Magnetic matrix containing metal magnetic particles and electronic component containing the magnetic matrix
By using amorphous silicon oxide film with structural defects as the insulating film in the magnetic matrix, the problem of insulating film failure under high forming pressure is solved, high filling rate and low eddy current loss are achieved, and the performance of the magnetic matrix is enhanced.
Patent Information
- Application Number
- CN201910688312.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-09
- Filing Date
- 2019-07-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-07-29
AI Technical Summary
The conventional magnetic matrix can easily lead to the destruction of the metal magnetic particle insulating film under high forming pressure, resulting in an increase in eddy current loss, and it is difficult to suppress eddy current loss.
Amorphous silicon oxide film with structural defects is used as an insulating film in a magnetic matrix, with a thickness of less than 100 nm to follow the deformation of metal magnetic particles and prevent the insulating film from being destroyed. The lamination process and heat treatment are used to form a soft oxidation with high flexibility Silicon film.
It effectively suppresses the damage of the insulating film, improves the filling rate and mechanical strength of metal magnetic particles in the magnetic matrix, reduces eddy current losses, and enhances high-frequency characteristics and magnetic permeability.
Smart Images

Figure CN110828108B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a magnetic matrix containing metal magnetic particles and an electronic component containing the magnetic matrix. Background Art
[0002] As the material of the magnetic base of electronic components, various magnetic materials have been used. For example, ferrite is often used as a magnetic material for coil components such as inductors. Ferrite is suitable as a magnetic material for inductors because of its high magnetic permeability.
[0003] As magnetic materials for electronic components other than ferrites, metal magnetic materials containing metal magnetic particles are known. Metal magnetic materials generally have a higher saturation flux density than ferrite materials, and are therefore suitable as materials for magnetic bases of coil components with large currents flowing. The magnetic base formed by a composite magnetic material containing metal magnetic particles is produced as follows: for example, by injecting a slurry obtained by mixing metal magnetic particles and a binder into a mold, and then press-forming the slurry by applying pressure to the mold. An insulating film is provided on the surface of each metal magnetic particle contained in the magnetic base, and the insulating film is used to prevent short circuits between adjacent metal magnetic particles.
[0004] The magnetic matrix used in electronic components is required to have a high magnetic permeability. In order to improve the magnetic permeability, a proposal has been made to increase the filling rate of magnetic particles in the magnetic matrix. For example, Japanese Patent Publication No. 2006-179621 discloses a composite magnetic material containing a first magnetic particle and a second magnetic particle, wherein the average particle size of the second magnetic particle is less than 50% of the average particle size of the first magnetic particle, and when the content of the first magnetic particle is X [wt%] and the content of the second magnetic particle is Y [wt%], by satisfying the relationship of 0.05≤Y / (X+Y)≤0.30, a molded body filled with magnetic particles at a high density can be obtained. In addition, Japanese Patent Publication No. 2010-34102 discloses a clay-like magnetic matrix obtained by mixing two or more amorphous metal magnetic particles having different average particle sizes with an insulating binder. According to the publication, a high filling rate and low iron loss can be achieved by the magnetic matrix.
[0005] [Prior technical literature]
[0006] [Patent Literature]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2006-179621
[0008] [Patent Document 2] Japanese Patent Application Publication No. 2010-034102
[0009] It is believed that the filling rate of metal magnetic particles can be increased by increasing the molding pressure during molding of the magnetic matrix. However, if the molding pressure becomes high, there is a problem that the insulating film provided on the surface of the metal magnetic particles is easily destroyed. If the insulating film is destroyed, adjacent metal magnetic particles are short-circuited to each other, thereby causing the adjacent metal magnetic particles to become a particle with a large diameter. Eddy currents are likely to occur in these large-diameter particles. Therefore, if insulation breakdown occurs between the metal magnetic particles contained in the magnetic matrix, there is a problem that eddy current losses become large. In order to suppress eddy current losses, it is hoped that even if a high molding pressure is applied, the insulating film provided on the metal magnetic particles will not be destroyed. Summary of the invention
[0010] The object of the present invention is to solve or alleviate at least a part of the above-mentioned problems. One of the more specific objects of the present invention is to suppress the destruction of the insulating film provided on the metal magnetic particles contained in the magnetic substrate. Other objects of the present invention are explained by the description of the entire specification.
[0011] A magnetic substrate according to one embodiment of the present invention comprises metal magnetic particles and an amorphous silicon oxide film provided on the surface of the metal magnetic particles and having structural defects introduced therein.
[0012] In the magnetic substrate according to one embodiment of the present invention, the silicon oxide film is formed to have a thickness of 100 nm or less.
[0013] In the magnetic substrate according to one embodiment of the present invention, the silicon oxide film is formed to have a thickness of 50 nm or less.
[0014] In the magnetic substrate according to one embodiment of the present invention, the metal magnetic particles contain Fe, and the content of Fe in the metal magnetic particles is 90 wt % or more.
[0015] One embodiment of the present invention relates to an electronic component. The electronic component includes the above-mentioned magnetic substrate.
[0016] An electronic component according to one embodiment of the present invention comprises the magnetic substrate described above, and a coil provided on the magnetic substrate. The coil may be embedded in the magnetic substrate. The coil may be provided on the magnetic substrate in such a manner that at least a portion of the coil is exposed to the outside of the magnetic substrate.
