Method for preparing core-shell coated conductive material from medium and low temperature coal tar and application of core-shell coated conductive material
Preparing core-shell coated conductive materials from medium-low temperature coal tar solves the problems of poor stability and poor electrochemical performance of existing conductive materials, achieves high specific capacitance and improved Coulombic efficiency, reduces costs, and is environmentally friendly .
Patent Information
- Application Number
- CN202410847727.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing conductive materials have poor stability, poor electrochemical performance, and high processing costs. In particular, graphite-like carbon anode materials used in lithium-ion batteries have small lithium ion diffusion coefficients, poor compatibility with electrolytes, and shortage of raw materials. problem.
Mid- to low-temperature coal tar is used to prepare core-shell coated conductive materials. Through steps such as fraction cutting, gradient extraction, oxidative cross-linking reaction and hydrogenation refining, an efficient core-shell structure is formed to improve the stability and electrochemical performance of the material, and The specific capacitance and Coulombic efficiency of the material are enhanced through the carbonization process.
It significantly improves the stability and electrochemical performance of conductive materials, increases specific capacitance and Coulomb efficiency, reduces process preparation costs, and utilizes easily available secondary coal resources to reduce environmental pollution.
Smart Images

Figure CN118851142A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive material preparation, and relates to a method for preparing a core-shell coated conductive material from medium- and low-temperature coal tar and application thereof. Background Art
[0002] In recent years, with the increasing interest in electric vehicles and hybrid vehicles, the global demand for lithium-ion batteries has increased year by year. Highly crystalline graphite carbon is often used as anode material for lithium-ion batteries due to its high capacity, excellent cycle performance and high coulombic efficiency. However, the diffusion coefficient of lithium ions between graphite layers is small, which seriously restricts the improvement of high-rate charge and discharge performance of lithium-ion batteries. In addition, graphite materials with high graphitization degree have poor compatibility with electrolytes, so further improvements must be made to improve the rate performance and compatibility of graphite-based negative electrode materials with electrolytes.
[0003] Modification methods can be roughly divided into three categories: surface oxidation or reduction treatment, doping and coating. For industrial production, the coating modification process is mainly used. Among them, the core-shell carbon material has a double-layer or multi-layer structure. The core and the shell achieve the coating effect through chemical bonds or other interactions, so that the advantages of the core and the shell are integrated, so that new materials that are different from or even better than the core or shell itself can be prepared. The properties of the material can be controlled by adjusting the type of core-shell material, and the properties of the core-shell material can be adjusted by controlling the preparation process and then controlling the thickness of the core layer and shell layer, so as to achieve the performance optimization of the overall material.
[0004] The Chinese patent document with application number CN201410205734.3 discloses a method for preparing a coated electrode material, an electrode material prepared according to the method, and a lithium ion battery containing the electrode material. A silicon compound containing an alkoxy group is used as a coating agent, and a negative electrode material is used as an electrode material. The electrode material and the coating agent are in contact with a gasified product, and a heating reaction is performed to form a coated electrode material. The method uses a gas phase method to achieve the coating of the existing electrode material and stabilize the electrode material structure; however, this method directly coats the negative electrode material with a silicon compound, and silicon is prone to pulverization during actual electrode use, which reduces the utilization rate of the active components of the conductive material, thereby affecting the electrochemical performance of the material. Shen Wanci of Tsinghua University used a spray granulation method to prepare a phenolic resin coated spherical graphite composite material, and then obtained a pyrolytic carbon coated spherical graphite composite material by carbonization. Compared with spherical graphite, the first coulomb efficiency of the composite graphite material is significantly improved, the cycle performance is significantly extended, and the compatibility of the electrode material electrolyte is also significantly improved, but the stability and electrochemical performance are still poor. In addition, the graphite carbon negative electrode materials currently used in lithium-ion batteries mainly use petroleum products as the main raw materials. With the shortage of energy, raw materials are becoming increasingly scarce, resulting in high processing costs. In addition, the products formed during the preparation of petroleum products seriously pollute the environment. Summary of the invention
[0005] In view of the technical problems of poor stability, poor electrochemical performance and high processing cost of existing conductive materials, the present invention provides a method for preparing core-shell coated conductive materials using medium- and low-temperature coal tar and application thereof.
