Coating compositions for use with overcoated photoresists

By using a primer composition of PDQ and resin between the photoresist layer and the substrate, the problem of uneven linewidth and resolution limitations caused by reflected radiation during the photoresist exposure process is solved, achieving higher lithography results and pattern quality.

CN111033381BActive Publication Date: 2024-10-11DUPONT SPECIALTY MATERIALS KOREA LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN201880038368.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-08-09
Publication Date
2024-10-11
Estimated Expiration
2038-08-09

AI Technical Summary

Technical Problem

The uneven line width and patterning resolution limitations caused by reflected radiation during the exposure process of existing photoresists make it difficult to effectively reduce the impact of reflected radiation on the photoresist layer.

Method used

Employing a primer composition containing a substituted photodecomposable quencher compound (PDQ) and a resin that reduces the migration of photogenerated acids by forming an absorbing layer between the photoresist layer and the substrate, and by ions after exposure The dissociation of the complex releases acidic anions, neutralizes strong acids in unexposed areas, and cooperates with the chromophore to absorb unwanted radiation and reduce reflection.

Benefits of technology

Improved resolution and focus latitude of lithography results, reduced acid neutralization of unexposed areas, enhanced photoresist layer planarization and via filling, and improved pattern collapse performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111033381B_ABST
    Figure CN111033381B_ABST
Patent Text Reader

Abstract

Organic coating compositions, particularly antireflective coating compositions for use with overcoated photoresists, are provided that include 1) one or more resins and 2) one or more PDQ compounds different from the 1) one or more resins.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application claims the benefit of priority to U.S. Application No. 15 / 626,872, filed on June 19, 2017, which is a continuation of U.S. Application No. 15624,699, filed on June 15, 2017, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to compositions for microelectronic applications, and in particular to anti-reflective coating compositions (eg, "BARC"). The compositions of the present invention comprise one or more substituted photodecomposable quencher compounds. Background Art

[0004] Photoresists are light-sensitive films used to transfer images onto substrates. A photoresist coating is formed on a substrate and the photoresist layer is then exposed to an activating radiation source through a photomask. After exposure, the photoresist is developed to provide a relief image that allows selective processing of the substrate.

[0005] Reflection of the activating radiation used to expose the photoresist generally limits the resolution of the image patterned in the photoresist layer. Reflection of radiation from the substrate / photoresist interface can cause spatial variations in the radiation intensity in the photoresist, resulting in non-uniform photoresist line widths when developed. Radiation can also be scattered from the substrate / photoresist interface into areas of the photoresist that are not intended to be exposed, again resulting in line width variations.

[0006] One approach for reducing the problem of reflected radiation is to use a radiation absorbing layer interposed between the substrate surface and the photoresist coating. See US 2016 / 0187778. See also US 2011 / 0200935; US 2012 / 0258405; and US 2015 / 0346599.

[0007] Electronic device manufacturers continually seek to increase the resolution of photoresist images patterned on anti-reflective coatings. Summary of the invention

[0008] We now provide novel coating compositions that can be used with overcoated photoresist compositions. In a preferred aspect, the coating compositions of the present invention can be used as effective antireflective layers for overcoated resist layers.

[0009] Preferred coating compositions may include 1) one or more resins (sometimes referred to herein as matrix resins) and 2) one or more substituted photodecomposable quencher compounds (PDQ) compounds different from 1) the one or more resins.

[0010] Without being bound by any theory, it is believed that the use of the preferred PDQ compounds as disclosed herein can minimize the migration of photogenerated acid from the exposed areas of the overcoated resist layer to the unexposed areas of the coated substrate (including the unexposed areas at the resist / underlayer interface). That is, the PDQ in the underlayer can inhibit the undesirable flow of photogenerated acid to the unexposed areas of the resist and underlayer coatings.

[0011] We have found that using one or more preferred PDGs in primer compositions can provide enhanced lithographic results. See the comparative results listed in the Examples below.

[0012] In one aspect, preferred PDQ compounds will react upon exposure to radiation used to image the overcoated photoresist layer. Exemplary imaging radiation is 193 nm and EUV. In particular, preferred PDQ compounds will react upon exposure to radiation used to image the overcoated photoresist layer and post-exposure baking (e.g., processing at 100° C. for 30 to 60 seconds) to release, such as by dissociation of the ionic complex (i.e., onium salt), the acidic anionic component.

[0013] In another aspect, preferred PDQ compounds are non-polymeric compounds. Suitable PDQ compounds may have a molecular weight of less than 3,000, or more typically less than 2500, or less than 2000, or less than 1500, or less than 1000, or less than 800, 700, 600, or 500.

[0014] In yet another aspect, preferred PDQ compounds are ionic compounds. Preferred ionic compounds for use as PDQ compounds are onium salts, such as sulfonium or iodonium compounds.

[0015] On the other hand, preferred PDQ compounds may have anions with high pKas (e.g., sulfamates with pKas greater than 0 or carboxylates with pKas greater than 3). As referred to herein, pKa values ​​are in aqueous solution at 23° C. and may be measured experimentally or calculated, for example, using Advanced Chemistry Development (ACD) Labs software version 11.02.

