can be used in a single piece, comprising a glass substrate and a composite film layer coated on a surface of one side of the glass substrate, wherein the composite film layer comprises a first anti-reflection medium film layer, a first high-temperature resistant flame-retardant film layer, a first metal isolation film layer, a functional film layer, a second metal isolation film layer, a second anti-reflection medium film layer, a second high-temperature resistant flame-retardant film layer and a protective film layer that are sequentially deposited from the glass substrate outward. The present invention optimizes the structure and thickness parameters of the composite film layer so that the glass product of the present invention has both the effects of low heat transfer coefficient and high light transmittance, and can be used in a single piece.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass production, and in particular to energy-saving glass with high light transmittance that can be used in a single piece. Background Art

[0002] The low-emissivity coated glass with the best performance and the highest market share currently sold on the market includes at least one silver-type metal functional layer, the main function of which is to reflect most of the incident infrared radiation back to the source of heat radiation. For example, in summer, it can block outdoor solar radiation from entering the room to reduce the cost of air conditioning; in winter, it can prevent indoor warm air from flowing through the glass to the outside, thereby reducing heating costs. This plays a role in energy conservation and environmental protection. However, this film layer is very easy to be oxidized, sulfurized, etc., resulting in the film surface of this type of silver-based low-emissivity coated glass must be used on the hollow inner surface of insulating glass to avoid being exposed to air and damaged.

[0003] In the current single-layer solar control glass with niobium as the functional layer, the only niobium functional layer is deposited on a separate glass substrate. Only when the thickness of the functional layer of such products is thicker (for example, at least about 10 nanometers or higher) can the value of the heat transfer coefficient U specified in the current national standards be met. However, when the functional layer is thicker, due to the non-selective absorption of the incident radiation energy, the light transmittance of such glass is very low (generally less than 30%, or even less than 20%).

[0004] In view of such characteristics, it is difficult for existing products to obtain an acceptable heat transfer coefficient U from such a film layer while maintaining a sufficiently high (light transmittance greater than 40%, preferably greater than 50%) solar transmittance. Summary of the invention

[0005] The present invention provides an energy-saving glass with high light transmittance that can be used in a single piece, which can solve the problem of low light transmittance while ensuring that the heat transfer coefficient is sufficiently low.

[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a high-transmittance energy-saving glass that can be used in a single piece, including a glass substrate and a composite film layer coated on one side surface of the glass substrate, the composite film layer including a first anti-reflection dielectric film layer, a first high-temperature resistant flame-retardant film layer, a first metal isolation film layer, a functional film layer, a second metal isolation film layer, a second anti-reflection dielectric film layer, a second high-temperature resistant flame-retardant film layer and a protective film layer deposited in sequence from the glass substrate to the outside.

[0007] Furthermore, the functional film layer is a metal niobium layer or a niobium nitride layer.

[0008] Furthermore, the thickness of the functional film layer is 5-40 nm.

[0009] Furthermore, the first anti-reflection dielectric film layer / the second anti-reflection dielectric film layer is any one of a zinc oxide / aluminum oxide composite layer and a zinc oxide / tin oxide composite layer, or a composite layer of the two, and the film layer structures of the first anti-reflection dielectric film layer and the second anti-reflection dielectric film layer are the same or different.

[0010] Furthermore, the thickness of the first anti-reflection dielectric film layer is 20-100 nm; the thickness of the second anti-reflection dielectric film layer is 30-100 nm.

[0011] Furthermore, the first high temperature resistant flame retardant film layer / the second high temperature resistant flame retardant film layer is a SbOx layer.

[0012] Furthermore, the thickness of the first high temperature resistant flame retardant film layer is 30-55 nm; the thickness of the second high temperature resistant flame retardant film layer is 25-50 nm.

[0013] Furthermore, the first metal isolation film layer / the second metal isolation film layer is any one layer or a composite layer of any multiple layers of a NiCrOx layer, a NiCr layer, a Ti layer and a TiOx layer, and the film layer structures of the first metal isolation film layer and the second metal isolation film layer are the same or different.

[0014] Furthermore, the thickness of the first metal isolation film layer is 0.5-5 nm; the thickness of the second metal isolation film layer is 0.5-6 nm.

[0015] Furthermore, the protective film layer is any one layer or a composite layer of any two layers of a SiNx layer, a SiOx layer, a SiNxOy layer and a TiOx layer, and the thickness of the protective film layer is 25-60 nm.

