Lead acid battery manufacturing method

By providing cross-configured convex strips in the separator of the lead-acid battery, the problem of insufficient strength of the joint is solved, the joint strength and penetration resistance are improved, and the performance of the battery is significantly improved.

CN111295780BActive Publication Date: 2024-11-05GS YUASA INT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880071253.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-10-31
Filing Date
2018-10-05
Publication Date
2024-11-05
Estimated Expiration
2038-10-05

AI Technical Summary

Technical Problem

In the existing lead-acid batteries, the joint strength of the bag-shaped spacer is insufficient, resulting in joint strength deviation and performance problems, especially in vibration tests and penetration short-circuitability.

Method used

By providing a plurality of first convex strips and second convex strips in the first and second regions of the spacer, and facing at the engaging portion in such a way that at least one first convex strip intersects at the at least one second convex strip, A cross configuration is formed to improve bonding strength and penetration short circuit resistance.

Benefits of technology

It effectively improves the bonding strength of the bag-shaped spacer in the lead-acid battery, reduces the bonding strength deviation, and significantly improves the penetration resistance, preventing the occurrence of short circuit in the lower part of the vibration test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111295780B_ABST
    Figure CN111295780B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a lead-acid battery, wherein the lead-acid battery is a lead-acid battery having a plate group formed by stacking a plurality of positive plates and a plurality of negative plates with a separator, and the method for manufacturing the lead-acid battery includes a step of processing the separator into a bag-like shape of a first region and a second region facing each other. The step of processing the separator into a bag-like shape includes a step of forming a joint, and the joint includes at least a portion in the first region and at least a portion in the second region. A plurality of first convex strips are provided in the first region, and a plurality of second convex strips are provided in the second region, and the step of forming the joint includes a step of making the first region and the second region face each other in a manner that at least one first convex strip and at least one second convex strip intersect in the joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a lead-acid battery. Background Art

[0002] Lead-acid batteries are used in various applications in addition to automotive and industrial applications. Lead-acid batteries include a negative electrode plate, a positive electrode plate, a separator interposed between the negative electrode plate and the positive electrode plate, and an electrolyte. An aqueous sulfuric acid solution is generally used as the electrolyte.

[0003] Patent Document 1 discloses an example in which a negative electrode plate is accommodated in a bag-shaped polyethylene separator, and the bag-shaped separator has convex lines on the negative electrode plate side. In this example, the convex lines are formed inside the bag-shaped separator.

[0004] When the separator is formed into a bag shape, the separator is usually bent into a U-shape and the two side edges are joined. As a method for joining the two side edges, there can be cited a method of meshing sealing, heat sealing and ultrasonic sealing, or a method using an adhesive material or an adhesive tape (for example, refer to Patent Document 2).

[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-22796

[0006] Patent Document 2: Japanese Patent Application Publication No. 2009-245901

[0007] In the production of the bag-shaped separator having ridges formed inside as exemplified in Patent Document 1, when both side edge portions of the separator are joined, the separator having ridges formed on the joining surface can be used.

[0008] However, when spacers having ridges formed on the joining surfaces are overlapped and both side edge portions are joined, sufficient joining strength may not be obtained depending on the arrangement of the ridges. Summary of the invention

[0009] One aspect of the present invention relates to a method for manufacturing a lead-acid battery, wherein the lead-acid battery is a lead-acid battery having an electrode plate group in which a plurality of positive electrode plates and a plurality of negative electrode plates are stacked with separators interposed therebetween.

[0010] The manufacturing method includes the step of processing the separator into a bag-like shape having a first region and a second region facing each other.

[0011] The step of processing the separator into a bag shape includes the step of forming a joint portion, the joint portion including at least a portion of the first region and at least a portion of the second region.

[0012] A plurality of first convex strips are arranged in the first area.

[0013] A plurality of second convex strips are arranged in the second area.

[0014] The step of forming the joining portion includes the step of causing the first region and the second region to face each other so that at least one of the first convex lines and at least one of the second convex lines intersect at the joining portion.

[0015] According to the present disclosure, it is possible to improve the strength of the joint portion of the bag-shaped separator used in the lead acid battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a front view schematically showing the appearance of a lead acid battery separator used in a method for producing a lead acid battery according to one aspect of the present invention.

[0017] Figure 2 This is a schematic diagram showing a separator sheet before the lead-acid battery separator is processed into a bag shape.

[0018] Figure 3 It is a schematic diagram showing the state of the inner convex strip when the separator sheets are overlapped.

[0019] Figure 4 Yes means Figure 2 A schematic diagram showing another embodiment of a separator sheet before the lead acid battery separator is processed into a bag shape.

[0020] Figure 5 Yes means Figure 2 A schematic diagram showing another embodiment of a separator sheet before the lead acid battery separator is processed into a bag shape.

[0021] Figure 6 Yes means Figure 2 A schematic diagram showing another embodiment of a separator sheet before the lead acid battery separator is processed into a bag shape.

[0022] Figure 7 This is a perspective view of a partially cutaway portion of a lead-acid battery using a bag-shaped separator. DETAILED DESCRIPTION

[0023] The manufacturing method of a lead-acid battery involved in one aspect of the present invention is a manufacturing method of a lead-acid battery having a plate group formed by stacking a plurality of positive plates and a plurality of negative plates with a separator, and the manufacturing method includes a process of processing the separator into a bag-like shape having a first region and a second region facing each other. The process of processing the separator into a bag-like shape includes a process of forming a joint, and the joint includes at least a portion in the first region and at least a portion in the second region. A plurality of first ridges are provided in the first region, and a plurality of second ridges are provided in the second region. The process of forming the joint includes a process of opposing the first region and the second region in a manner that at least one first ridge and at least one second ridge intersect in the joint.

[0024] According to the above aspect of the present invention, the joint portion for binding the first region and the second region into a bag shape is formed in a predetermined region (preferably, the inner peripheral edge portion) provided in the first region and the second region.

[0025] Specifically, for example, a separator having a first area and a second area on the same main surface is folded in half so that the first area is opposite to the second area, thereby forming a joint. In this case, a bag-shaped separator can be manufactured by overlapping a separator sheet into a U-shape, the bent portion of the bag-shaped separator becomes the lower end, a joint is provided on the left end side and the right end side, and an opening is provided on the upper end. However, a bag-shaped separator can also be manufactured by setting the right end (or left end) of the separator sheet as a bent portion, forming a joint on the left end side (or right end side) and the lower end side. Alternatively, a bag-shaped separator can also be manufactured by stacking a first half sheet having a first area on the main surface and a second half sheet having a second area on the main surface so that the first area and the second area are opposite. In this case, two half sheets are overlapped, and a joint is formed on the left end side, the right end side and the lower end side, so that a bag-shaped separator can be manufactured. The bag-shaped separator is used to accommodate the positive plate or negative plate of a lead-acid battery.

[0026] Here, in the bag-shaped separator, the direction in which the opening for inserting the positive electrode plate or the negative electrode plate is provided is defined as the upper side (vertical direction) of the separator, and the opposite side is defined as the lower side. In addition, when defining the upper and lower sides of the separator in this way, the direction toward the left is defined as the left side of the separator, and the direction toward the right is defined as the right side of the separator.

[0027] The convex stripes are protruding portions protruding from one side of the separator, and are provided to inhibit close contact between the separator and the electrode plate and to inhibit damage and / or permeation short circuit caused by oxidation degradation of the separator. The convex stripes are provided on the surface of the separator in a predetermined pattern.

[0028] The outer shape of the bag-shaped separator can be formed into a shape similar to the outer shape of the first area. Preferably, the outer shape of the first area is a quadrilateral shape. In this case, the bag-shaped separator has a roughly quadrilateral outer shape. By providing a joint portion in the area near at least two sides constituting the quadrilateral, the separator sheet (or two half sheets) can be processed into a bag shape. The outer shape of the bag-shaped separator is not limited to a quadrilateral, and can also be any shape (for example, a polygon or an arc shape, etc.). The sides constituting the polygon do not need to be precise straight lines, and can also have curved or tortuous parts. For example, in the case of a bag-shaped separator whose outer shape is roughly triangular by bending, it is sufficient that the joint area is provided on the side of one end corresponding to one side of the triangle.