[0016] The acid generated by the preferred PDQ is weaker than the acid generated by the photoacid generator compound of the outer coated resist layer. Therefore, without being bound by theory, when the strong acid generated by the photoacid generator in the exposed area migrates to the unexposed bottom area of ​​the photoresist and then the photodestructible quencher with a higher pKa in the unexposed area quenches the strong acid diffusing from the exposed area. This may result in the strong acid in the unexposed area being neutralized.

[0017] Thus, in certain preferred aspects, the acidic component of the PDQ in the primer composition differs in pKa from the acidic component of the photoacid generator compound of the overcoated photoresist composition layer by 0.5, 1, 2, 3, or 4 or more.

[0018] Particularly preferred PDQ compounds may include formula (A),

[0019]

[0020] Where R 1 and R 2 are each independently hydrogen, substituted or unsubstituted alkyl (e.g., C 1 -C 12 alkyl), substituted or unsubstituted cycloalkyl (e.g. C 3 -C 12 cycloalkyl), or substituted or unsubstituted aryl (eg, 5- to 12-membered aryl or phenyl); and Y is a cation, such as a sulfonium cation.

[0021] Also particularly preferred PDQ compounds may include formula (B),

[0022]

[0023] Where R 3 is a substituted or unsubstituted alkyl group (e.g., C 1 -C 12 alkyl), substituted or unsubstituted cycloalkyl (e.g. C 3 -C 12 cycloalkyl), or substituted or unsubstituted aryl (eg, 5- to 12-membered aryl or phenyl); and Y is a cation, such as a sulfonium cation.

[0024] In certain preferred aspects, one or more of the resins may also contain one or more PDQ moieties, either as pendant groups or as integral units to the resin chains.

[0025] The coating composition of the present invention may further comprise a crosslinker component different from the PDQ compound and the resin. In preferred crosslinking compositions, a coating of the composition may harden or crosslink after heat treatment at 180°C, 200°C or 250°C or higher for 60, 90, 120 or 180 seconds.

[0026] For anti-reflective applications, the bottom layer composition of the present invention also preferably contains a component containing a chromophore that can absorb the undesired radiation used to expose the overcoated resist layer without reflecting back into the resist layer. The matrix polymer or the substituted PDQ compound can contain such a chromophore, or the coating composition can contain another component containing a suitable chromophore.

[0027] Particularly preferred coating compositions of the present invention may also contain a thermal acid (TAG) generator compound that can promote the hardening of the applied composition coating. Preferred coating compositions may include 1) one or more resins (sometimes referred to herein as matrix resins); 2) one or more substituted photodecomposable quencher compounds (PDQ) compounds different from 1) one or more resins; and 3) one or more thermal acid generator compounds (TAGs) different from 1) one or more resins and 2) one or more PDQ compounds. Preferred primer coating compositions may further include a crosslinker component different from 1) one or more resins, 2) one or more PDQ compounds, and 3) one or more TAGs.

[0028] When used together with the photoresist of outer coating, coating composition can be applied on the substrate such as semiconductor wafer that can have one or more organic or inorganic coating thereon.Before coating with photoresist layer outer coating, can optionally heat-treat applied coating.In the case of crosslinked composition, this kind of heat treatment may cause the hardening of coating composition layer, comprises crosslinking.This kind of crosslinking can comprise the covalent bond formation reaction between hardening and / or one or more composition components, and can regulate the water contact angle of coating composition layer.

[0029] Thereafter, a photoresist composition can be applied over the coating composition layer, the applied photoresist composition layer subsequently imaged with patterned activating radiation, and the imaged photoresist composition layer developed to provide a photoresist relief image.

[0030] A variety of photoresists can be used in combination with the coating compositions of the present invention (i.e., overcoated). Preferred photoresists for use with the primer coating compositions of the present invention are chemically amplified resists, especially positive and negative photoresists, which contain one or more photoactive compounds and a resin component containing units that undergo a deblocking or cleavage reaction in the presence of a photogenerated acid.

[0031] In certain preferred aspects, the photoresist composition is designed for use with a negative-tone resist, wherein exposed areas remain after a development process, but positive-tone development can also be used to remove exposed portions of the photoresist layer.

[0032] The invention further provides methods for forming photoresist relief images and novel articles comprising substrates, such as microelectronic wafer substrates, coated with the coating compositions of the invention, either alone or in combination with a photoresist composition.

[0033] Other aspects of the invention are disclosed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1Scanning electron micrographs of imaged photoresist / undercoat samples and comparative samples are shown. DETAILED DESCRIPTION

[0035] We now provide novel organic coating compositions that are particularly suitable for overcoated photoresist layers. As discussed above, preferred coating compositions may include 1) a matrix polymer; and 2) one or more PDQ compounds. Preferred coating compositions of the present invention may be applied by spin coating (spin-on compositions) and formulated as solvent compositions. The coating compositions of the present invention are particularly suitable for use as antireflective compositions for overcoated photoresists and / or as planarization or via filling compositions for overcoated photoresist composition coatings.

[0036] Particularly preferred PDQ compounds may have formula (A),

[0037]

[0038] Where R 1 and R 2 are each independently hydrogen, substituted or unsubstituted alkyl (e.g., C 1 -C 12 alkyl), substituted or unsubstituted cycloalkyl (e.g. C 3 -C 12 cycloalkyl), or substituted or unsubstituted aryl (eg, 5- to 12-membered aryl or phenyl); and Y is a cation, such as a sulfonium group.