[0017] According to the disclosure of this specification, it is possible to suppress the destruction of the insulating film provided on the metal magnetic particles included in the magnetic substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a perspective view of a coil component according to one embodiment of the present invention.
[0019] Figure 2 yes Figure 1 An exploded perspective view of the coil components.
[0020] Figure 3 It is a schematic representation of the I-I line cut Figure 1 FIG. 4 is a diagram of a cross section of a coil component.
[0021] Figure 4A This is a diagram schematically showing metal magnetic particles contained in the slurry before press molding.
[0022] Figure 4B Yes Figure 3 The region A of the magnetic substrate is shown enlarged and schematically represented.
[0023] Explanation of symbols
[0024] 1 Inductor
[0025] 2 Circuit board
[0026] 10 Magnetic substrate
[0027] 25 Coil conductor
[0028] 31~37 Metal magnetic particles
[0029] 41~47 Silicon oxide film DETAILED DESCRIPTION
[0030] Reference Figures 1 to 3 , an inductor 1 according to an embodiment of the present invention is described. Figure 1 is a perspective view of an inductor 1 according to an embodiment of the present invention. Figure 2 yes Figure 1 An exploded perspective view of the inductor 1, Figure 3 It is a schematic representation of the I-I line cut Figure 1 FIG. 1 is a diagram of a cross section of an inductor 1. Figure 2 In FIG. 4 , for the sake of convenience of explanation, illustration of external electrodes is omitted.
[0031] In this specification, unless otherwise explained in the text, the "length" direction, "width" direction and "thickness" direction of the inductor 1 are respectively Figure 1 The “L” direction, “W” direction and “T” direction.
[0032] The inductor 1 shown in these figures is an example of a coil component to which the present invention can be applied. In addition to inductors, the present invention can also be applied to transformers, filters, reactors and various other coil components. The present invention can also be applied to coupled inductors, chokes and various other magnetic coupling type coil components.
[0033] As shown in the figure, the inductor 1 includes a magnetic base 10 , a coil conductor 25 provided in the magnetic base 10 , an external electrode 21 electrically connected to one end of the coil conductor 25 , and an external electrode 22 electrically connected to the other end of the coil conductor 25 .
[0034] The magnetic substrate 10 is formed of a magnetic material in a rectangular parallelepiped shape. The magnetic substrate 10 includes: a magnetic layer 20 in which a coil 25 is embedded; an upper cover layer 18 formed of a magnetic material provided on the upper surface of the magnetic layer 20; and a lower cover layer 19 formed of a magnetic material provided on the lower surface of the magnetic layer 20. The boundary between the magnetic layer 20 and the upper cover layer 18 and the boundary between the magnetic layer 20 and the lower cover layer 19 may not be clearly confirmed due to the manufacturing method of the magnetic substrate 10. In one embodiment of the present invention, the magnetic substrate 10 is formed so that the length dimension (dimension in the L direction) is 1.0 mm to 2.6 mm, the width dimension (dimension in the W direction) is 0.5 to 2.1 mm, and the height dimension (dimension in the H direction) is 0.5 to 1.0 mm. The dimension in the length direction may also be 0.3 mm to 1.6 mm.
[0035] The inductor 1 is mounted on the circuit substrate 2. A pad portion 3 may also be provided on the circuit substrate 2. When the inductor 1 has two external electrodes 21 and 22, two pad portions 3 are provided on the circuit substrate 2 corresponding thereto. The inductor 1 may also be mounted on the circuit substrate 2 by bonding the external electrodes 21 and 22 to the corresponding pad portions 3 of the circuit substrate 2, respectively. The circuit substrate 2 can be mounted on various electronic devices. Electronic devices that can be mounted with the circuit substrate 2 include smart phones, tablet computers, game consoles and various other electronic devices. As described later, since the insulation of the magnetic substrate 10 is improved, the inductor 1 can be miniaturized and / or thinned. Therefore, the inductor 1 can be suitable for a circuit substrate 2 with high-density mounted components. The inductor 1 may also be a built-in component buried inside the circuit substrate 2.
[0036] The magnetic substrate 10 has a first main surface 10a, a second main surface 10b, a first end surface 10c, a second end surface 10d, a first side surface 10e, and a second side surface 10f. The outer surface of the magnetic substrate 10 is defined by these six surfaces. The first main surface 10a and the second main surface 10b are opposite to each other, the first end surface 10c and the second end surface 10d are opposite to each other, and the first side surface 10e and the second side surface 10f are opposite to each other.
[0037] exist Figure 1In the figure, the first principal surface 10a is called the "upper surface" because the first principal surface 10a is located on the upper side of the magnetic substrate 10. Similarly, the second principal surface 10b is called the "lower surface". Since the inductor 1 is arranged so that the second principal surface 10b faces the circuit substrate 2, the second principal surface 10b is also called the "mounting surface". When referring to the up and down direction of the inductor 1, Figure 1 The up and down direction is used as the reference.
