A VCSEL chip and preparation method thereof
By employing a function gradient modulation process to adjust the potential barrier in VCSEL chips, the problems of low active region carrier gain and complex processes were solved, achieving high differential gain and low heat loss, and improving product stability.
Patent Information
- Application Number
- CN201911318203.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-19
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2039-12-19
AI Technical Summary
Existing VCSEL lasers have low active region carrier gain, making it impossible to simultaneously achieve high photon confinement and carrier confinement, and their manufacturing process is complex and costly.
By sequentially growing an N-type DBR layer, an N-type confinement layer, a first waveguide layer, a second waveguide layer, a quantum well, a second symmetric waveguide layer, a first symmetric waveguide layer, and a P-type confinement layer on the substrate surface of a VCSEL chip, and using a function-gradient modulation process to adjust the potential barrier, the potential barrier gradually changes to form a low resistance and high refractive index difference, thereby reducing heat loss and improving differential gain.
It improves the differential gain of VCSEL chips, reduces heat loss, and has a simple process, low cost, and high product stability.
Smart Images

Figure CN110943370B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of VCSEL technology, and in particular to a VCSEL chip and a preparation method thereof. Background Art
[0002] VCSEL, whose full name is Vertical Cavity Surface Emitting Laser, is developed based on gallium arsenide semiconductor materials. Different from other light sources such as LED (light emitting diode) and LD (Laser Diode), it has the advantages of small size, circular output spot, single longitudinal mode output, small threshold current, low price, easy integration into large-area arrays, etc. It is widely used in optical communication, optical interconnection, optical storage and other fields.
[0003] The epitaxial structure of the existing VCSEL laser usually includes a substrate, on which a buffer layer, an N-type doped DBR, an active layer, an oxidized confinement layer, a P-type doped DBR and a P-type cladding are sequentially deposited; wherein the active layer is composed of a confinement layer, a waveguide layer and a quantum well, a symmetric waveguide layer and a symmetric confinement layer. However, due to the growth quality of the active area material or the unreasonable design of the active area MQW structure, it is easy to cause the active area carrier gain of the epitaxial structure to be not large enough, and the VCSEL optical power is relatively small, which is difficult to meet the application requirements of most near-infrared sensors.
[0004] To solve the above problems, some VCSEL lasers set up symmetrical waveguide layers with gradient refractive index or gradient composition, such as patent publication number: CN107093841A, which proposes an epitaxial structure of a near-infrared VCSEL laser and its preparation method. By directly setting a group of symmetrical waveguide layers with gradient composition on the two contact surfaces of the quantum well, and coordinating them through the special structural design of the quantum well, that is, inserting multiple thick barrier layers in the active area to cooperate, it is possible to reduce the leakage loss of carriers and thus improve the differential gain of the active area. However, the light field of this patent solution is close to the current limiting layer. Due to the aggregation of carriers, the edge suppression mode is stronger than the fundamental mode, resulting in the generation of high-order modes and a larger divergence angle; at the same time, since the insertion of multiple thick barrier layers in the active area requires precise control, it is bound to cause complicated processes, high costs, affect the stability of the product, and affect the potential barriers of the quantum well.
[0005] In view of this, the inventor specially designed a VCSEL chip and a method for preparing the same, which resulted in this case. Summary of the invention
[0006] The purpose of the present invention is to provide a VCSEL chip and a method for preparing the same, so as to solve the problems in the prior art of low carrier gain in the active region, inability to simultaneously have high photon confinement and carrier confinement, and complex process and high cost.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a VCSEL chip, comprising:
[0009] providing a substrate;
[0010] An N-type DBR layer, an N-type confinement layer, a first waveguide layer, a second waveguide layer, a quantum well, a second symmetric waveguide layer, a first symmetric waveguide layer, and a P-type confinement layer are sequentially grown on the surface of the substrate; the first waveguide layer and the first symmetric waveguide layer are respectively obtained by performing a function-gradient modulation process on the potential barrier; and the potential barrier of the first waveguide layer is greater than the potential barrier of the second waveguide layer, the potential barrier of the second waveguide layer is greater than the potential barrier of the second symmetric waveguide layer, the potential barrier of the second symmetric waveguide layer is less than the potential barrier of the first symmetric waveguide layer, the potential barrier of the first symmetric waveguide layer is less than the barrier of the P-type confinement layer, and the barrier of the P-type confinement layer is greater than the minimum value of the potential barrier of the first waveguide layer;
[0011] A P-type oxidation interface stop layer, a P-type DBR layer and a P-type cladding layer are sequentially grown on the surface of the P-type confinement layer.
[0012] Preferably, the function includes but is not limited to a rational function or an elementary function.
[0013] Preferably, the method for preparing the VCSEL chip comprises the following steps:
[0014] S01, providing a substrate;
[0015] S02, growing the N-type DBR layer on the surface of the substrate;
[0016] S03, growing an N-type confinement layer, so that the potential barrier of the N-type confinement layer is R1;
[0017] S04, growing a first waveguide layer, so that the potential barrier of the first waveguide layer gradually changes from R2 to R5, and R1>R2>R5;
[0018] S05, maintaining the potential barrier R5 described in step S04, and growing a second waveguide layer;
[0019] S06, growing a quantum well, so that the potential barrier of the quantum well is smaller than the potential barrier of the second waveguide layer;
[0020] S07, growing a second symmetric waveguide layer, so that the potential barrier of the second symmetric waveguide layer is R6, and R6<R5;
[0021] S08, growing a first symmetric waveguide layer, so that the potential barrier of the first symmetric waveguide layer gradually changes from R5 to R3, and R5<R3<R2;
[0022] S09, growing a P-type confinement layer, so that the potential barrier of the P-type confinement layer is greater than or equal to R3 and less than R2;
[0023] S10, sequentially growing the P-type oxidation interface stop layer, the P-type DBR layer and the P-type cladding layer on the surface of the P-type confinement layer.
[0024] Preferably, the N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer each include Al x GaAs layer, and the first waveguide layer and the first symmetric waveguide layer are both obtained by performing a function-gradient modulation process on the Al element composition.
[0025] Preferably, the N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer each include Al x Ga y In z P layer, and the first waveguide layer and the first symmetric waveguide layer are both obtained by performing a function-gradient modulation process on the Al element composition.
[0026] Preferably, the N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer each include Al x InGaAs layer, and the first waveguide layer and the first symmetric waveguide layer are both obtained by performing a function-gradient modulation process on the Al element composition.
[0027] Preferably, the Al element composition of the first waveguide layer is greater than the Al element composition of the second waveguide layer, the Al element composition of the second waveguide layer is greater than the Al element composition of the second symmetric waveguide layer, the Al element composition of the second symmetric waveguide layer is less than the Al element composition of the first symmetric waveguide layer, the Al element composition of the first symmetric waveguide layer is less than the Al element composition of the P-type confinement layer, and the Al element composition of the P-type confinement layer is greater than the minimum value of the Al element composition of the first waveguide layer.