[0039] Preferred R 1 and R 2 are independently hydrogen or C 1 -C 4 Alkyl, which may be optionally substituted by methyl, ethyl, cyclohexyl, cyclopentyl and adamantyl. Other preferred R 1 and R 2 Independently for C 3 -C 12 Cycloalkyl groups such as cyclohexyl, cyclopentyl and adamantyl.

[0040] Preferably Y is a C 1 -C 12 Alkyl, 2-8 membered heteroalkyl, C 3 -C 12 a sulfonium cation of a cycloalkyl, 5-12 membered heterocycloalkyl or 5-12 membered aryl (e.g., phenyl, naphthyl or anthracenyl), each of which is optionally substituted by C 1 -C 3 Alkyl or C 3 -C 12Other preferred Y is a sulfonium cation having a phenyl, cyclopentyl, cyclohexyl, adamantyl, methyl, ethyl, propyl, butyl, tert-butyl or isopropyl group, each of which is optionally replaced by a linear or branched C 1 -C 4 The alkyl group is substituted with methyl, ethyl, propyl, butyl, tert-butyl or isopropyl. Further preferred Y includes a 5-6 membered heterocycloalkyl group formed by a sulfur atom and an alkyl substituent.

[0041] Exemplary preferred anions Y may include:

[0042]

[0043] Exemplary PDQ compounds having formula (A) may include:

[0044]

[0045] Also particularly preferred PDQ compounds may include formula (B),

[0046]

[0047] Where R 3 is a substituted or unsubstituted alkyl group (e.g., C 1 -C 12 alkyl), substituted or unsubstituted cycloalkyl (e.g. C 3 -C 12 cycloalkyl), or substituted or unsubstituted aryl (e.g., 5 to 12 membered aryl or phenyl); and Y is as described herein. Preferred R 3 Can include C 1 -C 4 Alkyl, which may be linear or branched and optionally substituted. Other preferred R 3 C 3 -C 12 Cycloalkyl, such as cyclohexyl, cyclopentyl and adamantyl, or phenyl, may be optionally substituted.

[0048] Exemplary PDQ compounds having formula (B) may include:

[0049]

[0050] PDQ compounds are commercially available or can be easily synthesized. See the examples below.

[0051] As mentioned herein, suitable heteroalkyl groups include optionally substituted C 1 -C 20Alkoxy, preferably optionally substituted alkylthio having 1 to about 20 carbon atoms; preferably optionally substituted alkylsulfinyl having 1 to about 20 carbon atoms; preferably optionally substituted alkylsulfonyl having 1 to about 20 carbon atoms; and preferably optionally substituted alkylamine having 1 to about 20 carbon atoms.

[0052] The various materials and substituents that are "optionally substituted" may be appropriately substituted at one or more available positions by, for example, halogen (F, Cl, Br, I); nitro; hydroxy; amino; alkyl, such as C 1-4 Alkyl; alkenyl, such as C 2-8 Alkenyl; alkylamino, such as C 1-8 Alkylamino; carbocyclic aromatic groups, such as phenyl, naphthyl, anthracenyl, etc.; and the like.

[0053] Preferably, the one or more resins and the one or more substituted PDQ compounds are different materials, ie, the one or more resins and the one or more substituted PDQ compounds are not covalently linked.

[0054] The one or more substituted PDQ compounds are suitably present in the coating composition in an amount of from 0.1 weight percent to 10, 15, 20, 30, 40 or more weight percent based on the total solids weight of the coating composition, more typically from 1, 2 or 3 weight percent to 5, 10, 15 or 20 or more weight percent based on the total solids weight of the coating composition. Total solids are as referred to herein.

[0055] A variety of resins can be used as the matrix polymer of the primer composition.

[0056] The particularly preferred matrix resin of the coating composition of the present invention may contain polyester bonds. Polyester resins can be easily prepared by the reaction of one or more polyol reagents with one or more carboxyl-containing compounds (such as carboxylic acids, esters, anhydrides, etc.). Suitable polyol reagents include glycols, glycerol and triols, such as glycols, such as glycols are ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, butanediol, pentanediol, cyclobutanediol, cyclopentanediol, cyclohexanediol, dimethylolcyclohexane, and triols, such as glycerol, trimethylolethane, trimethylolpropane, etc.

[0057] The matrix resin of the coating composition of the present invention may contain a variety of additional groups, such as cyanurate groups, as disclosed in US Pat. Nos. 6,852,421 and 8,501,383.

[0058] Particularly preferred matrix resins of the coating compositions of the present invention may contain one or more cyanurate groups and polyester linkages.

[0059] As discussed, for anti-reflective applications, suitably one or more of the compounds reacted to form the resin comprises a moiety that can act as a chromophore to absorb radiation used to expose the over-applied photoresist coating. For example, phthalate compounds (e.g., phthalic acid or dialkyl phthalate (i.e., diesters, such as esters each having 1 to 6 carbon atoms, preferably dimethyl phthalate or ethyl phthalate) can be polymerized with aromatic or non-aromatic polyols and optionally other reactive compounds to provide polyesters that are particularly useful in coating compositions for use with photoresists imaged at wavelengths below 200 nm (e.g., 193 nm). PDQ compounds can also be polymerized with one or more polyols to provide resins useful in the primer coating compositions of the present invention. The resins are to be used in compositions with overcoated photoresists imaged at wavelengths below 300 nm or below 200 nm (e.g., 248 nm or 193 nm), naphthyl compounds can be polymerized, such as naphthyl compounds containing one or two or more carboxyl substituents, such as dialkyl naphthalene dicarboxylates, particularly di-C naphthalene dicarboxylates. 1-6 Also preferred are reactive anthracene compounds, for example anthracene compounds having one or more carboxyl groups or ester groups, such as one or more methyl or ethyl ester groups.

