Implantable device and packaging method thereof
By forming a dense nano-level and micron-level double-layer coating on implantable devices, it solves the problem of difficulty in packaging accuracy, size and stability in the existing technology, and achieves effective protection of small molecules and macromolecule liquids. Significantly improve the accuracy and stability of the device.
Patent Information
- Application Number
- CN201910025937.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-01-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-01-11
AI Technical Summary
Existing implantable device packaging technology is difficult to meet high precision, small size, high sensitivity and long-term stability at the same time, especially in terms of preventing the influence of liquids, especially for devices with movable structures.
It adopts a double-layer packaging structure, including a dense nano-level coating to prevent the impact of liquids and a micron-level coating to prevent the impact of liquids. It is formed through technologies such as atomic layer deposition and vapor deposition, which respectively block the penetration of small molecules and large molecular groups, forming Double protection effect.
It achieves high precision, ultra-thin size and long-term stability of the device, reduces the impact of the external environment on accuracy, and is suitable for implantable devices with movable structures, such as intraocular pressure sensors.
Smart Images

Figure CN109626319B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of micro-nano manufacturing technology, and in particular to an implantable device and a packaging method thereof. Background Art
[0002] Packaging technology plays a pivotal role in the field of implantable device technology. It can even be said that without proper packaging technology, there will be no implantable devices for clinical applications. Among all implantable devices, there is a large class of implantable devices with movable structures, such as mechanical sensors and actuators. Because of their movable structures, this large class of implantable devices has higher requirements for packaging technology.
[0003] Taking an implantable intraocular pressure sensor as an example, its packaging needs to meet at least two conditions at the same time. First, the packaged intraocular pressure sensor must meet the requirements of high precision, small size, and high sensitivity. Among them, the main guarantee condition for the high precision and high sensitivity requirements is that the packaging structure cannot have a significant impact on the movement of the movable structure that plays a sensing role in the sensor. Second, the packaging structure of the intraocular pressure sensor must meet the stability requirements of long-term implantation (especially the long-term stability to prevent the influence of liquid).
[0004] In the prior art, micron-thick polymer materials such as polyparaxylene have been used to encapsulate implantable devices. However, due to the poor density of polymer materials, a larger thickness is required to achieve a better liquid-proof effect. In addition, this method has a better protective effect on liquids in the state of large molecular clusters, but it is difficult to block the invasion of liquids in the state of small molecular clusters. In recent years, atomic layer deposition processes have also been used to produce nanometer-thick dense oxides, nitrides, fluorides, metals, carbides, sulfides and other materials for waterproof packaging of electronic devices. Although this method has a better protective effect on liquids in the state of small molecular clusters, it has a poor protective effect on liquids in the state of large molecular clusters. In addition, the Young's modulus and hardness of dense oxides and other materials are relatively large, which has a greater impact on the performance of micro-devices with movable structures.
[0005] At the same time, since implantable devices will be affected by external environmental factors such as temperature, humidity, corrosive gases, vibration, etc. during operation, if they are not properly packaged and protected, the accuracy indicators of the devices will be greatly affected.
[0006] Therefore, if the above two packaging methods can be combined, the advantages of micron coating and nano coating can be brought into play respectively, a suitable packaging structure and packaging process can be provided for implantable devices (especially implantable devices with movable structures, such as implantable intraocular pressure sensors, etc.), and a new implantable packaging method with good liquid protection effect, ultra-thin size and little impact on device performance can be realized. At the same time, after packaging, it can not only compensate for the defects such as gap and hysteresis in the sensor, but also reduce the influence of the external environment on the accuracy of the sensor, thereby improving the accuracy of the device. This is of great significance to the research and application of implantable devices. Summary of the invention
[0007] Based on the above situation, the main purpose of the present invention is to provide a double-layer packaging method for implantable devices, which can meet the two requirements of small packaging size and long-term stability against liquid influence, while improving the accuracy of the device.
