Methods for making foam containers and foam containers

Using water-based foaming ink and flexo printing technology to produce foam containers solves the problems of poor insulation and health risks in existing refrigerated containers, achieves good insulation and environmentally friendly and healthy production, and improves product safety and user experience. .

CN109929324BActive Publication Date: 2024-10-11杭州顶正包材有限公司 +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN201910252212.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-03-29
Publication Date
2024-10-11
Estimated Expiration
2039-03-29

AI Technical Summary

Technical Problem

The packaging of existing refrigerated or frozen containers has poor insulation effect, which can easily lead to product deterioration and inconvenience to hold. In addition, gravure printing technology is complex and costly, and solvent-based inks pose health risks.

Method used

Water-based foaming ink and flexo printing technology are used to make foam containers through laminating, printing and heating steps to form a structure of ink layer, first polyethylene layer, paper layer and second polyethylene layer to achieve good heat insulation and Environmentally friendly and healthy production.

Benefits of technology

It improves the heat insulation capacity of the container, reduces the volatilization of harmful gases, avoids the risk of solvent residue, enhances the health and safety of workers and consumers, and improves hand-holding comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109929324B_ABST
    Figure CN109929324B_ABST
Patent Text Reader

Abstract

The present invention provides a method for making a foaming container and a foaming container. The method for making a foaming container comprises a laminating step, a printing step and a heating step. Laminating step: laminating on both sides of a paper layer to obtain a first polyethylene layer and a second polyethylene layer respectively; printing step: printing an aqueous foaming ink on the first polyethylene layer to obtain an ink layer; and heating step: heating the first polyethylene layer and the ink layer to foam. The foaming container is made by the method for making a foaming container, and the foaming container comprises a container wall and a container bottom, and the container wall comprises: an ink layer, a first polyethylene layer, a paper layer and a second polyethylene layer in sequence.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of packaging, in particular to a method for manufacturing a foaming container and the foaming container. Background Art

[0002] With the improvement of living standards, people's demands for the quality, functionality and user experience of containers for daily necessities are also constantly increasing. In particular, there are increasingly higher requirements for the thermal insulation capacity of containers. The packaging used for refrigerated and frozen containers on the market currently usually has a structure of ink layer / PE coating layer / paper layer / PE coating layer, and the thermal insulation effect of this packaging is poor. Therefore, some products that need to be refrigerated or frozen are prone to melting or deterioration. Secondly, the temperature difference between the container containing the product taken out of the freezing environment and the external environment is too large, and a large amount of water droplets are easily formed on the surface, which wets the paper layer of the container and causes damage to the packaging. Furthermore, the temperature of the container surface is too cold, and the cold insulation effect is poor when held in hand, and it is easy to slip.

[0003] The foam layer can effectively insulate heat. The structure of the main foam containers currently available on the market is: ink layer / polyethylene (PE) foam layer / paper layer / PE coating layer. However, the production of such foam containers requires gravure printing, and the ink used in the ink layer is solvent-based ink. However, gravure printing requires complex pre-press platemaking technology, long production cycles, and high platemaking costs. Furthermore, the use of volatile solvents results in high levels of harmful gases in the workshop, significantly harming the health of workers. Furthermore, gravure printing platemaking is complex, the salaries required by gravure printing practitioners are relatively high, and there is a high reliance on manual labor, resulting in high production costs. Furthermore, solvent-based inks carry the risk of residual solvents, posing a significant safety hazard to the health of sellers. Summary of the Invention

[0004] The object of the present invention is to provide a method for manufacturing a foaming container which has good heat insulation capability and does not require the use of oil-based ink, and the foaming container.

[0005] To address the above technical issues, the present invention provides a method for manufacturing a foaming container, comprising a laminating step, a printing step, and a heating step. The laminating step comprises laminating both sides of a paper layer to form a first polyethylene layer and a second polyethylene layer, respectively; the printing step comprises printing a water-based foaming ink on the first polyethylene layer to form an ink layer; and the heating step comprises heating the first polyethylene layer and the ink layer to form foaming layers.