[0060] The compound containing the chromophore unit may also contain one or preferably two or more hydroxyl groups and react with the carboxyl-containing compound. For example, a phenyl compound or an anthracene compound having one, two or more hydroxyl groups may react with the carboxyl-containing compound.

[0061] Additionally, the primer coating composition for anti-reflective purposes may include a material containing a chromophore unit separate from the resin component that provides water contact angle adjustment (e.g., a resin containing photoacid-labile groups and / or base-reactive groups). For example, the coating composition may include a polymer or non-polymer compound containing phenyl, anthracene, naphthyl, etc. units. However, it is generally preferred that the one or more resins that provide water contact angle adjustment also contain a chromophore portion.

[0062] Preferably, the matrix resin of the primer composition of the present invention will have a weight average molecular weight (Mw) of about 1,000 to about 10,000,000 Daltons, more typically about 2,000 to about 100,000 Daltons, and a number average molecular weight (Mn) of about 500 to about 1,000,000 Daltons. The molecular weight (Mw or Mn) of the polymer of the present invention is suitably determined by gel permeation chromatography.

[0063] In many preferred embodiments, the matrix polymer will be the major solid component of the primer composition. For example, the matrix polymer may be present in an amount of 50 to 99.9 weight percent based on the total solids content of the coating composition, more typically 80 to 95 weight percent based on the total solids content of the coating composition. As referred to herein, the solids of the coating composition refer to all materials of the coating composition excluding the solvent carrier.

[0064] As described, the preferred primer coating compositions of the present invention can be crosslinked, for example, by heat treatment and / or radiation treatment. For example, the preferred primer coating compositions of the present invention can contain a separate crosslinker component that can be crosslinked with one or more other components of the coating composition. Typically, preferred crosslinked coating compositions contain a separate crosslinker component.

[0065] A variety of crosslinking agents may be employed, including those disclosed in European Application 542008. For example, suitable coating composition crosslinking agents include amine-based crosslinking agents, such as melamine materials, including melamine resins such as those manufactured by Cytec Industries and sold under the trade names Cymel 300, 301, 303, 350, 370, 380, 1116, and 1130. Glycolurils are particularly preferred, including glycolurils available from Cytec Industries. Benzguanidine and urea-based materials will also be suitable, including resins such as benzoguanidine resins available from Cytec Industries under the names Cymel 1123 and 1125, and urea resins available from Cytec Industries under the names Powderlink 1174 and 1196. In addition to being commercially available, such amine-based resins can be prepared, for example, by the reaction of acrylamide or methacrylamide copolymers with formaldehyde in a solution containing an alcohol, or alternatively by copolymerization of N-alkoxymethylacrylamide or methacrylamide with other suitable monomers.

[0066] The crosslinker component of the coating composition of the present invention is typically present in an amount of about 5 to 50 weight percent of the total solids (all components excluding the solvent carrier) of the coating composition, more typically about 5 to 25 weight percent of the total solids.

[0067] As discussed, particularly preferred coating compositions of the present invention may also contain thermal acid (TAG) generator compounds. Thermally induced crosslinking of the coating composition activated by a thermal acid generator is generally preferred. As discussed, a layer of the primer coating composition may be suitably applied to the heat treated substrate surface to activate, i.e., generate the released acid from the TAG and harden or crosslink one or more composition components. Thereafter, a photoresist layer may be applied to the hardened primer.

[0068] Suitable thermal acid generator compounds for use in the coating composition include ionic or substantially neutral thermal acid generators, such as ammonium salts of aromatic hydrocarbon sulfonates (e.g., ammonium toluene sulfonates), for catalyzing or promoting crosslinking during the curing of the anti-reflective composition coating. Typically, one or more thermal acid generators are present in the coating composition at a concentration of about 0.1 to 10 weight percent of the total dry components (all components except the solvent carrier) of the composition, more preferably about 0.5 to 2 weight percent of the total dry components.

[0069] The coating compositions of the present invention, particularly those used for reflection control applications, may also contain additional dye compounds that absorb the radiation used to expose the overcoated photoresist layer. Other optional additives include surface leveling agents, such as those available under the trade name Silwet 7604, or surfactants FC 171 or FC 431 available from 3M Company.

[0070] The primer compositions of the present invention may also contain other materials such as photoacid generators, including photoacid generators used with overcoated photoresist compositions as discussed. For a discussion of such use of photoacid generators in antireflective compositions, see U.S. Pat. No. 6,261,743.

[0071] To make the liquid coating composition of the present invention, the components of the coating composition are dissolved in a suitable solvent, such as one or more oxyisobutyrates, particularly methyl-2-hydroxyisobutyrate, ethyl lactate or glycol ethers such as one or more of 2-methoxyethyl ether (diglyme), ethylene glycol monomethyl ether and propylene glycol monomethyl ether; solvents having both ether and hydroxyl moieties, such as methoxybutanol, ethoxybutanol, methoxypropanol and ethoxypropanol; methyl 2-hydroxyisobutyrate; esters such as methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate and other solvents such as dibasic esters, propylene carbonate and γ-butyrolactone. The concentration of dry components in the solvent will depend on several factors, such as the method of application. Typically, the solids content of the primer composition varies from about 0.5 to 20 weight percent of the total weight of the coating composition, preferably the solids content varies from about 0.5 to 10 weight percent of the coating composition.