[0038] The external electrode 21 is provided on the first end surface 10c of the magnetic base 10. The external electrode 22 is provided on the second end surface 10d of the magnetic base 10. As shown in the figure, each external electrode may extend to the upper surface and the lower surface of the magnetic base 10. The shape and arrangement of each external electrode are not limited to the example shown in the figure. For example, the external electrodes 21 and 22 may be provided on the lower surface 10b of the magnetic base 10. In this case, the coil conductor 25 is connected to the external electrodes 21 and 22 provided on the lower surface 10b of the magnetic base 10 via the through-hole conductor. The external electrode 21 and the external electrode 22 are arranged at intervals from each other in the longitudinal direction. The distance between the external electrode 21 and the external electrode 22 is the same as or slightly smaller than the dimension of the magnetic base 10 in the longitudinal direction, that is, 0.3 mm to 1.6 mm. As described later, in the magnetic base 10, since the insulation is improved, the distance between the external electrode 21 and the external electrode 22 can be reduced to about 0.3 mm to 1.6 mm.
[0039] Next, the main reference Figure 2 , the stacked structure of the inductor 1 will be further described. Figure 2 , an exploded perspective view of an inductor 1 manufactured by a stacking process is shown. Figure 2 As shown, the magnetic layer 20 includes magnetic films 11 to 17. In the magnetic layer 20, magnetic films 11, 12, 13, 14, 15, 16, and 17 are stacked in order from the positive side to the negative side in the T-axis direction. The inductor 1 may also be manufactured by a method other than the stacking process. For example, the inductor 1 may also be manufactured by a thin film process. In addition, the inductor 1 may also be a winding type coil in which a winding wire is wound around the outside of the core.
[0040] Conductor patterns C11 to C17 are formed on the upper surfaces of the magnetic films 11 to 17. The conductor patterns C11 to C17 are formed by, for example, printing a conductive paste made of a metal or alloy having excellent conductivity by screen printing. As the material of the conductive paste, Ag, Pd, Cu, Al, or an alloy thereof can be used. The conductor patterns C11 to C17 can also be formed by other materials and methods. The conductor patterns C11 to C17 can also be formed by, for example, a sputtering method, an inkjet method, or a known method other than these.
[0041] Through holes V1 to V6 are formed at predetermined positions of the magnetic films 11 to 16. The through holes V1 to V6 are formed by forming through holes penetrating the magnetic films 11 to 16 in the T-axis direction at predetermined positions of the magnetic films 11 to 16 and embedding a conductive material in the through holes.
[0042] The conductor patterns C11 to C17 are electrically connected to adjacent conductor patterns through via holes V1 to V6. The conductor patterns C11 to C17 connected in this way form a spiral coil conductor 25. That is, the coil conductor 25 includes the conductor patterns C11 to C17 and via holes V1 to V6.
[0043] The end portion of the conductor pattern C11 opposite to the end portion connected to the through hole V1 is connected to the external electrode 22. The end portion of the conductor pattern C17 opposite to the end portion connected to the through hole V6 is connected to the external electrode 21.
[0044] The upper cover layer 18 includes magnetic films 18a to 18d formed of a magnetic material, and the lower cover layer 19 includes magnetic films 19a to 19d formed of a magnetic material. In this specification, the magnetic films 18a to 18d and the magnetic films 19a to 19d are collectively referred to as "cover layer magnetic films".
[0045] As described above, the magnetic base 10 (magnetic films 11 to 17 and the cover layer magnetic film) is formed of a magnetic material. As the magnetic material for the magnetic base 10, a composite magnetic material containing a binder and a plurality of metal magnetic particles can be used. The inductor 1 may also have two or more regions formed of different magnetic materials. For example, the magnetic layer 20 and the upper cover layer 18 may also be formed of different magnetic materials.
[0046] An insulating film is formed on each of the metal magnetic particles contained in the composite magnetic material used for the magnetic substrate 10. The insulating film is an amorphous silicon oxide film. As described later, structural defects are introduced into the silicon oxide film.
[0047] Next, an example of a method for manufacturing the inductor 1 will be described. The inductor 1 can be manufactured, for example, by a lamination process. Hereinafter, an example of a method for manufacturing the inductor 1 by a lamination process will be described.
[0048] First, magnetic sheets are prepared as magnetic films 18a to 18d constituting the upper cover layer 18, magnetic films 11 to 17 constituting the magnetic layer 20, and magnetic films 19a to 19d constituting the lower cover layer 19. These magnetic sheets are formed of a composite magnetic material containing a binder and a plurality of metal magnetic particles.
[0049] In order to make a magnet sheet, first, metal magnetic particles are prepared. The metal magnetic particles used in the magnet sheet are formed of a crystalline or amorphous metal or alloy containing at least one element of iron (Fe), nickel (Ni), and cobalt (Co). The metal magnetic particles may also contain at least one element of silicon (Si), chromium (Cr), and aluminum (Al). The metal magnetic particles may be pure iron particles formed of Fe and inevitable impurities, or Fe-based amorphous alloys containing iron (Fe). This Fe-based amorphous alloy includes, for example, Fe-Si alloys, Fe-Si-Al alloys, Fe-Si-Cr-B alloys, Fe-Si-B-C alloys, and Fe-Si-P-B-C alloys. The metal magnetic particles may also contain particles of only a single type of metal or a single type of alloy. For example, the first metal magnetic particles 31 may also be particles formed entirely of pure iron or a specific type of Fe-based amorphous alloy. The metal magnetic particles contained in the composite magnetic material used for the magnetic substrate 10 may also contain particles of many different types of metals or alloys. For example, the first metal magnetic particles 31 may also include a plurality of particles formed of pure iron and a plurality of particles formed of an Fe-Si alloy. When the metal magnetic particles are formed of pure iron or an alloy containing Fe, the Fe content in the metal magnetic particles may be 90 wt% or more. Thus, a magnetic substrate 10 having good magnetic saturation characteristics can be obtained. The metal magnetic particles may also be carbonyl iron powder having an Fe content of 99.9 wt% or more.