[0006] The present invention uses medium-low temperature coal tar as a raw material to prepare a coating agent and a spherical core respectively, and then forms a core-shell coated conductive material through carbonization, which is beneficial to enhancing the stability of the material. The core-shell coated conductive material has a higher specific capacitance and coulombic efficiency, the electrochemical performance is improved, and the process preparation cost is low.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing a core-shell coated conductive material using medium- and low-temperature coal tar, comprising the following steps:
[0009] S1. Fraction cutting
[0010] Take two portions of medium and low temperature coal tar, cut the phenol oil of 180℃~220℃ fraction by atmospheric and vacuum distillation in the first portion, and the remaining fraction is recorded as dephenolized oil;
[0011] The second part uses atmospheric and vacuum distillation to cut out phenol oil in the 180℃~220℃ fraction and asphalt in the 350℃~550℃ fraction;
[0012] S2. Preparation of coating agent
[0013] The dephenolized oil in step S1 is separated into component a and component b in sequence by gradient extraction method, and component a and component b are mixed in a mass ratio of (1-3):1 to obtain a composite material;
[0014] Add a viscosity reducer to the composite material; then add a crosslinking agent and an oxidant in an inert gas atmosphere to obtain a coating agent through an oxidative crosslinking reaction; the oxidant is phenol oil in the 180°C to 220°C fraction in step S1; the amount of the viscosity reducer added is 1% to 5% of the mass of the composite material; the amount of the oxidant added is 5% to 10% of the mass of the composite material; and the amount of the crosslinking agent added is 7% to 14% of the mass of the composite material;
[0015] S3, Core Making
[0016] The 350°C to 550°C fraction asphalt cut out in step S1 is taken and subjected to hydrogenation, thermal polymerization and separation to obtain a core ball;
[0017] S4, coating
[0018] The coating agent obtained in step S2 is ground into powder, dissolved in tetrahydrofuran, the coating agent addition amount is 5wt% to 15wt%, and then the spherical core obtained in step S3 is added, and after stirring, ultrasonication, filtering, drying and carbonization, a core-shell coated conductive material is obtained.
[0019] It is further defined that in step S2, the specific steps of the gradient extraction process are:
[0020] S2.1. Mix the dephenolized oil from step S1 with toluene in a mass ratio of 1:(1.5-2.5), stir at 60-90°C for 50-80 min, let stand for 2-4 h, take the upper light phase to obtain component a, and the lower layer is the remaining component;
[0021] S2.2. Mix the remaining components with quinoline in a mass ratio of 1:(1.5-2.5), stir at 60°C-90°C for 50-80 min, let stand for 2-4 h, and take the upper light phase to obtain component b.
[0022] It is further defined that in step S2, the viscosity reducing agent is one or more of carboxymethyl cellulose, 2-acrylamido-2-methylpropane sulfonic acid, sodium dodecylbenzene sulfonate and sodium N and N-dimethyl-dithiocarbonylpropane sulfonate; the cross-linking agent is one or more of polydopamine, polyvinylidene fluoride, terminal hydroxyl polybutadiene, polytetrafluoroethylene and stearic acid.
[0023] It is further defined that in step S2, the process conditions of the oxidative crosslinking reaction are:
[0024] The first stage is heated to 260℃~290℃, kept constant for 2h~4h, and the heating rate is 2℃ / min~4℃ / min; the second stage is heated to 300℃~360℃, kept constant for 2h~5h, and the heating rate is 0.5℃ / min~2℃ / min.
[0025] It is further defined that the yield of the coating agent is ≥65.5%, and the properties of the coating agent are: a softening point of 244°C to 287°C, a coking value of ≥67.54%, a toluene insoluble content of 50% to 75%, and a quinoline insoluble content of 0.02% to 0.13%.