[0028] The present invention also provides a VCSEL chip, the VCSEL chip comprising:
[0029] substrate;
[0030] An N-type DBR layer, an N-type confinement layer, a first waveguide layer, a second waveguide layer, a quantum well, a second symmetric waveguide layer, a first symmetric waveguide layer, and a P-type confinement layer are sequentially grown on the surface of the substrate; the first waveguide layer and the first symmetric waveguide layer respectively include potential barriers with a gradual function change; and the potential barrier of the first waveguide layer is greater than the potential barrier of the second waveguide layer, the potential barrier of the second waveguide layer is greater than the potential barrier of the second symmetric waveguide layer, the potential barrier of the second symmetric waveguide layer is less than the potential barrier of the first symmetric waveguide layer, the potential barrier of the first symmetric waveguide layer is less than the barrier of the P-type confinement layer, and the potential barrier of the P-type confinement layer is greater than the minimum value of the potential barrier of the first waveguide layer;
[0031] A P-type oxidation interface stop layer, a P-type DBR layer and a P-type cladding layer are sequentially grown on the surface of the P-type confinement layer.
[0032] Preferably, the N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer each include Al x GaAs layer, where x is the composition of the Al element.
[0033] Preferably, the N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer each include Al x Ga y In z P layer, where x is the component of Al element.
[0034] Preferably, the N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer each include Al x In y GaAs layer, where x is the composition of the Al element.
[0035] Preferably, Al element composition functions of the first waveguide layer and the first symmetric waveguide layer vary gradually.
[0036] Preferably, the Al element composition of the first waveguide layer is greater than the Al element composition of the second waveguide layer, the Al element composition of the second waveguide layer is greater than the Al element composition of the second symmetric waveguide layer, the Al element composition of the second symmetric waveguide layer is less than the Al element composition of the first symmetric waveguide layer, the Al element composition of the first symmetric waveguide layer is less than the Al element composition of the P-type confinement layer, and the Al element composition of the P-type confinement layer is greater than the minimum value of the Al element composition of the first waveguide layer.
[0037] Preferably, Al element composition X of the N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer is greater than zero and less than or equal to 0.9.
[0038] Preferably, the Al element component X of the N-type confinement layer is 0.9; and the thickness of the N-type confinement layer is 30 - 100 nm, including the end values.
[0039] Preferably, the Al element component of the first waveguide layer varies gradually, wherein the Al element component X gradually changes from a range function of 0.6 to 0.9 to a range of 0.1 to 0.6, excluding the end values; and the thickness of the first waveguide layer is 10 - 50 nm, including the end values.
[0040] Preferably, the Al element component X of the second waveguide layer satisfies: 0.1 < X < 0.8; and the thickness of the second waveguide layer is 30 - 100 nm, including the end values.
[0041] Preferably, the Al element component X of the second symmetric waveguide layer satisfies: 0.1 < X < 0.8; and the thickness of the second symmetric waveguide layer is 30 - 100 nm, including the end values.
[0042] Preferably, the Al element component of the first symmetric waveguide layer varies gradually, wherein the Al element component X gradually changes from a range function of 0.1 to 0.6 to a range of 0.6 to 0.9, excluding the end values; and the thickness of the first symmetric waveguide layer is 10 - 50 nm, including the end values.
[0043] According to the above technical solutions, the VCSEL chip and its manufacturing method provided by the present invention grow an N-type DBR layer, an N-type confinement layer, a first waveguide layer, a second waveguide layer, a quantum well, a second symmetric waveguide layer, a first symmetric waveguide layer, and a P-type confinement layer on the surface of the substrate in sequence; the first waveguide layer and the first symmetric waveguide layer are respectively obtained by a modulation process of gradually changing the potential barrier; and the potential barrier of the first waveguide layer is greater than the potential barrier of the second waveguide layer, the potential barrier of the second waveguide layer is greater than the potential barrier of the second symmetric waveguide layer, the potential barrier of the second symmetric waveguide layer is less than the potential barrier of the first symmetric waveguide layer, the potential barrier of the first symmetric waveguide layer is less than the potential barrier of the P-type confinement layer, and the potential barrier of the P-type confinement layer is greater than the minimum value of the potential barrier of the first waveguide layer.
[0044] Firstly, growing the first waveguide layer between the N-type confinement layer and the second waveguide layer can effectively alleviate the potential barrier difference caused by the different Al components of the N-type confinement layer and the second waveguide layer; secondly, by adjusting the Al element component X, the potential barrier of the first symmetrical waveguide layer is gradually changed as a function, so that the potential barriers at the head and tail end points of the first waveguide layer are infinitely close to the potential barriers of the N-type confinement layer and the second waveguide layer, respectively, thereby reducing the potential barrier junction between the N-type confinement layer and the second waveguide layer to a greater extent, thereby obtaining a better series resistance value, and providing a better refractive index for the growth of the second waveguide layer; thirdly, through the transition of the first waveguide layer, a low resistance is formed between the N-type confinement layer and the second waveguide layer, thereby reducing the heat loss of the VCSEL chip to a certain extent, thereby achieving the effect of improving the differential gain of the VCSEL chip.
[0045] Similarly, growing the first symmetric waveguide layer between the second symmetric waveguide layer and the P-type confinement layer can effectively mitigate the barrier difference caused by the different Al components of the second symmetric waveguide layer and the P-type confinement layer; secondly, by adjusting the Al element composition X, the barrier of the first symmetric waveguide layer is gradually changed as a function, so that the barrier at the head and tail end points of the first symmetric waveguide layer are infinitely close to the barrier of the second symmetric waveguide layer and the P-type confinement layer, thereby reducing the barrier junction of the second symmetric waveguide layer and the P-type confinement layer to a greater extent, thereby obtaining a better series resistance; thirdly, through the transition of the first symmetric waveguide layer, a low resistance is formed between the second symmetric waveguide layer and the P-type confinement layer, thereby reducing the heat loss of the VCSEL chip to a certain extent, and further achieving the effect of improving the differential gain of the VCSEL chip.
[0046] Secondly, by setting the potential barrier of the first waveguide layer to be greater than the potential barrier of the second waveguide layer, the potential barrier of the second waveguide layer to be smaller than the potential barrier of the second symmetric waveguide layer, the potential barrier of the second symmetric waveguide layer to be smaller than the potential barrier of the first symmetric waveguide layer, the potential barrier of the first symmetric waveguide layer to be smaller than the potential barrier of the P-type confinement layer, and the potential barrier of the P-type confinement layer to be greater than the minimum value of the potential barrier of the first waveguide layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer form a refractive index difference, so that light can easily approach the high-refractive-index N-type confinement layer for concentrated propagation, and the impurity absorption of photons by the P-type material is reduced, thereby improving the fundamental mode capability of the VCSEL chip, reducing the generation of edge modes, thereby reducing the divergence angle, and further improving the gain of the fundamental mode.
[0047] Furthermore, the VCSEL chip and the preparation method thereof provided by the present invention can be simultaneously applicable to ternary / quaternary material systems containing Al components in different bands.