[0008] The above purpose is achieved through the following technical solutions:
[0009] According to a first aspect of the present invention, an implantable device is provided for implantation in a living body, wherein the implantable device comprises a device body and a packaging structure arranged around the device body, wherein the packaging structure comprises a first protective layer coated on the device body and a second protective layer arranged around the first protective layer, and wherein one of the first protective layer and the second protective layer is a dense nano-scale coating that prevents liquid influence, and the other of the first protective layer and the second protective layer is a micron-scale coating that prevents liquid influence.
[0010] Preferably, the first protective layer is a dense nano-scale coating that prevents liquids from affecting it, and the second protective layer is a micro-scale coating that prevents liquids from affecting it.
[0011] Preferably, the dense nanoscale coating that prevents liquid influence is an atomic layer deposition layer or a vapor deposition layer;
[0012] And / or, the micron-scale coating that protects against liquid influence is a vapor deposition layer, or an evaporation deposition layer, or a sputtering deposition layer, or a spraying deposition layer.
[0013] Preferably, the implantable device is an implantable device with a movable structure, preferably an implantable pressure-sensitive device, and more preferably an implantable intraocular pressure sensor.
[0014] Preferably, the thickness of the dense nano-scale coating for preventing liquid influence is between 0.1 and 1000 nanometers, and / or the thickness of the micro-scale coating for preventing liquid influence is between 0.1 and 3000 micrometers.
[0015] Preferably, in the packaging structure, at least the second protective layer is formed of a biocompatible material.
[0016] According to a second aspect of the present invention, a packaging method for the aforementioned implantable device comprises the steps of:
[0017] S40, forming the first protective layer on the periphery of the device body;
[0018] S50, forming the second protective layer on the periphery of the first protective layer.
[0019] Preferably, the implantable device comprises a chip and a substrate for mounting the chip, and before step S40, further comprises the following steps:
[0020] S10, cleaning the chip;
[0021] S20, attaching the cleaned chip to the substrate;
[0022] S30, performing wire bonding on the chip and the substrate to form the device body.
[0023] Preferably, the dense nanoscale coating that prevents liquid influence is formed on the device body by using atomic layer deposition technology or vapor deposition technology;
[0024] And / or, the micron-scale coating that protects against liquids is formed by using vapor deposition technology, evaporation technology, sputtering technology, or spraying technology.
[0025] Preferably, the dense nanoscale coating that prevents liquid influence is formed by one or more of oxides, nitrides, fluorides, metals, carbides, sulfides, and polymers;
[0026] And / or, the micron-scale coating that protects against liquids is formed by using one or more of polymers, oxides, sulfides, nitrides, carbides, and ceramics.
[0027] The implantable device and the packaging method thereof of the present invention can simultaneously meet the two requirements of small device packaging size and long-term stability against liquid influence, thereby meeting the requirements of long-term implantation and normal operation of the device.
[0028] In particular, the implantable device of the present invention utilizes the synergistic effect of a dense nanoscale coating that protects against liquid influence (such as an atomic layer deposition layer, a vapor deposition layer) and a micron-scale coating that protects against liquid influence (such as a chemical vapor deposition layer, etc.), so that the corresponding device has good stability against liquid influence, wherein the micron-scale coating that protects against liquid influence can prevent the erosion of larger liquid molecules (such as large molecular clusters composed of more than 10 liquid molecules), and the dense nanoscale coating that protects against liquid influence can prevent the erosion of gas molecules or small molecular clusters composed of less than 10 liquid molecules, thereby providing dual protection against liquid influence for the implantable device and significantly reducing the packaging size of the implantable device.
[0029] In particular, for implantable devices with movable structures, the packaging structure provided by the present invention can not only compensate for defects such as gaps and hysteresis in the sensor, but also isolate harmful media in the external environment that affect the accuracy of the sensor, thereby improving the accuracy of the device. In addition, the packaging structure provided by the present invention has little effect on the movement of its movable structure, thereby ensuring the high sensitivity of the device to a large extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The preferred embodiments of the implantable device and the packaging method thereof according to the present invention will be described below with reference to the accompanying drawings.