[0050] In one embodiment, the metal magnetic particles have an average particle size of 1 μm to 200 μm. The metal magnetic particles may also contain two or more metal magnetic particles having different average particle sizes. For example, the metal magnetic particles used in the composite magnetic material may also contain first metal magnetic particles having a first average particle size and second metal magnetic particles having a second average particle size smaller than the first average particle size. In one embodiment, the average particle size of the second metal magnetic particles is less than 1 / 10 of the average particle size of the first metal magnetic particles. When the average particle size of the second metal magnetic particles is less than 1 / 10 of the average particle size of the first metal magnetic particles, the second metal magnetic particles easily enter the gaps between the adjacent first metal magnetic particles 31, resulting in an increase in the filling rate (density) of the metal magnetic particles of the magnetic matrix 10. In one embodiment, the metal magnetic particles of the composite magnetic material used in the magnetic matrix 10 may also contain third metal magnetic particles having a third average particle size smaller than the second average particle size. The average particle size of the third metal magnetic particles may be less than 0.5 μm. As a result, even when the coil component is excited at a high frequency, the occurrence of eddy currents in the third metal magnetic particles can be suppressed. Thus, the coil component 10 having excellent high-frequency characteristics can be obtained.
[0051] The average particle size of the metal magnetic particles contained in the composite magnetic material is determined by cutting the magnetic matrix along the thickness direction (T direction) of the magnetic matrix to expose the cross section, photographing the particles larger than 1 μm at 2000 to 5000 times and photographing the particles smaller than 1 μm at 5000 to 10000 times using a scanning electron microscope (SEM) for the cross section, obtaining the particle size distribution based on the photographed photos, and determining the average particle size of the metal magnetic particles contained in the composite magnetic material based on the particle size distribution. For example, the 50% value of the particle size distribution obtained based on the SEM photo can be used as the average particle size of the metal magnetic particles.
[0052] An insulating film is formed on the surface of the metal magnetic particles to prevent the metal magnetic particles from short-circuiting with each other. The insulating film is preferably formed in a manner that covers the entire surface of the metal magnetic particles. As mentioned above, when the metal magnetic particles include three types of metal magnetic particles with different average particle sizes, it is desirable to set an insulating film on the powder with an average particle size of 1 μm or more, and it is also possible not to set an insulating film on the metal magnetic particles with an average particle size of less than 1 μm or the third metal magnetic particles with a small average particle size. This is because, even if the metal magnetic particles with a very small average particle size short-circuit with other metal magnetic particles, the effect on eddy current loss is slight.
[0053] In one embodiment, the insulating film provided on the surface of the metal magnetic particles is an amorphous silicon oxide film with structural defects. The amorphous silicon oxide film with structural defects is provided on the surface of each metal magnetic particle in the following manner. First, a SiO2 layer is formed on the surface of each metal magnetic particle, for example, by a coating process using a sol-gel method. Specifically, first, a treatment solution containing TEOS (tetraethoxysilane, Si(OC2H5)4), ethanol and water is mixed in a mixed solution containing metal magnetic particles, ethanol and ammonia water to prepare a mixed solution, and then the mixed solution is stirred, and then the stirred mixed solution is filtered to separate the metal magnetic particles with SiO2 provided on their respective surfaces. In one embodiment, the thickness of the SiO2 layer formed on the surface of the metal magnetic particles is less than 100nm when the average particle size of the metal magnetic particles is less than 200μm. The thickness of the SiO2 layer provided on the metal magnetic particles can be changed according to the average particle size of the metal magnetic particles.
[0054] Next, the metal magnetic particles formed with the SiO2 layer are heat treated in a reducing atmosphere. The heat treatment is performed as follows: for example, H2 gas is used as the atmosphere gas, and the temperature is 400 to 800°C for 20 to 60 minutes. The temperature and time of the heat treatment can be appropriately set according to the thickness of the SiO2 layer so that the SiO2 layer is sintered as an amorphous silicon oxide film instead of a crystalline substance. In addition, the hydrogen concentration, temperature and time of the heat treatment can be appropriately set according to the composition and average particle size of the metal magnetic particles in order to suppress the oxidation of the metal magnetic particles. The SiO2 layer formed on the surface of the metal magnetic particles has the effect of suppressing the bonding of the metal particles caused by the above-mentioned heat treatment. Therefore, by forming the SiO2 layer on the surface of the metal magnetic particles, the heat treatment can be performed at a higher temperature than when the SiO2 layer is not formed. In this way, the problem of bonding of particles in the heat treatment process is alleviated, so various materials can be used as metal magnetic particles. As a reducing atmosphere gas, in addition to H2 gas, various reducing atmosphere gases such as H2 diluted with nitrogen or argon can be used.