[0072] Exemplary Photoresist Systems

[0073] The photoresist used with the primer composition generally comprises a polymer and one or more acid generators. Positive resists are generally preferred, and the resist polymer has a functional group that imparts alkaline water solubility to the resist composition. For example, it is preferred to include a polar functional group (such as hydroxyl or carboxylate) or a polymer having an acid-labile group that can release such polar groups after the photolithography process. Preferably, the polymer is used in the resist composition in an amount sufficient to allow the resist to be developed with an alkaline aqueous solution.

[0074] Acid generators are also suitably used with polymers comprising repeating units containing aromatic groups, such as optionally substituted phenyl, including phenol, optionally substituted naphthyl and optionally substituted anthracene. Polymers containing optionally substituted phenyl (including phenol) are particularly suitable for many resist systems, including those imaged with EUV and electron beam radiation. For positive-acting resists, polymers also preferably contain one or more repeating units comprising acid-labile groups. For example, in the case of polymers containing optionally substituted phenyl or other aromatic groups, polymers may include repeating units containing one or more acid-labile parts, such as polymers formed by polymerization of monomers of acrylate or methacrylate compounds and acid-labile esters (such as tert-butyl acrylate or tert-butyl methacrylate). Such monomers can be copolymerized with one or more other monomers (such as styrene or vinylphenol monomers) comprising one or more aromatic groups (such as optionally phenyl).

[0075] Preferred monomers for forming such polymers include: acid labile monomers having the following formula (V), lactone-containing monomers or polarity-controlling monomers having the following formula (VI), or a combination comprising at least one of the foregoing monomers:

[0076]

[0077] Each R a are independently H, F, -CN, C 1-10 Alkyl, or C 1-10 In the acid-deprotectable monomer of formula (V), R b Independently for C 1-20 Alkyl, C 3-20 Cycloalkyl, C 6-20 Aryl or C 7-20 aralkyl, and each R b is independent or at least one R b With adjacent R b In the lactone-containing monomer of formula (VI), L is a monocyclic, polycyclic, or fused polycyclic C 4-20 Contains lactone group.

[0078] Exemplary acid-deprotectable monomers include, but are not limited to:

[0079]

[0080] or a combination comprising at least one of the foregoing, wherein R a H, F, -CN, C 1-6 Alkyl, or C 1-6 Fluoroalkyl.

[0081] Suitable lactone monomers may have the following formula (IX):

[0082]

[0083] Where R a H, F, -CN, C 1-6 Alkyl, or C 1-6 Fluoroalkyl, R is C 1-10 alkyl, cycloalkyl, or heterocycloalkyl, and w is an integer from 0 to 5. In formula (IX), R is directly connected to the lactone ring or is usually connected to the lactone ring and / or one or more R groups, and the ester portion is directly or indirectly connected to the lactone ring through R.

[0084] Exemplary lactone-containing monomers include:

[0085]

[0086] or a combination comprising at least one of the foregoing monomers, wherein R a H, F, -CN, C 1-10 Alkyl, or C 1-10 Fluoroalkyl.

[0087] Particularly suitable polymers having acid-labile deblocking groups for use in the positive-acting chemically amplified photoresists of the present invention have been disclosed in European Patent Application 0829766A2 (polymers having acetal and ketal polymers) and European Patent Application EP0783136A2 (terpolymers and other copolymers comprising units of 1) styrene; 2) hydroxystyrene; and 3) acid-labile groups, particularly acid-labile groups of alkyl acrylates.

[0088] Other preferred resins for photoresists for imaging below 200 nm (e.g. at 193 nm) include units of the following general formulae (I), (II) and (III):

[0089]

[0090] Where: R 1 Yes (C 1 -C 3 ) alkyl; R 2 Yes (C1 -C 3 ) alkylene; Li is a lactone group; and n is 1 or 2.

[0091] The molecular weight and polydispersity of the polymers used in the photoresists of the present invention may vary widely. Suitable polymers include w Those having a molecular weight distribution of about 1,000 to about 50,000, more typically about 2,000 to about 30,000, wherein the molecular weight distribution is about 3 or less, more typically about 2 or less.

[0092] Preferred negative-acting compositions of the present invention comprise a material that will cure, crosslink or harden upon exposure to an acid and a mixture of two or more acid generators as disclosed herein. Preferred negative-acting compositions comprise a polymeric binder (such as a phenolic or non-aromatic polymer), a crosslinker component and a photoactive component of the present invention. Such compositions and their uses have been disclosed in European Patent Application 0164248 and U.S. Patent No. 5,128,232 to Thackeray et al. Preferred phenolic polymers for use as polymeric binder components include novolacs and poly(vinylphenols), such as those discussed above. Preferred crosslinkers include amine-based materials (including melamine, glycoluril) benzoguanamine-based materials and urea-based materials. Melamine-formaldehyde polymers are generally particularly suitable. Such crosslinking agents are commercially available, for example, melamine polymers, glycoluril polymers, urea-based polymers and benzoguanamine polymers, such as those sold under the trade names Cymel 301, 303, 1170, 1171, 1172, 1123 and 1125 and Beetle 60, 65 and 80 by Cytec.