[0031] Figure 1 Schematic diagram of the appearance of an implantable device according to a preferred embodiment of the present invention, wherein the A region is partially cross-sectionally processed;
[0032] Figure 2 for Figure 1 A partial enlarged schematic diagram of the middle A area;
[0033] Figure 3 A flowchart of a preferred packaging method for an implantable device according to a preferred embodiment of the present invention;
[0034] Figure 4 A schematic diagram of the appearance of a chip involved in a preferred embodiment of the present invention;
[0035] Figure 5 for Figure 4 A schematic diagram of the appearance of a chip attached to a substrate;
[0036] Figure 6 A schematic diagram of the appearance of a chip-substrate assembly formed after the chip and the substrate are wire-bonded;
[0037] Figure 7 for Figure 6 A schematic diagram of the appearance of the chip substrate assembly after the first protective layer is formed, wherein the B area is partially cross-sectionally processed;
[0038] Figure 8 for Figure 7 A partial enlarged schematic diagram of area B in the middle.
[0039] Reference numerals in the figure: 10 - chip, 20 - substrate, 30, 31, 32, 33 - metal leads, 40 - first protective layer, 50 - second protective layer. DETAILED DESCRIPTION
[0040] In order to ensure the ability of implantable devices to prevent the influence of liquids, while improving the accuracy of devices and reducing the packaging volume of implantable devices, especially implantable devices with movable structures, the present invention abandons the metal, ceramic or glass packaging shells used in the prior art, and replaces them with a protective layer structure to prevent the influence of liquids, thereby forming a new packaging structure and packaging method.
[0041] According to a first aspect of the present invention, there is provided an implantable device for implantation in a living being (eg, a human being). Figure 1 and Figure 2 As shown, the implantable device includes a device body and a packaging structure arranged on the periphery of the device body. In the illustrated embodiment, the implantable device includes a chip 10 and a substrate 20 for mounting the chip 10, so that the device body is a chip-substrate assembly, that is, an assembly formed by assembling the chip 10 and the substrate 20. Wherein, the packaging structure includes a first protective layer 40 coated on the device body and a second protective layer 50 located on the periphery of the first protective layer 40, and wherein one of the first protective layer 40 and the second protective layer 50 is a dense nano-scale coating that prevents liquid influence, and the other is a micron-scale coating that prevents liquid influence. Preferably, the first protective layer 40 is a dense nano-scale coating that prevents liquid influence, and the second protective layer 50 is a micron-scale coating that prevents liquid influence; or, alternatively, the first protective layer 40 is a micron-scale coating that prevents liquid influence, and the second protective layer 50 is a dense nano-scale coating that prevents liquid influence.
[0042] In the prior art, the biocompatible coating used for the contact surface of the biomedical device to prevent the influence of liquid is mainly a polymer coating, and its function is to improve the interface compatibility between the corresponding biomedical device and the organs in the body. The main reason why the coating method of the prior art cannot maintain the effectiveness of the device's effect of preventing the influence of liquid for a long time is that the current coating method mainly uses a single coating as a protective layer of the device, and the single coating has limited effect on the protection of liquid due to its own material properties and other limitations. For example, a single micron-level polymer coating such as polyparaxylene has better protection against large molecules in the liquid, but poor protection against small molecules in the liquid; a single nano-level oxide coating has a dense structure and can better protect small molecules in the liquid, but poor protection against large molecules in the liquid, and due to its high Young's modulus and hardness, it will have a greater impact on the performance of the sensitive or moving parts of the device.
[0043] However, water in nature (including in organisms) often does not exist in the form of a single water molecule, but exists in the form of a number of water molecules that are aggregated together through hydrogen bonding to form a water molecule cluster, commonly known as a "water molecule cluster". Usually, a water molecule cluster composed of more than 10 water molecules is called a macromolecular cluster, which has poor activity and cannot break through the protection of the above-mentioned polymer coating. Such macromolecular clusters exist in large quantities in organisms and account for the vast majority of water in organisms; and a water molecule cluster composed of less than 10 water molecules is called a small molecule cluster, which has high activity and small volume. Although only a small amount exists in the organism, these small molecule clusters can pass through the porous structure of the polymer and accumulate over the years, and will slowly penetrate into the interior of the polymer coating. Therefore, if this polymer coating is directly applied to the implantable device of the present invention, due to the lack of the encapsulation shell used in the prior art, a part of the small molecule clusters of the liquid will gradually penetrate into the interior of the polymer coating. When a certain amount is reached, it will cause damage to the device, such as damaging the circuit of the chip, etc., making it difficult for the corresponding implantable device to meet the stability requirements of long-term implantation to prevent the influence of liquid.