[0055] By performing heat treatment under a reducing atmosphere, sintering of the SiO2 layer proceeds, an amorphous silicon oxide film is generated, and in the process of generating this silicon oxide film, N, O and / or C are discharged from the metal magnetic particles. The generation of the amorphous silicon oxide film and the discharge of N, O and / or C from the inside of the metal magnetic particles occur simultaneously in the initial process of the heat treatment, so it is believed that the gas containing N, O and / or C discharged from the metal magnetic particles is taken into the inside of the silicon oxide film as fine bubbles. The silicon oxide film thus formed becomes amorphous silicon dioxide with structural defects containing bubbles. That is, structural defects are introduced into this amorphous silicon oxide film (amorphous silicon dioxide film) by heat treatment under a reducing atmosphere. The amorphous silicon oxide film (amorphous silicon dioxide film) having such structural defects has the flexibility to follow the deformation of the metal magnetic particles caused by the forming pressure, etc., because of the introduced structural defects. The above-mentioned amorphous silicon oxide film has structural defects including bubbles and has a lower hardness than a silicon oxide film without structural defects, so it is considered that it is easy to follow the deformation of the metal magnetic particles. In addition, when the metal magnetic particles are deformed by the forming pressure, the amorphous silicon oxide film follows the deformation of the metal magnetic particles and deforms in a manner to fill the gaps between the metal magnetic particles. Therefore, the adhesion between the metal magnetic particles can be improved through the amorphous silicon oxide film.
[0056] If the film thickness of the SiO2 layer before the heat treatment under the above-mentioned reducing atmosphere is compared with the film thickness of the amorphous silicon oxide film after the heat treatment, the film thickness of the silicon oxide film after the heat treatment is about 1.2 to 1.6 times the film thickness of the SiO2 layer before the heat treatment. The rate of change varies depending on the treatment temperature. When the film thickness of the SiO2 layer before the heat treatment is 50nm, it can be confirmed that the film thickness of the silicon oxide film after the heat treatment is about 70nm. The change in its film thickness also changes according to the thickness of the SiO2 layer. Specifically, the thinner the film thickness of the SiO2 layer before the heat treatment, the smaller the change, and the thicker the film thickness, the greater the change. For example, when the SiO2 layer is 17nm, the film thickness of the silicon oxide film after the heat treatment is about 20nm, and when the SiO2 layer is 63nm, the film thickness of the silicon oxide film after the heat treatment is about 100nm. By making the film thickness of the silicon oxide film 20nm to 100nm, it has the flexibility to follow the deformation of the metal magnetic particles and deform, and can also exist continuously on the surface of the metal magnetic particles. Such an amorphous silicon oxide film can insulate the metal magnetic particles from other metal magnetic particles.
[0057] Next, the metal magnetic particles having the amorphous silicon oxide film formed thereon as described above are mixed with a binder to prepare a slurry. A portion of the metal magnetic particles dispersed in the slurry is shown in FIG. Figure 4A middle. Figure 4A 7 metal magnetic particles 31a to 37a are shown in the figure. As shown in the figure, silicon oxide films 41a to 47a are respectively provided on the surface of each of the metal magnetic particles 31a to 37a. As mentioned above, the silicon oxide films 41a to 47a are amorphous silicon oxide films (amorphous silicon dioxide) with structural defects introduced into the film. By introducing structural defects into the silicon oxide films 41a to 47a, the silicon oxide films 41a to 47a can deform along with the deformation of the metal magnetic particles 31a to 37a during the forming process of silicon oxide described later. In order to introduce structural defects into the silicon oxide films 41a to 47a to enable such silicon oxide films 41a to 47a to follow the deformation of the metal magnetic particles 31a to 37a, in one embodiment, the thickness of the SiO2 layer formed on the surface of the metal magnetic particles is 100nm or less. If the SiO2 layer is thicker than this thickness, the structural defects introduced into the silicon oxide films 41a to 47a during the heat treatment in a reducing atmosphere may not reach a sufficient amount to ensure the flexibility of the silicon oxide films 41a to 47a. As mentioned above, when H2 gas is used as the atmosphere gas and the heat treatment is performed at 400 to 800°C for 20 to 60 minutes, structural defects can be introduced from the surface to a range of 50nm, which has been confirmed by the experimental observation of the inventor. Therefore, by making the thickness of the SiO2 layer formed on the surface of the metal magnetic particles less than 50nm, it is possible to introduce structural defects into the entire region of the silicon oxide films 41a to 47a in the thickness direction.
[0058] The binder contained in the composite magnetic material is, for example, a thermosetting resin with excellent insulation properties, such as epoxy resin, phenolic resin, polyimide resin, silicone resin, polystyrene (PS) resin, high-density polyethylene (HDPE) resin, polyoxymethylene (POM) resin, polycarbonate (PC) resin, polyvinylidene fluoride (PVDF) resin, phenolic resin, polytetrafluoroethylene (PTFE) resin, polyparaphenylene benzobisoxazole (PBO) resin, polyvinyl alcohol (PVA) resin, polyvinyl butyral (PVB) resin or acrylic resin.
[0059] Next, the slurry is placed in a forming mold and a forming pressure is applied to obtain a plate-shaped magnet sheet. The magnet sheet can be formed by warm forming or cold forming. During warm forming, the forming is performed at a temperature higher than the curing temperature of the binder and which does not affect the crystallization of the metal magnetic particles. For example, in warm forming, the forming is performed at a temperature of 150°C to 400°C. The forming pressure is, for example, 40MPa to 120MPa. In order to obtain the desired filling rate, the forming pressure can be appropriately adjusted.