[0048] Finally, the above-mentioned preparation method has a simple process and low cost, and the VCSEL chip product obtained by the above-mentioned preparation method has high stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0050] Figure 1 A schematic diagram of the structure of the VCSEL chip provided in this application;
[0051] Figure 2 Schematic diagram of the variation of Al element composition during the growth process of the VCSEL chip provided in this application;
[0052] Explanation of symbols in the figure: 1. substrate, 2. buffer layer, 3. N-type DBR layer, 4. N-type confinement layer, 5. first waveguide layer, 6. second waveguide layer, 7. quantum well, 8. second symmetric waveguide layer, 9. first symmetric waveguide layer, 10. P-type confinement layer, 11. P-type oxide interface stop layer, 12. P-type DBR layer, 13. P-type cladding layer. DETAILED DESCRIPTION
[0053] To make the content of the present invention clearer, the content of the present invention is further described below in conjunction with the accompanying drawings. The present invention is not limited to this specific embodiment. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0054] Example 1
[0055] like Figure 1 As shown, a method for preparing a VCSEL chip comprises:
[0056] Providing a substrate 1;
[0057] A buffer layer 2, an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9, and a P-type confinement layer 10 are sequentially grown on the surface of the substrate 1; the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include Al xGaAs layer, wherein X is an Al element component, and the first waveguide layer 5 and the first symmetric waveguide layer 9 are respectively obtained by a modulation process of performing a function gradient on the potential barrier, specifically: performing a function gradient on the Al element flow rate, the Ga element flow rate and the Al element component X respectively to achieve a function gradient of the potential barrier; making the potential barrier of the first waveguide layer 5 greater than the potential barrier of the second waveguide layer 6, the potential barrier of the second waveguide layer 6 greater than the potential barrier of the second symmetric waveguide layer 8, the potential barrier of the second symmetric waveguide layer 8 less than the potential barrier of the first symmetric waveguide layer 9, the potential barrier of the first symmetric waveguide layer 9 less than the potential barrier of the P-type confinement layer 10, and the potential barrier of the P-type confinement layer 10 greater than the minimum value of the potential barrier of the first waveguide layer 5;
[0058] A P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 are sequentially grown on the surface of the P-type confinement layer 10 .
[0059] like Figure 2 As shown, the method for preparing a VCSEL chip includes the following steps:
[0060] S01, providing a GaAs substrate 1, and growing a buffer layer 2 on the surface of the substrate 1;
[0061] S02, growing an N-type DBR layer 3 on the surface of the buffer layer 2 at a growth temperature of 680-790° C. and a growth pressure of 50 mbar;
[0062] S03, growing an N-type limiting layer 4, the growth interval is as follows Figure 2 In the A1 segment shown, the N-type confinement layer 4 includes Al 0.9 GaAs, growth thickness is 30-100nm;
[0063] S04, lowering the growth temperature of step S02 to gradually change the temperature to 650-700°C, and adjusting the Al element composition X to make X=0.8; by functionally modulating the Al element flow rate, the Ga element flow rate, and the Al element composition X, a layer of Al is grown. x GaAs layer, X is modulated from 0.8 to 0.5, and the growth interval is as follows Figure 2 A2 segment shown; and then forming a first waveguide layer 5, the thickness of the first waveguide layer 5 is 10-50nm; wherein the Ga element flow rate satisfies the quadratic function equation Y (Ga_flow) = -3.381x 2 +45.49x-26.029, can also be transformed into other functions. The Al element flow rate satisfies the quadratic function equation Y(Al_flow)=9.5833x 2 -127.99x+539.71, can also be transformed into other functions including linear functions;
[0064] S05, maintaining the growth temperature of step S04, and adjusting the Al element composition X to grow a layer of Al x GaAs layer, where X = 0.5, the growth interval is as follows Figure 2 A3 segment shown; and then forming a second waveguide layer 6, the thickness of the second waveguide layer 6 is 30-100nm;
[0065] S06, grow quantum well 7, the growth interval is as follows Figure 2 Section A4 shown;
[0066] S07, maintaining the growth conditions of step S05, and growing a layer of Al x GaAs layer, where X = 0.4, the growth interval is as follows Figure 2 A5 segment shown; and then forming a second symmetric waveguide layer 8, the thickness of the second symmetric waveguide layer 8 is 30-100nm;
[0067] S08, increasing the growth temperature of step S07 to gradually change the temperature to 680-790°C, and adjusting the Al element composition X to make X=0.5; by functionally modulating the Al element flow rate, the Ga element flow rate, and the Al element composition X, a layer of Al is grown. x GaAs layer, X is modulated from 0.5 to 0.7, and the growth interval is as follows Figure 2 A6 segment shown; and then forming a first symmetrical waveguide layer 9, the thickness of the first symmetrical waveguide layer 9 is 10-50nm; wherein the Ga element flow rate satisfies the quadratic function equation Y(Ga_flow)=-3.381x 2 +45.49x-26.029, can also be transformed into other functions. The Al element flow rate satisfies the quadratic function equation Y(Al_flow)=9.5833x 2 -127.99x+539.71, can also be transformed into other functions including linear functions;
[0068] S09, grow a layer of Al x GaAs layer, where X = 0.7, the growth interval is as follows Figure 2 A7 segment shown; then forming a P-type confinement layer 10, the thickness of the P-type confinement layer 10 is 10-100nm;
[0069] S10 , sequentially growing a P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 on the surface of the P-type confinement layer 10 .
[0070] Functions include, but are not limited to, rational functions or elementary functions.
[0071] Adjustment of the growth temperature includes linear increase or linear decrease.
[0072] This embodiment further provides a VCSEL chip, the VCSEL chip comprising:
[0073] Substrate 1;
[0074] A buffer layer 2, an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9 and a P-type confinement layer 10 are sequentially stacked on the surface of the substrate 1; the first waveguide layer 5 and the first symmetric waveguide layer 9 respectively include potential barriers with gradual function changes;
[0075] A P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 are sequentially stacked on the surface of the P-type confinement layer 10 which faces away from the first symmetric waveguide layer 9 .
[0076] The N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include Al x GaAs layer, wherein X is a component of the Al element; and the potential barrier of the first waveguide layer 5 is greater than the potential barrier of the second waveguide layer 6, the potential barrier of the second waveguide layer 6 is greater than the potential barrier of the second symmetric waveguide layer 8, the potential barrier of the second symmetric waveguide layer 8 is smaller than the potential barrier of the first symmetric waveguide layer 9, the potential barrier of the first symmetric waveguide layer 9 is smaller than the potential barrier of the P-type confinement layer 10, and the potential barrier of the P-type confinement layer 10 is greater than the minimum value of the potential barrier of the first waveguide layer 5.
[0077] The Al element composition of the first waveguide layer 5 is greater than that of the second waveguide layer 6, the Al element composition of the second waveguide layer 6 is greater than that of the second symmetric waveguide layer 8, the Al element composition of the second symmetric waveguide layer 8 is less than that of the first symmetric waveguide layer 9, the Al element composition of the first symmetric waveguide layer 9 is less than that of the P-type confinement layer 10, and the Al element composition of the P-type confinement layer 10 is greater than the minimum value of the Al element composition of the first waveguide layer 5.