[0044] The dense nano-scale coating to prevent liquid influence in the present invention is a dense coating with a thickness of nanometers, which can block the penetration of small molecular groups; the micron-scale coating to prevent liquid influence is a coating to prevent liquid influence with a thickness of micrometers, and its density is lower than that of the dense nano-scale coating to prevent liquid influence, and its blocking ability relative to the penetration of small molecular groups is limited, but it can effectively block the penetration of large molecular groups. In addition, the packaging structure in the present invention can not only make up for the defects such as gap and hysteresis in the sensor, but also isolate harmful media in the external environment that affect the accuracy of the sensor, thereby improving the accuracy of the device.
[0045] Therefore, the present invention is provided with a first protective layer and a second protective layer on the periphery of the device body, and in a preferred embodiment, the first protective layer is a dense nano-scale coating that prevents the influence of liquids, and the second protective layer is a micron-scale coating that prevents the influence of liquids, wherein the micron-scale coating that prevents the influence of liquids is used to block the penetration of large molecular clusters (the vast majority of water molecular clusters are large molecular clusters), and the dense nano-scale coating that prevents the influence of liquids is used to block the penetration of small molecular clusters. Therefore, during the long-term working process after implantation in the body, even if a small number of small molecular clusters penetrate into the interior of the micron-scale coating that prevents the influence of liquids as the first line of defense, due to the presence of the dense nano-scale coating that prevents the influence of liquids as the second line of defense, these small molecular clusters will find it difficult to break through to the surface of the chip.
[0046] In another preferred embodiment, the first protective layer is a micron-scale coating that prevents the influence of liquids, and the second protective layer is a dense nano-scale coating that prevents the influence of liquids, wherein the dense nano-scale coating that prevents the influence of liquids acts as the first line of defense on the periphery to block the penetration of small molecular clusters and large molecular clusters at the same time, and the micron-scale coating acts as the second line of defense on the inside to continue to block the penetration of large molecular clusters when the first line of defense fails locally. Therefore, during the long-term operation of the implant in the body, if the dense nano-scale coating that prevents the influence of liquids on the periphery fails locally after a long period of operation, due to the existence of the micron-scale coating that prevents the influence of liquids, even if a small amount of small molecular clusters may penetrate into the micron-scale coating that prevents the influence of liquids through the local failure site, it will still take a long time to break through to the chip surface. It is particularly important to note that in the present embodiment, the dense nanoscale liquid-proof coating can penetrate into the micropores of the micrometer-scale liquid-proof coating during the formation process, thereby forming a three-dimensional second protective layer. At this time, even if the dense nanoscale liquid-proof coating as the first line of defense fails locally on the surface, small molecular clusters are actually still difficult to penetrate into the interior of the micrometer-scale liquid-proof coating, and the long-term working stability and reliability of the implantable device can be guaranteed.
[0047] Therefore, the packaging structure of the implantable device proposed by the present invention can withstand the test of long-term implantation to prevent the influence of liquid, thereby meeting the stability requirements. In addition, the packaging structure of the present invention can not only make up for the defects such as gap and hysteresis in the sensor, but also isolate the harmful media in the external environment that affect the accuracy of the sensor, thereby improving the accuracy of the device.
[0048] On the other hand, since the packaging structure of the implantable device proposed in the present invention can only include two layers of ultra-thin coatings, which are micron-level and nano-level respectively, the size of the implantable device can be significantly reduced compared to the existing implantable packaging devices using shells, which is very important for the application of implantable devices.
[0049] It can be seen that the implantable device of the present invention can simultaneously meet the requirements of small packaging size and long-term stability against liquid influence, and can meet the requirements of long-term implantation and normal operation of various implantable devices (especially implantable devices with movable structures, such as pressure sensitive devices, especially intraocular pressure sensors, etc.).
