Polyphenylene ether resin composition and silane-modified copolymer

By introducing silane-modified copolymers of polybutadiene and polystyrene frameworks into polyphenylene ether resin, the problem of insufficient adhesion between the polyphenylene ether resin substrate and copper foil is solved, and the dielectric characteristics and signal transmission efficiency are improved .

CN111378269BActive Publication Date: 2024-11-12SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911321399.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-28
Filing Date
2019-12-19
Publication Date
2024-11-12
Estimated Expiration
2039-12-19

AI Technical Summary

Technical Problem

The existing polyphenylene ether resin substrates have insufficient adhesion to copper foil, which affects the high-frequency signal transmission efficiency and dielectric characteristics of electronic equipment.

Method used

The adhesion between the cured product and the copper foil is improved by hydrogen silanization reaction using a silane-modified copolymer and a polyphenylene ether resin composition.

Benefits of technology

The adhesion between the polyphenylene ether resin composition and the copper foil is significantly improved, the dielectric characteristics are optimized, and signal transmission losses are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111378269B_ABST
    Figure CN111378269B_ABST
Patent Text Reader

Abstract

The present invention provides a polyphenylene ether resin composition which has excellent dielectric properties and improves the adhesion to copper foil. The polyphenylene ether resin composition contains a polyphenylene ether resin and a silane-modified copolymer represented by the following formula (1). 1 each independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, and R 2 Each of them independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, e, f, g and h independently represent a number greater than 0, and m represents an integer of 1 to 3. However, the order of each repeating unit is arbitrary).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyphenylene ether resin composition containing a silane-modified copolymer, and more particularly to a polyphenylene ether resin composition containing a silane-modified copolymer having a polybutadiene skeleton and a polystyrene skeleton. Background Art

[0002] In recent years, with the improvement of bonding and mounting technology, electronic equipment continues to develop with the high integration of semiconductor devices and the refinement of packaging and the high-density wiring of printed wiring boards carried on electronic equipment, especially in electronic equipment using high-frequency bands such as mobile communication, significant progress has been made. For the printed wiring board constituting such electronic equipment, multilayering and fine wiring are carried out simultaneously. For the high-speed signal transmission speed required for the high-speed information processing, it is effective to reduce the dielectric constant of the material. In addition, in order to reduce the loss during transmission, it is effective to use a material with a small dielectric loss tangent (dielectric loss).

[0003] Polyphenylene ether (PPE) has been studied as a substrate material because of its excellent dielectric properties such as dielectric constant and dielectric loss tangent. Resin compositions using modified polyphenylene ether have also been proposed (Patent Documents 1 and 2).

[0004] Although a substrate molded using a resin composition using polyphenylene ether has excellent dielectric properties, there is a problem that the adhesion with copper foil is insufficient.

[0005] On the other hand, silane-modified copolymers having a polybutadiene skeleton, a polystyrene skeleton, etc. are reported to be useful as a component of a filler-filled rubber composition (Patent Documents 3 and 4), but have not yet been used in a polyphenylene ether resin composition.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2004-339328

[0009] Patent Document 2: International Publication No. 2014 / 034103

[0010] Patent Document 3: U.S. Patent No. 3759869

[0011] Patent Document 4: Japanese Patent Application Publication No. 2017-8301 Summary of the invention

[0012] Problems to be solved by the invention

[0013] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a polyphenylene ether resin composition that provides a cured product having excellent dielectric properties and improved adhesion to copper foil.

[0014] Means for solving problems

[0015] The present inventors have conducted intensive studies to solve the above problems and have found that a silane-modified copolymer having a polybutadiene skeleton and a polystyrene skeleton improves the adhesion between a cured product of a polyphenylene ether resin composition and a copper foil, thereby completing the present invention.

[0016] That is, the present invention provides:

[0017] 1. A polyphenylene ether resin composition comprising a polyphenylene ether resin and a silane-modified copolymer represented by the following formula (1),

[0018]

Chemistry 1

[0019]

[0020] (Where R 1 each independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, and R 2 Each of the following independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms; each of e, f, g and h independently represents a number greater than 0; and m represents an integer of 1 to 3. However, the order of each repeating unit is arbitrary.)

[0021] 2. The polyphenylene ether resin composition according to 1 above, wherein in formula (1), f / (e+f+g+h) is 0.22 or more,

[0022] 3. A silane-modified copolymer represented by the following formula (1),

[0023]

Chemistry 2

[0024]

[0025] (Where R 1 each independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, and R 2 Each of the above-mentioned groups independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, e, f, g and h independently represent a number greater than 0, f / (e+f+g+h) is greater than 0.22, and m represents an integer from 1 to 3. However, the order of each repeating unit is arbitrary. ).