[0006] According to this aspect of the present invention, the aqueous foaming ink is a synchronous aqueous foaming ink, and the synchronous aqueous foaming ink comprises the following components by weight percentage:

[0007]

[0008]

[0009] According to this aspect of the present invention, in the laminating step, low-density polyethylene and the additive are laminarized to obtain a first polyethylene layer, and medium-density polyethylene and the additive are laminarized to obtain a second polyethylene layer.

[0010] According to this aspect of the invention, the low density polyethylene has a melt index of 11-14, and the medium density polyethylene has a melt index of 7-10.

[0011] According to this aspect of the present invention, the fineness of the aqueous foaming ink is less than 5 μm.

[0012] According to this aspect of the invention, printing is performed using flexographic or gravure techniques.

[0013] In the second aspect of the present invention, the present invention also provides a foam container, which is made by the foam container manufacturing method. The foam container includes a container wall and a container bottom. The container wall includes: an ink layer, a first polyethylene layer, a paper layer and a second polyethylene layer in sequence.

[0014] According to a second aspect of the present invention, a container bottom comprises a third polyethylene layer and a paper layer.

[0015] According to the second aspect of the present invention, the thickness of the first polyethylene layer is in the range of 800 μm to 900 μm.

[0016] According to the second aspect of the present invention, the heat seal strength of the second polyethylene layer and the paper layer is 4

[0017] N / 15mm~25N / 15mm.

[0018] In summary, the printing step in the foam container manufacturing method of the present invention utilizes water-based foaming ink, which has the advantages of being environmentally friendly and healthy compared to the oil-based inks used in the prior art. During the manufacturing process, since the water-based foaming ink contains essentially no organic solvents, there is essentially no volatilization of organic solvents during the printing step and the subsequent heating step, thereby preventing the problem of relatively high levels of harmful gases, which is beneficial for maintaining the safety of the manufacturing workers. Furthermore, solvent-based inks carry the risk of solvent residue, posing a significant safety hazard to the health of the seller. However, the foam container manufacturing method of the present invention utilizes water-based foaming ink, the solvent of which is primarily water, so there is no need to worry about the problem of organic solvent residue. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a flow chart of a method for manufacturing a foaming container provided in Example 1 of the present invention;

[0020] Figure 2 is a schematic diagram of a foaming container provided in Example 1 of the present invention;

[0021] Figure 3 It is a cross-sectional view of the container wall of the foaming container provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0023] Example 1

[0024] Please refer to Figure 1 The first invention of the present invention provides a method for manufacturing a foaming container, comprising a laminating step, a printing step, and a heating step.

[0025] Laminating step S01: laminating both sides of the paper layer 13 to obtain a first polyethylene layer 12 and a second polyethylene layer 14 respectively;

[0026] Printing step S02: printing water-based foaming ink on the first polyethylene layer 12 to obtain an ink layer 11; and

[0027] Heating step S03: The first polyethylene layer 12 and the ink layer 11 are heated and foamed.

[0028] The printing step in the foaming container manufacturing method uses water-based foaming ink, which is environmentally friendly and healthier than the oil-based inks used in the prior art. During the manufacturing process, since the water-based foaming ink contains essentially no organic solvents, there is essentially no volatilization of organic solvents during the printing step and the subsequent heating step, thus avoiding the problem of high levels of harmful gases and benefiting the safety of production workers. Furthermore, solvent-based inks carry the risk of solvent residue, posing a significant safety hazard to the health of sellers. However, the foaming container manufacturing method of the present invention uses water-based foaming ink, the solvent of which is primarily water, so there is no need to worry about organic solvent residue.

[0029] Furthermore, the first polyethylene layer 12 and ink layer 11 of the present invention form a foamed layer after foaming. The foamed layer contains air bubbles, which are poor conductors of heat. Therefore, the foamed layer has excellent thermal insulation capabilities. For products requiring insulation or frozen packaging, it can provide insulation and heat preservation, preventing burns and prolonging food cooling time. It also provides insulation and prolonged thawing time for frozen product packaging. Furthermore, the foamed container has excellent heat and cooling effects when held in the hand, and water is less likely to form on the outer walls.