[0050] In particular, for implantable devices with movable structures, their sensitivity depends on the sensitivity of the movable structure when it moves (for example, when the pressure-sensitive membrane is deformed). Obviously, the external package of the movable structure should not hinder the movement of the movable structure itself. In the present invention, a dense nano-scale coating that prevents liquid influence and a micron-scale coating that prevents liquid influence can be directly coated on the surface of the corresponding movable structure. Since the thickness of these two coatings that prevent liquid influence is very thin, the hindrance to the movement of the movable structure is very small, and thus only a small impact on the sensitivity of the device will be produced. The packaging structure of the present invention can not only make up for the defects of gap, hysteresis, etc. in the sensor, but also isolate harmful media in the external environment that affect the accuracy of the sensor, thereby improving the accuracy of the device.
[0051] Preferably, in the present invention, the dense nano-scale coating that prevents the influence of liquids can be an atomic layer deposition layer, a vapor deposition layer, but is not limited to an atomic layer deposition layer; the micron-scale coating that prevents the influence of liquids can be a chemical vapor deposition layer, or an evaporation deposition layer, or a sputtering deposition layer, or a spray deposition layer, but is not limited to the listed deposition layers.
[0052] Atomic layer deposition technology is a method that can deposit substances on the surface of a substrate layer by layer in the form of a single atomic film. During the atomic layer deposition process, the chemical reaction of a new layer of atomic film is directly related to the previous layer, so that only one layer of atoms is deposited each time. By precisely controlling the thickness of the deposited coating, a protective coating that meets the requirements and prevents the influence of liquids can be obtained. Preferably, the thickness of the first protective layer 40 (preferably an atomic layer deposition layer) is between 0.1 and 1000 nanometers, more preferably 0.5 to 400 nanometers, for example 300 nanometers. The density of the atomic layer deposition layer can well ensure its blocking of small molecular clusters.
[0053] Preferably, the material used to form the dense nanoscale liquid-resistant coating (preferably an atomic layer deposition layer) can be any liquid-resistant material, such as oxides, nitrides, fluorides, metals, carbides, sulfides or combinations thereof.
[0054] Preferably, the material used to form the micron-scale coating that protects against liquids may be any material that protects against liquids, such as polymers, oxides, sulfides, nitrides, carbides, ceramics or a combination thereof.
[0055] Preferably, different materials and / or different processes can be used to form the dense nano-scale coating that prevents the influence of liquids. Similarly, different materials and / or different processes can also be used to form the micron-scale coating that prevents the influence of liquids. Taking the micron-scale coating that prevents the influence of liquids as an example, the micron-scale coating that prevents the influence of liquids itself can have different materials and / or properties in the thickness direction. For example, the same material and different processes can be used to form the micron-scale coating that prevents the influence of liquids, different materials and different processes can be used to form the micron-scale coating that prevents the influence of liquids, or different materials and the same process can be used to form the micron-scale coating that prevents the influence of liquids, thereby making full use of the advantages of different materials and / or different process methods.
[0056] For example, in a preferred embodiment, a layer of liquid-proof coating with a thickness of, for example, 2 microns can be first deposited using silicon carbide, and then a layer of liquid-proof coating with a thickness of, for example, 2 microns can be deposited using polyparaxylene, and these two liquid-proof coatings together constitute the micron-level liquid-proof coating described in the present invention. In this way, the density and stability of the liquid-proof coating can be improved, and the hydrophobicity of polyparaxylene can be used to further improve the liquid-proof ability of the coating.
[0057] Preferably, the thickness of the second protective layer 50 (preferably a micron-level coating to prevent liquid influence, such as a chemical vapor deposition layer, an evaporation deposition layer, or a sputtering deposition layer) is between 0.1 and 3000 microns, more preferably between 1 and 100 microns, for example 4 microns.
[0058] As mentioned above, the implantable device of the present invention can be any type of implantable device, preferably an implantable device with a movable structure. Specifically, the implantable device with a movable structure includes, for example, an implantable mechanical quantity sensor and an implantable actuator.
