A kind of electrode material based on 3C-SiC film and preparation method thereof
By growing a porous 3C-SiC film on a single crystal Si substrate, the problem of supercapacitor electrode materials easily falling off at high temperatures is solved, the capacitance and cycle characteristics are improved, and it is suitable for micro supercapacitors, achieving high structural stability and high performance. Energy density electrode materials.
Patent Information
- Application Number
- CN201910703335.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-07-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2039-07-31
AI Technical Summary
The electrode materials of existing supercapacitors tend to fall off under high operating temperatures, resulting in reduced cycle characteristics, and the thermal expansion mismatch between the electrode energy storage active material and the current collection matrix affects stability and energy density.
The chemical vapor deposition method is used to grow a porous 3C-SiC film on a single crystal Si substrate. The concave and convex structure is formed by laser etching to promote the growth of the 3C-SiC film, increase the interface area with the electrolyte, and improve the structural stability of the electrode material. .
The specific capacitance and cycle characteristics of the supercapacitor are significantly improved, ensuring high performance under high temperature and large current conditions. It is suitable for micro supercapacitors, and the process is simple and does not require metal catalysts.
Smart Images

Figure CN110534348B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic materials, and in particular relates to an electrode material based on a 3C-SiC film and a preparation method thereof. Background Art
[0002] With the continuous use of non-renewable energy and the increasingly serious environmental pollution problem, research on improving energy conversion efficiency and storage device capacity is becoming more and more urgent. Compared with other energy storage devices, supercapacitors are considered to be perfect energy storage devices. Supercapacitors store electrical energy at the interface between electrodes and electrolytes without chemical reactions. Supercapacitors complement the existing rechargeable battery market, especially in the fields of high-speed charging and discharging and high energy density. Improving the safety, stability and energy density of supercapacitors in a large operating temperature range is one of the urgent problems to be solved in this field. In order to improve the stability of supercapacitors in a large temperature range, the following key issues need to be considered: 1) At high operating temperatures, the energy conversion is intense, which can cause the electrolyte to hit the electrode, causing the electrode material to fall off, thereby reducing the cycle characteristics of the battery; 2) There is a thermal expansion mismatch between the electrode energy storage active material and the current collection matrix. When the operating temperature fluctuates in a large range, it can cause the active material to fall off. Therefore, it is of great research significance to prepare electrode materials with high structural stability.
[0003] Cubic silicon carbide (3C-SiC) is the most popular third-generation wide bandgap semiconductor material, with excellent properties such as high electron mobility, high breakdown electric field strength, high thermal stability, high strength and corrosion resistance. In addition, 3C-SiC is deposited on the surface of the Si substrate through vapor deposition technology, and the substrate and the film interface are firmly connected. Therefore, 3C-SiC has excellent properties such as high temperature resistance, thermal shock resistance, and high cycle performance as an electrode material. At present, there are literature reports on the use of single crystal Si substrates to grow whisker-like SiC as a supercapacitor electrode material, but the resulting electrode material has a low specific capacitance. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an electrode material based on 3C-SiC film and a preparation method thereof in view of the above-mentioned deficiencies in the prior art. A chemical vapor deposition method (CVD) is adopted, and a single crystal Si is used as a substrate, on which a porous 3C-SiC film is grown. The porous structure film has a large interface area with the electrolyte, which is beneficial to improving the specific capacitance of the supercapacitor.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0006] Provided is an electrode material based on a 3C-SiC film, which consists of a single crystal Si substrate and a 3C-SiC film with a porous structure grown on the substrate.
[0007] According to the above scheme, the single crystal Si substrate is Si (111) with a purity of >99.999%.
[0008] According to the above scheme, the thickness of the 3C-SiC film with a porous structure is 20 to 60 μm.