[0093] Particularly preferred photoresists of the present invention can be used in immersion lithography applications. For a discussion of preferred immersion lithography photoresists and methods, see, for example, US Pat. No. 7,968,268 to Rohm and Haas Electronic Materials.

[0094] The photoresist of the present invention may also contain a single acid generator or a mixture of different acid generators, typically a mixture of 2 or 3 different acid generators, more typically a mixture consisting of a total of 2 different acid generators. The photoresist composition contains an acid generator used in an amount sufficient to generate a latent image in a coating of the composition after exposure to activating radiation. For example, the acid generator will suitably be present in an amount of 1 to 20 wt % based on the total solids of the photoresist composition.

[0095] Suitable acid generators are known in the art of chemically amplified photoresists and include, for example: onium salts such as triphenylsulfonium trifluoromethanesulfonate, (p-tert-butoxyphenyl)diphenylsulfonium trifluoromethanesulfonate, tris(p-tert-butoxyphenyl)sulfonium trifluoromethanesulfonate, triphenylsulfonium p-toluenesulfonate; nitrobenzyl derivatives such as 2-nitrobenzyl-p-toluenesulfonate, 2,6-dinitrobenzyl-p-toluenesulfonate, and 2,4-dinitrobenzyl-p-toluenesulfonate; sulfonates such as 1,2,3-tris(methylsulfonyloxy)benzene, 1,2,3-tris(trifluoromethanesulfonyloxy)benzene, and 1,2,3-tris(p-toluenesulfonyloxy)benzene; heavy metals such as styryl, ... Azomethane derivatives, such as bis(benzenesulfonyl)diazomethane and bis(p-toluenesulfonyl)diazomethane; glyoxime derivatives, such as bis-O-(p-toluenesulfonyl)-α-dimethylglyoxime and bis-O-(n-butanesulfonyl)-α-dimethylglyoxime; sulfonate derivatives of N-hydroxyimide compounds, such as N-hydroxysuccinimide methanesulfonate and N-hydroxysuccinimide trifluoromethanesulfonate; and halogen-containing triazine compounds, such as 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine and 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-1,3,5-triazine.

[0096] As referred to herein, an acid generator can generate an acid when exposed to activating radiation, such as EUV radiation, electron beam radiation, 193 nm wavelength radiation or other radiation sources. Acid generator compounds as referred to herein may also be referred to as photoacid generator compounds.

[0097] Photoresists of the present invention may also contain other materials. For example, other optional additives include actinic dyes and contrast dyes, anti-striation agents, plasticizers, speed increasers and sensitizers. Such optional additives will usually be present in the photoresist composition with a smaller concentration.

[0098] Alternatively or in addition, other additives may include quenchers, which are bases that are not destructible by light, such as those based on hydroxides, carboxylates, amines, imines and amides. Preferably, such quenchers include C 1-30 An organic amine, imine or amide, or a C-type compound which can be a strong base (such as a hydroxide or alkoxide) or a weak base (such as a carboxylate) 1-30 Quaternary ammonium salts. Exemplary quenchers include amines such as tripropylamine, dodecylamine, tri(2-hydroxypropyl)amine, tetra(2-hydroxypropyl)ethylenediamine; arylamines such as diphenylamine, triphenylamine, aminophenol, and 2-(4-aminophenyl)-2-(4-hydroxyphenyl)propane; hindered amines such as diazabicycloundecene (DBU) or diazabicyclononene (DBN); or ion quenchers including alkyl quaternary ammonium salts such as tetrabutylammonium hydroxide (TBAH) or tetrabutylammonium lactate.

[0099] Surfactants include fluorinated and non-fluorinated surfactants, and are preferably nonionic. Exemplary fluorinated nonionic surfactants include perfluoro-C 4 Surfactants, such as FC-4430 and FC-4432 surfactants available from 3M Corporation; and fluorodiols, such as POLYFOX PF-636, PF-6320, PF-656, and PF-6520 fluorosurfactants from Omnova.

[0100] The photoresist further includes a solvent generally suitable for dissolving, dispensing and coating the components used in the photoresist. Exemplary solvents include anisole; alcohols, including ethyl lactate, 1-methoxy-2-propanol and 1-ethoxy-2-propanol; esters, including n-butyl acetate, 1-methoxy-2-propyl acetate, methoxyethoxy propionate, ethoxyethoxy propionate; ketones, including cyclohexanone and 2-heptanone; and combinations comprising at least one of the foregoing solvents.

[0101] Photolithography

[0102] In use, the coating composition of the present invention is applied to the substrate in the form of a coating by any of a variety of methods (such as spin coating). The coating composition is usually applied to the substrate with a dry layer thickness of about 0.02 to 0.5 μm, preferably a dry layer thickness of about 0.04 to 0.20 μm. The substrate is suitably any substrate used in the method involving a photoresist. For example, the substrate can be silicon, silicon dioxide or aluminum-aluminum oxide microelectronic wafers. Gallium arsenide, silicon carbide, ceramics, quartz or copper substrates can also be used. It is also suitable to use substrates for liquid crystal displays or other flat panel display applications, such as glass substrates, indium tin oxide coated substrates, etc. It is also possible to use substrates for optical and optoelectronic devices (such as waveguides).