[0059] Among them, mechanical quantity sensors include, for example, pressure sensors, tactile sensors, acceleration sensors, gyroscopes (or angular velocity sensors), flow sensors, etc. When working, they use their movable structures to convert mechanical quantities into changes in parameters such as stress, deformation or resonant frequency of the movable structure, and then convert these changes into electrical quantities. For example, as a type of pressure sensitive device, the piezoresistive pressure sensor includes a silicon diaphragm that bears the measured pressure and a piezoresistor on the surface of the diaphragm. The silicon diaphragm acts as a transducer element and deforms under the action of the measured pressure to generate stress and strain; the piezoresistor converts the change in strain into a change in resistance, and measures the change in resistance by measuring the circuit to achieve pressure measurement. An intraocular pressure sensor is a typical type of pressure sensitive device.
[0060] Among them, the actuator is also called a driver or actuator, such as a micropump, microvalve, micromotor, microswitch, etc. When working, it converts the control signal and energy into controllable motion and power output of the movable structure, so that the actuator performs work externally under the action of the control signal.
[0061] In the implantable device with a movable structure of the present invention, an integrated coating is provided on the device body, so that a dense, thin, reliable coating that prevents the influence of liquid is deposited on the surface of the device body of the packaged mechanical quantity sensor or actuator. The package coating structure can not only meet the ability to prevent the influence of liquid, but also will not affect the indicators of the sensor or actuator (such as sensitivity, stability, etc.). In addition, it can also make up for the defects such as gap and hysteresis in the sensor, and can also isolate harmful media in the external environment that affect the accuracy of the sensor, thereby improving the accuracy of the device.
[0062] In particular, for implantable intraocular pressure sensors, their ideal size should be within the millimeter level. The size of the devices obtained by the packaging methods of the prior art is generally in the millimeter level or above, mainly because the existing packaging structure size is too large, for example, the ceramic or glass packaging shell is too thick. The packaging structure size of the implantable intraocular pressure sensor of the present invention is very small. For example, the packaging can be completed with the help of a coating of nanometer to micrometer level (such as 100 nanometers to 4000 microns), which meets the ability to prevent the influence of liquids for long-term implantation, so that the overall size of the packaged intraocular pressure sensor remains almost unchanged.
[0063] Preferably, at least the second protective layer 50 is formed of a biocompatible material; more preferably, both the first protective layer 40 and the second protective layer 50 are formed of a biocompatible material. Thus, the periphery of the second protective layer 50 does not need to be treated for biocompatibility, thereby reducing costs and shortening the time used in the packaging process.
[0064] It is easy to imagine that, under the premise that the second protective layer 50 is not formed of a biocompatible material, a biocompatible material coating can also be provided on the outermost layer of the packaging structure (i.e., the periphery of the second protective layer 50) to meet the biocompatibility requirements of implantation in a living body.
[0065] In summary, the implantable device of the present invention utilizes the synergistic effect of a dense nano-scale coating that protects against liquid influence (such as a vapor deposition layer, an atomic layer deposition layer) and a micron-scale coating that protects against liquid influence (such as a chemical vapor deposition layer, etc.), so that the corresponding implantable device has good ability to protect against liquid influence and stability when implanted in the body, wherein the micron-scale coating that protects against liquid influence can prevent the erosion of liquid molecules (such as large molecular clusters composed of more than 10 water molecules), and the dense nano-scale coating that protects against liquid influence can prevent the erosion of water vapor molecules or small molecular clusters composed of less than 10 water molecules, thereby providing dual protection against liquid influence for the implantable device and significantly reducing the packaging size of the implantable device.
[0066] According to a second aspect of the present invention, a packaging method for the above-mentioned implantable device is also provided. Figure 3 As shown, it includes the steps of:
[0067] S40, forming a first protective layer 40 on the periphery of the device body, preferably using atomic layer deposition technology to form an atomic layer deposition layer on the device body, that is, a dense nano-level coating that prevents liquid influence, to obtain Figure 7 and Figure 8 The structure shown;
[0068] S50, forming a second protective layer 50 on the periphery of the first protective layer 40, preferably using chemical vapor deposition technology, or evaporation deposition technology, or sputtering deposition technology, or spraying technology, etc. to form the second protective layer 50 on the periphery of the first protective layer 40, that is, a micron-level coating to prevent liquid influence, to obtain Figure 1 and Figure 2 Preferably, after this step, the packaging of the implantable device is completed.