[0009] The present invention also provides a method for preparing the above-mentioned electrode material based on 3C-SiC film, and the specific steps are as follows:
[0010] 1) Place a single crystal Si substrate on a substrate holder in a deposition chamber of a cold wall laser chemical vapor deposition device, and evacuate the chamber to reduce the pressure in the deposition chamber to below 10 Pa;
[0011] 2) H2 is introduced into the deposition chamber from the upper side of the deposition chamber, and the laser is turned on to irradiate the surface of the single-crystalline Si substrate to heat the single-crystalline Si substrate to 1200-1280°C, and the temperature is kept stable. The single-crystalline Si substrate is etched under high temperature conditions using H2 to form a concave-convex structure on the surface of the substrate. After the etching is completed, the temperature and the amount of gas introduced into the deposition chamber are kept unchanged, and a carrier gas containing HMDS (hexamethyldisilane) is introduced into the deposition chamber from the upper side of the deposition chamber. At the same time, H2 is introduced as a diluent gas, and the deposition pressure in the deposition chamber is adjusted to deposit and grow a 3C-SiC porous thin film. After the deposition is completed, the laser, H2 and the carrier gas are turned off, the deposition chamber is evacuated and naturally cooled to room temperature to obtain an electrode material based on a 3C-SiC thin film.
[0012] According to the above scheme, the flow rate of H2 introduced into the deposition chamber in step 2) is 1000-3000 sccm.
[0013] According to the above scheme, the wavelength of the laser in step 2) is 800-1000nm.
[0014] According to the above scheme, the etching time in step 2) is 1 to 3 minutes.
[0015] According to the above scheme, the carrier gas in step 2) is a mixed gas of Ar and HMDS, and the carrier gas flow rate is 25 sccm. When the HMDS-containing gas flow passes through the substrate surface from the upper side of the deposition chamber, it is difficult to blow into the depression, so there is basically no SiC generated in the depression.
[0016] According to the above scheme, the flow rate of HMDS in the carrier gas in step 2) is 2-10 sccm.
[0017] According to the above scheme, the conditions for depositing and growing the 3C-SiC porous film in step 2) are: deposition pressure of 300-500 Pa, and deposition time of 10-50 min.
[0018] The present invention uses single crystal Si as a substrate, irradiates the substrate with laser in advance, and makes the Si substrate etched by H2 under high temperature conditions. Under high temperature conditions, H2 reacts with Si to generate gaseous SiH x (x=1~4), thereby forming a concave-convex structure on the surface of the Si substrate, and then a carrier gas containing hydrogen and a precursor HMDS is introduced to deposit and grow a 3C-SiC film on the surface of the substrate. Since the Si substrate forms a concave-convex structure after etching, the 3C-SiC film is promoted to have a porous structure.
[0019] The beneficial effects of the present invention are as follows: 1. The present invention first uses a single crystal Si as a substrate, pre-irradiates the substrate with a laser, and etches the Si substrate with H2 under high temperature conditions to form a concave-convex structure surface, and then grows a porous 3C-SiC film on the substrate surface by a CVD process. The obtained electrode material has a high specific capacitance (up to 4.8mF / cm 2 ), which can significantly improve the capacitance of the supercapacitor, and the 3C-SiC film is firmly connected to the Si substrate, and the thermal expansion coefficients of 3C-SiC and Si are both small, so under high temperature and high current conditions, it can still maintain high cycle characteristics, so it is suitable for preparing electrode materials and has important application prospects in the field of integrated micro supercapacitors; 2. The process flow of the present invention is simple, and a porous structure 3C-SiC film can be obtained without the use of a metal catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Surface SEM images of the single crystal Si substrate before (a) and after (b) H2 etching in Example 1 of the present invention;
[0021] Figure 2 The XRD pattern of the 3C-SiC film obtained in Example 1;
[0022] Figure 3 The SEM images of the surface (a) and cross section (b) of the 3C-SiC film obtained in Example 1;
[0023] Figure 4 Schematic diagram of the formation mechanism of the porous structure of the 3C-SiC film in Example 1;
[0024] Figure 5 The electrochemical CV curve (a) and the specific capacitance variation trend diagram (b) of the porous 3C-SiC film obtained in Example 1 measured in a KCl solution with a concentration of 2 mol / L are shown. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.
[0026] The single crystal Si substrate used in the embodiment of the present invention is Si(111) with a purity of >99.999% and a thickness of 0.5 mm.