[0026] Effects of the Invention

[0027] The polyphenylene ether resin composition of the present invention contains a silane-modified copolymer having a polybutadiene skeleton, a polystyrene skeleton and a hydrolyzable silyl group. By using the silane-modified copolymer, the adhesion between the cured product and the copper foil can be improved. DETAILED DESCRIPTION

[0028] The present invention is described in detail below.

[0029] [Polyphenylene ether resin]

[0030] The polyphenylene ether resin used in the polyphenylene ether resin composition of the present invention is not particularly limited, but preferably a modified polyphenylene ether resin, preferably a polyphenylene ether resin terminally modified with a substituent having a carbon-carbon unsaturated double bond. As such a polyphenylene ether resin, commercially available products such as Noryl SA9000 (manufactured by SABIC Innovative Plastics) can be used. Even if it is not a commercially available product, a modified polyphenylene ether resin in which a vinyl group, a styryl group, a methacryloyl group, an acryloyl group, etc. are introduced using a polyphenylene ether modified with a terminal hydroxyl group can be used.

[0031] [Silane modified copolymer]

[0032] The silane-modified copolymer contained in the polyphenylene ether resin composition of the present invention is represented by formula (1). In formula (1), the order of the repeating units is arbitrary.

[0033]

Chemistry 3

[0034]

[0035] Among them, R 1 each independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, and R 2 Each of them independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms; each of e, f, g and h independently represents a number greater than 0; and m represents an integer of 1 to 3.

[0036] As R 1 and R 2 The alkyl group may be a linear, cyclic or branched alkyl group having 1 to 10 carbon atoms. Specific examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl groups.

[0037] Specific examples of the aryl group having 6 to 10 carbon atoms include phenyl, α-naphthyl, β-naphthyl and the like.

[0038] Among these, R1 , preferably a straight-chain alkyl group, more preferably a methyl group or an ethyl group.

[0039] In addition, as R 2 , preferably a straight-chain alkyl group, more preferably a methyl group or an ethyl group.

[0040] e is preferably 1-500, more preferably 5-300.

[0041] f is preferably 1-500, more preferably 5-300.

[0042] g is preferably 1-500, more preferably 2-100.

[0043] h is preferably 1-500, more preferably 5-300.

[0044] f / (e+f+g+h) is preferably 0.2 or more, more preferably 0.22 or more, further preferably 0.25 or more, and particularly preferably 0.30 or more. The upper limit is not particularly limited, but is preferably 1 or less, and more preferably 0.8 or less.

[0045] The silane-modified copolymer represented by formula (1) can be obtained by hydrosilylation of a butadiene-styrene copolymer represented by formula (2) with an organic silicon compound represented by formula (3) in the presence of a catalyst containing a platinum compound, preferably in the presence of a catalyst containing a platinum compound and a co-catalyst, as shown in the following synthesis route.

[0046]

Chemistry 4

[0047]

[0048] (Where R 1 , R 2 , e, f, g, h and m have the same meanings as above. )

[0049] The butadiene-styrene copolymer represented by formula (2) can be synthesized using butadiene and styrene as raw monomers by a known method such as emulsion polymerization and solution polymerization, and can also be obtained as a commercial product, for example, Ricon 100, Ricon 181, Ricon 184 (all manufactured by Cray Valley), L-SBR-820, L-SBR-841 (all manufactured by Kuraray Co., Ltd.) are already on the market.

[0050] On the other hand, examples of the organic silicon compound represented by the formula (3) include trimethoxysilane, methyldimethoxysilane, dimethylmethoxysilane, triethoxysilane, methyldiethoxysilane, and dimethylethoxysilane.

[0051] Regarding the reaction ratio of the copolymer of formula (2) and the compound of formula (3), relative to 1 mol of -[CH 2 -CH-(CH=CH 2 )] f+g - repeating unit, the compound of formula (3) is preferably less than 1 mol, more preferably 0.8 mol or less. The lower limit is not particularly limited, but is preferably 0.01 mol or more.