[0029] The first area and the second area constitute the inner surfaces of the bag-shaped separator that are opposite to each other. Preferably, the separator sheet or half sheet has a joint area and a pole plate area in the first area and in the second area. For the joint area, it is an area including a joint portion that stitches the first area and the second area into a bag shape, and a wider area than the joint portion is set in consideration of the positioning margin involved in the joint. Preferably, the joint area is arranged on the end side of the separator sheet or half sheet, and the peripheral area within a prescribed distance to the end can be set as the joint area. In contrast, the pole plate area is an area isolated from the joint area, and when the bag-shaped separator accommodates the positive plate or the negative plate, it is an area opposite to the positive plate or the negative plate.

[0030] In the case where the joining area is provided at the end side of the separator sheet or half sheet, the joining portion may be provided in a manner including the end. Alternatively, within the joining area, the joining portion may be formed extending in parallel with the contour of the end of the bag-shaped separator (i.e., the contour of the end of the separator sheet or half sheet), or may be formed extending in any contour shape different from the contour of the end of the bag-shaped separator.

[0031] A plurality of first ridges are provided in the first region, and a plurality of second ridges are provided in the second region. The inner surface of the joined bag-shaped separator is set as the first surface and the second surface. In the joined bag-shaped separator, the first region is on the first surface, and the second region is on the second surface. The first ridge is formed in the electrode plate region within the first region on the first surface, thereby preventing either the positive electrode plate or the negative electrode plate from being in close contact with the first surface. Similarly, the second ridge is formed in the electrode plate region within the second region on the second surface, thereby preventing either the above-mentioned electrode plate from being in close contact with the second surface. The first ridge and the second ridge provided in the electrode plate region prevent damage and / or penetration short circuit caused by oxidation degradation of the separator when accommodating the positive electrode plate or the negative electrode plate. In the following, the first ridge and the second ridge are collectively referred to as "inner ridges".

[0032] Typically, the first ridges and the second ridges are arranged in a linear pattern such that the plurality of ridges are parallel to adjacent ridges at predetermined intervals within a predetermined region.

[0033] The first convex strip and the second convex strip (inner convex strip) are also formed in the joining area in the first area and the second area. When the inner convex strip is formed in the joining area, the first convex strip and the second convex strip can overlap when the first area and the second area are placed opposite to each other and the joining portion is formed. However, using this overlapping method, sometimes sufficient joining strength cannot be obtained.

[0034] For example, when the joint is formed, the first area and the second area are overlapped so that the second ridge in the joint area of ​​the second area is embedded in the valley between the adjacent first ridges in the joint area of ​​the first area (or, the first ridge in the joint area of ​​the first area is embedded in the valley between the adjacent second ridges in the joint area of ​​the second area). In this case, the joint strength is lower than when the first ridge and the second ridge overlap. In particular, when the method of joining is a crimping method such as meshing seal, the trend of reduced joint strength becomes greater. However, if the positioning accuracy of the joint portion of the joint device is considered, it is difficult to completely prevent the second ridge from being embedded in the valley between the first ridge (or, the first ridge is embedded in the valley between the second ridge), and it becomes a factor in the deviation of the joint strength. As a result, the performance of the lead-acid battery also deviates.

[0035] This is a common problem in the manufacture of bag-shaped separators provided with inner convex strips, regardless of whether it is welded or bonded, but it is particularly prominent in methods of joining by compressing the joint portion to a predetermined thickness by a crimping joining method such as a meshing sealing method or a heat welding method, where the thickness of the joint portion before crimping is made thinner than the assumed thickness by embedding the convex strip of one of the first and second convex strips between the grooves of the convex strips of the other convex strip. As a result, the compression rate when compressed to the predetermined thickness is reduced, which easily leads to a reduction in the joint strength.

[0036] Therefore, one aspect of the present invention includes a step of making the first area and the second area face each other in such a manner that at least one of the first convex strips and at least one of the second convex strips intersect in the joint portion when forming the joint portion. According to the arrangement of the inner convex strips, the first area and the second area are made face each other in such a manner that the first convex strips intersect with the second convex strips, thereby preventing other convex strips from being embedded in the valleys between adjacent convex strips. By forming the joint in a state where the embedding of the convex strips is suppressed, the strength variation of the joint portion of the bag-shaped separator is reduced, and the joint strength can be maintained.

[0037] Here, the "intersection" of the first ridge and the second ridge refers to the state in which the first area and the second area are opposite, and the first ridge and the second ridge are in contact at least at a point. The first ridge and the second ridge may also be in contact with a line or a surface. In addition, the location of at least point contact is not limited to one location. The linear pattern of the ridge may be a straight line or a curve. In addition, it may be a dotted line in which a part of the straight line or curve is missing. The pattern of the ridge is preferably a stripe-shaped pattern composed of a plurality of ridges each consisting of parallel straight lines, because it makes the manufacture of the ridge easy. With respect to the angle at which the first ridge and the second ridge intersect, the pattern of the first ridge and the pattern of the second ridge preferably intersect at an angle of more than 0.2°, and more preferably at an angle of more than 0.3°. As long as the intersection angle is more than 0.2°, sufficient bonding strength can be obtained.

[0038] It is also considered that, depending on the method of forming the joint, it is difficult to distinguish whether the first ridge and the second ridge intersect in the joint based on the state of the joint of the bag-shaped separator after manufacture. Even in this case, it is possible to infer whether the first ridge and the second ridge intersect in the joint based on the configuration of the first ridge and the second ridge in the area around the joint. For example, in the joint area, when a plurality of first ridges and second ridges are formed at a predetermined interval as straight lines extending in a predetermined direction, it can be inferred that in the joint, the first ridge and the second ridge are formed at the same ridge interval as the ridge interval in the joint area as straight lines extending in the same direction as the ridge extension direction in the joint area. That is, the intersection of the first ridge and the second ridge can be inferred by interpolating or extrapolating the ridge pattern in the joint based on the ridge pattern in the peripheral area of ​​the joint.

[0039] As the arrangement pattern of the first convex strip and the second convex strip, for example, in the case of a separator sheet having a quadrilateral (rectangle, trapezoid or parallelogram) with substantially parallel opposite sides, in the region (joint region) in the first region of the separator sheet where at least the joint portion is provided and the region (joint region) in the second region where at least the joint portion is provided, the first convex strip and the second convex strip can be extended in a straight line in the same direction on the main surface of the separator sheet. In addition, the first convex strip and the second convex strip extending in the same direction on the main surface means that the first convex strip and the second convex strip extend in the same direction when the first region and the second region are on the same plane before the separator sheet is folded in half. The first convex strip and the second convex strip can extend in a straight line on the main surface of the separator sheet in a direction substantially parallel to the above-mentioned opposite sides of the separator sheet. Alternatively, the first convex strip and the second convex strip can extend in a straight line on the main surface of the separator sheet in a direction substantially perpendicular to the above-mentioned opposite sides of the separator sheet. In addition, "parallel" or "perpendicular" to the opposite sides does not mean that the extension direction of the convex strip is strictly parallel or perpendicular in a mathematical sense. In the above case, when the separator sheet is folded in half so that the first region and the second region are opposite to each other, the folding is performed with the direction inclined from the direction perpendicular to the opposite sides as the bending axis. For example, if the separator sheet is a rectangle with the opposite sides as the long sides, the separator sheet is folded in half with the direction inclined from the short side of the separator sheet as the axis. When the first region and the second region are opposite to each other by shifting the axis for bending the separator sheet from the symmetry axis, the second ridge can extend in a straight line along an inclined direction different from the extending direction of the first ridge.

[0040] In addition, as the configuration pattern of the first convex strip and the second convex strip, for example, the following configuration can be adopted: in the area (joining area) where at least the joint portion is provided in the first area of ​​the isolation sheet and the area (joining area) where at least the joint portion is provided in the second area, the first convex strip and the second convex strip extend linearly on the main surface of the isolation sheet along the same direction, that is, along the direction inclined from the direction parallel to the opposite side of the isolation sheet. In this case, when the isolation sheet is folded in half so that the first area and the second area are opposite to each other, the isolation sheet can be folded in half with the direction perpendicular to the opposite side as the axis. For example, as long as the isolation sheet is a rectangle with the opposite side as the long side, the isolation sheet can be folded in half with the short side direction of the isolation sheet as the axis. The first convex strip and the second convex strip extend obliquely from the direction parallel to the opposite side, so when the first area and the second area are opposite to each other, the second convex strip can extend linearly in the oblique direction relative to the extension direction of the first convex strip.