[0027] Example 1
[0028] An electrode material based on 3C-SiC film, the preparation method of which comprises the following steps:
[0029] 1) Place a single crystal Si substrate on a substrate holder in a deposition chamber of a cold wall laser chemical vapor deposition device, and evacuate the chamber to reduce the pressure in the deposition chamber to below 10 Pa;
[0030] 2) H2 was introduced into the deposition chamber from the upper side of the deposition chamber, and the H2 flow rate was 1500 sccm;
[0031] 3) Turn on the laser to irradiate the surface of the single crystal Si substrate, the wavelength of the laser is 1000nm, the temperature of the single crystal Si substrate is raised to 1250℃, and the temperature is kept for 2 minutes. The Si substrate is etched under high temperature conditions using H2 to form a concave-convex structure on the surface of the substrate;
[0032] 4) Keeping the temperature and gas flow rate in the deposition chamber unchanged, hydrogen and Ar carrier gas containing precursor HMDS are introduced into the deposition chamber from the upper side of the deposition chamber, with a carrier gas flow rate of 25 sccm, of which the HMDS flow rate is 3 sccm;
[0033] 5) Adjust the pressure in the deposition chamber to 400 Pa and maintain it for 30 minutes;
[0034] 6) Turn off the laser, the H2-containing and HMDS-containing carrier gases, evacuate the deposition chamber and cool it naturally to room temperature to obtain an electrode material based on a 3C-SiC film.
[0035] like Figure 1 The surface SEM images of the single crystal Si substrate before (a) and after (b) H2 etching in this embodiment show that a concave-convex structure is formed on the surface of the substrate after etching. The XRD spectrum of the film obtained in this embodiment is shown in Figure 2 The XRD spectrum shows diffraction peaks of 3C-SiC (111), (331) and (220), indicating that the film is 3C-SiC. Figure 3 The SEM images of the surface (a) and cross section (b) of the 3C-SiC film show that the surface of the film has a cauliflower-like morphology, and the cross section shows that the film grows in a columnar shape with gaps between the crystal columns. It can be seen that the film has a porous structure and the film thickness is about 38 μm. Figure 4As shown in FIG. 1 , after the Si substrate is etched by H2, a concave-convex structure is formed on the surface. When the precursor HMDS gas flow passes through the substrate surface, it is difficult to blow into the concave part, so no SiC is generated in the concave part. However, the protruding part of the Si substrate can be exposed to a large amount of HMDS gas flow, so SiC can grow in the protruding part, and a columnar porous structure film is formed as the growth time increases. The area specific capacitance test results of the porous 3C-SiC film prepared in this embodiment are shown in FIG. Figure 5 As shown in the figure, the electrochemical CV curve (a) and the specific capacitance change trend diagram (b) were measured in a KCl solution with a concentration of 2 mol / L. The CV curve is rectangular, indicating its double-layer capacitance properties. When the scan rate is 10 mV / s, the specific capacitance of the film reaches 4.80 mF / cm 2 , which is higher than similar materials reported in the literature. This is because the 3C-SiC film has a porous structure and the surface of the 3C-SiC crystal column is rough, which makes the film have a high specific surface area and thus a high specific capacitance.
[0036] Example 2
[0037] An electrode material based on 3C-SiC film, the preparation method of which comprises the following steps:
[0038] 1) Place a single crystal Si substrate on a substrate holder in a deposition chamber of a cold wall laser chemical vapor deposition device, and evacuate the chamber to reduce the pressure in the deposition chamber to below 10 Pa;
[0039] 2) H2 is introduced into the deposition chamber from the upper side of the deposition chamber, and the H2 flow rate is 1000 sccm;
[0040] 3) Turn on the laser to irradiate the surface of the single crystal Si substrate, the wavelength of the laser is 1000nm, the temperature of the single crystal Si substrate is raised to 1200℃, and the temperature is kept for 3 minutes. The Si substrate is etched under high temperature conditions using H2 to form a concave-convex structure on the surface of the substrate;
[0041] 4) Keeping the temperature and gas flow rate in the deposition chamber unchanged, hydrogen and Ar carrier gas containing precursor HMDS are introduced into the deposition chamber from the upper side of the deposition chamber, with a carrier gas flow rate of 25 sccm, of which the HMDS flow rate is 2 sccm;
[0042] 5) Adjust the pressure in the deposition chamber to 300 Pa and maintain it for 50 minutes;
[0043] 6) Turn off the laser and the carrier gas containing H2 and HMDS, evacuate the deposition chamber and cool it naturally to room temperature to obtain an electrode material based on a 3C-SiC film.