[0030] Furthermore, the water-based foaming ink in this embodiment is a synchronous water-based foaming ink. Synchronous ink means that it can maintain synchronous foaming with the first polyethylene layer 12. If the water-based foaming ink and the first polyethylene layer 12 cannot foam synchronously, the first polyethylene layer 12 may foam faster or slower than the ink layer 11, causing the first polyethylene layer 12 or the ink layer 11 to expand faster than the other layer, thereby affecting the adhesion of the ink layer 11 to the first polyethylene and seriously affecting the flatness of the ink layer 11 and the ink display effect. Using synchronous ink can avoid this situation.

[0031] The water-based ink in this embodiment uses water as the main solvent / dispersion medium, ammonia, organic amine, or ammonia and organic amine as the neutralizer, and water-based acrylic resin / emulsion as the binder. The synchronous water-based foaming ink in this embodiment is made by mixing the following components by weight:

[0032]

[0033]

[0034] The pigments in the present invention can be both organic and inorganic pigments. Pigments are used to color synchronous water-based foaming inks, which can meet the appearance requirements of foaming containers in different colors. Organic pigments have bright colors, strong tinting power, low density, and are non-toxic. Organic pigments look relatively loose, while inorganic pigments are heavier. Organic pigments generally have a higher brightness and higher tinting power than inorganic pigments. In other embodiments, water-based acrylic resins and water-based acrylic emulsions can also increase the water solubility of the resin by introducing hydrophilic groups such as hydroxyl groups, amido groups, or ether bonds through the selection of appropriate modifiers, thereby increasing the color saturation of the ink layer 11. Silicone is used for defoaming to avoid the appearance of a large number of bubbles during the stirring of the ink, which affects the appearance and color of the ink layer 11.

[0035] The silica used in this embodiment serves as a dispersant and flow control agent, and silica exhibits strong UV resistance and catalytic properties. The sun resistance of inks using silica as a filler can generally be improved by 2 to 3 levels, and the abrasion resistance, heat resistance, and adhesion strength of the ink layer 11 are significantly improved. Furthermore, the silica is fumed silica. Fumed silica (3% by mass) and aqueous acrylic acid are uniformly mixed and then dispersed, resulting in an ink with high stability. The polyethylene wax and polytetrafluoroethylene wax in this embodiment primarily serve to enhance gloss, leveling, and scratch resistance.

[0036] The preparation steps for the synchronous water-based ink in this embodiment are as follows: dissolution - pre-dispersion - grinding - conditioning. Dissolution involves dissolving the water-based acrylic resin into a uniform resin solution using ammonia, an organic amine, and water. Pre-dispersion and grinding are used to evenly distribute the pigment throughout the resin. Conditioning adjusts the ink's physical properties, including viscosity, color, and adhesion.

[0037] This embodiment also includes a drying or humidification step. Humidity levels vary depending on the storage environment, especially during the rainy season, which can lead to excessive moisture in the paper. Therefore, the paper needs to be dried before use. In northern winter, the air is too dry, and the moisture in the paper is insufficient to form bubbles during the foaming process. Therefore, the paper needs to be humidified before use. However, the present invention does not impose any restrictions on the drying or humidification steps; in other production methods, the paper can also be stored in a constant humidity environment.

[0038] In this embodiment, the laminating step precedes the heating step. However, in other embodiments, a first polyethylene layer 12 can be formed by laminating one side of the paper layer 13. Then, a water-based foaming ink is printed on the first polyethylene layer 12 to form the ink layer 11. Furthermore, the first polyethylene layer 12 and the ink layer 11 are heated and foamed. Finally, a second polyethylene layer 14 is formed by laminating the other side of the paper layer 13. Since the second polyethylene layer 14 is not formed on the other side of the paper layer 13 during heating, air, an inert gas, or the like can be introduced along the direction from the paper layer 13 to the foaming layer to ensure uniform bubbles in the foaming layer and enhance the foaming effect.