[0041] When the second ridge extends in a direction inclined relative to the first ridge, the first region and the second region are opposed to each other, thereby facilitating the intersection of the first ridge and the second ridge in the joint portion, thereby reducing the variation in the joint strength and maintaining the joint strength.

[0042] In addition, the first convex strip and the second convex strip may extend together in a direction inclined from a direction parallel to the above-mentioned opposite sides of the isolation sheet, and the isolation sheet may be folded in half with a direction inclined from a direction perpendicular to the above-mentioned opposite sides of the isolation sheet as an axis. The angle at which the first convex strip and the second convex strip intersect may be made larger. Thus, the first convex strip and the second convex strip may intersect more easily in the joint portion and may intersect more easily at multiple locations. As a result, the deviation of the joint strength is further reduced, and the joint strength may be further improved.

[0043] At this time, from the perspective of the ease of processing the convex strips, it is preferred that the first convex strips in the electrode plate region also extend in the same direction as the first convex strips in the bonding region. Similarly, from the perspective of the ease of processing the convex strips, it is preferred that the second convex strips in the electrode plate region extend in the same direction as the second convex strips in the bonding region.

[0044] Preferably, the first ridges include: a plurality of first joining ridges, which are arranged at a predetermined interval in the joining region within the first region; and a plurality of first electrode plate ridges, which are arranged at a predetermined interval in the electrode plate region within the first region. In this case, the intervals at which the first joining ridges are set may be narrower than the intervals at which the first electrode plate ridges are set. Thus, more first ridges can be crossed with second ridges in the joining region.

[0045] Similarly, preferably, the second ridges include: a plurality of second joining ridges, which are arranged at a predetermined interval in the joining area within the second region; and a plurality of second electrode plate ridges, which are arranged at a predetermined interval in the electrode plate area within the second region. In this case, the intervals at which the second joining ridges are set can also be narrower than the intervals at which the second electrode plate ridges are set. Thus, the first ridges can intersect with more second ridges in the joining area.

[0046] By increasing the number of intersections between the first ridges and the second ridges in the joint portion, the joint strength can be maintained high.

[0047] Preferably, for the separator, there is a third area on the back of the first area and a fourth area on the back of the second area, respectively, a plurality of third ridges are arranged in the third area, and a plurality of fourth ridges are arranged in the fourth area. The outer surface of the bag-shaped separator after bonding is set as the third surface and the fourth surface. In the bag-shaped separator after bonding, the third area is on the third surface, and the fourth area is on the fourth surface. The third ridge and the fourth ridge inhibit the close contact between the plate of the positive plate and the negative plate that is not contained in the bag of the separator and the separator. The third ridge and the fourth ridge arranged in the plate area inhibit the damage and / or penetration short circuit caused by the oxidation degradation of the separator caused by contact with the plate of the other party. In the following, the third ridge and the fourth ridge are collectively referred to as "outer ridges".

[0048] The performance of the battery can be improved by providing a bag-shaped separator with inner and outer convex strips. However, in this case, in order to maintain high charge and discharge characteristics, the total thickness of the separator needs to be suppressed, and the thickness of the base part of the separator has to be thinned. As a result, the bonding strength of the ends of the separator is easily reduced, making the problem of bonding strength deviation more serious.

[0049] The third ridge may also be provided in an area within the third area corresponding to the joining area within the first area (i.e., an area on the back side of the joining area within the first area). In addition, the fourth ridge may also be provided in an area within the fourth area corresponding to the joining area within the second area (i.e., an area on the back side of the joining area within the second area). In this case, the third ridge or the fourth ridge (external ridge) is also compressed together when the joining is formed by crimping or the like. Thus, the compression ratio is increased, and the joining strength can be obtained. On the other hand, the deviation in the joining strength is more significant due to the deviation in the positioning of the joining end. However, by making the first ridge intersect with the second ridge in the joining portion, it is possible to suppress the embedding of other ridges between the valleys between adjacent ridges, and the joining strength can be maintained at a high level.

[0050] In this way, the first area and the second area are opposed to each other in such a manner that the first convex strip and the second convex strip intersect in the joint portion to form a joint portion, thereby reducing the deviation of the joint strength of the bag-shaped separator and maintaining the joint strength. The above-mentioned effect is not limited to the compression method of meshing and sealing, and the effect can also be obtained in heat welding and the like. The step of forming the joint portion may include the step of joining at least a portion of the first area to at least a portion of the second area by compression welding or welding.

[0051] In one aspect of the present invention, the manufacturing method of the lead-acid battery can further include a process of configuring the negative electrode plate in a manner of accommodating the negative electrode plate in a separator processed into a bag shape. As a method of accommodating the negative electrode plate, after the negative electrode plate is pressed to the electrode plate area in the first area of ​​the separator sheet or the electrode plate area in the second area, the separator is folded in half, and a joint can be formed in a state where the negative electrode plate is sandwiched between the first area and the second area. In this case, the formation of the joint and the accommodation of the negative electrode plate to the bag-shaped separator are performed simultaneously. However, it is also possible to accommodate the negative electrode plate in the bag-shaped separator after forming the joint and processing the separator into a bag shape.

[0052] The bag-shaped separator is effective as a separator used in a lead-acid battery when housing a negative electrode plate, and can improve resistance to short circuiting due to permeation.

[0053] Hereinafter, with reference to the accompanying drawings, the manufacturing method of the lead-acid battery involved in the embodiment of the present invention, in particular, the form of the separator is described in detail. However, the present invention is not limited to the following embodiments. In addition, in the following drawings, the form of the inner convex strip in the joint area of ​​the separator is emphasized, and there is a situation where the composition ratio of each part of the actual separator is inconsistent with the composition ratio of each part corresponding to the accompanying drawings.

[0054] Figure 1 A schematic diagram showing a lead acid battery separator used in the method according to the embodiment of the present invention as viewed from the outside of a bag is shown. Figure 2 Schematically showing that Figure 1 The separator 100 is a separator sheet before being processed into a bag shape. The separator 100 comprises: a bag-shaped base 101, which is composed of a microporous film; inner convex strips 102a to 102d, which protrude from the inner surface (first surface or second surface) of the base 101; and outer convex strips 104a and 104b, which protrude from the outer surface (third surface) of the base 101. However, since the inner convex strips 102a to 102d are located inside the bag-shaped separator, Figure 1In the case where a negative electrode plate is housed in the separator 100, the inner convex strips 102a to 102d are located on the negative electrode plate side, and the outer convex strips 104a and 104b are located on the positive electrode plate side. In the case where a positive electrode plate is housed in the separator 100, the outer convex strips 104a and 104b are located on the negative electrode plate side, and the inner convex strips 102a to 102d are located on the positive electrode plate side. Both the structure in which the negative electrode plate is housed in the separator 100 and the structure in which the positive electrode plate is housed in the separator 100 are acceptable.

[0055] The separator 100 may be formed of a polymer material. At least the base portion is a porous sheet, which may also be referred to as a porous film. The separator 100 may also include a filler (e.g., a particulate filler such as silicon dioxide and / or a fibrous filler) dispersed in a matrix formed of a polymer material. Preferably, the separator 100 is composed of an acid-resistant polymer material. As such a polymer material, polyolefins such as polyethylene and polypropylene are preferred.

[0056] The average thickness of the base portion 101 is, for example, 0.15 mm to 0.3 mm, and preferably 0.18 mm to 0.27 mm. When the average thickness of the base portion is within such a range, the charge-discharge characteristics are maintained at a high level, and it is easy to ensure the height of the inner convex strip and the outer convex strip corresponding to the needs. The average thickness of the base portion is obtained by measuring the thickness of the base portion at 5 randomly selected locations in the cross-sectional photograph of the separator and averaging the thickness.

[0057] The separator 100 includes a plate region 106, a bonding region 108a disposed at the left end of the separator, and a bonding region 108b disposed at the right end of the separator. The bonding regions 108a and 108b are respectively formed with bonding (bonding portions) 109a and 109b between the first surface and the second surface.