[0026] It is further defined that in step S3, the conditions for hydrofining are: catalyst NiMo / Al2O3-SiO2; H2 atmosphere, pressure 6MPa-12MPa, time 0.5h-2.5h, temperature 330℃-390℃; the mass ratio of asphalt in the 350℃-550℃ fraction to the catalyst is (20-40):1;
[0027] The moderate thermal polymerization process is as follows: the first stage is heated to 300°C ~ 340°C, kept at a constant temperature for 1h ~ 2h, and the heating rate is 2°C / min ~ 4°C / min; the second stage is heated to 420°C ~ 450°C, kept at a constant temperature for 4h ~ 7h, and the heating rate is 0.5°C / min ~ 2°C / min.
[0028] It is further defined that in step S3, the yield of the spherical core is ≥35%, and the particle size is 5 μm to 15 μm.
[0029] It is further defined that in step S4, the carbonization process is: heating to 800°C to 1000°C at a rate of 0.5°C / min to 3°C / min, and maintaining the constant temperature for 0.5h to 2h.
[0030] The core-shell coated conductive material prepared by the method for preparing core-shell coated conductive material with medium-low temperature coal tar has the following properties: the first coulomb efficiency is 90% to 93%, and the capacity retention rate is 85% to 96%.
[0031] Application of the core-shell coated conductive material in the negative electrode material of lithium battery.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The present invention uses medium and low temperature coal tar as raw material, and obtains fractions and asphalt of different temperature sections through fraction cutting. The fractions of different temperature sections are mixed and oxidative cross-linking reactions are used to obtain a coating agent; the asphalt is subjected to hydrogenation and thermal polycondensation to obtain a spherical core, and finally carbonized, and the spherical core is wrapped with a coating agent to form a core-shell coated conductive material, and the coating agent and the spherical core are prepared respectively, and then the core-shell coated conductive material is formed by carbonization. The coating agent has a high yield, a high softening point, and a low content of quinoline insolubles; the shape of the spherical core is conducive to the uniformity of the coating of the coating agent, and can better enhance the stability of the material; the obtained core-shell coated material has a high specific capacitance and coulomb efficiency, improves the electrochemical properties of the conductive material, and has a low process preparation cost.
[0034] 2. The present invention reduces the content of quinoline insolubles in the raw materials by gradient extraction, thereby preparing a coating agent with a lower quinoline insoluble content; by adding a viscosity reducer, it is beneficial to reduce the viscosity of the system, improve the compatibility between components, and effectively prevent the rapid conversion of β-resin to quinoline insolubles caused by deposition on the wall of the vessel, so as to achieve the highest possible coating agent yield; at the same time, the oxidant uses phenol oil from the 180-220°C fraction cut from medium- and low-temperature coal tar by atmospheric and vacuum distillation, which effectively avoids the incompatibility and reaction activity mismatch between raw materials from different sources.
[0035] 3. The present invention, by adding a cross-linking agent, can, on the one hand, promote the cross-linking of light components in asphalt into large molecules, thereby increasing the coking value of the coating agent, which is beneficial for carbonizing the coating agent to form more amorphous carbon during the coating treatment, thereby improving its electrochemical performance as a negative electrode material; on the other hand, during the reaction process, bridge bonds can be formed between molecules with fewer aromatic rings to form polycyclic aromatic hydrocarbon molecules with higher molecular weight, so that the oxygen-containing functional groups are located at the side chain positions of the polycyclic aromatic hydrocarbons, which can effectively improve the removal of oxygen-containing functional groups during induced condensation and increase the yield of the coating agent product.
[0036] 4. The present invention uses an oxidative cross-linking reaction to fully convert the aromatic components in the raw materials into quinoline-soluble toluene-insoluble matter (β resin) and some macromolecular toluene-soluble matter (γ resin), thereby greatly improving the softening point of the coating agent.
[0037] 5. The oxidative cross-linking reaction of the present invention can suppress excessive polycondensation and the generation of quinoline insolubles through multi-stage gentle temperature increase, thereby improving product quality.