[0052] The catalyst containing a platinum compound used in the above-mentioned hydrosilylation reaction is not particularly limited. Specific examples thereof include chloroplatinic acid, an alcohol solution of chloroplatinic acid, a toluene or xylene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, tetrakis(triphenylphosphine)platinum, dichlorobis(triphenylphosphine)platinum, dichlorobisacetonitrile platinum, dichlorobisbenzonitrile platinum, dichlorocyclooctadiene platinum, and supported catalysts such as platinum-carbon, platinum-alumina, and platinum-silica.

[0053] From the viewpoint of selectivity during hydrosilylation, a zero-valent platinum complex is preferred, and a toluene or xylene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex is more preferred.

[0054] The amount of the catalyst containing the platinum compound is not particularly limited. From the perspective of reactivity, productivity, etc., it is preferred that the amount of platinum atoms contained is 1×10 -7 ~1×10 -2 The molar amount is more preferably 1×10 -7 ~1×10 -3 The amount of moles.

[0055] As the promoter in the above reaction, it is preferred to use one or more selected from ammonium salts of inorganic acids, amide compounds and carboxylic acids.

[0056] Specific examples of ammonium salts of inorganic acids include ammonium chloride, ammonium sulfate, ammonium sulfamate, ammonium nitrate, monoammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium diphosphite, ammonium carbonate, ammonium bicarbonate, ammonium sulfide, ammonium borate, and ammonium borofluoride. Among them, ammonium salts of inorganic acids having a pKa of 2 or more are preferred, and ammonium carbonate and ammonium bicarbonate are more preferred.

[0057] Specific examples of the amide compound include formamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, propionamide, acrylamide, malonamide, succinamide, maleamide, fumaramide, benzamide, phthalamide, palmitamide, and stearamide.

[0058] Specific examples of the carboxylic acid include formic acid, acetic acid, propionic acid, butyric acid, methoxyacetic acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, lactic acid, glycolic acid, and the like. Among these, formic acid, acetic acid, and lactic acid are preferred, and acetic acid is more preferred.

[0059] The amount of the co-catalyst used is not particularly limited, but is preferably 1×10 -5 ~5×10 -1 mole, more preferably 1×10 -4 ~1×10 -1 Moore.

[0060] The above reaction proceeds even in the absence of a solvent, but a solvent may also be used.

[0061] Specific examples of usable solvents include hydrocarbon solvents such as pentane, hexane, cyclohexane, heptane, isooctane, benzene, toluene, and xylene; ether solvents such as diethyl ether, tetrahydrofuran, and dioxane; ester solvents such as ethyl acetate and butyl acetate; aprotic polar solvents such as N,N-dimethylformamide; chlorinated hydrocarbon solvents such as dichloromethane and chloroform, etc. These solvents may be used alone or in combination of two or more.

[0062] The reaction temperature in the hydrosilylation reaction is not particularly limited, and the reaction can be carried out at a temperature ranging from 0°C to 200°C, preferably 0°C to 200°C.

[0063] In order to obtain an appropriate reaction rate, it is preferred to carry out the reaction under heating. From such a viewpoint, the reaction temperature is more preferably 40 to 110°C, and further preferably 40 to 90°C.

[0064] The reaction time is not particularly limited, but is usually about 1 to 60 hours, preferably 1 to 30 hours, and more preferably 1 to 20 hours.

[0065] In consideration of the handling properties of the polyphenylene ether resin composition of the present invention, the number average molecular weight of the silane-modified copolymer represented by formula (1) is preferably 500 to 100,000, more preferably 1,000 to 20,000.

[0066] In addition, the number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography.

[0067] The amount of the silane-modified copolymer represented by formula (1) in the polyphenylene ether resin composition of the present invention is preferably 0.001 to 20 parts by mass, more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the resin component (polyphenylene ether resin) in the composition, from the viewpoint of adhesion to copper foil.

[0068] [Other ingredients]

[0069] The polyphenylene ether resin composition of the present invention may further contain components other than the above-mentioned components. Examples of the other components include a high molecular weight body, an inorganic filler, a flame retardant, an additive, a curing agent, and a reaction initiator.

[0070] Examples of the high molecular weight body include polybutadiene, butadiene-styrene copolymers other than those represented by formula (1), and (meth)acrylic acid-based copolymers.

[0071] Examples of the inorganic filler include spherical silica, barium sulfate, silica powder, crushed silica, calcined talc, barium titanate, titanium oxide, clay, alumina, mica, boehmite, and the like.