[0058] On the first surface and the second surface of the electrode region 106, an inner convex strip 102a (first electrode convex strip) and an inner convex strip 102b (second electrode convex strip) are provided (refer to Figure 2 to Figure 5 ), an outer convex strip 104a is provided on the third surface of the electrode plate region 106. When a lead-acid battery is constructed, in the electrode plate region 106, the separator 100 is opposite to the positive electrode plate or the negative electrode plate. At this time, the inner convex strips 102a, 102b and the outer convex strip 104a prevent the base portion 101 from directly contacting the positive electrode plate or the negative electrode plate. On the other hand, an inner convex strip 102c (first joining convex strip) and an inner convex strip 102d (second joining convex strip) are provided on the first surface and the second surface of the joining region 108a, 108b (refer to Figure 2 to Figure 5 ). In addition, an outer convex strip 104b is provided on the third surface of the joint regions 108a and 108b.

[0059] Figure 1 The separator 100 shown is formed by folding a separator sheet having inner convex strips 102a to 102d and outer convex strips 104a and 104b formed in advance into a U shape and then joining the left end side and the right end side by a method such as meshing and sealing. Figure 2 The rectangular separator sheet 110 is schematically shown before being folded in half and joined at the left and right end portions. Figure 2 This is a schematic diagram of the separator sheet viewed from the surface where the inner convex strips 102a to 102d are formed, and the outer convex strips 104a and 104b are not shown in the figure because they exist on the back side.

[0060] The isolation sheet 110 has a first region (in Figure 2 , the region above the axis X parallel to the short side of the separator sheet) and the second region (in Figure 2 When the first region and the second region are opposed to each other, the first region becomes the first surface of the bag-shaped separator, and the second region becomes the second surface of the bag-shaped separator.

[0061] like Figure 2 As shown, the electrode area 106 in the first region is provided with an inner convex stripe 102a, and the electrode area 106 in the second region is provided with an inner convex stripe 102b. The bonding areas 108a and 108b in the first region are provided with inner convex stripes 102c, and the bonding areas 108a and 108b in the second region are provided with inner convex stripes 102d. The inner convex stripes 102a to 102d are formed as linear stripe patterns at predetermined intervals in a direction parallel to the long side of the separator sheet. Figure 2 In the embodiment, the ridge intervals of the inner ridges 102 c and 102 d provided in the bonding regions 108 a and 108 b are made narrower than the ridge intervals of the inner ridges 102 a and 102 b provided in the electrode region 106 .

[0062] In this embodiment, Figure 2 The separator sheet shown is folded in half to form Figure 1 In the case of the bag-shaped separator 100 shown in FIG. 1 , the separator sheet is not bent about an axis X parallel to the short side of the separator sheet, but is bent as shown in FIG. Figure 2As shown by the dotted line, the separator sheet is bent with the axis Y slightly offset from the direction parallel to the short side as the axis, so that the left and right end sides of the joint area 108a, 108b are joined. As a result, when the first area and the second area are opposed to each other to form a bag-shaped separator, the inner convex strips 102a to 102d extend in a direction slightly inclined from the vertical direction. In addition, the inner convex strips 102a, 102c on the first surface and the inner convex strips 102b, 102d on the second surface extend obliquely from the vertical direction in opposite directions to each other, so when the first area and the second area are opposed to each other, in each joint area 108a, 108b, the inner convex strips 102c and the inner convex strips 102d can be made to cross. At this time, even in the electrode area 106, the inner convex strips 102a and the inner convex strips 102b cross. Moreover, when the joint is formed, at least one intersection of the inner convex strips 102c and the inner convex strips 102d is included in the joint portion.

[0063] When the left and right end sides of the joining regions 108a and 108b are joined, the inner convex strips 102c and the inner convex strips 102d are intersected at the joining portion, thereby easily preventing one inner convex strip 102c from being embedded in the valley between the inner convex strips 102d arranged at a predetermined interval on the second region, or one inner convex strip 102d from being embedded in the valley between the inner convex strips 102c arranged at a predetermined interval on the first region. As a result, the variation in the joining strength is reduced, and the joining strength can be maintained.

[0064] Figure 3 The state of the inner convex strip of the separator sheet in the joint area 108a when the first area and the second area are opposed to each other is shown. Figure 3 In order to avoid cumbersome records, the records of the outer convex strips are omitted.

[0065] In the Figure 2 After the isolation sheet shown in the figure is folded in half, when the bending axis is offset from the axis X parallel to the short side of the isolation sheet and the offset angle is small, due to the positional relationship between the inner convex strips 102c and 102d, there is a Figure 3 (a) shows a case where the inner convex stripes 102c and the inner convex stripes 102d do not overlap. In this case, the inner convex stripes 102d are embedded in the valleys between the inner convex stripes 102c, and the inner convex stripes 102c are embedded in the valleys between the inner convex stripes 102d.

[0066] On the other hand, in the case of large offset angles, such as Figure 3 As shown in (b), the inner convex line 102c intersects with the inner convex line 102d regardless of the positional relationship between the inner convex lines 102c and 102d. In this case, the joining strength can be maintained high.

[0067] When the separator sheet is folded in half, even if the offset angle of the bending axis is the same, the relative position of the inner convex strip 102d with respect to the inner convex strip 102c may deviate in the left-right direction depending on the position of the separator sheet being bent (the position in the long side direction of the separator sheet). Even when the offset angle is small, the inner convex strip 102c can cross the inner convex strip 102d at the joint. However, depending on the bending position, the inner convex strip 102c may cross or may not cross the inner convex strip 102d ( Figure 3 (a)) In both cases, the bonding strength may vary. However, compared with the case where the separator sheet is bent about the X axis, the variation in bonding strength is reduced.

[0068] The interval at which the inner convex strip 102c is set is set as D, and the length of the inner convex strip 102c is set as L. If the angle of the axis Y for the separator sheet to be bent from the direction X parallel to the short side is set as θ, the inner convex strip 102c and the inner convex strip 102d are tilted in opposite directions by only θ, so the intersection angle is 2θ. In this case, when tan2θ≥D / L is satisfied, the inner convex strip 102c and the inner convex strip 102d can be reliably crossed at more than one position, the bonding strength can be improved, and the deviation of the bonding strength can be maintained at a low level. In this case, if the width of the joint portion from the end of the separator sheet is set in a manner including the inner convex strip 102d located at the second position from the end side, the joint portion includes at least one intersection of the inner convex strip 102c and the inner convex strip 102d. If the distance from the inner convex strip 102d located at the end side to the end is set as W, the joint portion including the end portion can be set to a region with a width of more than D+W. In order to prevent the generation of unjoined portions, the width of the joint portion is preferably greater than the offset of the end portion of the separator (the length of the end portion of the separator on the joint portion side when folded in half is set to L). 2 , L 2 tan2θ) method.

[0069] Figure 4 , 5 It means Figure 2 Schematic diagram of the morphology of different isolation sheets. Figure 4 In the isolation sheet 111 shown, the inner convex strips 102a to 102d are not formed as shown in FIG. Figure 2In this case, if the separator sheet 111 is folded in half with the axis X in the direction parallel to the short side of the separator sheet as the axis, the inner convex strips 102a, 102c in the first area and the inner convex strips 102b, 102d in the second area extend obliquely from the vertical direction in opposite directions. Therefore, when the first area and the second area are placed opposite to each other and the joint is formed on the left and right end sides, the inner convex strips 102c and the inner convex strips 102d can be crossed in the joint portion in the joint area 108a, 108b. In addition, at this time, in the plate area 106, the inner convex strips 102a and the inner convex strips 102b cross each other.

[0070] exist Figure 4 In the embodiment, the axis used for folding the isolation sheet 111 may be as follows: Figure 2 The inner convex strips 102c and 102d can be inclined from the direction parallel to the short side of the separator sheet as shown in the axis Y. The angle at which the inner convex strips 102c and 102d intersect can be made larger, and the inner convex strips 102c and 102d can be easily intersected in the joint.