[0038] 6. The present invention uses medium- and low-temperature coal tar as raw material to prepare conductive materials. The raw materials are easily available, and the secondary resources of coal are fully utilized without pollution to the environment. The purpose of cost reduction, efficiency improvement, energy conservation and environmental protection is achieved, and a new method for the preparation of core-shell coated conductive materials is provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The present invention provides a flow chart of the preparation process. DETAILED DESCRIPTION
[0040] The technical solution protected by the present invention is now described in detail with reference to the accompanying drawings and embodiments, but this should not be used as a limitation to the protection scope of the present invention.
[0041] See also Figure 1 The present invention provides a method for preparing a core-shell coated conductive material using medium- and low-temperature coal tar, comprising the following steps:
[0042] S1. Fraction cutting
[0043] Take two portions of medium and low temperature coal tar, cut the phenol oil of 180℃~220℃ fraction by atmospheric and vacuum distillation in the first portion, and the remaining fraction is recorded as dephenolized oil;
[0044] The second part uses atmospheric and vacuum distillation to cut out phenol oil in the 180°C to 220°C fraction and asphalt in the 350°C to 550°C fraction.
[0045] S2. Preparation of coating agent
[0046] The dephenolized oil in step S1 is separated into component a and component b in sequence by gradient extraction method, and component a and component b are mixed in a mass ratio of (1-3):1 to obtain a composite material.
[0047] A viscosity reducer is added to the compound material; then, a crosslinking agent and an oxidant are added under an inert gas atmosphere to obtain a coating agent through an oxidative crosslinking reaction.
[0048] In the present invention, the oxidant is the phenol oil in the 180°C to 220°C fraction in step S1; the added amount of the viscosity reducer is 1% to 5% of the mass of the composite material; the added amount of the oxidant is 5% to 10% of the mass of the composite material; and the added amount of the cross-linking agent is 7% to 14% of the mass of the composite material.
[0049] In step S2 of the present invention, the specific steps of the gradient extraction process are:
[0050] S2.1. Mix the dephenolized oil from step S1 with toluene in a mass ratio of 1:(1.5-2.5), stir at 60-90°C for 50-80 min, let stand for 2-4 h, take the upper light phase to obtain component a, and the lower layer is the remaining component;
[0051] S2.2. Mix the remaining components with quinoline in a mass ratio of 1:(1.5-2.5), stir at 60°C-90°C for 50-80 min, let stand for 2-4 h, and take the upper light phase to obtain component b.
[0052] In step S2 of the present invention, the viscosity reducing agent is one or more of carboxymethyl cellulose, 2-acrylamido-2-methylpropane sulfonic acid, sodium dodecylbenzene sulfonate and sodium N and N-dimethyl-dithiocarbonylpropane sulfonate; the cross-linking agent is one or more of polydopamine, polyvinylidene fluoride, terminal hydroxyl polybutadiene, polytetrafluoroethylene and stearic acid.
[0053] In step S2 of the present invention, the process conditions for the oxidative crosslinking reaction are:
[0054] The first stage is heated to 260℃~290℃, kept constant for 2h~4h, and the heating rate is 2℃ / min~4℃ / min; the second stage is heated to 300℃~360℃, kept constant for 2h~5h, and the heating rate is 0.5℃ / min~2℃ / min.
[0055] In step S2 of the present invention, the yield of the coating agent is ≥65.5%, and the properties of the coating agent are: a softening point of 244°C to 287°C, a coking value of ≥67.54%, a toluene insoluble content of 50% to 75%, and a quinoline insoluble content of 0.02% to 0.13%.
[0056] S3, Core Making
[0057] The 350°C to 550°C fraction asphalt cut out in step S1 is subjected to hydrogenation refining, moderate thermal polymerization reaction and separation to obtain a core ball.
[0058] In step S3 of the present invention, the conditions for hydrotreating are: catalyst NiMo / Al2O3-SiO2; under H2 atmosphere, pressure 6MPa-12MPa, time 0.5-2.5h, temperature 330℃-390℃, and the mass ratio of asphalt to catalyst in the 350℃-550℃ fraction is (20-40):1.