[0016] After adopting the above technical scheme, the present invention has the following advantages compared with the prior art:

[0017] 1. The present invention optimizes the structure and thickness parameters of the composite film layer so that the glass product of the present invention has both low heat transfer coefficient and high light transmittance.

[0018] 2. The functional film layer of the present invention is made of metal niobium or niobium nitride. The thermal radiation in sunlight is mainly non-selectively absorbed by the metal niobium layer or the niobium nitride layer. Metal niobium (Nb) is a particularly stable material that can withstand various heat treatments without damaging its optical properties. Niobium nitride (NbN) has a high level of chemical stability. Using the above two materials as the functional film layer allows the glass product to be used in a single piece.

[0019] 3. The first anti-reflection medium film layer and the second anti-reflection medium film layer of the present invention have a relatively high refractive index to offset the absorption of the functional film layer, so that the light transmittance of the glass product of the present invention can reach 50% or more, and the product appearance is clear and transparent, which can ensure good heat insulation and thermal insulation effects, meeting the needs of consumers for natural and environmental protection.

[0020] 4. The present invention uses flame-retardant antimony oxide as a coating material, which improves the film's ability to withstand high-temperature impacts and solves the problem of many appearance defects in tempered glass products. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Attached Figure 1 It is a schematic diagram of the structure of the energy-saving glass with high light transmittance that can be used in a single piece in the present invention.

[0022] in,

[0023] 100. Glass substrate;

[0024] 200, composite film layer;

[0025] 201, a first anti-reflection dielectric film layer; 202, a first high-temperature resistant flame-retardant film layer; 203, a first metal isolation film layer; 204, a functional film layer; 205, a second metal isolation film layer; 206, a second anti-reflection dielectric film layer; 207, a second high-temperature resistant flame-retardant film layer; 208, a protective film layer. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0027] like Figure 1 As shown, a high-transmittance energy-saving glass that can be used in a single piece includes a glass substrate 100 and a composite film layer 200 coated on one side of the glass substrate 100. The composite film layer 200 includes a first anti-reflection medium film layer 201, a first high-temperature resistant flame-retardant film layer 202, a first metal isolation film layer 203, a functional film layer 204, a second metal isolation film layer 205, a second anti-reflection medium film layer 206, a second high-temperature resistant flame-retardant film layer 207 and a protective film layer 208 deposited in sequence from the glass substrate 100 to the outside.

[0028] Specific:

[0029] The functional film layer 204 is a metal niobium (Nb) layer or a niobium nitride (NbN) layer, and the thickness of the functional film layer 204 is 5-40nm. Metal niobium (Nb) is a particularly stable material that can withstand various heat treatments without damaging its optical properties; niobium nitride (NbN) has a high level of chemical stability. Using metal niobium or niobium nitride as a functional film layer is not easy to oxidize or sulfide, and the composite film layer 200 of the glass product can be directly exposed to the air and can be used as a single piece.

[0030] The first anti-reflection dielectric film layer 201 / the second anti-reflection dielectric film layer 206 is any one of a zinc oxide / aluminum oxide composite layer (ZnAlOx layer) and a zinc oxide / tin oxide composite layer (ZnSnOx layer) or a composite layer of the two, and the film layer structures of the first anti-reflection dielectric film layer 201 and the second anti-reflection dielectric film layer 206 can be the same or different. Preferably, the thickness of the first anti-reflection dielectric film layer 201 is 20-100 nm; the thickness of the second anti-reflection dielectric film layer 206 is 30-100 nm.

[0031] The first anti-reflection dielectric film layer 201 and the second anti-reflection dielectric film layer 206 of the present invention use coating materials with better performance as protective materials, which can improve the high temperature resistance of the glass product, thereby providing better protection for the functional film layer 204. In addition, the zinc oxide / aluminum oxide composite layer and the zinc oxide / tin oxide composite layer both have a high refractive index, thereby offsetting the absorption of the functional film layer 204, thereby improving the light transmittance of the glass product of the present invention, which can be as high as 50% or even higher. The glass product not only has a clear and transparent appearance, but also can ensure good heat insulation and thermal insulation effects, meeting the needs of consumers for natural and environmental protection.

[0032] In addition, since the film materials selected for the first anti-reflection dielectric film layer 201 and the second anti-reflection dielectric film layer 206 have better physical properties and chemical corrosion resistance, the deposited first anti-reflection dielectric film layer 201 and the second anti-reflection dielectric film layer 206 have excellent corrosion resistance, mechanical scratch resistance, and high temperature resistance, thereby improving the subsequent processing performance and service life of the glass product.