[0103] Preferably, before the photoresist composition is applied to the bottom coating composition, the applied coating is cured. Curing conditions will vary with the components of the bottom coating composition. In particular, the curing temperature will depend on the specific acid or acid (heat) generator adopted in the coating composition. Typical curing conditions are from about 80 ℃ to 225 ℃ for about 0.5 to 5 minutes. Curing conditions preferably make the coating composition coating substantially insoluble in the photoresist solvent to be used and the developer solution.

[0104] After such solidification, the photoresist is applied on the surface of the applied coating composition. As with the application of one or more bottom coating composition layers, the outer coated photoresist can be applied by any standard means, such as by spin coating, dip coating, meniscus coating or roller coating. After application, the photoresist coating is usually dried by heating to remove the solvent, preferably until the resist layer is not sticky. Optimally, the intermixing of the bottom composition layer and the outer coated photoresist layer should not occur substantially.

[0105] The resist layer is then imaged in a conventional manner through a mask with activating radiation (e.g., 248 nm, 193 nm, or EUV radiation). The exposure energy is sufficient to effectively activate the photosensitive components of the resist system to produce a patterned image in the resist coating. Typically, the exposure energy is about 3 to 300 mJ / cm 2 , and depends in part on the exposure tool and the specific resist and resist processing employed. If desired, the exposed resist layer can be subjected to a post-exposure bake to create or enhance solubility differences between exposed and unexposed areas of the coating. For example, negative-acting acid-hardened photoresists typically require post-exposure heating to induce acid-promoted crosslinking reactions, and many chemically enhanced positive-acting resists require post-exposure heating to induce acid-promoted deprotection reactions. Typically, post-exposure bake conditions include temperatures of about 50°C or higher, and more specifically, temperatures of about 50°C to about 160°C.

[0106] The photoresist layer may also be exposed in an immersion lithography system, i.e. where the space between the exposure tool (particularly the projection lens) and the photoresist-coated substrate is occupied by an immersion fluid such as water or water mixed with one or more additives such as cesium sulfate, which may provide the fluid with an increased refractive index. Preferably, the immersion fluid (e.g. water) has been treated to avoid bubbles, e.g. the water may be degassed to avoid nanobubbles.

[0107] Reference herein to "immersion exposure" or other similar terms indicates that exposure is performed with such a fluid layer (eg, water or water with additives) interposed between the exposure tool and the applied photoresist composition layer.

[0108] The exposed photoresist layer is then treated with a suitable developer, which can selectively remove parts of the film to form a photoresist pattern. In the negative development method, the unexposed areas of the photoresist layer can be selectively removed by treating with a suitable non-polar solvent. For suitable procedures for negative development, see US2011 / 0294069. Typical non-polar solvents for negative development are organic developers, such as solvents selected from ketones, esters, hydrocarbons and mixtures thereof, such as acetone, 2-hexanone, 2-heptanone, methyl acetate, butyl acetate and tetrahydrofuran. The photoresist material used in the NTD process preferably forms a photoresist layer, which can form a negative image with an organic solvent developer, or a positive image with an aqueous alkaline developer (such as a tetraalkylammonium hydroxide solution). Preferably, the NTD photoresist is based on a polymer with an acid-sensitive (deprotectable) group, which forms a carboxylic acid group and / or a hydroxyl group when deprotected.

[0109] Alternatively, the development of the exposed photoresist layer can be achieved by treating the exposed layer with a suitable developer capable of selectively removing the exposed portions of the film (where the photoresist is positive) or removing the unexposed portions of the film (where the photoresist is crosslinkable in the exposed areas, i.e., negative). Preferably, the photoresist is positive, based on a polymer having acid-sensitive (deprotectable) groups that form carboxylic acid groups upon deprotection, and the developer is preferably a tetraalkylammonium hydroxide solution free of metal ions, such as, for example, a 0.26N aqueous solution of tetramethylammonium hydroxide. The pattern is formed by development.

[0110] The developed substrate can then be selectively processed according to procedures well known in the art on those substrate areas lacking photoresist, such as chemical etching or plating substrate areas lacking photoresist. Suitable etchants include hydrofluoric acid etching solutions and plasma gas etching, such as oxygen plasma etching. Plasma gas etching removes the underlying coating.

[0111] The following non-limiting examples illustrate the invention.

[0112] Example 1-2: PDQ synthesis

[0113] Example 1:

[0114]

[0115] To a mixture of 75.0 parts of compound (a) (Tokyo Industrial Chemistry, Co., Ltd.), 600 parts of chloroform, 240 parts of 10% aqueous sodium hydroxide solution are added. The resulting mixture is stirred at room temperature for 1 hour, and then the organic layer is separated and dried. 106 parts of triethylamine are added to the filtered organic layer. The resulting mixture is cooled to -10°C, and 51.2 parts of compound (c) are added, followed by stirring at room temperature for 1 hour. Then a compound of formula (d) is added, followed by overnight stirring and then aqueous extraction. The obtained organic layer is concentrated under reduced pressure. The solid is purified to provide compound (2).

[0116] Example 2

[0117]

[0118] To a mixture of 2.2 parts of compound (e) (Tokyo Industrial Chemical Co., Ltd.) and 50 parts of chloroform, 2.8 parts of triethylamine are added. The mixture is cooled to -10 ° C, and 1.6 parts of compound (f) are added, followed by stirring at room temperature. Then 4.0 parts of compound (g) are added to the reaction mixture, followed by overnight stirring and then aqueous extraction. The obtained organic layer is concentrated under reduced pressure. The solid is purified to provide compound (4).