[0059] The thermal polymerization process of the present invention is as follows: the first stage is heated to 300°C-340°C, kept at a constant temperature for 1h-2h, and the heating rate is 2°C / min-4°C / min; the second stage is heated to 420°C-450°C, kept at a constant temperature for 4h-7h, and the heating rate is 0.5°C / min-2°C / min.
[0060] In step S3 of the present invention, the yield of the spherical core is ≥35%, and the particle size is 5 μm to 15 μm.
[0061] S4, coating
[0062] The coating agent obtained in step S2 is ground into powder, dissolved in tetrahydrofuran, and the spherical core obtained in step S3 is added, and the core-shell coated conductive material is obtained by stirring, ultrasonication, filtering, drying and carbonization.
[0063] In step S4 of the present invention, the carbonization process is: heating to 800°C to 1000°C at a rate of 0.5°C / min to 3°C / min, and maintaining the constant temperature for 0.5h to 2h.
[0064] The core-shell coated conductive material prepared by the method of the present invention has the following properties: the first coulomb efficiency is 90% to 93% and the capacity retention rate is about 85% to 96%.
[0065] The core-shell coated conductive material prepared by the present invention has high performance and can be used in negative electrode materials of lithium batteries.
[0066] The preparation method of the present invention is described below with reference to several groups of embodiments, and the performance of the core-shell coated conductive material is verified through experiments.
[0067] It should be noted that, unless otherwise specified, the reagents and drugs used in the following examples and experiments are conventional commercially available products.
[0068] It should be noted that, unless otherwise specified, the operations used in the following examples and experiments are routine operations in the art.
[0069] Example 1
[0070] This embodiment provides a method for preparing a core-shell coated conductive material using medium- and low-temperature coal tar, comprising the following steps:
[0071] S1. Fraction cutting
[0072] 1 kg of medium and low temperature coal tar is subjected to vacuum distillation to obtain phenol oil in the 180-220°C fraction, and the remaining portion is retained and recorded as dephenolized oil; another 1 kg of medium and low temperature coal tar is subjected to vacuum distillation cutting to cut out phenol oil in the 180-220°C fraction and asphalt in the 350-550°C fraction;
[0073] S2. Ingredients
[0074] 100 g of dephenolized oil and toluene were mixed in a mass ratio of 1:2, placed in a constant temperature water bath at 80°C and stirred for 60 min, allowed to stand for 3 h, and the upper light phase a was taken; the remaining components in the lower layer were collected and extracted with quinoline under the same conditions as above, and the upper light phase b was taken; the obtained upper light phase a and upper light phase b were respectively subjected to rotary evaporation to evaporate the solvent to obtain the corresponding component a and component b.
[0075] Component a and component b are mixed in a mass ratio of 1:1 to obtain a compound raw material, and the viscosity reducer is added in an amount of 1%, the oxidant is added in an amount of 5%, and the cross-linking agent is added in an amount of 7%, and the mixture is evenly mixed to prepare a compound mixed raw material.
[0076] S3. Preparation of coating agent
[0077] The composite mixed raw materials are placed in a reactor, and a crosslinking agent and an oxidant are added under a nitrogen atmosphere. The oxidant is the phenol oil of the 180°C to 220°C fraction in step S1, and the amount of the oxidant added is 5% of the mass of the composite material; the viscosity reducer is carboxymethyl cellulose, and the amount of the viscosity reducer added is 1% of the mass of the composite material; the crosslinking agent is polydopamine, and the amount of the crosslinking agent added is 7% of the mass of the composite material. The oxidation crosslinking reaction is carried out under the following conditions: the first stage is heated to 260°C, kept at a constant temperature for 2h, and the heating rate is 2°C / min; the second stage is heated to 310°C, kept at a constant temperature for 2h, and the heating rate is 0.5°C / min, to obtain a coating agent.
[0078] S4, Ball Core
[0079] 150g of 350℃~550℃ fraction asphalt was placed in a magnetically driven high-pressure reactor, and the catalyst was added at an oil-to-catalyst ratio of 30:1. The oil refers to the 350℃~550℃ fraction asphalt, and the catalyst NiMo / Al2O3-SiO 2。 After N2 replacement, H2 was added to 8MPa and the reaction was carried out at 350°C for 1.5h. After the reaction was completed, the hydrogenation product and the catalyst were separated to obtain a refined raw material.