[0033] The first high temperature resistant flame retardant film layer 202 / the second high temperature resistant flame retardant film layer 207 is a SbOx layer. Preferably, the thickness of the first high temperature resistant flame retardant film layer 202 is 30-55nm; the thickness of the second high temperature resistant flame retardant film layer 207 is 25-50nm. The present invention uses flame retardant antimony oxide as a coating material, which not only improves the high temperature impact resistance of the first high temperature resistant flame retardant film layer 202 / the second high temperature resistant flame retardant film layer 207, but also improves the protective effect on the functional film layer 204, so that the heat resistance of the glass product is better than that of traditional coated glass, and the appearance defects of the tempered glass product can be reduced.

[0034] The first metal isolation film layer 203 / the second metal isolation film layer 205 is any one of a NiCrOx layer, a NiCr layer, a Ti layer and a TiOx layer or a composite layer of any multiple layers, and the film structure of the first metal isolation film layer 203 and the second metal isolation film layer 205 is the same or different. Preferably, the thickness of the first metal isolation film layer 203 is 0.5-5nm; the thickness of the second metal isolation film layer 205 is 0.5-6nm.

[0035] The functional film layer 204 is protected by any one or a composite layer of any multiple layers of the NiCrOx layer, the NiCr layer, the Ti layer and the TiOx layer, so that the film layer structure is more complete and the bonding force is higher, which effectively ensures the density of the film layer and the stability of the glass product.

[0036] In particular, when the first metal isolation film layer 203 / the second metal isolation film layer 205 includes a NiCrOx layer, during the heating process, NiCrOx has a good affinity for partially permeated oxygen, thereby effectively capturing oxygen molecules and better protecting the functional film layer 204. In addition, since the NiCrOx layer combines with oxygen, the visible light transmittance of the product can be effectively improved, thereby improving the transparency of the glass product.

[0037] The protective film layer 208 is any one layer of a SiNx layer, a SiOx layer, a SiNxOy layer and a TiOx layer, or a composite layer of any two layers. Preferably, the protective film layer 208 has a thickness of 25-60 nm.

[0038] The various film layers of the present invention are sequentially plated from the glass substrate 100 to the outside by magnetron sputtering. According to the well-known technology, the NiCrOx layer, TiOx layer, SbOx layer, SiOx layer, ZnAlOx layer and ZnSnOx layer are deposited using corresponding targets in a reactive atmosphere containing oxygen; the SiNx layer and NbN layer are deposited using corresponding targets in a reactive atmosphere containing nitrogen; the Nb layer, NiCr layer and Ti layer are deposited using corresponding targets in an inert atmosphere containing pure argon; the SiNxOy layer is deposited using corresponding targets in a reactive atmosphere containing both nitrogen and oxygen.

[0039] After the coating is completed, it is placed in a tempering furnace for tempering treatment. The heating temperature of the coated surface is 680-690°C, and the heating temperature of the non-coated surface of the glass substrate 100 is slightly lower than that of the coated surface, which is 670-680°C. This is because the composite film layer 200 of the present invention is a functional film layer, and its performance determines that the heat absorption capacity of the coated surface is weaker than that of the non-coated surface. In order to ensure that the coated surface and the non-coated surface absorb heat consistently and avoid bending and deformation during the tempering treatment, the temperature of the coated surface needs to be higher than that of the non-coated surface, and the tempering treatment time is 570-590s.

[0040] The following are specific embodiments:

[0041] Example 1

[0042] After cleaning and drying the glass substrate 100, the following film layers are sequentially plated on one side of the glass substrate: ZnSnOx / SbOx / NiCrOx / Nb / NiCrOx / ZnSnOx / SbOx / TiOx; the thickness of each film layer in the composite film layer 200 is: 39nm / 36.5nm / 0.5nm / 28nm / 0.6 nm / 38nm / 48.9nm / 40.6nm;

[0043] For light transmission greater than 50% after tempering, the following results were obtained:

[0044] Transmittance T=62.7%; Heat transfer coefficient U=4.18W / m 2 .k;

[0045] Rout=9.0; a*=-3.2; b*=-16.3 (glass surface);

[0046] Rinside = 21.3; a* = -4.6; b* = 0.8 (membrane surface).

[0047] Note that in this embodiment and the following embodiments, Rout is the reflectance of the laminate view from the glass side, and its corresponding a* and b* values ​​correspond to the visual color on the glass side; while Rin and the corresponding a* and b* values ​​are the values ​​obtained when viewing the laminate from the film layer side.