[0044] Example 3
[0045] An electrode material based on 3C-SiC film, the preparation method of which comprises the following steps:
[0046] 1) Place a single crystal Si substrate on a substrate holder in a deposition chamber of a cold wall laser chemical vapor deposition device, and evacuate the chamber to reduce the pressure in the deposition chamber to below 10 Pa;
[0047] 2) H2 is introduced into the deposition chamber from the upper side of the deposition chamber, and the H2 flow rate is 3000 sccm;
[0048] 3) Turn on the laser to irradiate the surface of the single crystal Si substrate, the wavelength of the laser is 1000nm, the temperature of the single crystal Si substrate is raised to 1280℃, and the temperature is kept for 1min. The Si substrate is etched under high temperature conditions using H2 to form a concave-convex structure on the surface of the substrate;
[0049] 4) Keeping the temperature and gas flow rate in the deposition chamber unchanged, hydrogen and Ar carrier gas containing precursor HMDS are introduced into the deposition chamber from the upper side of the deposition chamber, with a carrier gas flow rate of 25 sccm, of which the HMDS flow rate is 10 sccm;
[0050] 5) Adjust the pressure in the deposition chamber to 500 Pa and maintain it for 10 minutes;
[0051] 6) Turn off the laser, the H2 and HMDS carrier gases, evacuate the deposition chamber and cool it naturally to room temperature to obtain an electrode material based on a 3C-SiC film.
Claims
1. A method for preparing an electrode material based on 3C-SiC film, characterized in that: The specific steps are as follows: 1) Place the single crystal Si substrate on the substrate holder of the deposition chamber of the cold wall laser chemical vapor deposition device, and evacuate the chamber to reduce the pressure to below 10Pa; 2) H2 is introduced into the deposition chamber from the upper side of the deposition chamber, and the laser is turned on to irradiate the surface of the single crystal Si substrate, so that the temperature of the single crystal Si substrate is raised to 1200-1280°C, and the temperature is kept stable. The single crystal Si substrate is etched under high temperature conditions using H2 to form a concave-convex structure on the surface of the substrate. After the etching is completed, the temperature and the amount of gas introduced into the deposition chamber are kept unchanged, and a carrier gas containing HMDS is introduced into the deposition chamber from the upper side of the deposition chamber. At the same time, H2 is introduced as a dilution gas, and the deposition pressure in the deposition chamber is adjusted to deposit and grow a 3C-SiC porous film. After the deposition is completed, the laser, H2 and the carrier gas are turned off, and the deposition chamber is evacuated and naturally cooled to room temperature to obtain an electrode material based on a 3C-SiC film. The surface of the 3C-SiC film has a cauliflower-like morphology, grows in a columnar shape, and there are gaps between the crystal columns.
2. The method for preparing an electrode material based on a 3C-SiC film according to claim 1, characterized in that: Step 2) The flow rate of H2 introduced into the deposition chamber is 1000~3000sccm.
3. The method for preparing an electrode material based on a 3C-SiC film according to claim 1, characterized in that: Step 2) The wavelength of the laser is 800-1000 nm.
4. The method for preparing an electrode material based on a 3C-SiC thin film according to claim 1, characterized in that: Step 2) Etching time is 1~3min.
5. The method for preparing an electrode material based on a 3C-SiC thin film according to claim 1, characterized in that: Step 2) The carrier gas is a mixture of Ar and HMDS, and the carrier gas flow rate is 25 sccm.
6. The method for preparing an electrode material based on a 3C-SiC film according to claim 1, characterized in that: Step 2) The flow rate of HMDS in the carrier gas is 2-10 sccm.
7. The method for preparing an electrode material based on a 3C-SiC film according to claim 1, characterized in that: Step 2) The conditions for deposition and growth of 3C-SiC porous film are: deposition pressure of 300~500Pa, and deposition time of 10~50min.
8. The electrode material based on 3C-SiC film obtained by the preparation method according to any one of claims 1 to 7, characterized in that: It consists of a single crystal Si substrate and a 3C-SiC film with a porous structure grown on the substrate. The surface of the 3C-SiC film has a cauliflower-like morphology and grows in a columnar shape with gaps between the crystal columns.
9. The electrode material based on 3C-SiC film according to claim 8, characterized in that: The single crystal Si substrate is Si(111) with a purity of >99.999%.
10. The electrode material based on 3C-SiC film according to claim 8, characterized in that: The 3C-SiC film with a porous structure has a thickness of 20-60 μm.