[0069] It can be seen that the packaging method of the present invention can be completed mainly through two steps of atomic layer deposition and chemical vapor deposition (or evaporation deposition, or sputtering deposition, or spraying, etc.). Compared with the packaging method of the prior art using glass, ceramic, metal and other packaging shells, it has the advantages of high packaging efficiency, low cost, and small size after packaging.
[0070] Illustratively, in step S40, the device body of the implantable device (such as an implantable intraocular pressure sensor) may be placed in an atomic layer deposition chamber, and a coating that prevents liquid influence may be deposited layer by layer on the surface of the device body in the form of a single atomic film.
[0071] Preferably, in step S40, any material that can prevent the influence of liquid, such as one or more of oxides, nitrides, fluorides, metals, carbides, and sulfides (such as a combination of the foregoing materials) can be used to form the first protective layer (such as an atomic layer deposition layer).
[0072] In an exemplary embodiment of atomic layer deposition, for example, tantalum oxide material can be used. For example, the device body is placed in an atomic layer deposition chamber, and the tantalum oxide coating is deposited layer by layer on the surface of the device body in the form of a single atomic film. Specific parameters include, for example: 3000 cycles, thickness 300nm, and so on.
[0073] Illustratively, in step S50, one or more compounds, elemental gases, etc. containing thin film elements can be introduced into a reaction chamber where an implantable device (such as an implantable intraocular pressure sensor) processed in step S40 is placed, and a thin film that prevents the influence of liquids can be deposited on the surface of the implantable device (such as an implantable intraocular pressure sensor) by means of a spatial gas phase chemical reaction.
[0074] Preferably, in step S50, any material that can prevent the influence of liquid, such as one or more of polymers, oxides, sulfides, nitrides, carbides, and ceramics (such as a combination of the foregoing materials) can be used to form the second protective layer (such as a chemical vapor deposition layer).
[0075] In an exemplary embodiment of chemical vapor deposition, for example, polyparaxylene material can be used. For example, the device body is placed in a deposition chamber, and the polyparaxylene coating is uniformly deposited on the surface of the device body (for example, on the periphery of the first protective layer). Specific parameters include, for example: the deposition temperature is room temperature, the thickness is 40 microns, the deposition time is about 10 hours, and so on.
[0076] Preferably, the implantable device comprises a chip 10 and a substrate 20 for mounting the chip 10, such as Figure 3 As shown, before step S40, the following steps may also be included:
[0077] S10, cleaning: cleaning the chip 10;
[0078] S20, chip mounting: the cleaned chip 10 is mounted on the substrate 20. Figure 5 As shown;
[0079] S30, wire bonding: the chip 10 is wire bonded to the substrate 20, for example, by metal wires 30, 31, 32, 33. Figure 6 As shown, after this step is completed, the device body referred to in the present invention is obtained.
[0080] For example, the chip 10 has an outer structure as shown in FIG. Figure 4 shown.
[0081] Among them, the main purpose of step S10 is to clean the surface of the chip 10. For example, the chip can be first immersed in an acetone solution for ultrasonic cleaning for several minutes to several tens of minutes (such as 20 minutes), and then immersed in an isopropanol solution for ultrasonic cleaning for several minutes to several tens of minutes (such as 20 minutes), or directly cleaned by plasma cleaning or the like.
[0082] In step S20 , the cleaned chip 10 may be attached to the substrate 20 preferably by adhesive bonding, conductive adhesive bonding, Au—Si alloy eutectic method, Pb—Sn alloy bonding, or the like.
[0083] In step S30, metal wires are preferably used to connect the electrode lead pads on the chip 10 and the outer lead pads on the base of the substrate 20. Usually, the chip 10 and the substrate 20 can be wire-bonded by methods such as heat pressing, thermal ultrasound and ultrasound.