[0078] The Al element composition X of the N-type confinement layer 4 , the first waveguide layer 5 , the second waveguide layer 6 , the second symmetric waveguide layer 8 , the first symmetric waveguide layer 9 , and the P-type confinement layer 10 is greater than zero and less than or equal to 0.9.
[0079] The N-type confinement layer 4 includes Al x GaAs layer, wherein X=0.9; and the thickness of the N-type confinement layer 4 is 30-100 nm, including end values.
[0080] The first waveguide layer 5 includes Al with a gradient Al element composition. x GaAs layer, wherein the Al element composition X gradually changes from the range of 0.6 to 0.9 to the range of 0.1 to 0.6, excluding the end value; and the thickness of the first waveguide layer 5 is 10-50nm, including the end value.
[0081] The second waveguide layer 6 includes an Al x GaAs layer, where 0.1 < X < 0.8; and the thickness of the second waveguide layer 6 is 30 - 100 nm, including the end values.
[0082] The second symmetric waveguide layer 8 includes an Al x GaAs layer, where 0.1 < X < 0.8; and the thickness of the second symmetric waveguide layer 8 is 30 - 100 nm, including the end values.
[0083] The first symmetric waveguide layer 9 includes an AlGaAs layer with a gradually changing Al elemental composition, where x the Al elemental composition X gradually changes from a range of 0.1 to 0.6 to a range of 0.6 to 0.9, excluding the end values; and the thickness of the first symmetric waveguide layer 9 is 10 - 50 nm, including the end values.
[0084] Based on the above technical solutions, in other embodiments of the present application, the thicknesses of the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 and their Al elemental composition X only need to meet the aforementioned ranges and requirements, and be adaptively changed with reference to the above embodiments. The present application does not enumerate them here.
[0085] As can be seen from the above technical solutions, the VCSEL chip and its manufacturing method provided in this embodiment grow an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9, and a P-type confinement layer 10 on the surface of the substrate 1 in sequence; the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include an Al x GaAs layer, where X is the Al elemental composition, and the first waveguide layer 5 is obtained through a modulation process of gradually changing the flow rates of the Al element, the Ga element, and the Al elemental composition X respectively; the first symmetric waveguide layer 9 is obtained through a modulation process of gradually changing the flow rates of the Al element, the Ga element, and the Al elemental composition X respectively.
[0086] Firstly, growing the first waveguide layer 5 between the N-type confinement layer 4 and the second waveguide layer 6 can effectively mitigate the potential barrier difference caused by the different Al components of the N-type confinement layer 4 and the second waveguide layer 6; secondly, by adjusting the Al element component X, the potential barrier of the first waveguide layer 5 is gradually changed as a function, so that the potential barriers at the head and tail end points of the first waveguide layer 5 are infinitely close to the potential barriers of the N-type confinement layer 4 and the second waveguide layer 6, respectively, thereby reducing the potential barrier junction between the N-type confinement layer 4 and the second waveguide layer 6 to a greater extent, thereby obtaining a better series resistance value, and providing a better refractive index for the growth of the second waveguide layer 6; thirdly, through the transition of the first waveguide layer 5, a low resistance is formed between the N-type confinement layer 4 and the second waveguide layer 6, thereby reducing the heat loss of the VCSEL chip to a certain extent, thereby achieving the effect of improving the differential gain of the VCSEL chip.
[0087] Similarly, growing the first symmetric waveguide layer 9 between the second symmetric waveguide layer 8 and the P-type confinement layer 10 can effectively mitigate the potential barrier difference caused by the different Al components of the second symmetric waveguide layer 8 and the P-type confinement layer 10; secondly, by adjusting the Al element composition X, the potential barrier of the first symmetric waveguide layer 9 is gradually changed as a function, so that the potential barriers at the head and tail end points of the first symmetric waveguide layer 9 are infinitely close to the potential barriers of the second symmetric waveguide layer 8 and the P-type confinement layer 10, respectively, thereby reducing the barrier junction between the second symmetric waveguide layer 8 and the P-type confinement layer 10 to a greater extent, and thus obtaining a better series resistance; thirdly, through the transition of the first symmetric waveguide layer 9, a low resistance is formed between the second symmetric waveguide layer 8 and the P-type confinement layer 10, thereby reducing the heat loss of the VCSEL chip to a certain extent, and further achieving the effect of improving the differential gain of the VCSEL chip.
[0088] Furthermore, by setting that the Al element composition of the N-type confinement layer 4 is greater than the Al element composition of the first waveguide layer 5, the Al element composition of the first waveguide layer 5 is greater than the Al element composition of the second waveguide layer 6, the Al element composition of the second waveguide layer 6 is greater than the Al element composition of the second symmetric waveguide layer 8, the Al element composition of the second symmetric waveguide layer 8 is less than the Al element composition of the first symmetric waveguide layer 9, the Al element composition of the first symmetric waveguide layer 9 is less than the Al element composition of the P-type confinement layer 10, and the Al element composition of the P-type confinement layer 10 is greater than the minimum value of the Al element composition of the first waveguide layer 5, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 form a refractive index difference, so that light is easily close to the high-refractive index N-type confinement layer 4 for concentrated propagation, and the impurity absorption of photons by the P-type material is reduced, thereby improving the fundamental mode capability of the VCSEL chip, reducing the generation of edge modes, thereby reducing the divergence angle, and further improving the gain of the fundamental mode.
[0089] Finally, the above-mentioned preparation method has a simple process and low cost, and the VCSEL chip product obtained by the above-mentioned preparation method has high stability.
[0090] Example 2
[0091] like Figure 1 As shown, a method for preparing a VCSEL chip comprises:
[0092] Providing a substrate 1;
[0093] A buffer layer 2, an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9, and a P-type confinement layer 10 are sequentially grown on the surface of the substrate 1; the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include Al x Ga y In z P layer, wherein X is an Al element component, and the first waveguide layer 5 and the first symmetric waveguide layer 9 are respectively obtained by a modulation process of performing a function gradient on the potential barrier, specifically: the function gradient of the potential barrier is realized by performing a function gradient on the Al element flow rate, the Ga element flow rate and the Al element component X respectively; the potential barrier of the first waveguide layer 5 is greater than the potential barrier of the second waveguide layer 6, the potential barrier of the second waveguide layer 6 is greater than the potential barrier of the second symmetric waveguide layer 8, the potential barrier of the second symmetric waveguide layer 8 is less than the potential barrier of the first symmetric waveguide layer 9, the potential barrier of the first symmetric waveguide layer 9 is less than the potential barrier of the P-type confinement layer 10, and the potential barrier of the P-type confinement layer 10 is greater than the minimum value of the potential barrier of the first waveguide layer 5;
[0094] A P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 are sequentially grown on the surface of the P-type confinement layer 10 .