[0039] In this embodiment, the first polyethylene layer 12 is obtained by laminating low-density polyethylene and an additive, and the second polyethylene layer 14 is obtained by laminating medium-density polyethylene and an additive. The melt index of low-density polyethylene is 11 to 14, and the melt index of medium-density polyethylene is 7 to 10. The low-density polyethylene (LDPE) mentioned in the present invention is generally produced by high-pressure polymerization and has a density of 0.910 g / cm 3 ~0.925g / cm 3 The molecular structure of low-density polyethylene (LDPE) is a linear macromolecule with numerous branches. The varying lengths of the branches on the main chain affect the regularity of the macromolecular arrangement, resulting in loose packing and hindering crystallization. Consequently, the crystallinity is generally between 55% and 65%. LDPE has a low melting point and a soft texture. The long branches give it low viscosity at high shear rates during processing and high melt strength during stretching. LDPE and additive coatings exhibit foaming properties at certain temperatures.

[0040] Medium density polyethylene (MDPE) is a polyethylene produced by copolymerizing α-olefins with high efficiency catalysts at low to medium pressure to control its density (0.926 g / cm 3~0.940g / cm 3 ), with a crystallinity of 70% to 80%. Due to its numerous and long side chains, its density and crystallinity decrease, resulting in medium-density polyethylene (MDPE) having better flexibility and low-temperature properties, but inferior tensile strength, hardness, and heat resistance to high-density polyethylene (HDPE). Because co-olefins increase the number of interlamellar links within the MDPE crystals, its resistance to slow cracking and long-term mechanical strength are significantly improved compared to LDPE. Placing the higher-density MDPE close to the side of a foam container containing beverages, food, or other items effectively isolates the contents from the environment.

[0041] In this embodiment, the fineness of the water-based foaming ink is less than 5 μm. When the fineness of the ink is greater than this value, the foaming effect of the ink layer 11 will be affected.

[0042] In this embodiment, flexographic printing is performed using a 130# high-line-count flexographic printing technique, which improves printing precision, achieves rich colors, vivid patterns, and can achieve metallic, tactile, and concave-convex three-dimensional effects.

[0043] Please refer to Figure 2 and Figure 3 This embodiment also provides a foam container manufactured by the foam container manufacturing method. The foam container includes a container wall 1 and a container bottom 2. The container wall 1 includes an ink layer 11, a first polyethylene layer 12, a paper layer 13, and a second polyethylene layer 14 in sequence.

[0044] In this embodiment, the container wall 1 further includes a protective layer, which is disposed on the outside of the ink layer 11 and is used to protect the ink layer 11 from being scratched or dissolved.

[0045] In this embodiment, the paper layer 13 is made of high-density base paper with uniform moisture content. When heated, the moisture in the paper layer turns into water vapor and enters the PE layer, thereby forming the PE into a foamed layer with uniform bubble size.

[0046] In this embodiment, the container bottom 2 is composed of a third polyethylene layer and a paper layer 13. In other embodiments, the container bottom 2 can also be made of the same material as the container wall 1. That is, the entire foam container can be pressed from the same material, eliminating the need to splice different materials and saving steps.

[0047] In this embodiment, the thickness of the first polyethylene layer 12 is 800 μm, which refers to the thickness of the first polyethylene layer 12 after foaming. In other embodiments, the thickness of the first polyethylene layer 12 may also be 900 μm or 850 μm.

[0048] In this embodiment, the heat sealing strength between the second polyethylene layer 14 and the paper layer 13 is 4 N / 15 mm. In other embodiments, the heat sealing strength between the second polyethylene layer 14 and the paper layer 13 is 25 N / 15 mm, or the heat sealing strength between the second polyethylene layer 14 and the paper layer 13 is 20 N / 15 mm, or the heat sealing strength between the second polyethylene layer 14 and the paper layer 13 is 10 N / 15 mm.

[0049] Example 2

[0050] The steps for making the foaming container and the foaming container in Example 2 are basically the same as those in Example 1, with only slight differences in the composition of the water-based foaming ink. The same structures are numbered the same, and the differences are described below.

[0051] The water-based foaming ink is a synchronous water-based foaming ink. In this embodiment, the synchronous water-based foaming ink comprises the following components by weight:

[0052]

[0053] Example 3

[0054] The steps for making the foaming container and the foaming container in Example 3 are basically the same as those in Example 1, with only slight differences in the composition of the water-based foaming ink. The same structure is numbered the same, and the differences are described below.