[0060] The pressurization treatment for obtaining the magnet sheet can also be performed on a plurality of sheets at once. Specifically, the slurry can be applied to the surface of a plastic base film and dried, the dried slurry can be cut into sheets of a specified size, and the laminated body obtained by stacking a plurality of sheets can be pressurized.
[0061] Next, coil conductors are provided for the magnetic pieces produced in the above manner. Specifically, through holes are formed in the T-axis direction at predetermined positions of each magnetic piece, which is the magnetic film 11 to the magnetic film 16. Next, conductive paste is printed on the upper surface of each magnetic piece, which is the magnetic film 11 to the magnetic film 17, by screen printing to form a conductor pattern on the magnetic piece. In addition, conductive paste is buried in each through hole formed in each magnetic piece. In this way, the conductor patterns formed on the first magnetic piece, which is the magnetic film 11 to the magnetic film 17, become conductor patterns C11 to conductor patterns C17, respectively, and the metal buried in each through hole becomes through holes V1 to V6. Each conductor pattern can be formed by various known methods other than screen printing.
[0062] Next, the coil laminate is obtained by laminating the first magnetic sheets as the magnetic films 11 to 17. The magnetic sheets as the magnetic films 11 to 17 are laminated so that the conductor patterns C11 to C17 formed on the magnetic sheets are electrically connected to adjacent conductor patterns through the through holes V1 to V6.
[0063] Next, a plurality of magnet sheets are stacked to form an upper stacked body as the upper cover layer 18. Also, a plurality of magnet sheets are stacked to form a lower stacked body as the lower cover layer 19.
[0064] Next, the lower laminate, coil laminate, and upper laminate are stacked in order from the negative side to the positive side in the T-axis direction, and the stacked laminates are heat-pressed by a press to obtain a main laminate. The main laminate may not be formed into a lower laminate, coil laminate, and upper laminate, but may be formed by stacking all the prepared magnet sheets in order and heat-pressing the stacked magnet sheets together.
[0065] Next, the main body laminate is cut into pieces of a desired size using a cutting machine such as a slicer or a laser processing machine to obtain a chip laminate. Next, the chip laminate is degreased and the degreased chip laminate is subjected to a heat treatment. The ends of the chip laminate are subjected to a grinding treatment such as polishing as required.
[0066] Next, conductive paste is applied to both ends of the chip laminate to form external electrodes 21 and external electrodes 22. If necessary, at least one of a solder resist layer and a solder wet layer may be formed on the external electrodes 21 and external electrodes 22. As described above, the inductor 1 can be obtained.
[0067] Part of the steps included in the above-mentioned manufacturing method can be omitted as appropriate. In the manufacturing method of the inductor 1, steps not explicitly described in this specification can be performed as needed. Part of each step included in the above-mentioned manufacturing method of the inductor 1 can be performed in a different order at any time without departing from the purpose of the present invention. Part of each step included in the above-mentioned manufacturing method of the inductor 1 can be performed simultaneously or in parallel if possible.
[0068] Figure 4B The magnetic base 10 of the inductor 1 manufactured as described above is cut along the TW plane, and the area A of the cut cross section is enlarged (see Figure 3 ) and schematically shown in FIG. The metal magnetic particles 31 to 37 contained in the magnetic matrix 10 are Figure 4A The metal magnetic particles 31a to 37a contained in the slurry before the pressure molding shown in the figure are deformed under the pressure applied during the molding. Silicon oxide films 41 to 47 are respectively provided on the surfaces of the metal magnetic particles 31 to 37. The silicon oxide films 41 to 47 are deformed to follow the deformation of the metal magnetic particles 31a to 37a during the molding of the magnet piece.
[0069] like Figure 4AAs shown, in the slurry before forming, there are gaps between adjacent metal magnetic particles 31a to 37a. The gaps are filled with a binder. In contrast, in the magnetic matrix 10, the metal magnetic particles 31 to 37 are more densely filled with the help of the pressure applied during forming. In one embodiment, each metal magnetic particle 31 to 37 is in gapless contact with at least one of the adjacent metal magnetic particles. The pressure applied during forming is set so that each metal magnetic particle 31 to 37 is in contact with at least one of the adjacent metal magnetic particles via the silicon oxide film 41 to 47. Figure 4B In the illustrated embodiment, for example, the metal magnetic particle 31 is in contact with each of the adjacent metal magnetic particles 32 to 37 via the silicon oxide films 41 to 47 .
[0070] The thickness of the silicon oxide films 41 to 47 is considered to be the same if it is thicker than the thickness of the silicon oxide films 41a to 47a before sintering. The change in film thickness can be confirmed by using a scanning electron microscope (SEM) to confirm the particle cross section before and after heat treatment. Therefore, in one embodiment, the thickness of the silicon oxide films 41 to 47 is 100 nm or less. In another embodiment, the thickness of the silicon oxide films 41 to 47 is 50 nm or less. The thickness of the silicon oxide films 41 to 47 can be measured as follows: the magnetic substrate 10 is cut along the thickness direction (T direction) of the magnetic substrate to expose the cross section, and the cross section is photographed with a scanning electron microscope (SEM) at a magnification of 50,000 to 100,000 times, and the measurement is performed based on the photographed photograph. For example, the thickness of an insulating layer provided on a metal magnetic particle included in a SEM photograph can be the size of the insulating layer in the direction along the imaginary straight line connecting the geometric center of gravity of the metal magnetic particle in the SEM photograph and the geometric center of gravity of other metal magnetic particles adjacent to the metal magnetic particle. The thickness of the insulating layer provided on a certain metal magnetic particle included in the SEM photograph may also be the dimension of the insulating layer along an imaginary line extending from the geometrical center of gravity (centroid) of the metal magnetic particle in the SEM photograph in the up-down direction of the SEM photograph. In this case, since the dimensions at the upper side and the dimensions at the lower side relative to the center of gravity are measured, the average of the dimensions may be used as the thickness of the insulating layer of the metal magnetic particle. When there are multiple first metal magnetic particles in the SEM photograph, the thickness of the insulating layer is obtained for each of the multiple metal magnetic particles, and the average value thereof is used as the thickness of the insulating layer provided on the first metal magnetic particle of the magnetic substrate.