[0095] like Figure 2 As shown, the method for preparing a VCSEL chip includes the following steps:
[0096] S01, providing a substrate 1, and growing a buffer layer 2 on the surface of the substrate 1;
[0097] S02, growing an N-type DBR layer 3 on the surface of the buffer layer 2 at a growth temperature of 680-790° C. and a growth pressure of 50 mbar;
[0098] S03, growing an N-type limiting layer 4, the growth interval is as follows Figure 2 In the A1 segment shown, the N-type confinement layer 4 includes Al 0.9 GaInP, growth thickness is 30-100nm;
[0099] S04, lowering the growth temperature of step S02 to gradually change the temperature to 650-700°C, and adjusting the Al element composition X to make X=0.8; by functionally modulating the Al element flow rate, the Ga element flow rate, and the Al element composition X, a layer of Al is grown. x Ga y In z P layer, so that X is modulated from 0.8 to 0.5, the growth interval is Figure 2 A2 segment shown; and then forming a first waveguide layer 5, the thickness of the first waveguide layer 5 is 10-50nm; wherein the Ga element flow rate satisfies the quadratic function equation Y (Ga_flow) = -3.381x 2 +45.49x-26.029, can also be transformed into other functions. The Al element flow rate satisfies the quadratic function equation Y(Al_flow)=9.5833x 2 -127.99x+539.71, can also be transformed into other functions including linear functions;
[0100] S05, maintaining the growth temperature of step S04, and adjusting the Al element composition X to grow a layer of Al x Ga y In z P layer, where X = 0.5, and the growth interval is Figure 2 A3 segment shown; and then forming a second waveguide layer 6, the thickness of the second waveguide layer 6 is 30-100nm;
[0101] S06, grow quantum well 7, the growth interval is as follows Figure 2 Section A4 shown;
[0102] S07, maintaining the growth conditions of step S05, and growing a layer of Al x Ga y In z P layer, where X = 0.4, the growth interval is as follows Figure 2 A5 segment shown; and then forming a second symmetric waveguide layer 8, the thickness of the second symmetric waveguide layer 8 is 30-100nm;
[0103] S08, increasing the growth temperature of step S07 to gradually change the temperature to 680-790°C, and adjusting the Al element composition X to make X=0.5; by functionally modulating the Al element flow rate, the Ga element flow rate, and the Al element composition X, a layer of Al is grown. x Ga y In z P layer, so that X is modulated from 0.5 to 0.7, the growth interval is Figure 2A6 segment shown; and then forming a first symmetrical waveguide layer 9, the thickness of the first symmetrical waveguide layer 9 is 10-50nm; wherein the Ga element flow rate satisfies the quadratic function equation Y(Ga_flow)=-3.381x 2 +45.49x-26.029, can also be transformed into other functions. The Al element flow rate satisfies the quadratic function equation Y(Al_flow)=9.5833x 2 -127.99x+539.71, can also be transformed into other functions including linear functions;
[0104] S09, grow a layer of Al x Ga y In z P layer, where X = 0.7, and the growth interval is Figure 2 A7 segment shown; then forming a P-type confinement layer 10, the thickness of the P-type confinement layer 10 is 10-100nm;
[0105] S10 , sequentially growing a P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 on the surface of the P-type confinement layer 10 .
[0106] Functions include, but are not limited to, rational functions or elementary functions.
[0107] Adjustment of the growth temperature includes linear increase or linear decrease.
[0108] This embodiment further provides a VCSEL chip, the VCSEL chip comprising:
[0109] Substrate 1;
[0110] A buffer layer 2, an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9 and a P-type confinement layer 10 are sequentially stacked on the surface of the substrate 1; the first waveguide layer 5 and the first symmetric waveguide layer 9 respectively include potential barriers with gradual function changes;
[0111] A P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 are sequentially stacked on the surface of the P-type confinement layer 10 which faces away from the first symmetric waveguide layer 9 .
[0112] The N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include Al x Ga y In zP layer, where X is the component of Al element; and the potential barrier of the first waveguide layer 5 is greater than that of the second waveguide layer 6, the potential barrier of the second waveguide layer 6 is greater than that of the second symmetric waveguide layer 8, the potential barrier of the second symmetric waveguide layer 8 is less than that of the first symmetric waveguide layer 9, the potential barrier of the first symmetric waveguide layer 9 is less than that of the P-type confinement layer 10, and the potential barrier of the P-type confinement layer 10 is greater than the minimum value of the potential barrier of the first waveguide layer 5.
[0113] The Al element component of the first waveguide layer 5 is greater than that of the second waveguide layer 6, the Al element component of the second waveguide layer 6 is greater than that of the second symmetric waveguide layer 8, the Al element component of the second symmetric waveguide layer 8 is less than that of the first symmetric waveguide layer 9, the Al element component of the first symmetric waveguide layer 9 is less than that of the P-type confinement layer 10, and the Al element component of the P-type confinement layer 10 is greater than the minimum value of the Al element component of the first waveguide layer 5.
[0114] The Al element component X of the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 is greater than zero and less than or equal to 0.9.
[0115] The N-type confinement layer 4 includes Al x Ga y In z P layer, where X = 0.9; and the thickness of the N-type confinement layer 4 is 30 - 100 nm, including the end values.
[0116] The first waveguide layer 5 includes Al with a gradually changing Al element component x Ga y In z P layer, where the Al element component X gradually changes from the range of 0.6 - 0.9 to the range of 0.1 - 0.6, excluding the end values; and the thickness of the first waveguide layer 5 is 10 - 50 nm, including the end values.
[0117] The second waveguide layer 6 includes Al x Ga y In z P layer, where 0.1 < X < 0.8; and the thickness of the second waveguide layer 6 is 30 - 100 nm, including the end values.
[0118] The second symmetric waveguide layer 8 includes Al x Ga y In z P layer, where 0.1 < X < 0.8; and the thickness of the second symmetric waveguide layer 8 is 30 - 100 nm, including the end values.
[0119] The first symmetric waveguide layer 9 includes Al with a gradually changing Al element component x Gay In z P layer, wherein the Al element composition X gradually changes from the range of 0.1 to 0.6 to the range of 0.6 to 0.9, excluding the end value; and the thickness of the first symmetric waveguide layer 9 is 10-50nm, including the end value.
[0120] On the basis of the above technical solution, in other embodiments of the present application, the thickness of the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 and their Al element composition X only need to meet the aforementioned ranges and requirements and be adaptively changed with reference to the above embodiments, and the present application does not enumerate them all here.
[0121] Through the above technical solution, it can be known that the VCSEL chip and the preparation method thereof provided in this embodiment are characterized by sequentially growing an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9, and a P-type confinement layer 10 on the surface of a substrate 1; the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include Al x Ga y In z P layer, wherein X is the Al element component, and the first waveguide layer 5 is obtained by performing a function-gradient modulation process on the Al element flow rate, the Ga element flow rate and the Al element component X respectively; the first symmetric waveguide layer 9 is obtained by performing a function-gradient modulation process on the Al element flow rate, the Ga element flow rate and the Al element component X respectively.