[0071] Figure 5 The separator sheet 112 shown is a stripe pattern in which the inner convex stripes 102c and 102d in the joining area are not straight lines but curves that undulate and extend substantially in the vertical direction. In this case, if the separator sheet is folded in half with the direction parallel to the short side of the separator sheet as an axis so that the first area and the second area are opposite, one inner convex stripe 102c can intersect with one or more inner convex stripes 102d at multiple locations in the joining areas 108a and 108b. In addition, one inner convex stripe 102d can intersect with one or more inner convex stripes 102c at multiple locations. Since the number of intersections increases, the deviation of the joining strength is further reduced, and a high joining strength can be maintained.

[0072] For the average height of the inner ridges in the joint area, it is preferably 0.05 mm or more from the perspective of puncture strength at the end, and preferably 0.5 mm or less from the perspective of suppressing poor joining caused by insufficient joining energy, etc. For the average height of the inner ridges in the plate area, it is preferably 0.3 mm or more in order to suppress oxidative degradation when facing the positive plate, and it is preferably 0.05 mm or more in order to suppress penetration short circuit when facing the negative plate. On the other hand, the average height of the inner ridges in the plate area is preferably 0.5 mm or less from the perspective of maintaining a higher discharge capacity. In addition, the height of the inner ridge refers to the distance from the main surface (first area or second area) of the substrate of the separator sheet at the specified position of the inner ridge to the top of the inner ridge. The average height of the inner ridge is obtained by averaging the height of the inner ridges measured at 10 arbitrarily selected locations of the inner ridges on one main surface of the substrate.

[0073] exist Figure 2 to Figure 5 In the example of the inner convex stripes 102a to 102d, a stripe pattern is shown. However, the pattern of the inner convex stripes is not particularly limited. The inner convex stripes may be formed randomly, or may be formed in a stripe shape, a curve shape, a lattice shape, etc. In addition, as shown in FIG. Figure 5 As illustrated, the pattern of the inner convex stripes may also be different in the electrode area and the bonding area. From the viewpoint of making it easier for the electrolyte to diffuse, it is preferred that a plurality of inner convex stripes are formed in a stripe-like manner in at least the electrode area in the first area or the second area. The orientation of the stripe-like inner convex stripes is not particularly limited, for example, a plurality of inner convex stripes may also be formed in the height direction or the width direction. From the viewpoint of suppressing the increase in internal resistance caused by the retention of gas generated during charging, it is preferred that a plurality of inner convex stripes be formed in the stripe-like shape along the height direction. On the other hand, from the viewpoint of suppressing the precipitation of high-concentration sulfuric acid generated during charging and suppressing stratification, it is preferred that a plurality of inner convex stripes be formed in the stripe-like shape along the width direction. In addition, the height direction refers to the direction in which the opening of the bag-like separator is located, and the width direction refers to the direction perpendicular to the height direction.

[0074] Figure 6 It means Figure 2 , Figure 4 as well as Figure 5 Schematic representation of the morphology of different separator sheets. Figure 6This is a diagram of observing the isolation sheet 114 from the third region (fourth region) side, but by folding the right triangle region in the upper right corner back to the paper side, the state of the first region (second region) side is also shown. The isolation sheet 114 is folded in half (mountain fold) so that the first region and the second region are opposite to each other, with the paper side of the isolation sheet 114 as the outer surface and the back side of the paper as the inner surface, thereby forming a bag-shaped isolation member. At this time, one of the mutually opposite inner surfaces of the isolation sheet 114 after folding constitutes the first surface, and the other surface constitutes the second surface. The outer surface of the outer surface of the isolation sheet 114 after folding that is located on the back of the first surface constitutes the third surface, and the outer surface located on the back of the second surface constitutes the fourth surface.

[0075] exist Figure 6 In the isolation sheet 114 shown, a plurality of outer convex strips 104a and 104b are formed to be arranged in stripes along the height direction (the direction parallel to the long side of the sheet). On the other hand, a plurality of inner convex strips 102e are formed to be arranged in stripes along the width direction (the direction parallel to the short side of the sheet). The spacing of the inner convex strips 102e is the same in both the joint area and the electrode plate area. On the other hand, the spacing of the outer convex strips 104b in the joint area is made narrower than the spacing of the outer convex strips 104a in the electrode plate area. The isolation sheet 114 can be appropriately used in the case where the negative electrode plate is accommodated in a bag-shaped separator. The isolation sheet 114 can also be formed by bending the isolation sheet with a direction Y slightly offset from the direction parallel to the short side of the isolation sheet as an axis to form a joint, so that the opposing inner convex strips 102e intersect each other.

[0076] By using Figure 2 as well as Figures 4 to 6 The separator sheet shown may have a plurality of inner convex strips extending in a direction slightly inclined from the height direction of the bag-shaped separator or in a direction slightly inclined from the width direction. Even in this case, the above-mentioned effect can be obtained.

[0077] From the viewpoint of puncture strength, oxidation resistance and permeation short circuit resistance, the interval between the stripe-shaped or grid-shaped inner ridges in the electrode region is preferably 0.5 mm to 10 mm. For example, the inner ridges are preferably formed at such intervals over 70% of the area of ​​the electrode region.

[0078] In contrast, the spacing of the inner convex stripes in the junction area is denser than that in the electrode area, so that the inner convex stripes can be reliably crossed and the number of crossing parts can be increased, which is preferred. Specifically, the spacing of the inner convex stripes in the stripe or grid shape is preferably narrower than that in the electrode area, and is between 0.5 mm and 2.0 mm.

[0079] The interval between inner convex lines refers to the distance between the tops of adjacent first convex lines or second convex lines (more specifically, the distance between the centers of adjacent inner convex lines in a direction crossing the inner convex lines).

[0080] The average height of the outer convex strips in the electrode area is preferably 0.3 mm or more in order to suppress oxidative degradation when facing the positive electrode plate, and preferably 0.05 mm or more in order to suppress penetration short circuit when facing the negative electrode plate. On the other hand, from the perspective of maintaining the charge and discharge characteristics at a high level, the average height of the outer convex strips in the electrode area is preferably 0.5 mm or less. For the average height of the outer convex strips in the junction area, it is preferably 0.05 mm or more from the perspective of puncture strength at the end, and preferably 0.5 mm or less from the perspective of suppressing poor junctions caused by insufficient junction energy, etc.

[0081] The height of the outer ridges is the distance from the main surface of the base of the separator sheet (third region or fourth region) at a predetermined position of the outer ridges to the top of the outer ridges.

[0082] As with the inner convex stripes, the pattern or orientation of the outer convex stripes is not particularly limited. For example, it can be selected from the above contents for the inner convex stripes. The spacing of the stripe-shaped or grid-shaped outer convex stripes in the electrode area is preferably 0.5 mm or more and 10 mm or less from the viewpoint of puncture strength, oxidation resistance, and resistance to permeation short circuit. For example, it is preferred that the outer convex stripes with such spacing are formed on more than 70% of the area of ​​the electrode area.

[0083] In contrast, from the perspective of increasing the compression rate during bonding by crimping or the like and improving bonding strength, the spacing between the outer ridges in the bonding area is narrower than that in the electrode area, preferably being 0.5 mm to 2.0 mm.

[0084] In addition, the interval between the outer convex lines refers to the distance between the tops of the adjacent third convex lines or fourth convex lines (more specifically, the distance between the centers of the adjacent outer convex lines in the direction crossing the outer convex lines).

[0085] Unless otherwise specified, the range of the spacing and height of the inner convex strips and the range of the spacing and height of the outer convex strips are preferred ranges, especially when the separator accommodates the negative electrode plate. When the separator accommodates the positive electrode plate, the range of the spacing and height of the inner convex strips in the electrode plate region can be selected from the range of the spacing and height of the outer convex strips in the electrode plate region, and the range of the spacing and height of the outer convex strips in the electrode plate region can be selected from the range of the spacing and height of the inner convex strips in the electrode plate region.

[0086] For example, the separator can be obtained by extruding a resin composition containing a pore former (a solid pore former such as polymer powder and / or a liquid pore former such as oil) and a polymer material into a sheet, removing the pore former, and forming pores in the matrix of the polymer material. For example, the convex stripes can be formed during extrusion molding, or after molding into a sheet or removing the pore former, they can be formed by transfer using a roller having grooves corresponding to the convex stripes. When a filler is used, it is preferred to add the filler to the resin composition.