[0119] Examples 3-6: Preparation of Primer Coating Compositions

[0120] Four different primer coating compositions (compositions of Examples 3, 4, 5 and 6, respectively) were prepared by mixing the materials (polymer, crosslinker, TAG, PDQ, solvent) of the types and amounts specified in Table 1 immediately below. The structures of the polymer, crosslinker, TAG, PDQ and solvent for each composition of Examples 3-6 follow Table 1. In each of Examples 3-6, the same polymer, crosslinker, TAG and solvent and their amounts were used. The only difference among the examples was the PDQ used and its amount (in Example 3, PDQ was not present). All weight percentages (wt.%) listed in Table 1 are based on the total solids of the coating composition (total solids are all materials of the composition excluding solvent).

[0121] Table 1. Sample formulations

[0122]

[0123]

[0124] The structure of the polymer for each of Examples 3-6.

[0125]

[0126] Structures of crosslinkers and TAGs of Examples 3-6

[0127]

[0128] The structure of the specified PDQ for Examples 4, 5, and 6.

[0129]

[0130] Solvent for each of Examples 3-6.

[0131] Example 7: Lithography Evaluation

[0132] Each coating composition of each of Examples 3 to 6 is spin-coated on a 4 cm x 4 cm wafer, which is pre-coated with a 65 nm cross-linked organic layer sold by Dow Chemical under the trade name AR46. The wafer coated with the composition of Examples 3-6 is then baked at 215° C. for one minute using a small coater. The BARC coating thickness after baking is 22 nm. A commercially available chemically enhanced photoresist composition is then spin-coated on each sample with the coating of Examples 3-6. The applied photoresist layer is soft-baked at 110° C. for 50 seconds, imaged through a mask with 193 nm radiation, and then exposed post-baking at 95° C. for 60 seconds.

[0133] The image samples were then processed with 0.26N TMAH aqueous developer. The photolithography results are listed below in Table 2. The coated system with PDQ in the primer composition showed better results, including wider focus latitude (FL) margin and improved pattern collapse performance. Figure 1 Scanning electron micrographs of the imaged and developed samples are further shown. Figure 1 As shown, Sample 1 is a sample imaged with the coating composition of Example 3; Sample 2 is a sample imaged with the coating composition of Example 4; Sample 3 is a sample imaged with the coating composition of Example 5; and Sample 4 is a sample imaged with the coating composition of Example 6;

[0134] Table 2. Lithography results

[0135]

Claims

1. A method for forming a photoresist relief image, comprising: a) applying a coating composition on a substrate, the coating composition comprising: 1) a resin, the resin comprising cyanurate groups; and 2) PDQ compounds; as well as b) applying a layer of photoresist composition on the coating composition layer, The PDQ compound has the following structure: in: R1 and R2 are each independently hydrogen, C1-C 12 Alkyl, or C3-C 12 Cycloalkyl; R3 is C3-C 12 cycloalkyl; and Y is a cation selected from the group consisting of: , Wherein, the coating composition further comprises 1) a crosslinker component and / or 2) a thermal acid generator compound, each different from the PDQ compound and the resin.

2. The method of claim 1, wherein: The PDQ compound has a sulfamate anion.

3. The method of claim 2, wherein: The PDQ compound comprises an anion with a pKa greater than zero.

4. The method of claim 1, wherein: Y is: 。 5. The method of claim 1, wherein: R1 and R2 are independently hydrogen, methyl, cyclohexyl or adamantyl and / or R3 is adamantyl.

6. The method according to any one of claims 1 to 5, wherein: The PDQ compound is: 。 7. A coated substrate comprising: A substrate having thereon: a) a coating composition comprising: 1) a resin comprising cyanurate groups; and 2) PDQ compounds; and b) a layer of photoresist composition on the coating composition layer, The PDQ compound has the following structure: in: R1 and R2 are each independently hydrogen, C1-C 12 Alkyl or C3-C 12 Cycloalkyl; R3 is C3-C 12 cycloalkyl; and Y is a cation selected from the group consisting of: ; Wherein, the coating composition further comprises 1) a crosslinker component and / or 2) a thermal acid generator compound, each different from the PDQ compound and the resin.

8. A coating composition for use with an overcoat photoresist composition, the coating composition comprising: 1) a resin comprising cyanurate groups; and 2) PDQ compounds, The PDQ compound has the following structure: in: R1 and R2 are each independently hydrogen, C1-C 12 Alkyl or C3-C 12 Cycloalkyl; R3 is C3-C 12 cycloalkyl; and Y is a cation selected from the group consisting of: ; Wherein, the coating composition further comprises 1) a crosslinker component and / or 2) a thermal acid generator compound, each different from the PDQ compound and the resin.

9. The coating composition according to claim 8, wherein The PDQ compound comprises a sulfamate anion.

Citation Information

Patent Citations

  • Chemically amplified positive photoresists

    EP0783136A2

  • Novel polymers and photoresist compositions

    EP0829766A2

  • Photoresist composition

    US20110200935A1

  • Photoresist compositions and methods of forming photolithographic patterns

    US20110294069A1

  • Resist composition and method for producing resist pattern

    US20120258405A1