[0080] The refined raw materials were placed in a magnetically driven reactor for thermal polymerization. The thermal polymerization process was as follows: the temperature was raised to 320°C in the first stage, kept constant for 1 hour, and the heating rate was 4°C / min; the temperature was raised to 430°C in the second stage, kept constant for 6 hours, and the heating rate was 0.5°C / min. After the reaction was completed, the thermal polymerization product was taken out.
[0081] The thermal polymerization product was subjected to Soxhlet extraction with pyridine, and the insoluble matter obtained by the extraction was washed with anhydrous ethanol and then dried in an oven at 150° C. for 12 h to obtain a spherical core.
[0082] S5, coating
[0083] The coating agent of step S3 is ground into powder, dissolved in tetrahydrofuran at a doping amount of 6%, and the spherical core obtained in step S4 is added, and a uniformly dispersed coating agent and spherical core mixture is obtained by stirring and ultrasonication. The organic solvent is removed by decompression using a rotary evaporator, and the sample is dried at 120°C, and then heated to 800°C in a tube furnace at a heating rate of 0.5°C / min, and kept at a constant temperature for 0.5h under a nitrogen atmosphere to obtain a core-shell coated conductive material.
[0084] Embodiment 2 to Embodiment 6
[0085] The preparation methods provided in Examples 2 to 6 are the same as those in Example 1, except that the amounts of raw materials used and the process parameters are different, as shown in Table 1.
[0086] Table 1 Process parameters of Example 2 to Example 6
[0087]
[0088]
[0089] Comparative Example 1
[0090] The difference between this comparative example and Example 1 is that the dephenolized oil is directly used for the oxidative cross-linking reaction without gradient extraction and preparation.
[0091] Comparative Example 2
[0092] The difference between this comparative example and Example 2 is that the component a and the component b obtained by gradient extraction are directly mixed to obtain a mixture, and the mixing mass ratio is not within the range of (1-3):1, and then the mixture continues to undergo subsequent reactions.
[0093] Comparative Example 3
[0094] This comparative example is different from Example 3 in that a one-stage temperature-raising oxidation cross-linking reaction is adopted.
[0095] Comparative Example 4
[0096] This comparative example is different from Example 4 in that no viscosity reducer is added.
[0097] Comparative Example 5
[0098] The difference between Comparative Example 5 and Example 5 is that no oxidant is added.
[0099] Comparative Example 6
[0100] The difference between Comparative Example 6 and Example 6 is that no cross-linking agent is added.
[0101] Test 1
[0102] The 12 groups of coating agents prepared in the above embodiments and comparative examples were tested for softening point (SP), toluene insoluble matter (TI), quinoline insoluble matter (QI), and coking value (CV) of the coating agents according to the national standards for coking products in the metallurgical industry GB / T4507-1999, GB / T2292-1997, GB / T2293-1997, and GB / T2727-88, respectively. The results are shown in Table 2.
[0103] Table 2 Performance test results of coating agents of examples and comparative examples
[0104]
[0105] It can be seen from Table 2 above that in Examples 1 to 6, the yield of the coating agent is ≥65.5%, the softening point of the coating agent is 244°C to 287°C, the coking value is ≥67.54%, the toluene insoluble matter is 50% to 75%, and the quinoline insoluble matter is 0.02% to 0.13%. Compared with the comparative example, the coating agent prepared in Examples 1 to 6 has a reduced quinoline insoluble matter, and the yield, softening point, and toluene insoluble coking value are greatly improved. This shows that through gradient extraction and component blending, under the joint action of an oxidant, a cross-linking agent, a viscosity reducer, and a two-stage temperature-raising oxidation cross-linking reaction, the prepared coating agent exhibits good performance, further improving the electrochemical properties of the final core-shell coated conductive material.
[0106] Test 2
[0107] Lithium-ion batteries were prepared using the core-shell coated conductive materials obtained in Examples 1 to 6 and Comparative Examples 1 to 6 as negative electrode materials, and the electrochemical properties of the batteries were measured.