[0087] Hereinafter, an example of a lead-acid battery using a bag-shaped separator manufactured by the method of this embodiment will be described in detail according to each main component, but the present invention is not limited to the following embodiment. In addition, since the bag-shaped separator is used as a separator of a lead-acid battery, the components other than the separator will be described.

[0088] (Electrolyte)

[0089] The electrolyte solution contains sulfuric acid in an aqueous solution. The electrolyte solution may be gelled as needed. The electrolyte solution may contain additives used in lead-acid batteries as needed.

[0090] The specific gravity of the electrolyte in a fully charged lead-acid battery after chemical conversion at 20°C is, for example, 1.10 g / cm 3 Above 1.35g / cm 3 the following.

[0091] (Positive plate)

[0092] There are two types of positive plates in lead-acid batteries: a pasted type and a clad type.

[0093] The paste-coated positive electrode plate comprises a positive electrode collector and a positive electrode material. The positive electrode material is retained by the positive electrode collector. In the paste-coated positive electrode plate, the positive electrode material is the portion after the positive electrode collector is removed from the positive electrode plate. The positive electrode collector can be formed in the same manner as the negative electrode collector, and can be formed by casting lead or lead alloy, or processing lead or lead alloy sheets.

[0094] The clad positive plate comprises a plurality of porous tubes, a core metal inserted into each tube, a positive electrode material filled in the tube into which the core metal is inserted, and a connecting seat connecting the plurality of tubes. In the clad positive plate, the positive electrode material is the portion of the positive plate after removing the tubes, the core metal, and the connecting seat.

[0095] Lead alloys used for positive electrode current collectors are preferably Pb-Ca alloys and Pb-Ca-Sn alloys from the perspective of corrosion resistance and mechanical strength. The positive electrode current collector may also have lead alloy layers with different compositions, and the number of alloy layers may also be multiple. Pb-Ca alloys and Pb-Sb alloys are preferably used for the core.

[0096] The positive electrode material contains a positive electrode active material (lead dioxide or lead sulfate) that develops capacity through an oxidation-reduction reaction. The positive electrode material may also contain other additives such as antimony (Sb) as needed.

[0097] In the case of the negative electrode plate, the positive electrode current collector is filled with positive electrode paste, and the paste is aged and dried to obtain a non-chemically converted pasted positive electrode plate. The positive electrode paste is prepared by kneading lead powder, additives, water and sulfuric acid.

[0098] The non-chemically converted clad positive electrode plate is formed by filling a tube into which a core bar is inserted with a mixture of an additive and lead powder or lead powder in a slurry form as required, and connecting a plurality of tubes with a connecting seat.

[0099] Thereafter, the positive electrode plate which has not been chemically converted is chemically converted to form a positive electrode plate.

[0100] (Negative plate)

[0101] The negative plate of the lead-acid battery is composed of a negative electrode collector and a negative electrode material. The negative electrode material is the portion of the negative electrode plate from which the negative electrode collector is removed. The negative electrode collector can also be formed by casting lead (Pb) or a lead alloy, or by processing a lead or lead alloy sheet. As a processing method, for example, a drawing process and a punching process can be cited.

[0102] The lead alloy used for the negative electrode current collector may be any one of a Pb-Sb alloy, a Pb-Ca alloy, and a Pb-Ca-Sn alloy. These lead or lead alloys may also contain at least one selected from Ba, Ag, Al, Bi, As, Se, and Cu as an additive element.

[0103] The negative electrode material contains a negative electrode active material (lead or lead sulfate) that develops capacity through redox reaction, and may also contain an anti-shrinkage agent, a carbonaceous material such as carbon black, barium sulfate, and other additives as needed.

[0104] The active material of the negative electrode in the charged state is spongy lead, but the negative plate that has not been chemically converted is usually made of lead powder.

[0105] The negative electrode plate can be formed by filling a negative electrode paste into a negative electrode current collector, aging and drying the negative electrode paste to form a non-chemically converted negative electrode plate, and then chemically converting the non-chemically converted negative electrode plate. The negative electrode paste is prepared by adding water and sulfuric acid to lead powder, an organic shrink-proof agent, and various additives as needed.

[0106] The chemical conversion can be carried out by accommodating the unconverted positive and negative electrode groups in the battery tank of the lead-acid battery. As required, the chemical conversion can also be carried out by injecting electrolyte into the battery tank after connecting the battery cells and welding the covers. In addition, the lead-acid battery or the electrode group can be assembled after the chemical conversion of the positive and negative plates is respectively carried out.

[0107] Figure 7 The external appearance of an example of a lead acid battery using a bag-shaped separator is shown.

[0108] The lead-acid battery 1 includes a battery tank 12 for accommodating a plate group 11 and an electrolyte (not shown). The battery tank 12 is divided into a plurality of battery cell chambers 14 by partition walls 13. Each battery cell chamber 14 accommodates a plate group 11. The opening of the battery tank 12 can be sealed by a cover 15 having a negative terminal 16 and a positive terminal 17. A unit liquid port plug 18 is provided on the cover 15 for each battery cell chamber. When replenishing water, the liquid port plug 18 is removed to replenish the replenishing liquid. The liquid port plug 18 can also have the function of discharging the gas generated in the battery cell chamber 14 to the outside of the battery.

[0109] The electrode group 11 is formed by stacking a plurality of negative plates 2 and positive plates 3 respectively with separators 4 interposed therebetween. Here, a bag-shaped separator 4 for accommodating the negative plates 2 is shown, but the bag-shaped separator 4 can also accommodate the positive plates 3. In the battery cell chamber 14 located at one end of the battery tank 12, the negative electrode frame 6 in which the plurality of negative plates 2 are connected in parallel is connected to the through connector 8, and the positive electrode frame 5 in which the plurality of positive plates 3 are connected in parallel is connected to the positive electrode column 7. The positive electrode column 7 is connected to the positive electrode terminal 17 on the outside of the cover 15. In the battery cell chamber 14 located at the other end of the battery tank 12, the negative electrode column 9 is connected to the negative electrode frame 6, and the through connector 8 is connected to the positive electrode frame 5. The negative electrode column 9 is connected to the negative electrode terminal 16 on the outside of the cover 15. Each through connector 8 passes through the through hole provided in the partition 13, and connects the electrode group 11 of the adjacent battery cell chambers 14 in series.

[0110] [Example]

[0111] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0112] 《Lead-acid battery A1》

[0113] (1) Preparation of negative electrode plate

[0114] Lead powder, water, dilute sulfuric acid, carbon black and an organic shrinkage-proofing agent are mixed to obtain a negative electrode paste. The negative electrode paste is filled in the mesh of a Pb-Ca-Sn alloy expanded mesh grid as a negative electrode collector, and the grid is aged and dried to obtain a negative electrode plate that is not chemically converted. Sodium lignin sulfonate is used as an organic shrinkage-proofing agent. The amount of carbon black and the organic shrinkage-proofing agent added is adjusted so that the content of each negative electrode material is 0.2% by mass, and the negative electrode paste is prepared.

[0115] (2) Preparation of positive electrode plate

[0116] Lead powder, water and sulfuric acid are kneaded to prepare a positive electrode paste, which is filled into the mesh of a Pb-Ca-Sn alloy expanded grid as a positive electrode current collector, aged and dried to obtain a non-chemically converted positive electrode plate.

[0117] (3) Preparation of Isolators

[0118] A separator S1 in the form of a bag is formed by folding a separator sheet made of a polyethylene microporous film and having ridges formed on both sides thereof in half and joining the left and right ends thereof. Figure 2 In the separator sheet shown, the spacing of the inner convex strips is set to 2.0 mm in the electrode area, 1.0 mm in the bonding area (the peripheral area of ​​5 mm from the left and right ends), and the height of the inner convex strips is set to 0.1 mm in both the electrode area and the bonding area. In addition, the spacing of the outer convex strips is set to 8.0 mm in the electrode area, 1.0 mm in the bonding area, and the height of the outer convex strips is set to 0.4 mm in the electrode area and 0.2 mm in the bonding area. In addition, the average thickness of the base portion of the separator is 0.25 mm.