[0122] Firstly, the first waveguide layer 5 is arranged between the N-type confinement layer 4 and the second waveguide layer 6, which can effectively alleviate the potential barrier difference caused by the different Al components of the N-type confinement layer 4 and the second waveguide layer 6; secondly, by adjusting the Al element component X, the potential barrier of the first waveguide layer 5 is gradually changed as a function, so that the potential barriers at the head and tail end points of the first waveguide layer 5 are infinitely close to the potential barriers of the N-type confinement layer 4 and the second waveguide layer 6, respectively, thereby reducing the potential barrier junction between the N-type confinement layer 4 and the second waveguide layer 6 to a greater extent, thereby obtaining a better series resistance value, and providing a better refractive index for the growth of the second waveguide layer 6; thirdly, through the transition of the first waveguide layer 5, a low resistance is formed between the N-type confinement layer 4 and the second waveguide layer 6, thereby reducing the heat loss of the VCSEL chip to a certain extent, thereby achieving the effect of improving the differential gain of the VCSEL chip.
[0123] Similarly, growing the first symmetric waveguide layer 9 between the second symmetric waveguide layer 8 and the P-type confinement layer 10 can effectively mitigate the potential barrier difference caused by the different Al components of the second symmetric waveguide layer 8 and the P-type confinement layer 10; secondly, by adjusting the Al element composition X, the potential barrier of the first symmetric waveguide layer 9 is gradually changed as a function, so that the potential barriers at the head and tail end points of the first symmetric waveguide layer 9 are infinitely close to the potential barriers of the second symmetric waveguide layer 8 and the P-type confinement layer 10, respectively, thereby reducing the barrier junction between the second symmetric waveguide layer 8 and the P-type confinement layer 10 to a greater extent, and thus obtaining a better series resistance; thirdly, through the transition of the first symmetric waveguide layer 9, a low resistance is formed between the second symmetric waveguide layer 8 and the P-type confinement layer 10, thereby reducing the heat loss of the VCSEL chip to a certain extent, and further achieving the effect of improving the differential gain of the VCSEL chip.
[0124] Furthermore, by setting that the Al element composition of the N-type confinement layer 4 is greater than the Al element composition of the first waveguide layer 5, the Al element composition of the first waveguide layer 5 is greater than the Al element composition of the second waveguide layer 6, the Al element composition of the second waveguide layer 6 is greater than the Al element composition of the second symmetric waveguide layer 8, the Al element composition of the second symmetric waveguide layer 8 is less than the Al element composition of the first symmetric waveguide layer 9, the Al element composition of the first symmetric waveguide layer 9 is less than the Al element composition of the P-type confinement layer 10, and the Al element composition of the P-type confinement layer 10 is greater than the minimum value of the Al element composition of the first waveguide layer 5, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 form a refractive index difference, so that light is easily close to the high-refractive index N-type confinement layer 4 for concentrated propagation, and the impurity absorption of photons by the P-type material is reduced, thereby improving the fundamental mode capability of the VCSEL chip, reducing the generation of edge modes, thereby reducing the divergence angle, and further improving the gain of the fundamental mode.
[0125] Finally, the above-mentioned preparation method has a simple process and low cost, and the VCSEL chip product obtained by the above-mentioned preparation method has high stability.
[0126] Example 3
[0127] like Figure 1 As shown, a method for preparing a VCSEL chip comprises:
[0128] Providing a substrate 1;
[0129] A buffer layer 2, an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9, and a P-type confinement layer 10 are sequentially grown on the surface of the substrate 1; the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include Alx In y GaAs layer, wherein X is an Al element component, and the first waveguide layer 5 and the first symmetric waveguide layer 9 are respectively obtained by a modulation process of performing a function gradient on the potential barrier, specifically: performing a function gradient on the Al element flow rate, the Ga element flow rate and the Al element component X respectively to achieve a function gradient of the potential barrier; making the potential barrier of the first waveguide layer 5 greater than the potential barrier of the second waveguide layer 6, the potential barrier of the second waveguide layer 6 greater than the potential barrier of the second symmetric waveguide layer 8, the potential barrier of the second symmetric waveguide layer 8 less than the potential barrier of the first symmetric waveguide layer 9, the potential barrier of the first symmetric waveguide layer 9 less than the potential barrier of the P-type confinement layer 10, and the potential barrier of the P-type confinement layer 10 greater than the minimum value of the potential barrier of the first waveguide layer 5;
[0130] A P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 are sequentially grown on the surface of the P-type confinement layer 10 .
[0131] like Figure 2 As shown, the method for preparing a VCSEL chip includes the following steps:
[0132] S01, providing a substrate 1, and growing a buffer layer 2 on the surface of the substrate 1;
[0133] S02, growing an N-type DBR layer 3 on the surface of the buffer layer 2 at a growth temperature of 680-790° C. and a growth pressure of 50 mbar;
[0134] S03, growing an N-type limiting layer 4, the growth interval is as follows Figure 2 In the A1 segment shown, the N-type confinement layer 4 includes Al 0.9 In y GaAs, growth thickness is 30-100nm;
[0135] S04, lowering the growth temperature of step S02 to gradually change the temperature to 650-700°C, and adjusting the Al element composition X to make X=0.8; by functionally modulating the Al element flow rate, the Ga element flow rate, and the Al element composition X, a layer of Al is grown. x In y GaAs layer, X is modulated from 0.8 to 0.5, and the growth interval is as follows Figure 2 A2 segment shown; and then forming a first waveguide layer 5, the thickness of the first waveguide layer 5 is 10-50nm; wherein the Ga element flow rate satisfies the quadratic function equation Y (Ga_flow) = -3.381x 2 +45.49x-26.029, can also be transformed into other functions. The Al element flow rate satisfies the quadratic function equation Y(Al_flow)=9.5833x 2-127.99x+539.71, can also be transformed into other functions including linear functions;
[0136] S05, maintaining the growth temperature of step S04, and adjusting the Al element composition X to grow a layer of Al x In y GaAs layer, where X = 0.5, the growth interval is as follows Figure 2 A3 segment shown; and then forming a second waveguide layer 6, the thickness of the second waveguide layer 6 is 30-100nm;
[0137] S06, grow quantum well 7, the growth interval is as follows Figure 2 Section A4 shown;
[0138] S07, maintaining the growth conditions of step S05, and growing a layer of Al x In y GaAs layer, where X = 0.4, the growth interval is as follows Figure 2 A5 segment shown; and then forming a second symmetric waveguide layer 8, the thickness of the second symmetric waveguide layer 8 is 30-100nm;
[0139] S08, increasing the growth temperature of step S07 to gradually change the temperature to 680-790°C, and adjusting the Al element composition X to make X=0.5; by functionally modulating the Al element flow rate, the Ga element flow rate, and the Al element composition X, a layer of Al is grown. x In y GaAs layer, X is modulated from 0.5 to 0.7, and the growth interval is as follows Figure 2 A6 segment shown; and then forming a first symmetrical waveguide layer 9, the thickness of the first symmetrical waveguide layer 9 is 10-50nm; wherein the Ga element flow rate satisfies the quadratic function equation Y(Ga_flow)=-3.381x 2 +45.49x-26.029, can also be transformed into other functions. The Al element flow rate satisfies the quadratic function equation Y(Al_flow)=9.5833x 2 -127.99x+539.71, can also be transformed into other functions including linear functions;
[0140] S09, grow a layer of Al x In y GaAs layer, where X = 0.7, the growth interval is as follows Figure 2 A7 segment shown; then forming a P-type confinement layer 10, the thickness of the P-type confinement layer 10 is 10-100nm;
[0141] S10 , sequentially growing a P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 on the surface of the P-type confinement layer 10 .