[0071] Defects are introduced into the silicon oxide films 41 to 47, and the magnetic substrate can be cut to expose the cross section, which can be confirmed by observing the cross section with a transmission electron microscope (TEM). Specifically, the cross section is irradiated with an electron beam at an acceleration voltage of 5V, and the cross section is photographed at a magnification of 100,000 times. In the photograph taken this way, the region where the defects are introduced into the silicon oxide films 41 to 47 is reflected darker than other regions. Due to the presence of such dark regions, the presence of structural defects in the silicon oxide films 41 to 47 can be confirmed. The region where the structural defects are introduced into the film is reflected darkly because the electron beam irradiated to the region is damaged when the region is photographed.
[0072] If the metal magnetic particles 31 to 37 and the silicon oxide films 41 to 47 are compared, the composition, especially the oxygen content, is different. Therefore, by analyzing the composition in each region of the cross section of the magnetic substrate 10, the boundary between the metal magnetic particles 31 to 37 and the corresponding silicon oxide films 41 to 47 can be determined. [Example]
[0073] Next, an embodiment of the present invention is described. First, metal magnetic particles formed of pure iron (99.92wt% Fe) with an average particle size of 5μm are prepared, and a SiO2 film with a thickness of 50nm is formed on the metal magnetic particles by a sol-gel method. Secondly, the metal magnetic particles formed with the SiO2 film are heat treated at 700°C for 60 minutes in an H2 atmosphere to form metal magnetic particles having an amorphous silicon oxide film with structural defects. Next, the metal magnetic particles provided with the amorphous silicon oxide film are mixed with polyvinyl butyral to form a slurry. Next, the slurry is injected into a molding mold, and a specified molding pressure is applied to produce a plurality of plate-shaped magnet pieces. As molding pressures, three pressures of 40MPa, 80MPa, and 120MPa are used. Thus, three types of magnet pieces molded with different molding pressures are obtained. For the sake of convenience, the magnet piece formed by a forming pressure of 40MPa is called the first magnet piece, the magnet piece formed by a forming pressure of 80MPa is called the second magnet piece, and the magnet piece formed by a forming pressure of 120MPa is called the third magnet piece. Then, a through hole for a through-hole conductor is set at a specified position of the magnet piece thus made. Then, a conductive paste containing Cu is buried in the through hole, and a conductive paste containing Cu is printed on the surface of each magnet piece according to a specified pattern. The magnet pieces with conductor patterns thus formed are stacked in such a way that adjacent conductor patterns are electrically connected by the conductors buried in the through holes to obtain a stack. In the stack, three types of stacks are included according to the type of magnet pieces used. That is, the first stack is formed by stacking the first magnet piece with a conductor pattern, the second stack is formed by stacking the second magnet piece with a conductor pattern, and the third stack is formed by stacking the third magnet piece with a conductor pattern. Next, the laminate was singulated using a slicer to obtain a chip laminate. The chip laminate thus obtained was heated at 650°C for 30 minutes in a H2 gas atmosphere. Next, a conductive paste was applied to both ends of the heated chip laminate to form a set of external electrodes. The external electrodes were plated with Ni and Sn to obtain three types of inductors. In these three types of inductors, the molding pressures used to mold the magnetic sheets constituting each magnetic matrix were different.
[0074] When the three types of inductors thus produced were cut along the T-axis direction and the cut cross-section was observed with a SEM at a magnification of 50,000 times, it was confirmed that a thin film of approximately 50 nm was formed on the surface of the metal magnetic particles with a substantially uniform thickness. The thin film on the surface of the metal magnetic particles was confirmed to be an amorphous silicon oxide film by SEM-EDS mapping.
[0075] In addition, the cross-sections of the three types of inductors were photographed at a magnification of 100,000 times using TEM. When observing with TEM, the cross-section of the inductor was irradiated with an electron beam at an accelerating voltage of 5 V. In the TEM photograph obtained in this way, black dot-shaped patterns can be observed in the area of the silicon oxide film. This confirmed that structural defects caused by electron beam damage were introduced into the silicon oxide film.
[0076] In addition, the magnetic permeability and Q value of 0.1MHz to 100MHz of the inductor obtained in the above manner were measured using an impedance analyzer (E4991A manufactured by Keysight Technologies Inc.). As a result, the magnetic permeabilities of the inductors made of magnetic sheets made at molding pressures of 40MPa, 80MPa, and 120MPa were 30, 55, and 66, respectively. In each of these inductors, a peak of the Q value appeared in the frequency region above 1MHz. This confirmed that the insulation between particles is guaranteed in the high-frequency region.