[0119] In addition, for all the convex strips including the inner convex strips and the outer convex strips, the cross-sectional shape of the protrusion is a substantially isosceles trapezoidal shape, and the width of the convex strips is 0.25 mm at the bottom of the separator base surface and 0.15 mm at the top. The convex strips are arranged in the first to fourth regions in the separator sheet in such a manner that the inner convex strips are formed on the two surfaces (the first surface and the second surface) of the inner surface of the bag-shaped separator and the outer convex strips are formed on the two surfaces (the third surface and the fourth surface) of the outer surface. For the separator sheet, it is a rectangle with a long side length of 250 mm and a short side length of 152 mm, and all the convex strips are formed by a stripe pattern extending in a straight line parallel to the long side of the separator sheet.

[0120] When the separator sheet is folded in half, the direction of the separator sheet being folded is slightly offset from the direction parallel to the short side so that the opposing inner convex strips do not overlap each other ( Figure 3(a)) is bent. Thereafter, the 3 mm area at the left and right ends is joined by a meshing sealing method to obtain a bag-shaped separator. The length L of the inner convex strip except the bent portion is 124 mm in any joining area and the electrode plate area of ​​the first area and the second area, and the interval D between the tops of the inner convex strips in the joining area is 1.0 mm as described above. The distance W between the top of the inner convex strip located on the endmost side and the end is 0.4 mm. The angle θ at which the axis Y of the bent separator sheet is offset from the direction X parallel to the short side is 0.2° (the angle formed by the inner convex strips 2θ=0.4°).

[0121] The separator is folded while the unconverted negative electrode plate is pressed on the first region of the separator, and the left and right ends are joined to form a bag of the separator and accommodate the negative electrode plate at the same time.

[0122] (4) Manufacturing of lead-acid batteries

[0123] The bag-shaped separator S1 containing the negative electrode plate and the positive electrode plate are stacked, and each battery cell is formed into an electrode plate group by 8 chemically unconverted negative electrode plates and 8 chemically unconverted positive electrode plates.

[0124] The electrode assembly was inserted into a polypropylene battery container, and an electrolyte was injected to perform chemical conversion in the battery container to assemble a liquid lead-acid battery A1 having a rated voltage of 12 V and a rated capacity of 48 Ah (5 hour rate).

[0125] 《Lead-acid battery A2》

[0126] In the preparation of the separator S1, when the separator sheet is folded in half, the axis of the folding separator sheet is changed. Figure 3 (b)) The angle θ of the axis Y of the bent separator sheet offset from the direction X parallel to the short side was set to 0.5° (intersection angle 2θ between the inner convex lines = 1°). Except for this, lead acid battery A2 was prepared in the same manner as lead acid battery A1.

[0127] 《Lead-acid battery A3》

[0128] A bag-shaped separator is made different from separator S1.

[0129] A separator S2 in the form of a bag is formed by folding a separator sheet made of a polyethylene microporous film and having ridges formed on both surfaces and joining the left and right ends thereof. Figure 6In the separator sheet shown, the spacing of the inner convex strips in the electrode area and the bonding area (the peripheral area of ​​5 mm from the left and right ends) is set to 0.5 mm, and the height of the inner convex strips in the electrode area and the bonding area is set to 0.1 mm. In addition, the spacing of the outer convex strips in the electrode area is set to 8.0 mm, and in the bonding area is set to 0.5 mm, and the height of the outer convex strips in the electrode area is set to 0.4 mm, and in the bonding area is set to 0.2 mm. In addition, the average thickness of the base portion of the separator is 0.25 mm.

[0130] In addition, for all the convex strips including the inner convex strips and the outer convex strips, the cross-sectional shape of the protrusion is a substantially isosceles trapezoidal shape, and the width of the convex strips is 0.2 mm at the bottom of the separator base surface and 0.1 mm at the top. The convex strips are arranged in the first to fourth regions in the separator sheet in such a manner that the inner convex strips are formed on two surfaces (the first surface and the second surface) of the inner surface of the bag-shaped separator and the outer convex strips are formed on two surfaces (the third surface and the fourth surface) of the outer surface. For the separator sheet, it is a rectangle with a long side length of 250 mm and a short side length of 152 mm, and all the inner convex strips are formed by a stripe pattern extending in a straight line perpendicular to the long side of the separator sheet, and all the outer convex strips are formed by a stripe pattern extending in a straight line parallel to the long side of the separator sheet.

[0131] When folding the separator sheet in half, the direction of the bending separator sheet is slightly offset from the direction parallel to the short side, and the opposite inner convex strips are bent in a manner that does not overlap each other. Thereafter, the 3mm area of ​​the left and right ends is joined by the meshing sealing method to obtain a bag-shaped separator. The length L of the inner convex strips other than the bending portion is 152mm, which is equal to the length of the short side of the separator sheet in any joining area and the plate area of ​​the first area and the second area, and the spacing D between the tops of the inner convex strips in the joining area is 0.5mm as described above. The distance W between the top of the inner convex strip located at the endmost side and the end is 0mm. The angle θ of the offset of the axis Y for bending the separator sheet from the direction X parallel to the short side is 0.05° (the angle 2θ formed by the inner convex strips is 0.1°). In addition, the length of the outer convex strips other than the bending portion is 124mm in the joining area and the main area, and the spacing between the tops of the outer convex strips in the joining area is 0.5mm as described above. The distance between the top of the outer convex line located at the endmost side and the endmost side is 0.4 mm.

[0132] The negative electrode plate was housed in the separator S2 to form an electrode plate group, thereby completing the lead storage battery A3.

[0133] 《Lead-acid battery A4》

[0134] In the preparation of the separator S2, the axis for bending the separator sheet was changed when the separator sheet was folded in half. The angle θ of the axis Y of the separator sheet that was bent from the direction X parallel to the short side was set to 0.5° (the intersection angle 2θ between the inner convex strips = 1°) in such a way that the opposing inner convex strips intersected each other. In addition, the lead-acid battery A4 was prepared in the same manner as the lead-acid battery A3.

[0135] 《Lead-acid battery B1》

[0136] A lead acid battery B1 was produced in the same manner as the lead acid battery A1 except that the positive electrode plate was housed in the separator S1 to form an electrode plate group.

[0137] 《Lead-acid battery B2》

[0138] A lead acid battery B2 was produced in the same manner as the lead acid battery A2 except that the positive electrode plate was housed in the separator S1 to form an electrode plate group.

[0139] In lead-acid batteries B1 and B2, the spacing of the inner convex strips of the separator sheet was set to 8.0 mm in the plate region and 1.0 mm in the joint region (the peripheral region of 5 mm from the left and right ends), and the height of the inner convex strips was set to 0.4 mm in the plate region and 0.2 mm in the joint region. In addition, the spacing of the outer convex strips was set to 2.0 mm in the plate region and 1.0 mm in the joint region, and the height of the outer convex strips was set to 0.1 mm in both the plate region and the joint region.

[0140] 《Lead-acid battery B3》

[0141] In the manufacture of the separator S2, the direction of bending the separator sheet is reversed to manufacture the separator S3. That is, for the separator S3, the relationship between the inner convex strip and the outer convex strip is opposite to that of the separator S2, the inner convex strip extends in a straight line parallel to the long side of the separator sheet, and the outer convex strip extends in a straight line perpendicular to the long side of the separator sheet. The spacing, height and length of the inner convex strips of the separator S3 are respectively the same as the spacing, height and length of the outer convex strips of the separator S2, and the spacing, height and length of the outer convex strips in the separator S3 are respectively the same as the spacing, height and length of the inner convex strips in the separator S2.

[0142] A lead acid battery B3 was produced in the same manner as the lead acid battery A3 except that the positive electrode plate was housed in the separator S3 to form an electrode plate group.

[0143] 《Lead-acid battery B4》

[0144] A lead acid battery B4 was produced in the same manner as the lead acid battery A4 except that the positive electrode plate was housed in the separator S3 to form an electrode plate group.

[0145] [Evaluation 1: Short circuit occurred in the lower part due to vibration]

[0146] After 150 cycles of the heavy-duty life test specified in JIS D 5301:2006, the following vibration test was performed and the incidence of lower short circuit was compared.