[0072] Examples of the curing agent include triallyl isocyanurate (TAIC) and other triallyl isocyanurate compounds, polyfunctional methacrylate compounds having two or more methacryloyl groups in the molecule, polyfunctional acrylate compounds having two or more acryloyl groups in the molecule, and vinylbenzyl compounds such as styrene and divinylbenzene having a vinylbenzyl group in the molecule.

[0073] [Method for producing composition]

[0074] The composition of the present invention can be prepared by dissolving the polyphenylene ether resin in a solvent according to a conventional method and then mixing the silane-modified copolymer with other components. As the solvent, aromatic solvents such as toluene and xylene are preferred; ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone are preferred; and ether solvents such as tetrahydrofuran are preferred. Among these, toluene and xylene are more preferred.

[0075] Example

[0076] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0077] In addition, the molecular weight is a polystyrene-equivalent number average molecular weight determined by gel permeation chromatography (GPC) measurement. The viscosity is a value at 25° C. measured using a rotational viscometer.

[0078] [Examples 1-1 to 1-4, Reference Examples 1-5 to 1-8]

[0079] [1] Production of silane-modified copolymers

[0080] [Example 1-1]

[0081] In a 2 L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 1000 g of Ricon 100 (e=19, (f+g)=44, h=11 in the above formula (2); number average molecular weight 4500; manufactured by Cray Valley Co., Ltd., the same below) was placed, 200 g of toluene, and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (3.1×10 -4 mol) and 0.2 g (3.1 × 10 -3 122 g (1.0 mol) of trimethoxysilane was added dropwise thereto at an internal temperature of 75 to 85°C over 2 hours, followed by stirring at 80°C for 3 hours.

[0082] After the stirring was completed, the mixture was concentrated under reduced pressure and filtered to obtain a yellow transparent liquid having a viscosity of 600,000 mPa·s and a number average molecular weight of 5,000.

[0083] The molecular weight and 1 The average structure determined by H-NMR spectrum was a silane-modified copolymer represented by the above formula (1) where e=19, f=40, g=4, and h=11. f / (e+f+g+h) was 0.54. This was designated as silane-modified copolymer A.

[0084] [Example 1-2]

[0085] In a 2L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel, and a thermometer, 1000 g of Ricon 100, 200 g of toluene, and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (3.1×10 -4 mol) and 0.2 g (3.1 × 10 -3 244 g (2.0 mol) of trimethoxysilane was added dropwise thereto at an internal temperature of 75 to 85°C over 2 hours, followed by stirring at 80°C for 3 hours.

[0086] After the stirring was completed, the mixture was concentrated under reduced pressure and filtered to obtain a yellow transparent liquid having a viscosity of 650,000 mPa·s and a number average molecular weight of 5,600.

[0087] The molecular weight and 1 The average structure determined by H-NMR spectrum was a silane-modified copolymer represented by the above formula (1) where e=19, f=36, g=8, and h=11. f / (e+f+g+h) was 0.49. This was designated as silane-modified copolymer B.

[0088] [Examples 1-3]

[0089] In a 2L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel, and a thermometer, 1000 g of Ricon 100, 200 g of toluene, and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (3.1×10 -4 mol) and 0.2 g (3.1 × 10 -3 366 g (3.0 mol) of trimethoxysilane was added dropwise thereto at an internal temperature of 75 to 85°C over 2 hours, followed by stirring at 80°C for 3 hours.

[0090] After the stirring was completed, the mixture was concentrated under reduced pressure and filtered to obtain a yellow transparent liquid having a viscosity of 700,000 mPa·s and a number average molecular weight of 6,100.

[0091] The molecular weight and 1 The average structure determined by H-NMR spectrum was a silane-modified copolymer represented by the above formula (1) where e=19, f=31, g=13, and h=11. f / (e+f+g+h) was 0.42. This was designated as silane-modified copolymer C.

[0092] [Examples 1-4]

[0093] In a 2L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel, and a thermometer, 1000 g of Ricon 100, 200 g of toluene, and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (3.1×10 -4 mol) and 0.2 g (3.1 × 10 -3 610 g (5.0 mol) of trimethoxysilane was added dropwise thereto at an internal temperature of 75 to 85°C over 2 hours, followed by stirring at 80°C for 3 hours.

[0094] After the stirring was completed, the mixture was concentrated under reduced pressure and filtered to obtain a yellow transparent liquid having a viscosity of 800,000 mPa·s and a number average molecular weight of 7,200.

[0095] The molecular weight and 1 The average structure determined by H-NMR spectrum was a silane-modified copolymer represented by the above formula (1) where e=19, f=22, g=22, and h=11. f / (e+f+g+h) was 0.29. This was designated as silane-modified copolymer D.