[0142] Functions include, but are not limited to, rational functions or elementary functions.
[0143] Adjustment of the growth temperature includes linear increase or linear decrease.
[0144] This embodiment further provides a VCSEL chip, the VCSEL chip comprising:
[0145] Substrate 1;
[0146] A buffer layer 2, an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9 and a P-type confinement layer 10 are sequentially stacked on the surface of the substrate 1; the first waveguide layer 5 and the first symmetric waveguide layer 9 respectively include potential barriers with gradual function changes;
[0147] A P-type oxidized interface stop layer 11 , a P-type DBR layer 12 and a P-type cladding layer 13 are sequentially stacked on the surface of the P-type confinement layer 10 which faces away from the first symmetric waveguide layer 9 .
[0148] The N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include Al x In y GaAs layer, wherein X is a component of the Al element; and the potential barrier of the first waveguide layer 5 is greater than the potential barrier of the second waveguide layer 6, the potential barrier of the second waveguide layer 6 is greater than the potential barrier of the second symmetric waveguide layer 8, the potential barrier of the second symmetric waveguide layer 8 is smaller than the potential barrier of the first symmetric waveguide layer 9, the potential barrier of the first symmetric waveguide layer 9 is smaller than the potential barrier of the P-type confinement layer 10, and the potential barrier of the P-type confinement layer 10 is greater than the minimum value of the potential barrier of the first waveguide layer 5.
[0149] The Al element composition of the first waveguide layer 5 is greater than that of the second waveguide layer 6, the Al element composition of the second waveguide layer 6 is greater than that of the second symmetric waveguide layer 8, the Al element composition of the second symmetric waveguide layer 8 is less than that of the first symmetric waveguide layer 9, the Al element composition of the first symmetric waveguide layer 9 is less than that of the P-type confinement layer 10, and the Al element composition of the P-type confinement layer 10 is greater than the minimum value of the Al element composition of the first waveguide layer 5.
[0150] The Al element composition X of the N-type confinement layer 4 , the first waveguide layer 5 , the second waveguide layer 6 , the second symmetric waveguide layer 8 , the first symmetric waveguide layer 9 , and the P-type confinement layer 10 is greater than zero and less than or equal to 0.9.
[0151] The N-type confinement layer 4 includes Al x In yGaAs layer, where X = 0.9; and the thickness of the N-type confinement layer 4 is 30 - 100 nm, including the end values.
[0152] The first waveguide layer 5 includes Al with a gradually changing Al x In y GaAs layer, where the Al element composition X gradually changes from the range of 0.6 - 0.9 to the range of 0.1 - 0.6, excluding the end values; and the thickness of the first waveguide layer 5 is 10 - 50 nm, including the end values.
[0153] The second waveguide layer 6 includes Al x In y GaAs layer, where 0.1 < X < 0.8; and the thickness of the second waveguide layer 6 is 30 - 100 nm, including the end values.
[0154] The second symmetric waveguide layer 8 includes Al x In y GaAs layer, where 0.1 < X < 0.8; and the thickness of the second symmetric waveguide layer 8 is 30 - 100 nm, including the end values.
[0155] The first symmetric waveguide layer 9 includes Al with a gradually changing Al x In y GaAs layer, where the Al element composition X gradually changes from the range of 0.1 - 0.6 to the range of 0.6 - 0.9, excluding the end values; and the thickness of the first symmetric waveguide layer 9 is 10 - 50 nm, including the end values.
[0156] Based on the above technical solutions, in other embodiments of the present application, the thicknesses of the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 and their Al element compositions X only need to meet the aforementioned ranges and requirements, and can be adaptively changed with reference to the above embodiments. The present application does not list them exhaustively here.
[0157] From the above technical solutions, it can be seen that for the VCSEL chip and its manufacturing method provided in this embodiment, by sequentially growing an N-type DBR layer 3, an N-type confinement layer 4, a first waveguide layer 5, a second waveguide layer 6, a quantum well 7, a second symmetric waveguide layer 8, a first symmetric waveguide layer 9, and a P-type confinement layer 10 on the surface of the substrate 1; the N-type confinement layer 4, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 all include Al x In yGaAs layer, wherein X is the Al element component, and the first waveguide layer 5 is obtained by performing a function-gradient modulation process on the Al element flow rate, the Ga element flow rate and the Al element component X respectively; the first symmetric waveguide layer 9 is obtained by performing a function-gradient modulation process on the Al element flow rate, the Ga element flow rate and the Al element component X respectively.
[0158] Firstly, the first waveguide layer 5 is arranged between the N-type confinement layer 4 and the second waveguide layer 6, which can effectively alleviate the potential barrier difference caused by the different Al components of the N-type confinement layer 4 and the second waveguide layer 6; secondly, by adjusting the Al element component X, the potential barrier of the first waveguide layer 5 is gradually changed as a function, so that the potential barriers at the head and tail end points of the first waveguide layer 5 are infinitely close to the potential barriers of the N-type confinement layer 4 and the second waveguide layer 6, respectively, thereby reducing the potential barrier junction between the N-type confinement layer 4 and the second waveguide layer 6 to a greater extent, thereby obtaining a better series resistance value, and providing a better refractive index for the growth of the second waveguide layer 6; thirdly, through the transition of the first waveguide layer 5, a low resistance is formed between the N-type confinement layer 4 and the second waveguide layer 6, thereby reducing the heat loss of the VCSEL chip to a certain extent, thereby achieving the effect of improving the differential gain of the VCSEL chip.
[0159] Similarly, growing the first symmetric waveguide layer 9 between the second symmetric waveguide layer 8 and the P-type confinement layer 10 can effectively mitigate the potential barrier difference caused by the different Al components of the second symmetric waveguide layer 8 and the P-type confinement layer 10; secondly, by adjusting the Al element composition X, the potential barrier of the first symmetric waveguide layer 9 is gradually changed as a function, so that the potential barriers at the head and tail end points of the first symmetric waveguide layer 9 are infinitely close to the potential barriers of the second symmetric waveguide layer 8 and the P-type confinement layer 10, respectively, thereby reducing the barrier junction between the second symmetric waveguide layer 8 and the P-type confinement layer 10 to a greater extent, and thus obtaining a better series resistance; thirdly, through the transition of the first symmetric waveguide layer 9, a low resistance is formed between the second symmetric waveguide layer 8 and the P-type confinement layer 10, thereby reducing the heat loss of the VCSEL chip to a certain extent, and further achieving the effect of improving the differential gain of the VCSEL chip.