[0048] Example 2

[0049] After the glass substrate 100 is cleaned and dried, the following film layers are sequentially plated on one surface thereof: ZnAlOx / SbOx / TiOx / Nb / TiOx / ZnAlOx / SbOx / SiOx; the thicknesses of the corresponding film layers in the above-mentioned composite film layer 200 are: 62.9nm / 48.3nm / 3.3nm / 22nm / 3.5nm / 58.3nm / 32.2nm / 21.6nm.

[0050] For light transmission greater than 50% after tempering, the following results were obtained:

[0051] Transmittance T=56.2%; Heat transfer coefficient U=3.75W / m 2 .k;

[0052] Rout=7.6; a*=-4.2; b*=-21.3 (glass surface);

[0053] Rinside = 18.6; a* = -3.2; b* = 0.2 (membrane surface).

[0054] Example 3

[0055] After the glass substrate 100 is cleaned and dried, the following film layers are sequentially plated on one surface thereof: ZnSnOx / SbOx / Ti / NbN / Ti / ZnSnOx / SbOx / SiNxOy; the thicknesses of the corresponding film layers in the above-mentioned composite film layer 200 are: 83nm / 54.7nm / 4.8nm / 26.3nm / 4.8nm / 62.4nm / 45.2nm / 52.8nm.

[0056] For light transmission greater than 50% after tempering, the following results were obtained:

[0057] Transmittance T=53%; Heat transfer coefficient U=3.52W / m 2 .k;

[0058] Rout=9.0; a*=-2.5; b*=-13.1 (glass surface);

[0059] Rinside = 16.9; a* = -4.8; b* = 0.7 (membrane surface).

[0060] It can be seen from the above embodiments that the high-transmittance energy-saving glass that can be used in a single piece of the present invention has both a low heat transfer coefficient and a high light transmittance, and the glass product has a clear and transparent appearance and a neutral transmitted color.

[0061] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-transmittance energy-saving glass that can be used in a single piece, comprising a glass substrate and a composite film layer coated on one side of the glass substrate. Features: The composite film layer comprises a first anti-reflection dielectric film layer, a first high temperature resistant flame retardant film layer, a first metal isolation film layer, a functional film layer, a second metal isolation film layer, a second anti-reflection dielectric film layer, a second high temperature resistant flame retardant film layer and a protective film layer sequentially deposited from the glass substrate outward; the functional film layer is a metal niobium layer or a niobium nitride layer; The thickness of the functional film layer is 5-40nm; the first anti-reflection medium film layer / the second anti-reflection medium film layer is any one of a zinc oxide / aluminum oxide composite layer and a zinc oxide / tin oxide composite layer or a composite layer of the two, and the film layer structures of the first anti-reflection medium film layer and the second anti-reflection medium film layer are the same or different.

2. The high-transmittance energy-saving glass that can be used in a single piece according to claim 1 is characterized in that: the thickness of the first anti-reflection dielectric film layer is 20-100nm; the thickness of the second anti-reflection dielectric film layer is 30-100nm.

3. The high-transmittance energy-saving glass that can be used in a single piece according to claim 1 is characterized in that the first high-temperature resistant flame-retardant film layer / the second high-temperature resistant flame-retardant film layer is a SbOx layer.

4. The high-transmittance energy-saving glass that can be used in a single piece according to claim 3 is characterized in that: the thickness of the first high-temperature resistant flame-retardant film layer is 30-55nm; the thickness of the second high-temperature resistant flame-retardant film layer is 25-50nm.

5. The high-transmittance energy-saving glass that can be used in a single piece according to claim 1 is characterized in that: the first metal isolation film layer / the second metal isolation film layer is any one layer or a composite layer of any multiple layers among NiCrOx layer, NiCr layer, Ti layer and TiOx layer, and the film layer structures of the first metal isolation film layer and the second metal isolation film layer are the same or different.

6. The high-transmittance energy-saving glass that can be used in a single piece according to claim 5 is characterized in that: the thickness of the first metal isolation film layer is 0.5-5nm; the thickness of the second metal isolation film layer is 0.5-6nm.

7. The high-transmittance energy-saving glass that can be used in a single piece according to claim 1 is characterized in that: the protective film layer is any one layer or a composite layer of any two layers of SiNx layer, SiOx layer, SiNxOy layer and TiOx layer, and the thickness of the protective film layer is 25-60nm.