[0084] Preferably, after step S30, a step of applying glue for protection may be further included: that is, applying a protective glue layer on at least the periphery of each metal lead of the device body to protect the chip 10 and each metal lead 30, 31, 32, 33 from damage during the pressure measurement process. The protective glue used in this step may be any suitable glue material or polymer material, such as polyparaxylene, silicone, PET, PVC or a combination thereof.
[0085] In summary, the present invention realizes the encapsulation of implantable devices by directly performing surface treatment on the device body. On the one hand, the encapsulation scale and thickness can be significantly reduced, and on the other hand, the process steps can be reduced. At the same time, it is easy to obtain good biocompatibility and stability to prevent liquid influence during long-term implantation in the body. In addition, for pressure-sensitive devices with movable parts inside, the ultra-thin coating will not have a significant impact on sensor characteristics such as sensitivity, thereby meeting the requirements of long-term implantation and normal operation of devices (such as intraocular pressure sensors). In addition, after encapsulation, not only can the defects of gap and hysteresis in the sensor be compensated, but also harmful media in the external environment that affect the accuracy of the sensor can be isolated, thereby improving the accuracy of the device.
[0086] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned preferred schemes can be freely combined and superimposed (such as a composite structure of more than two layers composed of a nano-scale coating and a micro-scale coating and a surface protection method thereof).
[0087] It should be understood that the above-mentioned embodiments are merely illustrative and not restrictive. Without departing from the basic principles of the present invention, various obvious or equivalent modifications or substitutions that can be made by those skilled in the art to the above-mentioned details will all be included in the scope of the claims of the present invention.
Claims
1. An implantable device for implantation in a living body, characterized in that: The implantable device comprises a device body and a packaging structure arranged around the device body, wherein the packaging structure comprises a first protective layer covering the device body and a second protective layer located around the first protective layer. The first protective layer is a coating that prevents liquids from being affected by nanometers, and the second protective layer is a coating that prevents liquids from being affected by micrometers; The thickness of the nano-level coating that prevents liquid influence is between 0.1 and 1000 nanometers, and the thickness of the micro-level coating that prevents liquid influence is between 0.1 and 3000 micrometers; The implantable device is an implantable intraocular pressure sensor with a movable structure; The nano-scale coating that protects against liquid influence is an atomic layer deposition layer; The micron-level coating that prevents liquid influence is a vapor deposition layer, or an evaporation deposition layer, or a sputtering deposition layer, or a spraying deposition layer; The micron-scale coating that prevents liquid influence can prevent erosion by macromolecular groups composed of more than 10 liquid molecules, and the nano-scale coating that prevents liquid influence can prevent erosion by gas molecules or small molecular groups composed of less than 10 liquid molecules; In the packaging structure, at least the second protective layer is formed of a biocompatible material.
2. A packaging method for the implantable device according to claim 1, characterized in that: Includes steps: S40, forming the first protective layer on the periphery of the device body; S50, forming the second protective layer on the periphery of the first protective layer.
3. The packaging method according to claim 2, characterized in that: The implantable device includes a chip and a substrate for mounting the chip, and before step S40, further includes the following steps: S10, cleaning the chip; S20, attaching the cleaned chip to the substrate; S30, performing wire bonding on the chip and the substrate to form the device body.
4. The packaging method according to claim 2 or 3, characterized in that: Using atomic layer deposition technology to form the nano-scale coating that prevents liquid influence on the device body; And / or, the micron-scale coating that protects against liquids is formed by using vapor deposition technology, evaporation technology, sputtering technology, or spraying technology.
5. The packaging method according to claim 4, characterized in that: One or more of oxides, nitrides, fluorides, metals, carbides, sulfides, and polymers are used to form the nano-scale coating that protects against liquids; And / or, the micron-scale coating that protects against liquids is formed by using one or more of polymers, oxides, sulfides, nitrides, carbides, and ceramics.
Citation Information
Patent Citations
Implantable device
CN209411765U
Micro-miniature implantable coated device
US20060173497A1