[0160] Furthermore, by setting that the Al element composition of the N-type confinement layer 4 is greater than the Al element composition of the first waveguide layer 5, the Al element composition of the first waveguide layer 5 is greater than the Al element composition of the second waveguide layer 6, the Al element composition of the second waveguide layer 6 is greater than the Al element composition of the second symmetric waveguide layer 8, the Al element composition of the second symmetric waveguide layer 8 is less than the Al element composition of the first symmetric waveguide layer 9, the Al element composition of the first symmetric waveguide layer 9 is less than the Al element composition of the P-type confinement layer 10, and the Al element composition of the P-type confinement layer 10 is greater than the minimum value of the Al element composition of the first waveguide layer 5, the first waveguide layer 5, the second waveguide layer 6, the second symmetric waveguide layer 8, the first symmetric waveguide layer 9, and the P-type confinement layer 10 form a refractive index difference, so that light is easily close to the high-refractive index N-type confinement layer 4 for concentrated propagation, and the impurity absorption of photons by the P-type material is reduced, thereby improving the fundamental mode capability of the VCSEL chip, reducing the generation of edge modes, thereby reducing the divergence angle, and further improving the gain of the fundamental mode.
[0161] Finally, the above-mentioned preparation method has a simple process and low cost, and the VCSEL chip product obtained by the above-mentioned preparation method has high stability.
[0162] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same and similar parts between the embodiments can be referred to each other. The above description of the disclosed embodiments enables professionals and technicians in this field to implement or use the present application. Various modifications to these embodiments will be obvious to professionals and technicians in this field, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will comply with the widest range consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a VCSEL chip, characterized in that: include: providing a substrate; An N-type DBR layer, an N-type confinement layer, a first waveguide layer, a second waveguide layer, a quantum well, a second symmetric waveguide layer, a first symmetric waveguide layer, and a P-type confinement layer are sequentially grown on the surface of the substrate; the first waveguide layer and the first symmetric waveguide layer are respectively obtained by performing a function-gradient modulation process on the potential barrier; and the potential barrier of the first waveguide layer is greater than the potential barrier of the second waveguide layer, the potential barrier of the second waveguide layer is greater than the potential barrier of the second symmetric waveguide layer, the potential barrier of the second symmetric waveguide layer is less than the potential barrier of the first symmetric waveguide layer, the potential barrier of the P-type confinement layer is greater than the minimum value of the potential barrier of the first symmetric waveguide layer, and the potential barrier of the P-type confinement layer is greater than the minimum value of the potential barrier of the first waveguide layer; A P-type oxidation interface stop layer, a P-type DBR layer and a P-type cladding layer are sequentially grown on the surface of the P-type confinement layer.
2. The method for preparing a VCSEL chip according to claim 1, characterized in that: The method for preparing the VCSEL chip comprises the following steps: S01, providing a substrate; S02, growing the N-type DBR layer on the surface of the substrate; S03, growing an N-type confinement layer, so that the potential barrier of the N-type confinement layer is R1; S04, growing a first waveguide layer, so that the potential barrier of the first waveguide layer gradually changes from R2 to R5, and R1>R2>R5; S05, maintaining the potential barrier R5 described in step S04, and growing a second waveguide layer; S06, growing a quantum well, so that the potential barrier of the quantum well is smaller than the potential barrier of the second waveguide layer; S07, growing a second symmetric waveguide layer, so that the potential barrier of the second symmetric waveguide layer is R6, and R6<R5; S08, growing a first symmetric waveguide layer, so that the potential barrier of the first symmetric waveguide layer gradually changes from R5 to R3, and R5<R3<R2; S09, growing a P-type confinement layer, so that the potential barrier of the P-type confinement layer is greater than or equal to R3 and less than R2; S10, sequentially growing the P-type oxidation interface stop layer, the P-type DBR layer and the P-type cladding layer on the surface of the P-type confinement layer.
3. The method for preparing a VCSEL chip according to claim 2, characterized in that: The N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer respectively include Al x GaAs layer, and the first waveguide layer and the first symmetric waveguide layer are both obtained by performing a function-gradient modulation process on the Al element composition.
4. The method for preparing a VCSEL chip according to claim 2, characterized in that: The N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer respectively include Al x Ga y In z P layer, and the first waveguide layer and the first symmetric waveguide layer are both obtained by performing a function-gradient modulation process on the Al element composition.
5. The method for preparing a VCSEL chip according to claim 2, characterized in that: The N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer respectively include Al x InGaAs layer, and the first waveguide layer and the first symmetric waveguide layer are both obtained by performing a function-gradient modulation process on the Al element composition.
6. The method for preparing a VCSEL chip according to claim 3, 4 or 5, characterized in that: The Al element composition of the first waveguide layer is greater than the Al element composition of the second waveguide layer, the Al element composition of the second waveguide layer is greater than the Al element composition of the second symmetric waveguide layer, the Al element composition of the second symmetric waveguide layer is less than the Al element composition of the first symmetric waveguide layer, the Al element composition of the first symmetric waveguide layer is less than the Al element composition of the P-type confinement layer, and the Al element composition of the P-type confinement layer is greater than the minimum value of the Al element composition of the first waveguide layer.
7. A VCSEL chip, characterized in that: The VCSEL chip comprises: substrate; An N-type DBR layer, an N-type confinement layer, a first waveguide layer, a second waveguide layer, a quantum well, a second symmetric waveguide layer, a first symmetric waveguide layer, and a P-type confinement layer are sequentially grown on the surface of the substrate; the first waveguide layer and the first symmetric waveguide layer respectively include potential barriers with a gradual function change; and the potential barrier of the first waveguide layer is greater than the potential barrier of the second waveguide layer, the potential barrier of the second waveguide layer is greater than the potential barrier of the second symmetric waveguide layer, the potential barrier of the second symmetric waveguide layer is less than the potential barrier of the first symmetric waveguide layer, the potential barrier of the first symmetric waveguide layer is less than the barrier of the P-type confinement layer, and the potential barrier of the P-type confinement layer is greater than the minimum value of the potential barrier of the first waveguide layer; Growing a P-type oxide interface cutoff layer, a P-type DBR layer and a P-type cladding layer in sequence on the surface of the P-type confinement layer; The N-type confinement layer, the first waveguide layer, the second waveguide layer, the second symmetric waveguide layer, the first symmetric waveguide layer, and the P-type confinement layer each include Al x GaAs layer or Al x Ga y In z P layer or Al x In y GaAs layer, wherein x is a composition of Al element; Furthermore, Al element composition functions of the first waveguide layer and the first symmetric waveguide layer vary gradually.
8. The VCSEL chip according to claim 7, characterized in that: The Al element composition of the first waveguide layer is greater than the Al element composition of the second waveguide layer, the Al element composition of the second waveguide layer is greater than the Al element composition of the second symmetric waveguide layer, the Al element composition of the second symmetric waveguide layer is less than the Al element composition of the first symmetric waveguide layer, the Al element composition of the first symmetric waveguide layer is less than the Al element composition of the P-type confinement layer, and the Al element composition of the P-type confinement layer is greater than the minimum value of the Al element composition of the first waveguide layer.
Citation Information
Patent Citations
Epitaxial structure of near-infrared VCSEL laser and manufacturing method thereof
CN107093841A
Semiconductor laser with low working voltage and high power conversion efficiency
CN104242057A
M-shaped gradually varied waveguide semiconductor laser device structure
CN107579431A
VCSEL chip
CN210866775U
Semiconductor laser element and laser device using the same
JP2818029B2