[0147] Vibration direction: single vibration up and down

[0148] Acceleration: 6G

[0149] Vibration frequency: 30Hz

[0150] Vibration time: 2 hours

[0151] [Evaluation 2: Resistance to penetration short circuit]

[0152] The charge and discharge were repeated in the following cycle, and the number of cycles at which permeation short circuit occurred was evaluated.

[0153] 1. Discharge: 9.6A (end voltage 10.5V)

[0154] 2. Constant resistance discharge: 10Ω resistor connected × 7 days

[0155] 3. Charging: 14.4V / 50A×60 minutes

[0156] The above steps 1 to 3 were repeated as one cycle, and the number of cycles at which the charging current and voltage fluctuated due to the occurrence of penetration short circuit was determined. The penetration short circuit resistance of each lead acid battery was evaluated by comparing the number of cycles of lead acid battery A1 to 100.

[0157] Table 1 shows the results of evaluations 1 and 2 of lead-acid batteries A1 to A4 and B1 to B4.

[0158] [Table 1]

[0159] Battery Isolation containment Cross-ribbed Ratio of short circuit occurrence in the lower part during vibration test (%) Permeation short circuit cycle number (%) A1 Negative plate none 20 100 A2 Negative plate have 0 120 A3 Negative plate none 20 100 A4 Negative plate have 0 120 B1 Positive plate none 20 120 B2 Positive plate have 0 120 B3 Positive plate none 20 120 B4 Positive plate have 0 120

[0160] As shown in Table 1, in lead-acid batteries A2 and A4 configured to cross the inner convex strips in the joint area, no lower short circuit occurs during the vibration test. This is believed to be due to the improved joint strength of the bag-shaped separator, so the seal at the end of the separator does not fall off, suppressing the short circuit caused by the contact between the sediment produced by the positive active material accumulated in the lower part of the battery tank due to the heavy-load life test and the negative plate. In contrast, in lead-acid batteries A1 and A3, a lower short circuit occurs with a high probability of 20%. This is believed to be due to the insufficient joint strength of the bag-shaped separator, so in the middle of the vibration test, a part of the joint of the bag-shaped separator falls off, and the sediment produced by the positive active material contacts the negative plate via the part that has fallen off, resulting in a short circuit.

[0161] Furthermore, the lead-acid batteries A2 and A4 also had improved resistance to penetration short circuits compared to the lead-acid batteries A1 and A3. This is believed to be because the crimping portion after the meshing seal is slightly thickened due to the intersection of the inner convex strips, thereby slightly widening the distance between the negative electrode plate and the separator in the bonding area at the end of the separator or in the area between the bonding area and the plate area, thereby suppressing the contact between the negative electrode plate and the separator around the end, and suppressing penetration short circuits.

[0162] As described above, the method for manufacturing the bag-shaped separator of the present embodiment has a remarkable effect when the bag-shaped separator accommodates a negative electrode plate, and can partially solve the unique problems that occur in lead-acid batteries having a structure in which the bag-shaped separator accommodates a negative electrode plate.

[0163] When the positive plate is contained in the bag-shaped separator and the lead-acid battery is manufactured in the same way, the vibration test is carried out in the same way, and the resistance to penetration short circuit is evaluated, the results shown in Table 1 are obtained for lead-acid batteries B1 to B4. As in the case where the negative plate is contained in the bag-shaped separator, the lower short circuit is suppressed by crossing the inner convex strips in the joint. On the other hand, when the positive plate is contained in the bag-shaped separator, the distance between the negative plate at the end of the separator and the separator is fully ensured because the negative plate is not contained. Therefore, lead-acid batteries B2 and B4 in which the inner convex strips are crossed in the joint and lead-acid batteries B1 and B3 in which the inner convex strips are not crossed in the joint can obtain the same resistance to penetration short circuit as lead-acid batteries A2 and A4.

[0164] Industrial Applicability

[0165] A method for manufacturing a lead acid battery according to one aspect of the present invention can be applied to the manufacture of separators used in valve-regulated and liquid-type lead acid batteries, and can be suitably used as a power source for starting automobiles, motorcycles, and the like.

[0166] Description of Reference Numerals

[0167] 1...lead-acid battery; 2...negative plate; 3...positive plate; 4...spacer; 5...positive frame; 6...negative frame; 7...positive pole; 8...through connector; 9...negative pole; 11...plate group; 12...battery tank; 13...partition wall; 14...battery cell chamber; 15...cover; 16...negative terminal; 17...positive terminal; 8...liquid port plug; 100...spacer; 101...base; 102a~102e...inner convex strip; 104a, 104b...outer convex strip; 106...plate region; 108a, 108b...joining region; 109a, 109b...joining; 110~112, 114...spacer sheet.

Claims

1. A method for manufacturing a lead-acid battery, the lead-acid battery having an electrode plate group formed by stacking a plurality of positive electrode plates and a plurality of negative electrode plates with separators interposed therebetween, wherein: The method for manufacturing a lead acid battery includes the steps of processing the separator into a bag shape having a first region and a second region facing each other, The step of processing the separator into a bag shape includes the step of forming a joint portion, wherein the joint portion includes at least a portion within the first region and at least a portion within the second region. A plurality of first convex strips are arranged in the first area, A plurality of second convex strips are arranged in the second area, The step of forming the joint portion includes the step of making the first region and the second region face each other in such a manner that at least one of the first ridges and at least one of the second ridges intersect in the joint portion. The step of forming the joining portion includes the step of folding a quadrilateral-shaped separator sheet having the first region and the second region on the same main surface and having parallel opposite sides in a direction inclined from a direction perpendicular to the opposite sides so that the first region and the second region are opposite to each other, In at least a region where the joining portion is provided in the first region and in at least a region where the joining portion is provided in the second region of the separator, the first convex stripes and the second convex stripes extend linearly in the same direction on the main surface.

2. The method for manufacturing a lead acid battery according to claim 1, wherein: In at least the region where the joining portion is provided in the first region and in at least the region where the joining portion is provided in the second region of the isolation sheet, the first convex stripes and the second convex stripes extend on the main surface in parallel with the opposite sides.

3. The method for manufacturing a lead acid battery according to claim 1, wherein: In at least the region where the joining portion is provided in the first region of the isolation sheet and in at least the region where the joining portion is provided in the second region, the first convex stripes and the second convex stripes extend together on the main surface in a direction perpendicular to the opposite sides.

4. The method for producing a lead acid battery according to any one of claims 1 to 3, wherein: The first region has a quadrilateral outer shape, and the joining portion is provided in a region near at least two sides constituting the quadrilateral.

5. The method for producing a lead acid battery according to any one of claims 1 to 3, wherein: A bonding area and a plate area are respectively provided in the first area and the second area, wherein the bonding area is provided with the bonding portion, and the plate area is separated from the bonding area. The first convex strip comprises: a plurality of first engaging ridges provided at predetermined intervals in the engaging region within the first region; and A plurality of first electrode plate convex strips are arranged at predetermined intervals in the electrode plate region within the first region, The first joining ridges are set at intervals narrower than the intervals between the first electrode plate ridges.

6. The method for manufacturing a lead acid battery according to claim 5, wherein: The second convex strip comprises: a plurality of second joining ridges, arranged at predetermined intervals in the joining region within the second region; and A plurality of second electrode plate convex strips are arranged at predetermined intervals in the electrode plate region within the second region, The intervals between the second joining ridges are narrower than the intervals between the second electrode plate ridges.

7. The method for producing a lead acid battery according to any one of claims 1 to 3, wherein: A third area is provided on the back of the first area, and a fourth area is provided on the back of the second area, respectively. A plurality of third convex strips are arranged in the third area. A plurality of fourth convex strips are arranged in the fourth area.

8. The method for manufacturing a lead acid battery according to claim 7, wherein: The third convex strip is provided at least in the third region corresponding to a region in the first region where the joint portion is provided.

9. The method for producing a lead acid battery according to any one of claims 1 to 3, wherein: The step of forming the joining portion includes the step of joining at least a portion of the first region and at least a portion of the second region by crimping or welding.

10. The method for producing a lead acid battery according to any one of claims 1 to 3, wherein: The method for manufacturing a lead-acid battery further includes the step of arranging the negative electrode plate so as to accommodate the negative electrode plate in the separator processed into a bag shape.