[0096] [Reference Example 1-5]

[0097] In a 2 L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 1000 g of Ricon 181 (e=30, (f+g)=13, h=9 in the above formula (2); number average molecular weight 3200; manufactured by Cray Valley Company. Same below) was placed, 200 g of toluene, and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.5×10 -4 mol) and 0.4 g (0.5 × 10 -2 73 g (0.6 mol) of trimethoxysilane was added dropwise thereto at an internal temperature of 75 to 85°C over 2 hours, followed by stirring at 80°C for 1 hour.

[0098] After the stirring was completed, the mixture was concentrated under reduced pressure and filtered to obtain a yellow transparent liquid having a viscosity of 12500 mPa·s and a number average molecular weight of 3400.

[0099] The molecular weight and 1 The average structure determined by H-NMR spectrum was a silane-modified copolymer represented by the above formula (1) where e=30, f=11, g=2, and h=9. f / (e+f+g+h) was 0.21. This was designated as silane-modified copolymer E.

[0100] [Reference Example 1-6]

[0101] In a 2L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel, and a thermometer, 1000 g of Ricon 100, 200 g of toluene, and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (3.1×10 -4 mol) and 0.2 g (3.1 × 10 -3 976 g (8.0 mol) of trimethoxysilane was added dropwise thereto at an internal temperature of 75 to 85°C over 2 hours, followed by stirring at 80°C for 3 hours.

[0102] After the stirring was completed, the mixture was concentrated under reduced pressure and filtered to obtain a yellow transparent liquid having a viscosity of 1,200,000 mPa·s and a number average molecular weight of 8,900.

[0103] The molecular weight and 1 The average structure determined by H-NMR spectrum was a silane-modified copolymer represented by the above formula (1) where e=19, f=9, g=35, and h=11. f / (e+f+g+h) was 0.12. This was designated as silane-modified copolymer F.

[0104] [Reference Example 1-7]

[0105] In a 2L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel, and a thermometer, 1000 g of Ricon 100, 200 g of toluene, and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (3.1×10 -4 mol) and 0.2 g (3.1 × 10 -3 854 g (7.0 mol) of trimethoxysilane was added dropwise thereto at an internal temperature of 75 to 85°C over 2 hours, followed by stirring at 80°C for 3 hours.

[0106] After the stirring was completed, the mixture was concentrated under reduced pressure and filtered to obtain a yellow transparent liquid having a viscosity of 1,100,000 mPa·s and a number average molecular weight of 8,300.

[0107] The molecular weight and 1 The average structure determined by H-NMR spectrum was a silane-modified copolymer represented by the above formula (1) where e=19, f=13, g=31, and h=11. f / (e+f+g+h) was 0.18. This was designated as silane-modified copolymer G.

[0108] [Reference Example 1-8]

[0109] A 2L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel, and a thermometer was charged with 1000 g of Ricon 181, 200 g of toluene, and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.5×10 -4 mol) and 0.4 g (0.5 × 10 -2 244 g (2.0 mol) of trimethoxysilane was added dropwise thereto at an internal temperature of 75 to 85°C over 2 hours, followed by stirring at 80°C for 1 hour.

[0110] After the stirring was completed, the mixture was concentrated under reduced pressure and filtered to obtain a yellow transparent liquid having a viscosity of 14500 mPa·s and a number average molecular weight of 3900.

[0111] The molecular weight and 1 The average structure determined by H-NMR spectrum was a silane-modified copolymer represented by the above formula (1) where e=30, f=6, g=7, and h=9. f / (e+f+g+h) was 0.12. This was referred to as silane-modified copolymer H.

[0112] [Examples 2-1 to 2-8, Comparative Examples 2-1 to 2-5]

[0113] [2] Production of polyphenylene ether resin composition

[0114] (Polyphenylene ether)

[0115] Modified polyphenylene ether (Noryl SA9000: manufactured by SABIC Innovative Plastics) whose terminal is modified with a methacryloyl group

[0116] (High molecular weight)

[0117] High molecular weight product having a methacrylic acid-based skeleton (ARUFON UP-1080; weight average molecular weight 6000: manufactured by Toagosei Co., Ltd.)

[0118] (Cross-linking curing agent)

[0119] Triallyl isocyanurate (TAIC: manufactured by Nippon Chemical Co., Ltd.)