[0108] The specific steps are as follows: weigh the negative electrode material, acetylene black and binder PVDF (polyvinylidene fluoride), and mix them in a mass ratio of 89:3:8, then add an appropriate amount of N,N-dimethylpyrrolidone, and after magnetic stirring for 5 hours, coat the resulting slurry on a copper foil with a thickness of 9μm, dry it with air at 80℃ for 6 hours, press it into shape at a pressure of 1.0MPa, and cut a Φ12mm electrode sheet as the working electrode of the battery. Use a metal lithium sheet as the counter electrode, the electrolyte is 1mol / LLiPF6 / EC+EMC+DMC (volume ratio: 1:1:1), and the diaphragm is a lithium battery diaphragm from Asahi Kasei of Japan, and assemble it into a button battery in a glove box filled with high-purity argon.
[0109] The experimental battery was charged and discharged using the CT2001A LAND battery test system, with a cut-off voltage of 0.001V to 2.0V and a current density of 37.2mA / g, equivalent to 0.1C. The electrochemical test performance results are shown in Table 3.
[0110] Table 3 Test results of battery prepared by negative electrode materials of examples and comparative examples
[0111]
[0112]
[0113] It can be seen from the data in Table 3 that the core-shell coated conductive material prepared by the present invention has an initial coulombic efficiency of 90% to 93%, and a capacity retention rate of 85% to 96% after 50 cycles. Compared with Comparative Examples 1 to 6, the core-shell coated conductive material prepared by the present invention has good stability and electrochemical performance, thereby improving the electrochemical performance of the lithium battery.
[0114] The viscosity reducer used in the above method is carboxymethyl cellulose and the cross-linking agent is polydopamine; however, when the types of the viscosity reducer and the cross-linking agent are changed according to the material range defined by the present invention, the prepared coating agent and the core-shell coated conductive material also show similar effects as shown in Table 2 and Table 3. In the preparation of the conductive material by the present invention, the obtained spherical core shape is conducive to the uniformity of the coating agent coating, which can better enhance the stability of the material; the core-shell coated material has a higher specific capacitance and coulomb efficiency, and improves the electrochemical performance of the negative electrode material; and the process preparation cost is low, the yield is high, and there is no pollution to the environment, thereby developing a new way to prepare core-shell coated conductive materials.
[0115] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a core-shell coated conductive material using medium- and low-temperature coal tar, characterized in that: The following steps are involved: S1. Fraction cutting Take two portions of medium and low temperature coal tar, cut the phenol oil of 180℃~220℃ fraction by atmospheric and vacuum distillation in the first portion, and the remaining fraction is recorded as dephenolized oil; The second part uses atmospheric and vacuum distillation to cut out phenol oil in the 180℃~220℃ fraction and asphalt in the 350℃~550℃ fraction; S2. Preparation of coating agent The dephenolized oil in step S1 is separated into component a and component b in sequence by gradient extraction method, and component a and component b are mixed in a mass ratio of (1-3):1 to obtain a composite material; Add a viscosity reducer to the composite material; then add a crosslinking agent and an oxidant in an inert gas atmosphere to obtain a coating agent through an oxidative crosslinking reaction; the oxidant is phenol oil in the 180°C to 220°C fraction in step S1; the amount of the viscosity reducer added is 1% to 5% of the mass of the composite material; the amount of the oxidant added is 5% to 10% of the mass of the composite material; and the amount of the crosslinking agent added is 7% to 14% of the mass of the composite material; S3, Core Making The 350°C to 550°C fraction asphalt cut out in step S1 is taken and subjected to hydrogenation, thermal polymerization and separation to obtain a core ball; S4, coating The coating agent obtained in step S2 is ground into powder, dissolved in tetrahydrofuran, the coating agent addition amount is 5wt% to 15wt%, and then the spherical core obtained in step S3 is added, and after stirring, ultrasonication, filtering, drying and carbonization, a core-shell coated conductive material is obtained.
2. The method for preparing a core-shell coated conductive material from medium and low temperature coal tar according to claim 1, characterized in that: In step S2, the specific steps of the gradient extraction process are: S2.