[0055] The water-based foaming ink is a synchronous water-based foaming ink. In this embodiment, the synchronous water-based foaming ink comprises the following components by weight:

[0056]

[0057]

[0058] Example 4

[0059] The steps for making the foaming container and the foaming container in Example 4 are basically the same as those in Example 1, with only slight differences in the composition of the water-based foaming ink. The same structures are numbered the same, and the differences are described below.

[0060] The water-based foaming ink is a synchronous water-based foaming ink. In this embodiment, the synchronous water-based foaming ink comprises the following components by weight:

[0061]

[0062] Example 5

[0063] The steps for making the foaming container and the foaming container in Example 5 are basically the same as those in Example 1, with only slight differences in the composition of the water-based foaming ink. The same structures are numbered the same, and the differences are described below.

[0064] The water-based foaming ink is a synchronous water-based foaming ink. In this embodiment, the synchronous water-based foaming ink comprises the following components by weight:

[0065]

[0066] In the manufacturing methods of the foaming containers in Examples 1 to 5, the ink layer and the first polyethylene layer can maintain synchronous foaming, and the inks are relatively stable. The finished foaming containers also have good stability in water and will not fall off or be scratched due to the ink being easily dissolved by water due to the water-based ink.

[0067] Those skilled in the art should understand that, in the disclosure of the present invention, the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the above terms cannot be understood as limiting the invention.

[0068] Although the present invention has been disclosed above by means of preferred embodiments, this is not intended to limit the present invention. Anyone skilled in the art may make slight changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the scope of protection required by the claims.

Claims

1. A method for making a foaming container, characterized in that: include: Laminating step: laminating one side of the paper layer to obtain a first polyethylene layer; Printing step: printing water-based foaming ink on the first polyethylene layer to obtain an ink layer; Heating step: the first polyethylene layer and the ink layer are heated and foamed; and Finally, a second polyethylene layer is formed by laminating the other side of the paper layer; The aqueous foaming ink is a synchronous aqueous foaming ink, and the synchronous aqueous foaming ink comprises the following components by weight percentage: Organic pigment or inorganic pigment 10%~40%; Water-based acrylic resin 14%~20%; Water-based acrylic emulsion 54%~64%; Fumed silica 3%; Silicone defoamer 0.1%~1%; Polyethylene wax and polytetrafluoroethylene wax 0.1%~5%; Ammonia and organic amine 0.1%~5%; The sum of the contents of the components of the synchronous water-based foaming ink should be equal to 100%; Wherein, the water-based acrylic resin and water-based acrylic emulsion are modified by introducing a hydrophilic group to increase the water solubility of the resin, and the hydrophilic group includes a hydroxyl group, an amide group or an ether bond; Among them, the synchronous water-based foaming ink can maintain synchronous foaming with the first polyethylene layer; wherein the fumed silica and aqueous acrylic acid are uniformly mixed and then dispersed; The preparation steps of the synchronous water-based foaming ink are as follows: dissolving-pre-dispersing-grinding-conditioning; wherein dissolving means dissolving the water-based acrylic resin into a uniform resin liquid, pre-dispersing and grinding are to evenly distribute the pigment into the resin, and conditioning is to adjust the various physical properties of the ink; Wherein, in the coating step, low-density polyethylene and the additive are coated to obtain a first polyethylene layer, and medium-density polyethylene and the additive are coated to obtain a second polyethylene layer; Wherein, the melt index of the low-density polyethylene is 11-14, and the melt index of the medium-density polyethylene is 7-10.

2. The method for making a foaming container according to claim 1, characterized in that: The fineness of the aqueous foaming ink is less than 5 μm.

3. The method for making a foaming container according to claim 1, characterized in that: The printing adopts flexographic printing technology or gravure printing technology.

4. A foaming container, made by the method for making a foaming container according to any one of claims 1 to 3, characterized in that: The foaming container comprises a container wall and a container bottom, wherein the container wall comprises in sequence: an ink layer, a first polyethylene layer, a paper layer and a second polyethylene layer; The container bottom includes a third polyethylene layer and a paper layer; The thickness of the first polyethylene layer ranges from 800 μm to 900 μm; The heat sealing strength between the second polyethylene layer and the paper layer is 4 N / 15mm to 25 N / 15mm.

Citation Information

Cited By

  • Tactile heat-insulating packaging film and packaging bag