[0120] (Inorganic filler)

[0121] Silica surface-treated with vinyl silane (SC2300-SVJ: manufactured by Advantex Corporation)

[0122] (Reaction initiator)

[0123] 1,3-Bis(tert-butylperoxydiisopropyl)benzene (Perbutyl P: manufactured by NOF Corporation)

[0124] [Preparation method]

[0125] (Varnish)

[0126] First, a modified polyphenylene ether (Noryl SA9000) and toluene were mixed, and the mixed solution was heated to 80°C to dissolve the mixture, thereby obtaining a 50% by mass toluene solution. Then, a high molecular weight body (ARUFON UP-1080), a crosslinking agent (TAIC), and silane-modified copolymers A to H were added to the obtained toluene solution in the proportions (parts by mass) described in Tables 1 and 2, and the mixture was stirred for 30 minutes to completely dissolve the mixture. Then, an inorganic filler (SC2300-SVJ) and a reaction initiator (Perbutyl P) were further added, and the mixture was dispersed using a bead mill to obtain a varnish-like resin composition.

[0127] (Prepreg)

[0128] A prepreg was prepared using the above varnish and used for the following evaluation.

[0129] In the prepreg, as the woven fabric substrate, a glass cloth of type #1078, WEA1078 manufactured by Nitto Boseki Co., Ltd. was used. Then, the above resin varnish was impregnated into the woven fabric substrate so that the thickness after curing became 60 μm, and at the same time, it was heated and dried at 120 °C for 3 minutes until it became a semi-cured state, thereby obtaining a prepreg.

[0130] (Laminated board)

[0131] For one piece of the above prepreg, copper foils with a thickness of 12 μm (GT-MP manufactured by Furukawa Electric Co., Ltd.) were arranged on both sides thereof to form a pressed body. Under vacuum conditions, at a temperature of 220 °C and a pressure of 40 kgf / cm 2 it was heated and pressed for 90 minutes to obtain an evaluation laminated board 1 with a thickness of 84 μm having copper foils bonded on both sides.

[0132] In addition, 12 pieces of the above prepregs were overlapped, copper foils were arranged on the topmost and bottommost layers, and heat molding was performed in the same manner as above. After obtaining a copper-clad laminate, the copper foils were peeled off to obtain an evaluation laminated board 2 with a thickness of 720 μm.

[0133] [Evaluation method]

[0134] For the evaluation laminated boards 1 and 2 prepared as described above, the following methods were used for evaluation.

[0135] (Copper foil adhesion)

[0136] In the evaluation laminated board 1, the peel strength of the copper foil from the insulating layer was measured in accordance with JIS C 6481:1996. A pattern with a width of 10 mm and a length of 100 mm was formed, and using a tensile testing machine, it was peeled at a speed of 50 mm / minute, and the peel strength (peel strength) at this time was measured. The obtained peel strength was used as the copper foil adhesion (adhesion strength). The measurement unit was kN / m.

[0137] (Dielectric properties (relative dielectric constant and dielectric loss tangent))

[0138] The relative dielectric constant and dielectric loss tangent of the evaluation substrate at 10 GHz were measured using the cavity resonator perturbation method. The above evaluation laminated board 2 was used as the evaluation substrate. Specifically, using a Network-Analyzer (N5230A: manufactured by Agilent-Technology Co., Ltd.), the relative dielectric constant (DK) and dielectric loss tangent (Df) of the evaluation substrate at 10 GHz were measured.

[0139]

Table 1

[0140]

[0141]

Table 2

[0142]

[0143] *1 Organic silicon compound I: Vinyltrimethoxysilane (KBM-1003 manufactured by Shin-Etsu Chemical Co., Ltd.)

[0144] *2 Organic silicon compound J: 3-methacryloylpropyltrimethoxysilane (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.)

Claims

1. A silane-modified copolymer represented by the following formula (1): In the formula, R 1 each independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, and R 2 independently represent an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, e, f, g and h independently represent a number greater than 0, f / (e+f+g+h) satisfies 0.25≤f / (e+f+g+h)<1, and m represents an integer of 1 to 3, in, The order of the repeating units is arbitrary.

2. The silane-modified copolymer according to claim 1, in, In the formula (1), f / (e+f+g+h) is 0.30 or more and 0.8 or less.

3. A polyphenylene ether resin composition comprising a polyphenylene ether resin and the silane-modified copolymer according to claim 1 or 2, in, The blending amount of the silane-modified copolymer is 0.001 to 20 parts by mass based on 100 parts by mass of the polyphenylene ether resin.