1. Mix the dephenolized oil from step S1 with toluene in a mass ratio of 1:(1.5-2.5), stir at 60-90°C for 50-80 min, let stand for 2-4 h, take the upper light phase to obtain component a, and the lower layer is the remaining component; S2.
2. Mix the remaining components with quinoline in a mass ratio of 1:(1.5-2.5), stir at 60°C-90°C for 50-80 min, let stand for 2-4 h, and take the upper light phase to obtain component b.
3. The method for preparing core-shell coated conductive materials from medium and low temperature coal tar according to claim 1, characterized in that: In step S2, the viscosity reducing agent is one or more of carboxymethyl cellulose, 2-acrylamido-2-methylpropane sulfonic acid, sodium dodecylbenzene sulfonate and sodium N and N-dimethyl-dithiocarbonylpropane sulfonate; the cross-linking agent is one or more of polydopamine, polyvinylidene fluoride, terminal hydroxyl polybutadiene, polytetrafluoroethylene and stearic acid.
4. The method for preparing a core-shell coated conductive material from medium- and low-temperature coal tar according to claim 1, characterized in that: In step S2, the process conditions of the oxidative crosslinking reaction are: The first stage is heated to 260℃~290℃, kept constant for 2h~4h, and the heating rate is 2℃ / min~4℃ / min; the second stage is heated to 300℃~360℃, kept constant for 2h~5h, and the heating rate is 0.5℃ / min~2℃ / min.
5. The method for preparing core-shell coated conductive materials from medium and low temperature coal tar according to claim 4, characterized in that: The yield of the coating agent is ≥65.5%, and the properties of the coating agent are: a softening point of 244°C to 287°C, a coking value of ≥67.54%, a toluene insoluble content of 50% to 75%, and a quinoline insoluble content of 0.02% to 0.13%.
6. The method for preparing a core-shell coated conductive material from medium- and low-temperature coal tar according to claim 1, characterized in that: In step S3, the conditions for hydrofining are: catalyst NiMo / Al2O3-SiO2; H2 atmosphere, pressure 6MPa-12MPa, time 0.5h-2.5h, temperature 330℃-390℃, mass ratio of asphalt to catalyst in the 350℃-550℃ fraction is (20-40):1; The thermal polymerization process is as follows: the first stage is heated to 300°C ~ 340°C, kept at a constant temperature for 1h ~ 2h, and the heating rate is 2°C / min ~ 4°C / min; the second stage is heated to 420°C ~ 450°C, kept at a constant temperature for 4h ~ 7h, and the heating rate is 0.5°C / min ~ 2°C / min.
7. The method for preparing core-shell coated conductive materials from medium and low temperature coal tar according to claim 1, characterized in that: In the step S3, the yield of the spherical core is ≥35%, and the particle size is 5 μm to 15 μm.
8. The method for preparing core-shell coated conductive materials from medium and low temperature coal tar according to claim 1, characterized in that: In step S4, the carbonization process is: heating to 800°C to 1000°C at a rate of 0.5°C / min to 3°C / min, and maintaining the constant temperature for 0.5h to 2h.
9. The core-shell coated conductive material prepared by the method for preparing a core-shell coated conductive material from medium- and low-temperature coal tar according to any one of claims 1 to 8, characterized in that: The performance of the core-shell coated conductive material is: the first coulomb efficiency is 90% to 93%, and the capacity retention rate is 85% to 96%.
10. Use of the core-shell coated conductive material as claimed in claim 9 in negative electrode materials for lithium batteries.
Citation Information
Patent Citations
Preparation method of coated electrode material
CN105098163A
Technology for producing coal-series needle coke by taking middle-temperature and low-temperature coal tar asphalt as raw material
CN107694552A
Method for preparing lithium battery negative electrode material from medium and low temperature coal tar and application of lithium battery negative electrode material
CN113979432A
Preparation method and system of petroleum-based coated asphalt with low quinoline insolubles and high softening point
CN115093874A
Preparation process of isotropic asphalt and high-softening-point coated asphalt