[0077] Next, the effects of the above-mentioned embodiment will be described. According to the magnetic substrate 10 of the above-mentioned embodiment, an amorphous silicon oxide film 41 to 47 is provided on the surface of each metal magnetic particle 31 to 37 in such a manner that adjacent metal magnetic particles 31 to 37 do not short-circuit each other. The amorphous silicon oxide films 41 to 47 are formed by introducing amorphous silicon dioxide with structural defects. This structural defect is considered to be caused by the gas containing N, O and / or C discharged from the metal magnetic particles being taken in as bubbles by the amorphous silicon dioxide when the SiO2 layer is fired in a reducing atmosphere to generate amorphous silicon dioxide. In the magnetic substrate 10 of the above-mentioned embodiment, since the structural defects are introduced into the silicon oxide films 41 to 47, the silicon oxide films 41 to 47 have flexibility. Therefore, the silicon oxide films 41 to 47 are easily deformed due to the structural defects in the film. Therefore, when the metal magnetic particles 31 to 37 are deformed due to the molding pressure applied when the magnetic base 10 is molded, the silicon oxide films 41 to 47 can also deform following the deformation of the metal magnetic particles 31 to 37. Therefore, the silicon oxide films 41 to 47 are difficult to be damaged during molding. Thus, the damage of the silicon oxide films 41 to 47 caused by the molding pressure applied when the magnetic base 10 is molded can be suppressed, and as a result, the short circuit between adjacent metal magnetic particles 31 to 37 can be prevented. Thus, in the magnetic base 10 of the above-mentioned embodiment, the occurrence of eddy current loss is suppressed.
[0078] In one embodiment described above, each metal magnetic particle 31 to 37 is connected to at least one of the adjacent metal magnetic particles through the silicon oxide film 41 to 47 without a gap. At this time, the distance between the adjacent metal magnetic particles (the distance between the outer surface of a metal magnetic particle and the outer surface of the metal magnetic particle adjacent to the metal magnetic particle) is the amount of two layers of silicon oxide film. Thus, in one embodiment described above, the distance between the adjacent metal magnetic particles can be reduced to the amount of two layers of silicon oxide film, thereby increasing the filling rate of the metal magnetic particles 31 to 37 of the magnetic substrate 10.
[0079] In one embodiment described above, a third metal magnetic particle having a third average particle size smaller than the second average particle size and having a third insulating layer formed on the surface thereof is further provided. The third metal magnetic particle 33 can further improve the filling rate of the metal magnetic particles of the magnetic matrix 10. In addition, the third metal magnetic particle 33 enters between the first metal magnetic particles 31, between the second metal magnetic particles 32, and between the first metal magnetic particles 31 and the second metal magnetic particles 32, thereby improving the mechanical strength of the magnetic matrix 10. In this way, the third metal magnetic particle 33, because it has a third average particle size smaller than the first metal magnetic particles 31 and the second metal magnetic particles 32, although it has little effect on the magnetic saturation characteristics of the magnetic matrix 10, it contributes to the improvement of the filling rate of the magnetic matrix 10 and the improvement of the mechanical strength of the magnetic matrix 10.
[0080] According to the above-described embodiment, the filling rate of the metal magnetic particles in the magnetic base 10 can be increased, and thus the inductor 1 having high inductance can be obtained.
[0081] The size, material and configuration of each component described in this specification are not limited to the contents clearly described in the embodiment, and each component can be deformed in a manner having any size, material, and configuration that can be included in the scope of the present invention. In addition, the components that are not clearly described in this specification can be added to the described embodiment, and a part of the components described in each embodiment can also be omitted.
Claims
1. A magnetic substrate, comprising: a first metal magnetic particle having a first amorphous silicon oxide film on a surface thereof; and a second metal magnetic particle having a second amorphous silicon oxide film on a surface thereof and adjacent to the first metal magnetic particle; Structural defects are introduced into the first amorphous silicon oxide film and the second amorphous silicon oxide film, respectively. The first metal magnetic particle and the second metal magnetic particle are in contact with each other via the first amorphous silicon oxide film and the second amorphous silicon oxide film. In a photograph obtained by irradiating the cross section of the magnetic substrate with an electron beam at an accelerating voltage of 5 V using a transmission electron microscope and taking the cross section at a magnification of 100,000 times, the structural defect appears darker than other regions.
2. The magnetic substrate according to claim 1, in, The first amorphous silicon oxide film and the second amorphous silicon oxide film are formed to have a thickness of 100 nm or less.
3. The magnetic substrate according to claim 2, in, The first amorphous silicon oxide film and the second amorphous silicon oxide film are formed to have a thickness of 50 nm or less.
4. The magnetic substrate according to claim 2, in, The first amorphous silicon oxide film and the second amorphous silicon oxide film are formed to have a thickness of 20 nm or more.
5. The magnetic substrate according to claim 3, in, The first amorphous silicon oxide film and the second amorphous silicon oxide film are formed to have a thickness of 20 nm or more.
6. The magnetic substrate according to any one of claims 1 to 5, in, The metal magnetic particles contain Fe, and the content of Fe in the metal magnetic particles is 90 wt % or more. 7 . An electronic component comprising the magnetic substrate according to claim 1 .
8. An electronic component comprising: The magnetic substrate according to any one of claims 1 to 6; and A coil is arranged on the magnetic substrate.